Easy-to-open packaging materials and packaging bags
A laminated packaging material with a paper base, anchor coat, vapor deposition, and sealant layers addresses poor tearability and high plastic content by using polyolefin resins, ensuring excellent tearability and barrier properties while reducing plastic use.
Patent Information
- Application Number
- JP2024094527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-16
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-09-12
AI Technical Summary
Existing packaging materials with gas barrier properties have poor tearability, especially when notched, and contain high amounts of plastic, which is environmentally detrimental.
A laminated packaging material structure comprising a paper base material, an anchor coat layer, a metal or metal oxide vapor deposition layer, and a sealant layer, with the paper base material weighing 50% or more, and a sealant layer thickness of 2 to 40 μm, utilizing polyolefin resins with carboxyl groups for improved tearability and barrier properties.
The packaging material achieves excellent tearability regardless of the tearing direction, maintains high water vapor barrier properties, and reduces plastic usage, making it environmentally friendly.
Smart Images

Figure 0007563646000004 
Figure 0007563646000005 
Figure 0007563646000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an easy-open packaging material and a packaging bag. [Background technology]
[0002] In recent years, the trend towards a plastic-free society has been growing due to growing environmental awareness sparked by the problem of marine plastic waste. In the field of packaging materials, there is also a growing demand to replace plastic with paper packaging materials. Packaging materials with gas barrier properties are being used to prevent the permeation of water vapor, which deteriorates the quality of the contents.
[0003] Patent Document 1 discloses a packaging material in which a paper base material, an adhesive layer containing a specific material, a metal layer in contact with the adhesive layer, and a sealant layer are laminated in this order, and the thickness of the adhesive layer is within a specific range. Patent Document 2 discloses a packaging material in which a paper base material, an adhesive layer in contact with the paper base material, and a sealant layer are laminated in this order, and the arithmetic mean roughness of the paper base material and the tensile strength of the packaging material satisfy specific conditional expressions. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-116880 A [Patent Document 2] JP 2020-49913 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the inventors' investigations have revealed that the packaging materials disclosed in the above Patent Documents 1 and 2 have poor tearability when the packaging materials do not have a notch. Furthermore, the inventors' investigations have revealed that the packaging materials disclosed in the above Patent Documents 1 and 2 have poor tearability when the tearing direction is not along the orientation direction of the fibers of the paper base material, although the fibers of the paper base material have orientation.
[0006] Furthermore, from the perspective of the Law for Promoting Effective Utilization of Resources, there is a demand to reduce the amount of plastic used in packaging materials as well.
[0007] The present disclosure provides an easy-open packaging material and packaging bag that have excellent tearability regardless of the tearing direction even when not having a notch, have excellent water vapor barrier properties, and are environmentally friendly. [Means for solving the problem]
[0008] An easy-open packaging material according to one aspect of the present disclosure is a packaging material having a laminated structure including, in this order, a paper base material, an anchor coat layer, a vapor-deposited layer of a metal or metal oxide, and a sealant layer, wherein the weight of the paper base material is 50 mass% or more based on the entire packaging material, the thickness of the sealant layer is 2 to 40 μm, the sealant layer contains a first polyolefin resin, and has a tensile breaking strength of 40 to 70 N / 15 mm.
[0009] The first polyolefin resin may have at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
[0010] The sealant layer may have a thickness of 2 to 20 μm.
[0011] The film may further include an adhesive layer between the deposition layer and the sealant layer.
[0012] The film may further include an overcoat layer between the vapor deposition layer and the adhesive layer, and the overcoat layer may contain a second polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
[0013] The anchor coat layer may contain a third polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
[0014] The anchor coat layer may contain a polyvinyl alcohol resin.
[0015] Another aspect of the present disclosure may be a packaging bag including the above-described easy-open packaging material.
[0016] The packaging bag may have a folded portion. Effect of the Invention
[0017] According to the present disclosure, there is provided an easy-open packaging material and packaging bag that has excellent tearability regardless of the tearing direction even if it does not have a notch, has excellent water vapor barrier properties, and is environmentally friendly. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view showing an easy-open packaging material according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an easy-open packaging material according to another embodiment of the present disclosure. [Diagram 3] FIG. 1 is a perspective view showing a packaging bag according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings where necessary. However, the present disclosure is not limited to the following embodiments.
