Method for producing (meth)acrylic resin film
The (meth)acrylic resin film addresses adhesive interface unevenness issues by controlling protruding defects and haze, enhancing optical and decorative film performance.
Patent Information
- Application Number
- JP2020160704
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Existing acrylic resin films used in optical applications, such as polarizing plates, suffer from insufficient suppression of adhesive interface unevenness, leading to visible defects and poor quality for high-definition displays.
A (meth)acrylic resin film with controlled adhesive interface properties, characterized by low protruding defects, high pencil hardness, and low haze, produced using a specific melt extrusion process with mirror-finished rolls and optimized temperature and pressure conditions.
The film effectively suppresses actual defects in laminated films, ensuring high optical quality and durability, suitable for applications like polarizing plates and decorative films.
Smart Images

Figure 0007563926000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a (meth)acrylic resin film and a method for producing the same. [Background technology]
[0002] Acrylic resin films are used as various optical films because of their excellent optical performance. However, in order to be used as optical films, the film must have few defects. For example, Patent Document 1 discloses a method for producing an optical film in which a barrier flight type screw or a screw with a mixing section is used as the screw of an extruder, the temperature of some members of the extruder is set to less than a certain temperature, and a resin is molded by a melt extrusion method. Patent Document 2 discloses that, in an optical laminate having a first outer layer, an intermediate layer, and a second outer layer in this order, a laminate with few fisheye defects is produced by setting the ratio of the thickness of the intermediate layer to the total thickness of the first outer layer and the second outer layer in a specific range. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-39935 A [Patent Document 2] JP 2017-68227 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the method disclosed in Patent Document 1 was able to reduce the content of foreign matter, but was not sufficient for the quality required by recent high-definition displays. The method disclosed in Patent Document 2 also reduced foreign matter, but like Patent Document 1, it did not yet provide sufficient quality. In particular, in polarizing plates, the adhesive interface between films with different refractive indexes is required to be as flat as possible, but the films disclosed in Patent Documents 1 and 2 were not necessarily capable of sufficiently suppressing unevenness at the adhesive interface.
[0005] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a (meth)acrylic resin film that, when used as a component of a laminate film such as a polarizing plate, can suppress visible defects in the polarizing plate caused by unevenness at the adhesive interface (hereinafter, sometimes referred to as "actual defects"), and a manufacturing method thereof. [Means for solving the problem]
[0006] As a result of investigating the above-mentioned problems, the inventors gained knowledge about the specific state in which the adhesive interface needs to be controlled, and further investigations based on this knowledge led to the completion of the present invention.
[0007] That is, the present invention provides the following [1] to
[10] . [1] One protruding defect with a height of 1 μm or more per 10 m 2 (Meth)acrylic resin film having a viscosity of less than 10000000000. [2] 10 fisheye defects / m 2 The (meth)acrylic resin film according to the above item [1], [3] The (meth)acrylic resin film according to the above [1] or [2], having a film thickness of 20 to 500 μm. [4] The (meth)acrylic resin film according to any one of the above [1] to [3], at least one surface of which has a pencil hardness of 5B or more. [5] The (meth)acrylic resin film according to any one of the above [1] to [4], which has a haze of 1.5% or less. [6] A laminate film comprising the (meth)acrylic resin film according to any one of the above [1] to [5]. [7] The laminate film according to the above [6], further comprising a functional layer on the surface of the laminate film. [8] A polarizing plate comprising the (meth)acrylic resin film according to any one of the above [1] to [5]. [9] A method for producing a (meth)acrylic resin composition, comprising: a melt extruding step of melt extruding a (meth)acrylic resin composition through a T-die; and a holding step of holding the melt extruded material between a pair of mirror-finished rolls or mirror-finished belts, The method for producing a (meth)acrylic resin film according to any one of the above [1] to [5], wherein the surface temperatures of the pair of mirror-finished rolls and the mirror-finished belt are both 60°C or higher, and the thickness of at least one of the outer cylinders of the pair of mirror-finished rolls and the thickness of at least one of the pair of mirror-finished belts are both more than 3 mm.
[10] The method for producing a (meth)acrylic resin film according to the above [9], wherein in the clamping step, the melt-extruded molten material is clamped between a pair of mirror-surface rolls, the pair of mirror-surface rolls comprising a mirror-surface elastic roll and a mirror-surface rigid roll. Effect of the Invention
[0008] According to the present invention, it is possible to provide a (meth)acrylic resin film that, when used as a constituent member of a laminate film such as a polarizing plate, can suppress actual damage and defects of the polarizing plate caused by unevenness at the adhesive interface, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] An example of an embodiment to which the present invention is applied will be described below. The numerical values specified in this specification are values determined by the methods disclosed in the embodiments or examples. Other embodiments are also included in the scope of the present invention as long as they are in accordance with the gist of the present invention. In this specification, "(meth)acrylic" means "acrylic or methacrylic", and "(meth)acrylic resin film" means a resin film made of a (meth)acrylic resin composition.
