Polarizing plate and display device using the same
The polarizing plate design with balanced moisture permeability films addresses durability issues by managing moisture ingress and egress, ensuring longevity and optical stability in high-temperature environments.
Patent Information
- Application Number
- JP2020040767
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-03-10
AI Technical Summary
Polarizing plates used in display devices for vehicles face durability issues under high-temperature environments due to moisture penetration through protective films, leading to polarizer deterioration.
A polarizing plate design with a protective film A having a hydrophobic hard coat layer on a TAC film and a low-moisture permeability film B, such as COP or PET, where the moisture permeabilities of both films are carefully balanced to allow moisture release while preventing ingress, using specific ranges (TA > 215 g/m²/day and TB ≥ 5 g/m²/day).
The design effectively suppresses polarizer deterioration by managing moisture within the plate, maintaining optical performance even in harsh high-temperature and high-humidity conditions.
Smart Images

Figure 0007563888000003 
Figure 0007563888000001 
Figure 0007563888000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing plate and a display device using the same. [Background technology]
[0002] Polarizing plates used in liquid crystal display devices are equipped with a polarizer in which an iodine compound or an organic dye is adsorbed onto a polyvinyl alcohol (PVA) film, and the PVA film is stretched to orient the iodine compound or the organic dye. Since polarizers made of PVA films are inferior in strength and water resistance, protective films are attached to both sides of the polarizer to protect the polarizer.
[0003] Conventionally, a hard coat film having a hard coat layer provided on one side of a triacetyl cellulose (TAC) film has been generally used as a protective film for a polarizing plate (see, for example, Patent Document 1). However, the moisture permeability of a hard coat film using a TAC film as a substrate is 300 to 1000 g / m 2 / day, and moisture absorption of the polarizer cannot be sufficiently suppressed under high temperature and high humidity conditions, which causes deterioration of the polarizer. Therefore, in order to improve moisture resistance compared to protective films using TAC film as a base material, various protective films using cycloolefin polymer (COP) or polyethylene terephthalate (PET) as a base material have been developed (see, for example, Patent Document 2). The moisture permeability of the protective film is 5 to 100 g / m 2 / day. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-175991 A [Patent Document 2] JP 2006-30807 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the number of display devices mounted on vehicles has increased. Since display devices for vehicle use may be used in extremely harsh high-temperature environments, the polarizing plates are also required to have durability in high-temperature environments.
[0006] By using a protective film using a low moisture permeable base material such as COP or PET, it is possible to sufficiently reduce the intrusion of moisture from the outside of the polarizing plate into the polarizer. However, it has been found that when a polarizing plate is exposed to a high temperature environment such as the inside of a car, moisture contained in the base material of the protective film and moisture contained in the adhesive used to attach the protective film to the polarizer penetrates and remains inside the polarizing plate, causing deterioration of the polarizer due to this moisture.
[0007] Therefore, an object of the present invention is to provide a polarizing plate having excellent durability at high temperatures and a display device using the same. [Means for solving the problem]
[0008] The polarizing plate according to the present invention has a protective film A bonded to one surface of a polarizer and a protective film B bonded to the other surface of the polarizer, Protective film A is a hard coat film having a hard coat layer laminated on one side of a triacetyl cellulose film, protective film B is a film made of a cycloolefin polymer, the hard coat layer contains a cycloolefin polymer as a hydrophobic material, the content of the cycloolefin polymer is 0.1 / 45 to 2.0 / 46.8 parts by weight when the total solid content of the hard coat layer is taken as 100 parts by weight, and the film thickness of the hard coat layer is 7 to 12 μm, The moisture permeabilities TA and TB of protective films A and B at 40° C. and 90% RH simultaneously satisfy the following conditions (1) and (2). 215 g / m 2 / day>TA> 80 g / m 2 / day ···(1) 5g / m 2 / day≧TB (2)
[0009] A display device according to the present invention includes the above polarizing plate. Effect of the Invention
[0010] According to the present invention, it is possible to provide a polarizing plate having excellent durability at high temperatures and a display device using the same. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic configuration of a polarizing plate according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] FIG. 1 is a cross-sectional view showing a schematic configuration of a polarizing plate according to an embodiment of the present invention.