[0020] <Easy-to-open packaging material> {First embodiment} The easy-open packaging material according to the first embodiment will be described below. Fig. 1 is a schematic cross-sectional view showing the packaging material according to the first embodiment. The packaging material 10 according to one embodiment has a laminated structure including a paper base material 1, an anchor coat layer 2, a deposition layer 3, and a sealant layer 4 in this order.
[0021] [Paper base material] The paper base material 1 is not particularly limited, and may be appropriately selected depending on the application of the packaging bag to which the packaging material 10 is applied. There is no particular limitation as long as the paper is made mainly of plant-derived pulp. Specific examples of the paper base material 1 include fine paper, special fine paper, coated paper, art paper, cast-coated paper, imitation paper, kraft paper, and glassine paper. The basis weight of the paper base material 1 is, for example, 20 g / m2, which provides better tearability. 2 More than 30g / m 2 More than 35g / m 2 or more than 40g / m 2 or more, and 2 Below 300g / m 2 or less than 100g / m 2 It may be the following:
[0022] The paper base material 1 may have a coating layer at least on the side in contact with the anchor coat layer 2 described below. By providing the coating layer, it is possible to prevent the anchor coat layer from penetrating into the paper, and it also plays a role of filling the unevenness of the paper, and the anchor coat layer can be formed uniformly without defects. For example, the coating layer may contain various copolymers such as styrene-butadiene, styrene-acrylic, and ethylene-vinyl acetate copolymers, polyvinyl alcohol resin, cellulose resin, and paraffin (WAX) as binder resins, and may contain clay, kaolin, calcium carbonate, talc, mica, and the like as fillers.
[0023] The thickness of the coating layer is not particularly limited, but may be, for example, 1 to 10 μm, or 3 to 8 μm.
[0024] When the weight of the paper base material 1 is 50% by mass or more based on the entire packaging material, the packaging material 10 has excellent tearability regardless of the tearing direction even if it does not have a notch. In addition, the amount of plastic material used can be sufficiently reduced, so that the entire packaging material can be said to be made of paper and has excellent recyclability. From the same viewpoint, the weight of the paper base material is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more.
[0025] The fibers contained in the paper base material 1 are preferably non-oriented, since even if the paper base material does not have a notch, the paper base material has excellent tearability regardless of the tearing direction.
[0026] [Anchor coat layer] The anchor coat layer 2 is provided on the surface of the paper base material 1 to improve adhesion between the paper base material 1 and the deposition layer 3 described below, and to improve the gas barrier properties of the packaging material. The material of the anchor coat layer 2 is not particularly limited, but examples thereof include polyurethane resins, polyvinyl alcohol resins, and a third polyolefin resin having a polar group.
[0027] The anchor coat layer 2 contains a polyurethane resin, which provides good wettability and therefore excellent coating stability, and provides good adhesion between the paper substrate 1 and the deposition layer 3. The good surface smoothness of the anchor coat layer 2 also makes it easier to form a dense deposition layer 3, resulting in even better gas barrier properties. Use of a polyurethane resin with gas barrier properties is expected to further improve gas barrier properties.
[0028] From the viewpoint of barrier properties, the polyurethane resin preferably contains at least one of a metaxylylene diisocyanate-derived structural unit and a hydrogenated metaxylylene diisocyanate-derived structural unit. When the polyurethane resin contains such a structural unit, it exhibits high cohesive strength due to hydrogen bonds and stacking effect between xylylene groups, and therefore tends to have better gas barrier properties. From the viewpoint of coatability, the coating liquid used when forming an anchor coat layer containing a polyurethane resin is preferably a coating liquid dispersed in water, such as a dispersion or emulsion. An example of such a coating liquid is Takelac WPB manufactured by Mitsui Chemicals.
[0029] The anchor coat layer 2 contains the third polyolefin resin, which allows the formation of a dense film due to the crystallinity of the polyolefin, and exhibits water vapor barrier properties. The crystallinity of the polyolefin exhibits water vapor barrier properties, and the inclusion of polar groups exhibits adhesion to the deposition layer 3.
[0030] The third polyolefin resin may have at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0031] As the third polyolefin-based resin, copolymers of ethylene or propylene with unsaturated carboxylic acids (unsaturated compounds having a carboxyl group, such as acrylic acid, methacrylic acid, and maleic anhydride), unsaturated carboxylic acid esters, and salts of carboxylic acids neutralized with basic compounds may be used, as well as copolymers of vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, and the like.