[0010] The (meth)acrylic resin film of the present invention (hereinafter, sometimes simply referred to as the film) has a protruding defect having a height of 1 μm or more at 1 piece / 10 m. 2 It is characterized in that it is less than.
[0011] A protruding defect with a height of 1 μm or more can become a harmful defect when used in a laminated film such as a polarizing plate, and the number of protruding defects with a height of 1 μm or more per 10 m is 1. 2 If the number is more than this, when the laminated film is made into a polarizing plate or the like, the number of defects that actually cause damage increases and the yield decreases. From this point of view, the number of protruding defects with a height of 1 μm or more is set at 0.5 pieces / 10 m. 2 Preferably less than 0.2 pieces / 10m 2 It is more preferable that the number of pieces is less than 0.1 pieces / 10m. 2 It is even more preferable that: When a laminated film containing a film having a protruding defect is used for a polarizing plate, etc., only the thickness ratio of each layer in the part of the protruding defect is different from the surrounding area, resulting in a laminated film with a locally different refractive index, and the corresponding part is detected as a distortion by visual inspection, and it was found to be a harmful defect. On the other hand, protruding defects occur on the film due to various causes, but it is possible to absorb the protruding parts to a certain extent during the film manufacturing process by combining the viscosity and glass transition temperature of the raw resin of the film, the manufacturing conditions of the film, etc. In this way, by absorbing the height of the protruding defect generated on the film into the surrounding area and lowering it, it is thought that it is possible to suppress the visual distortion (harmful defect) caused by the difference in thickness ratio when the laminated film is made. The number of protruding defects having a height of 1 μm or more can be determined by observation with a laser microscope, specifically by the method described in the examples. In the present invention, the fisheye defect refers to all defects that can be detected by visual inspection, and the protruding defect refers to a defect having a protrusion on the film (convex defect) among fisheye defects. Fisheye defects and protruding defects can be detected and measured by the methods described in the Examples. The height of the fisheye defect is usually 0.1 to 3 μm.
[0012] The (meth)acrylic resin film of the present invention has a protruding defect having a height of 1 μm or more of 1 defect / 10 m. 2 By having a fisheye defect density of less than 10 / m2, it is possible to obtain a (meth)acrylic resin film with few defects that will cause practical harm when it is made into a laminate film for a polarizing plate or the like, regardless of the presence or absence or number of other fisheye defects. However, the number of fisheye defects must be less than 10 / m2. 2 It is preferable that the number of pieces is 5 pieces / m or less. 2 More preferably, 2 pieces / m or less. 2 More preferably, it is 1.2 pieces / m or less. 2 On the other hand, since it is necessary to spend many steps such as installing a filter and improving the polymer to remove fish-eye defects, the number of fish-eye defects in this invention is preferably 0.1 / m or less. 2 More than 0.2 pieces / m 2 More than 0.5 pieces / m is acceptable 2 More than 1.0 pieces / m is acceptable 2 There may be more than one.
[0013] The (meth)acrylic resin film of the present invention preferably has a pencil hardness of at least one surface of 5B or more, more preferably 2B or more, even more preferably HB or more, and even more preferably F or more. A high pencil hardness makes the surface of the film less susceptible to scratches, and is therefore preferable as a decorative and surface protective film for the surface of a molded product that requires design, and is also preferable in polarizer protective film applications, since it can suppress the occurrence of scratches that occur during manufacturing processes such as lamination. The pencil hardness can be adjusted by the compounding composition of the (meth)acrylic resin composition, the type of (meth)acrylic resin used, and the type of (meth)acrylic crosslinked rubber particles used. The pencil hardness can be measured by a method in accordance with JIS K5600-5-4:1999, and specifically, can be determined by the method described in the examples.
[0014] The (meth)acrylic resin film of the present invention preferably has a haze of 1.5% or less, more preferably 1.2% or less, and even more preferably 1.0% or less. When the film is used in applications requiring design, a haze of 1.5% or less provides better surface gloss and clarity of the pattern layer printed on the film of the present invention. In addition, in optical applications such as polarizer protective films and light guiding films, this is preferable because it increases the utilization efficiency of the light source. Furthermore, this is preferable because it provides excellent shaping accuracy when performing surface shaping. The haze can be adjusted by the type and amount of the (meth)acrylic resin, the die temperature, roll temperature, film formation speed, pressing pressure, and the like during film formation. The haze can be measured by a method in accordance with JIS K7136:2000, and specifically, can be determined by the method described in the examples.
[0015] <(Meth)acrylic resin composition> The (meth)acrylic resin film of the present invention is made of a (meth)acrylic resin composition containing a (meth)acrylic resin (A) as a main component.