[0013] The polarizing plate 10 includes a polarizer 1, a protective film A laminated on one side of the polarizer 1, and a protective film B laminated on the other side of the polarizer 1. The polarizer 1 is formed by adsorbing iodine or a dye onto a polyvinyl alcohol (PVA) film and orienting it. Since the PVA constituting the polarizer 1 is poor in strength and water resistance, protective films A and B are attached to both sides of the polarizer 1.
[0014] The protective film A is a hard-coated film in which a hard-coat layer is laminated on one side of a TAC film. The hard-coat layer is a functional layer that coats a flexible TAC film and imparts hardness to the protective film A, and can be formed by applying and curing a coating liquid containing an ultraviolet-curable material. The pencil hardness of the protective film A (hard-coated film) is preferably 3H or more. In addition, since the TAC film has low water vapor barrier properties (high moisture permeability), the moisture permeability of the protective film A is adjusted by the hard-coat layer. Specifically, the moisture permeability of the protective film A can be set within the range described below by blending a hydrophobic material in the hard-coat layer. As the hydrophobic material to be contained in the hard-coat layer, for example, a cycloolefin polymer can be used. The TAC film of the protective film A is attached to the polarizer 1 using water paste (PVA aqueous solution).
[0015] The thickness of the TAC film used in the protective film A is not particularly limited, but is preferably 25 to 100 μm. The thickness of the hard coat layer is not particularly limited, but is preferably 2 to 15 μm. However, the thickness of the TAC film and the thickness of the hard coat layer can be appropriately changed as long as the moisture permeability of the protective film A is within the range described below.
[0016] The protective film B is a low moisture permeable film and can be made of any one of cycloolefin polymer, polyethylene terephthalate, and polymethyl methacrylate. The protective film B is attached to the polarizer 1 via an ultraviolet-curable adhesive. The thickness of the protective film B is not particularly limited, but is preferably 10 to 100 μm.
[0017] In the display device, protective film B is disposed on the display panel side, and the hard coat layer of protective film A is disposed on the viewing side (the side opposite to the display panel).
[0018] As described above, the polarizer 1 and the TAC film of the protective film A are bonded together using a water-based adhesive, so moisture may remain in the adhesive layer and the TAC film even after a drying process. If both protective films A and B were constructed using films with low moisture permeability, the intrusion of moisture from the outside would be suppressed, but moisture would be generated from the adhesive layer and / or the TAC film in an extremely high-temperature environment such as the inside of a car in summer and remain inside the polarizing plate 10, leading to deterioration of the polarizer 1. Therefore, in the polarizing plate 10 according to this embodiment, a difference is provided between the moisture permeability of the protective film A and the moisture permeability of the protective film B, In addition, by setting the moisture permeability of protective film A and the moisture permeability of protective film B to be within specific ranges, respectively, deterioration of polarizer 1 due to moisture is suppressed.
[0019] Specifically, assuming that the moisture permeabilities of protective films A and B at 40°C and 90% RH are TA and TB, respectively, TA and TB simultaneously satisfy the following conditions (1) and (2). Note that both the moisture permeabilities TA and TB are values measured in accordance with JIS Z 0208-1976. 240g / m 2 / day>TA>70g / m 2 / day ···(1) 70 g / m 2 / day≧TB (2)
[0020] By simultaneously satisfying the above conditions (1) and (2), it is possible to suppress the intrusion of moisture from the outside into the polarizing plate, while at the same time making it possible to expel moisture generated from the adhesive layer for bonding protective film A and polarizer 1 and / or the TAC film of protective film A to the outside when exposed to a high-temperature environment, for example, at 85°C.
[0021] The moisture permeability TA of protective film A is 180g / m 2 / day or more. In this case, the amount of hydrophobic material contained in the hard coat layer for adjusting the moisture permeability of protective film A can be reduced, so that the surface hardness of the hard coat layer is excellent. In addition, since protective film B is intended to completely block the ingress and egress of moisture, it is preferable that the moisture permeability TB of protective film B is small.