[0032] Specific examples of the third polyolefin resin include a copolymer of an acrylic acid ester and maleic anhydride, an ethylene-vinyl acetate copolymer, and an ethylene glycidyl methacrylate copolymer.
[0033] The polyvinyl alcohol resin is, for example, a fully saponified polyvinyl alcohol resin, a partially saponified polyvinyl alcohol resin, a modified polyvinyl alcohol resin, an ethylene-vinyl alcohol copolymer resin, etc. The degree of polymerization of the polyvinyl alcohol resin is preferably 300 or more and 1700 or less. If the degree of polymerization is 300 or more, the gas barrier property and bending resistance of the packaging material become good, and if the degree of polymerization is 1700 or less, the viscosity of the coating liquid of the polyvinyl alcohol resin described below becomes low, and the coating property becomes good.
[0034] When the anchor coat layer 2 contains a polyvinyl alcohol-based resin, it has excellent flexibility, and can suppress cracking of the vapor deposition layer 3 after bending (folding), thereby suppressing deterioration of the gas barrier properties, and can improve adhesion between the vapor deposition layer 3 and the anchor coat layer 2.
[0035] The anchor coat layer 2 may contain other components in addition to the polyurethane resin, the third polyolefin resin, and the polyvinyl alcohol resin. Examples of the other components include polyolefin resins other than the third polyolefin resin, silane coupling agents, organic titanates, polyacrylics, polyesters, polyurethanes, polycarbonates, polyureas, polyamides, polyimides, melamines, and phenols.
[0036] The content of the polyurethane resin in the anchor coat layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0037] The content of the third polyolefin resin in the anchor coat layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0038] The content of the polyvinyl alcohol-based resin in the anchor coat layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0039] The thickness of the anchor coat layer 2 may be, for example, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the anchor coat layer 2 is 1 μm or more, the unevenness of the paper base material 1 can be efficiently filled, and the deposition layer 3 can be laminated uniformly. Also, if the thickness of the anchor coat layer 2 is 20 μm or less, the deposition layer 3 can be laminated uniformly while suppressing costs.
[0040] The method of providing the anchor coat layer 2 includes a method of applying a coating liquid containing at least a material for forming the anchor coat layer and a solvent on a paper substrate, and drying the coating liquid. When the anchor coat layer 2 contains a third polyolefin resin, the third polyolefin resin in the coating liquid should have a small particle size. The particle size is not particularly limited, but is preferably 0.1 to 0.7 μm. When the particle size is small, the anchor coat layer 2 has excellent smoothness, and the deposited layer 3 tends to be uniform with little variation in thickness. As a result, the gas barrier property of the packaging material 10 tends to be further improved.
[0041] Examples of the solvent contained in the coating liquid of the anchor coat layer 2 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Also, from the viewpoint of environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0042] [Vapour-deposited layer] The deposition layer 3 is a layer obtained by depositing an inorganic oxide, a metal, or a metal oxide. The deposition layer may be obtained by depositing silica or aluminum, or may be obtained by depositing aluminum oxide (AlO x ) etc.
[0043] The thickness of the deposited layer 3 may be appropriately set depending on the application, but may be preferably 10 nm or more, 30 nm or more, 50 nm or more, and may be 300 nm or less, 100 nm or less, 80 nm or less. By setting the thickness of the deposited layer 3 to 10 nm or more, it is easy to ensure sufficient continuity of the deposited layer 3, and by setting the thickness to 300 nm or less, it is easy to sufficiently suppress the occurrence of curling and cracking, and to easily achieve sufficient gas barrier performance and flexibility.
[0044] From the viewpoint of oxygen gas barrier performance and film uniformity, it is preferable to form the deposition layer 3 by a vacuum deposition method. There are known deposition methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its fast deposition rate and high productivity. Among the vacuum deposition methods, deposition by electron beam heating is particularly effective because the deposition rate can be easily controlled by the irradiation area and electron beam current, and the temperature of the deposition material can be raised and lowered in a short time.
[0045] [Sealant layer] The sealant layer 4 is provided on the surface of the vapor-deposited layer 3 so as to be in contact with the vapor-deposited layer 3. The sealant layer 4 has a thickness of 2 to 40 μm. The sealant layer 4 contains a first polyolefin resin. The first polyolefin resin has a polar group.
[0046] The sealant layer 4 contains the first polyolefin resin, which allows the formation of a dense film due to the crystallinity of the polyolefin, and exhibits water vapor barrier properties. Furthermore, the polyolefin resin has a polar group, which allows it to adhere closely to the deposition layer 3, eliminating the need for a separate adhesive layer. This increases the proportion of paper in the packaging material, further improving tearability.
[0047] Examples of the polar group include a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0048] The first polyolefin resin may be a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxyl group, such as acrylic acid, methacrylic acid, or maleic anhydride), an unsaturated carboxylic acid ester, or a salt of a carboxylic acid neutralized with a basic compound. In addition, copolymers of ethylene or propylene with vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, or the like may also be used.
[0049] Specific examples of the first polyolefin resin include a copolymer of an acrylic acid ester and maleic anhydride, an ethylene-vinyl acetate copolymer, and an ethylene glycidyl methacrylate copolymer.
[0050] The sealant layer 4 may contain other components in addition to the first polyolefin resin, such as a silane coupling agent, an organic titanate, polyacrylic, polyester, polyurethane, polycarbonate, polyurea, polyamide, a polyolefin emulsion, polyimide, melamine, and phenol.
[0051] The content of the first polyolefin resin in the sealant layer 4 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0052] The thickness of the sealant layer 4 is 2 to 40 μm. When the thickness of the sealant layer 4 is 2 μm or more, sufficient seal strength for protecting the contents can be obtained. When the thickness of the sealant layer 4 is 40 μm or less, the packaging material 10 has excellent tearability regardless of the tearing direction even if it does not have a notch, and the amount of plastic material used can be sufficiently reduced. From the same viewpoint, the thickness of the sealant layer 4 may be 10 μm or less, or may be 5 μm or less. The packaging material 10 having a sealant layer 4 of such a thickness can be suitably used as a packaging material for packaging light-weight contents.
[0053] The sealant layer 4 may be a single layer, or may be a multilayer consisting of two or more layers.
[0054] The sealant layer 4 can be provided by applying a coating liquid containing the first polyolefin resin and a solvent onto the vapor deposition layer 3, and drying the coating liquid.
[0055] Examples of the solvent contained in the coating liquid of the sealant layer 4 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0056] The melting point of the first polyolefin resin in the coating liquid is preferably 70 to 160°C, more preferably 80 to 120°C. A low melting point has the advantage of lowering the start-up temperature during heat sealing. A high melting point of the first polyolefin resin increases the risk of blocking in a high-temperature environment. In order to prevent blocking, the particle size is preferably large so that the contact area is small. Although not particularly limited, the particle size may be specifically 1 nm or more, 0.1 μm or more, 1 μm or less, 0.7 μm or less, or 0.5 μm or less.
[0057] The tensile breaking strength of the packaging material 10 is 40 to 70 N / 15 mm. When the tensile breaking strength is 40 N / 15 mm or more, the packaging bag obtained from the packaging material 10 has sufficient strength, and the occurrence of defects such as tearing during transportation can be suppressed. When the tensile breaking strength is 70 N / 15 mm or less, the packaging material 10 has excellent tearability even if it does not have a notch. The tensile breaking strength is measured by pulling a test piece (longitudinal length: 100 mm, lateral length: 15 mm) cut out from the packaging material 10 in the longitudinal direction using a tensile tester (test length: 50 mm, pulling speed: 200 mm / min). When the fibers contained in the paper base material 1 are non-oriented, the tensile breaking strength of the packaging material 10 in any direction and in a direction perpendicular to the any direction may be in the above-mentioned numerical range. When the fibers contained in the paper base material 1 have an orientation, the tensile breaking strength of the packaging material 10 may be within the above numerical range in the direction of fiber orientation of the paper base material 1 in the packaging material 10 and in the direction perpendicular to the orientation direction.
[0058] {Second embodiment} The easy-open packaging material according to the second embodiment will be described below. Any points not described below are the same as those according to the first embodiment unless inconsistencies arise. Fig. 2 is a schematic cross-sectional view showing a packaging material according to the second embodiment. A packaging material 15 according to one embodiment has a laminated structure including a paper base material 1, an anchor coat layer 2, a deposition layer 3, an overcoat layer 11, an adhesive layer 12, and a sealant layer 4 in this order.