[0022] As described above, the polarizing plate 10 according to this embodiment includes, as protective films for the polarizer 1, a protective film A having a moisture permeability satisfying the above condition (1) and a protective film B having a moisture permeability satisfying the above condition (2). In this configuration, the protective film B arranged on the display panel side almost completely blocks the ingress and egress of moisture. On the other hand, the protective film A arranged on the viewing side suppresses the ingress of moisture from the outside into the polarizing plate 10, but allows the release of moisture generated inside the polarizing plate 10. Therefore, when the polarizing plate 10 according to this embodiment is used in a high-temperature environment, moisture generated inside the polarizing plate 10 does not remain, thereby suppressing deterioration of the polarizer and enabling the optical performance of the polarizing plate 10 to be maintained for a longer period of time. EXAMPLES
[0023] Examples of the present invention will now be described in detail.
[0024] Example 1 Composition 1 shown in Table 1 was applied as a coating solution for forming a hard coat layer to a 40 μm-thick TAC film (product name: TJ40UL, manufactured by Fujifilm Corporation) using a wire bar coater and dried, and then the coating film was irradiated with ultraviolet light at 100 mJ / cm. 2 The hard coat layer was cured by irradiating the hard coat layer with an exposure amount of 1000 μm to prepare a protective film A (hard coat film) according to Example 1. The film thickness of the hard coat layer after curing was set to the value shown in Table 2. A COP film having a thickness of 5 μm was used as a protective film B.
[0025] A polarizer was attached to the TAC film surface of protective film A using water-based glue and dried, and then the protective film was attached to the polarizer using a UV-curable adhesive, and the UV-curable adhesive was cured by irradiating it with UV rays to obtain a polarizing plate of Example 1.
[0026] [Table 1]
[0027] (Examples 2 to 7) Polarizing plates according to Examples 2 to 7 were produced in the same manner as in Example 1, except that compositions 2 to 7 shown in Table 1 were used as the coating liquids for forming a hard coat layer.
[0028] Comparative Example 1 The composition 8 shown in Table 1 was used as the coating liquid for forming the hard coat layer, and the exposure dose of ultraviolet light was 75 mJ / cm 2 A polarizing plate according to Comparative Example 1 was produced in the same manner as in Example 1, except for the above.
[0029] Comparative Example 2 A polarizing plate according to Comparative Example 2 was produced in the same manner as in Example 1, except that Composition 9 shown in Table 1 was used as the coating liquid for forming a hard coat layer.
[0030] Comparative Example 3 A polarizing plate according to Comparative Example 3 was produced in the same manner as in Example 1, except that a PMMA film having a thickness of 40 μm was used as the protective film A.
[0031] Comparative Example 4 A polarizing plate according to Comparative Example 4 was produced in the same manner as in Example 1, except that a COP film having a thickness of 5 μm was used as the protective film A.
[0032] (moisture permeability) Before being attached to the polarizer, the moisture permeability TA of the protective film A and the moisture permeability TB of the protective film B were measured under conditions of 40° C. and 90% humidity in accordance with JIS Z 0208-1976.
[0033] (Polarization degree after high temperature and high humidity durability test) The polarizing plates according to Examples 1 to 7 and Comparative Examples 1 to 4 were placed in a thermostatic chamber at 85°C and 85% RH, and the polarization degree was measured 240 hours and 500 hours after the placement. The polarization degree was calculated by performing luminosity correction using a 2-degree visual field (C light source) of "JIS Z 8701" on a value measured using an absorptiometer with an integrating sphere ("V7100" manufactured by JASCO Corporation).
[0034] Table 2 shows the measured values of the moisture permeability TA of protective film A, the moisture permeability TB of protective film B, and the polarization degree of the polarizing plate (initial value, before and after high temperature and high humidity durability test) used in Examples 1 to 7 and Comparative Examples 1 to 4.
[0035] [Table 2]
[0036] The polarizing plates according to Examples 1 to 7 had moisture permeability TA of protective film A and moisture permeability TB of protective film B satisfying the above conditions (1) and (2), and showed high polarization degree values even when placed in a thermostatic chamber at 85°C and 85% RH for 500 hours. The polarization degree test results after the high temperature and high humidity durability test according to Examples 1 to 7 mean that even when exposed to high temperature and high humidity, there was no deterioration of the polarizer caused by moisture penetrating into the polarizing plate from the outside, and no deterioration of the polarizer caused by moisture contained in protective film A and / or the adhesive for bonding protective film A.