[0059] [Sealant layer] The sealant layer 4 is provided on the surface of the adhesive layer 12 so as to be in contact with the adhesive layer 12. The sealant layer 4 contains a first polyolefin resin. Examples of the first polyolefin resin include low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE), high-density polyethylene resin (HDPE), linear low-density polyethylene resin (LLDPE), ethylene-vinyl acetate copolymer (EVA), propylene homopolymer, ethylene-propylene block copolymer, and ethylene-propylene random copolymer. These may be used alone or in combination of two or more.
[0060] The thickness of the sealant layer 4 is 2 to 40 μm. The thickness of the sealant layer 4 may be 10 μm or more since this tends to improve the strength of the packaging material 15, or may be 20 μm or less since this provides better tearability and allows for a further reduction in the amount of plastic material used. The packaging material 15 having a sealant layer 4 of such a thickness can be suitably used as a packaging material for packaging heavy contents.
[0061] Examples of methods for forming the sealant layer 4 include extrusion lamination and dry lamination, and from the viewpoint of protecting the vapor-deposited layer 3, the dry lamination is preferred.
[0062] [Overcoat layer] The overcoat layer 11 is provided on the surface of the deposition layer 3 so as to be in contact with the deposition layer 3, and contains a second polyolefin resin having a polar group. The gas barrier property of the packaging material 15 is further improved by providing the overcoat layer 11. In addition, the adhesion between the overcoat layer 11 and the deposition layer 3 and the adhesion between the overcoat layer 11 and the adhesive layer 12 are superior to the adhesion between the deposition layer 3 and the adhesive layer 12, so that the packaging material 15 including the overcoat layer 11 has excellent adhesion. The packaging material 15 does not need to include the overcoat layer 11.
[0063] The second polyolefin resin may have at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0064] The second polyolefin resin may be a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxyl group, such as acrylic acid or methacrylic acid), an unsaturated carboxylic acid ester, or a salt of a carboxylic acid neutralized with a basic compound. In addition, copolymers of ethylene or propylene with vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, or the like may also be used.
[0065] Specific examples of the second polyolefin resin include a copolymer of an acrylic acid ester and maleic anhydride, an ethylene-vinyl acetate copolymer, and an ethylene glycidyl methacrylate copolymer.
[0066] Such an overcoat layer 11 has excellent flexibility, can suppress cracking of the deposition layer 3 after bending (folding), and has excellent adhesion to the deposition layer 3. Furthermore, by including the second polyolefin resin, a dense film can be formed due to the crystallinity of the polyolefin, and water vapor barrier properties are exhibited. Furthermore, by having a polar group, adhesion to the deposition layer 3 is exhibited.
[0067] The overcoat layer 11 may contain other components in addition to the second polyolefin resin, such as a silane coupling agent, an organic titanate, polyacrylic, polyester, polyurethane, polycarbonate, polyurea, polyamide, a polyolefin emulsion, polyimide, melamine, and phenol.
[0068] The content of the second polyolefin resin in the overcoat layer 11 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0069] The thickness of the overcoat layer 11 may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the overcoat layer 11 is 20 μm or less, the adhesion to the deposition layer and the gas barrier property can be sufficiently exhibited while suppressing the cost.
[0070] The overcoat layer 11 can be provided by applying a coating liquid containing the second polyolefin resin and a solvent onto the deposition layer 3, and drying the coating liquid.
[0071] Examples of the solvent contained in the coating liquid for the overcoat layer 11 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0072] The melting point of the second polyolefin resin in the coating liquid is preferably 70 to 160°C, more preferably 80 to 120°C. If the melting point of the second polyolefin resin is high, there is a high possibility of blocking in a high temperature environment. From the viewpoint of preventing blocking, it is better that the particle size is large so that the contact area is small. Although not particularly limited, the particle size may specifically be 1 nm or more, 0.1 μm or more, 1 μm or less, 0.7 μm or less, or 0.5 μm or less.
[0073] [Adhesive layer] The adhesive layer 12 is provided on the surface of the overcoat layer 11. As the adhesive layer 12, various materials can be used as long as they can bond the overcoat layer 11 and the sealant layer 4 to each other, and an example of the adhesive layer 12 is a cured product of a urethane adhesive.
[0074] The urethane adhesive is a resin composition containing a polyol having two or more hydroxyl groups in one molecule and an isocyanate compound having two or more isocyanate groups in one molecule. The urethane adhesive is cured to generate a urethane bond. The urethane adhesive is preferably a two-liquid curing type. The urethane adhesive may have gas barrier properties.
[0075] The thickness of the adhesive layer 12 is preferably 0.1 μm or more from the viewpoint of improving the adhesiveness of the adhesive layer 12, and is preferably 5 μm or less from the viewpoint of further reducing the amount of plastic material used.
[0076] <Packaging bag> 3 is a perspective view showing a gusset bag 20 made of packaging material 10. A packaging bag is manufactured by sealing the opening at the top of the gusset bag 20. The gusset bag 20 has portions where the packaging material 10 is folded (folded portions B1, B2). Folded portion B1 is a portion where the packaging material 10 is folded in a valley direction when viewed from the innermost layer side, while folded portion B2 is a portion where the packaging material 10 is folded in a mountain direction when viewed from the innermost layer side.
[0077] The packaging bag may be formed by folding one sheet of packaging material in half so that the sealant layers 4 face each other, and then folding and heat sealing the sheet into the desired shape, or may be formed by stacking two sheets of packaging material together so that the sealant layers 4 face each other, and then heat sealing the sheet into the bag shape.
[0078] In the packaging bag according to the present embodiment, the heat seal strength is not particularly limited. The heat seal strength can be appropriately changed by changing the thickness of the sealant layer 4. For example, when a light-weight content is to be stored, the heat seal strength may be 2N or more and 10N or less. When a heavy-weight content is to be stored, the heat seal strength is preferably 10N or more.
[0079] The packaging bag can contain food, medicine, and the like. It is particularly suitable for containing food, such as sweets. The packaging bag according to the present embodiment can maintain high gas barrier properties even in a shape having a folded portion.
[0080] In the present embodiment, a gusset bag is given as an example of a packaging bag, but the packaging material according to the above embodiment may be used to produce, for example, a pillow bag, a three-side sealed bag, or a standing pouch. The packaging bag may be made of packaging material 15. EXAMPLES
[0081] Hereinafter, the present disclosure will be described more specifically based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0082] <Production of packaging materials> Example 1 Paper (clay coated paper, basis weight: 60g / m 2A coating solution containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group (product name: Chemipearl S500, ionomer type, particle size: <0.5 μm, solvent: water and IPA, manufactured by Mitsui Chemicals, Inc.) was applied onto the surface of the paper (paper thickness: 55 μm, clay coat thickness: 5 μm) using a bar coater and dried in an oven to form an anchor coat layer (thickness: 3 μm). Subsequently, AL was vapor-deposited on the anchor coat layer to form an AL vapor-deposited layer (thickness: 50 nm). A non-oriented polypropylene resin (CPP) film (thickness: 20 μm) as a sealant layer was dry-laminated on the vapor-deposited layer using an adhesive (product name: Takelac A525 / Takenate A52, urethane-based two-component type, manufactured by Mitsui Chemicals, Inc.) to obtain a packaging material. The thickness of the adhesive layer was 2 μm. The weight of the paper in the packaging material is shown in Table 1.
[0083] Example 2 An anchor coat layer was formed on the surface of the paper in the same manner as in Example 1, and an AL vapor deposition layer was formed on the anchor coat layer. A coating liquid containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group (product name: Chemipearl S500, ionomer type, particle size: <0.5 μm, solvent: water and IPA, manufactured by Mitsui Chemicals, Inc.) was applied on the surface of the vapor deposition layer with a bar coater, and dried in an oven to form an overcoat layer (thickness: 3 μm). A non-oriented polypropylene resin (CPP) film (thickness: 20 μm) as a sealant layer was dry laminated on the overcoat layer using an adhesive (product name: Takelac A525 / Takenate A52, urethane-based two-component type, manufactured by Mitsui Chemicals, Inc.) to obtain a packaging material. The thickness of the adhesive layer was 2 μm. The weight of the paper in the packaging material is shown in Table 1.