[0037] The polarizing plates according to Comparative Examples 1 and 2 have a high moisture permeability TA of the protective film A exceeding the upper limit of the above condition (1). The polarizing plates according to Comparative Examples 1 and 2 have a lower polarization degree after being placed in a thermostatic chamber at 85°C and 85% RH for 240 hours than those of Examples 1 to 7. When the polarizing plates according to Comparative Examples 1 and 2 are placed in a thermostatic chamber at 85°C and 85% RH for 500 hours, the deterioration of the polarizer progresses too much, and the amount of light transmitted through the polarizing plate (i.e., the amount of leaked light) becomes too large, making it impossible to measure the polarization degree. Comparing Comparative Examples 1 and 2 with Examples 1 to 7, it is considered that the polarizer of the polarizing plates according to Comparative Examples 1 and 2 is deteriorated as a result of moisture penetrating from the protective film A into the polarizing plate under high temperature and high humidity.
[0038] In the polarizing plates according to Comparative Examples 3 and 4, the moisture permeability TA of the protective film A is lower than the lower limit of the above condition (1). In the polarizing plates according to Comparative Examples 3 and 4, the polarization degree after being placed in a thermostatic chamber at 85°C and 85% RH for 240 hours was also lower than that of Examples 1 to 7. In addition, when the polarizing plates according to Comparative Examples 3 and 4 were placed in a thermostatic chamber at 85°C and 85% RH for 500 hours, the deterioration of the polarizer progressed too much, and the amount of light transmitted through the polarizing plate (i.e., the amount of leaked light) became too large, making it impossible to measure the polarization degree. From the comparison between Comparative Examples 3 and 4 and Examples 1 to 7, it is considered that in the polarizing plates according to Comparative Examples 3 and 4, the intrusion of moisture into the polarizing plate under high temperature and high humidity is suppressed, but the polarizer is deteriorated due to moisture contained in the protective film A and / or the adhesive for bonding the protective film A.
[0039] From the above, it has been confirmed that according to the present invention, by making the moisture permeability TA of protective film A and the moisture permeability TB of protective film B satisfy the above conditions (1) and (2), the deterioration of the polarizer can be suppressed and the optical performance of the polarizing plate can be maintained even when exposed to an extremely harsh environment of high temperature and high humidity for a long period of time. [Industrial Applicability]
[0040] The present invention can be used as a polarizing plate for use in a display device, and is particularly suitable as a polarizing plate for a display device used in a high-temperature environment, such as for in-vehicle use. [Explanation of symbols]
[0041] 1 Polarizer 10 Polarizing plate A, B protective film
Claims
1. A polarizing plate in which a protective film A is bonded to one surface of a polarizer and a protective film B is bonded to the other surface of the polarizer, The protective film A is a hard coat film having a hard coat layer laminated on one surface of a triacetyl cellulose film, The protective film B is a film made of a cycloolefin polymer, the hard coat layer contains a cycloolefin polymer as a hydrophobic material, and the content of the cycloolefin polymer is 0.1 / 45 to 2.0 / 46.8 parts by weight when the total solid content of the hard coat layer is 100 parts by weight; The hard coat layer has a thickness of 7 to 12 μm, A polarizing plate characterized in that the moisture permeabilities TA and TB of protective films A and B at 40° C. and 90% RH simultaneously satisfy the following conditions (1) and (2): 215g / m 2 / day>TA>80g / m 2 / day ・・・(1) 5g / m 2 / day≧TB ・・・(2)
2. 2. The polarizing plate according to claim 1, wherein the hard coat film has a pencil hardness of 3H or more.
3. A display device comprising the polarizing plate according to claim 1.
Citation Information
Patent Citations
Caster for preventing deflection of chassis and slidable contact abrasion of wheels
JP1987061802A
Spectacle frame and lens hanger
JP2006030807A
Polarizing plate and manufacturing method thereof, and liquid crystal display device
JP2013174861A
Polarizing plate protection film, polarizing plate, liquid crystal display device, and method for manufacturing polarizing plate protection film
JP2016175991A
Resin laminate with polarizing plate and display including the same
JP2017215582A