[0084] Example 3 An anchor coat layer was formed on the surface of the paper, and an aluminum vapor deposition layer was formed on the anchor coat layer in the same manner as in Example 1. A coating liquid containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group (product name: Chemipearl S500, ionomer type, particle size: <0.5 μm, solvent: water and IPA, manufactured by Mitsui Chemicals, Inc.) was applied on the surface of the vapor deposition layer with a bar coater, and dried in an oven to form a sealant layer (thickness: 3 μm) to obtain a packaging material. The weight of the paper in the packaging material is shown in Table 1.
[0085] Example 4 A packaging material was obtained in the same manner as in Example 1, except that the anchor coat layer was formed using a polyvinyl alcohol resin (saponification degree: 98%, polymerization degree: 500) instead of the coating liquid containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group. The weight of the paper in the packaging material is shown in Table 1.
[0086] Example 5 A packaging material was obtained in the same manner as in Example 1, except that a sealant layer was formed using a linear low-density polyethylene resin (LLDPE) film (thickness: 20 μm) instead of the non-oriented polypropylene resin (CPP) film. The weight of the paper in the packaging material is shown in Table 2.
[0087] Example 6 A packaging material was obtained in the same manner as in Example 1, except that a sealant layer was formed using a linear low-density polyethylene resin (LLDPE) film (thickness: 40 μm) instead of the non-oriented polypropylene resin (CPP) film. The weight of the paper in the packaging material is shown in Table 2.
[0088] Comparative Example 1 Except for changing the thickness of the non-oriented polypropylene resin (CPP) to 60 μm, a packaging material was obtained in the same manner as in Example 1. The weight of the paper in the packaging material is shown in Table 2.
[0089] Comparative Example 2 A packaging material was obtained in the same manner as in Example 1, except that a sealant layer was formed using a polyethylene terephthalate (PET) film (thickness: 30 μm) instead of the non-oriented polypropylene resin (CPP) film. The weight of the paper in the packaging material is shown in Table 2.
[0090] Example 7 Except for using silica as the vapor deposition layer, a packaging material was obtained in the same manner as in Example 1. The weight of the paper in the packaging material is shown in Table 3.
[0091] Example 8 Except for using alumina as the vapor-deposited layer, a packaging material was obtained in the same manner as in Example 1. The weight of the paper in the packaging material is shown in Table 3.
[0092] Example 9 Paper as paper (clay coated paper, basis weight: 50g / m 2 A packaging material was obtained in the same manner as in Example 1, except that the following materials were used: paper thickness: 45 μm, clay coat thickness: 5 μm. The weight of the paper in the packaging material is shown in Table 3.
[0093] Example 10 A packaging material was obtained in the same manner as in Example 1, except that the anchor coat layer was formed using a polyurethane resin instead of the coating liquid containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group. The weight of the paper in the packaging material is shown in Table 3.
[0094] Example 11 A packaging material was obtained in the same manner as in Example 3, except that the anchor coat layer was formed using a polyurethane resin instead of the coating liquid containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group. The weight of the paper in the packaging material is shown in Table 3.
[0095] Comparative Example 3 A packaging material was obtained in the same manner as in Example 10, except that the thickness of the non-oriented polypropylene resin (CPP) was 60 μm. The weight of the paper in the packaging material is shown in Table 3.
[0096] <Evaluation of tearability> The packaging materials according to the examples and the comparative examples were bonded together with the sealant layers facing each other to prepare a three-sided pouch (size: 10 cm square, seal width: 5 mm). Five evaluators were randomly selected from 10 men and 10 women, and the selected evaluators tore the three-sided pouch and evaluated the ease of tearing according to the following criteria. The three-sided pouch was torn in the direction along the flow direction in the papermaking process (MD) and in the direction perpendicular to the flow direction in the papermaking process (CD). The worst evaluation result among the evaluation results of the selected evaluators was regarded as the evaluation result of the packaging material. The results are shown in Tables 1 to 3. (Evaluation Criteria) A: Easily torn and no stretching of the sealant layer observed B: It can be torn, but the sealant layer is stretched. C: Non-tearable
[0097] <Measurement of tensile breaking strength> Test pieces were cut out from the packaging materials according to the examples and comparative examples. The size of the test pieces was 100 mm in length in the direction along the papermaking process (MD) and 15 mm in length in the direction perpendicular to the papermaking process (CD). The test pieces were pulled in the longitudinal direction (MD) using a tensile tester, and the tensile breaking strength was measured. The test length was 50 mm, and the pulling speed was 200 mm / min. The measurement was performed on five test pieces. The average value of the measured values obtained from the five test pieces was taken as the MD tensile breaking strength of the packaging material. In addition, the tensile breaking strength was measured in the same manner as the MD tensile breaking strength for test pieces with a length of 100 mm in the direction perpendicular to the papermaking process (CD) and a length of 15 mm in the direction along the papermaking process (MD), and was taken as the CD tensile breaking strength. The results are shown in Tables 1 to 3.
[0098] <Measurement of water vapor permeability> The water vapor permeability of the packaging materials according to the examples and comparative examples was measured by the MOCON method. The measurement conditions were a temperature of 40°C and a relative humidity of 90%. The measurement device used was a PERMATRAN (product name, manufactured by MOCON). While rolling a 600g roller at a speed of 300mm / min, the packaging material was folded 180 degrees so that the paper base material was on the inside, and the water vapor permeability of the packaging material after opening was also measured in the same manner. The results are shown in Tables 1 to 3 in units of [g / m 2 ·day].
[0099] [Table 1]
[0100] [Table 2]
[0101] [Table 3]
[0102] The gist of the present disclosure lies in the following [1] to [9]. [1] A paper base material; An anchor coat layer; a vapor-deposited layer of a metal or metal oxide; A sealant layer; A packaging material having a laminated structure comprising, in this order, The weight of the paper base material is 50% or more by mass based on the entire packaging material, The thickness of the sealant layer is 2 to 40 μm, the sealant layer comprises a first polyolefin-based resin; An easy-to-open packaging material having a tensile breaking strength of 40 to 70 N / 15 mm. [2] The easy-open packaging material according to [1], wherein the first polyolefin resin has at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group. [3] The easy-open packaging material according to [1] or [2], wherein the sealant layer has a thickness of 2 to 20 μm. [4] The easy-open packaging material according to any one of [1] to [3], further comprising an adhesive layer between the deposition layer and the sealant layer. [5] An overcoat layer is further provided between the deposition layer and the adhesive layer, The easy-open packaging material according to [4], wherein the overcoat layer contains a second polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group. [6] The easy-open packaging material according to any one of [1] to [5], wherein the anchor coat layer contains a third polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group. [7] The easy-open packaging material according to any one of [1] to [5], wherein the anchor coat layer contains a polyvinyl alcohol-based resin. [8] A packaging bag comprising the easy-open packaging material according to any one of [1] to [7]. [9] The packaging bag described in [8], having a folded portion. [Explanation of symbols]
[0103] 1...paper base material, 2...anchor coat layer, 3...vapor deposition layer, 4...sealant layer, 10, 15...packaging material, 11...overcoat layer, 12...adhesive layer, 20...gusset bag, B1, B2...folded portion.
Claims
1. A paper substrate; a vapor-deposited layer of a metal or metal oxide; A sealant layer; A packaging material having a laminated structure comprising, in this order, The weight of the paper base material is 50% by mass or more based on the entire packaging material, The thickness of the sealant layer is 2 to 40 μm, the sealant layer comprises a first polyolefin-based resin, An easy-open packaging material having a tensile breaking strength of 40 to 70 N / 15 mm.
2. The easy-open packaging material according to claim 1 , wherein the first polyolefin resin has at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
3. 2. The easy-open packaging material according to claim 1, wherein the sealant layer has a thickness of 2 to 20 μm.
4. The easy-open packaging material according to claim 1 , further comprising an adhesive layer between the deposition layer and the sealant layer.
5. an overcoat layer between the deposition layer and the adhesive layer; The easy-open packaging material according to claim 4 , wherein the overcoat layer comprises a second polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
6. A packaging bag comprising the easy-open packaging material according to any one of claims 1 to 5.
7. The packaging bag according to claim 6, having a folded portion.
Citation Information
Patent Citations
Packaging laminate, packaging bag using it and package using packaging bag
JP2006142597A
Laminated packaging material and packaging bag using it
JP2007076281A
Packaging material for paper container
JP2016003016A
Laminate and packaging material using laminate
JP2017226186A
Low-adsorption laminate for hand-opening and packaging material using the same and package
JP2019038569A