[0016] [(Meth)acrylic resin (A)] The (meth)acrylic resin (A) used in the present invention may be, for example, one that is mainly composed of structural units derived from methyl methacrylate (hereinafter, sometimes referred to as methyl methacrylate units). From the viewpoint of heat resistance, the content of methyl methacrylate units in the (meth)acrylic resin (A) is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, and all structural units may be methyl methacrylate units.
[0017] The (meth)acrylic resin (A) may contain structural units derived from monomers other than methyl methacrylate. The other monomer is not particularly limited as long as it is copolymerizable with methyl methacrylate, and examples thereof include acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate, phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-ethoxyethyl acrylate, glycidyl acrylate, allyl acrylate, cyclohexyl acrylate, norbornyl acrylate, and isobornyl acrylate; ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, methacrylic acid esters such as ... Methacrylic acid esters other than methyl methacrylate, such as n-hexyl methacrylate, 2-ethylhexyl methacrylate, pentadecyl methacrylate, dodecyl methacrylate, phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, 2-hydroxyethyl methacrylate, 2-ethoxyethyl methacrylate, glycidyl methacrylate, allyl methacrylate, cyclohexyl methacrylate, norbornyl methacrylate, and isobornyl methacrylate; acrylic acid, methacrylic acid, maleic anhydride, Examples of the monomer include unsaturated carboxylic acids or acid anhydrides thereof, such as maleic acid and itaconic acid; olefins, such as ethylene, propylene, 1-butene, isobutylene and 1-octene; conjugated dienes, such as butadiene, isoprene and myrcene; aromatic vinyl compounds, such as styrene, α-methylstyrene, p-methylstyrene and m-methylstyrene; acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, vinyl acetate, vinylpyridine, vinyl ketone, vinyl chloride, vinylidene chloride and vinylidene fluoride.
[0018] The stereoregularity of the (meth)acrylic resin (A) is not particularly limited, and for example, those having stereoregularity such as isotactic, heterotactic, syndiotactic, etc. can be used.
[0019] The (meth)acrylic resin composition used in the present invention may contain two or more (meth)acrylic resins (A), and preferably contains three (meth)acrylic resins (A) from the viewpoint of the balance between melt viscosity and mechanical properties. For example, the (meth)acrylic resin composition of the present invention preferably contains two (meth)acrylic resins (A-1) and (A-2) having different melt flow rates (MFR), more preferably contains three (meth)acrylic resins (A-1), (A-2) and (A-3) having different MFR, and particularly preferably consists of three (meth)acrylic resins (A-1), (A-2) and (A-3) having different MFR. By containing multiple types of resins (e.g., (A-1) and (A-2), or (A-1), (A-2) and (A-3)) in the (meth)acrylic resin (A) as described above, the effect on the resin of slight changes in conditions such as temperature in the film production process can be suppressed, making it less likely for protrusion defects to occur in the film, and is particularly effective in suppressing protrusion defects having a height of 1 μm or more.
[0020] [(Meth)acrylic resin (A-1)] The (meth)acrylic resin (A-1) mainly plays a role in maintaining high performance in heat resistance and mechanical properties of the obtained film while decreasing the complex viscosity of the (meth)acrylic resin composition. The weight average molecular weight of the (meth)acrylic resin (A-1) is preferably lower than the weight average molecular weight of the (meth)acrylic resin (A-3) described below. From the viewpoint of heat resistance and moldability of the film, the content of methyl methacrylate units in the (meth)acrylic resin (A-1) is preferably 85 to 97% by mass, more preferably 90 to 96.5% by mass, and even more preferably 94 to 96% by mass.
[0021] The weight average molecular weight of the (meth)acrylic resin (A-1) is preferably 67,000 to 92,000, more preferably 68,000 to 80,000, and even more preferably 70,000 to 75,000. When the weight average molecular weight of the (meth)acrylic resin (A-1) is 67,000 or more, the mechanical properties can be improved, and when it is 92,000 or less, an effect similar to that of a compatibilizer can be exhibited.
[0022] The (meth)acrylic resin (A-1) preferably has an MFR of more than 5 g / 10 min and less than 20 g / 10 min at a temperature of 230° C. and a load of 3.8 kg, more preferably 7 g / 10 min or more and 18 g / 10 min or less, and even more preferably 9 g / 10 min or more and 16 g / 10 min or less. When the (meth)acrylic resin (A-1) has an MFR of more than 5 g / 10 min, the melt viscosity of the (meth)acrylic resin composition used in the present invention can be reduced, and the productivity of the film can be improved. Also, when the MFR is less than 20 g / 10 min, the mechanical properties can be improved. As described in the Examples, the MFR can be measured under the above conditions in accordance with JIS K7210-1:2014.
[0023] From the viewpoint of heat resistance, the glass transition temperature (hereinafter sometimes referred to as Tg) of the (meth)acrylic resin (A-1) is preferably 90° C. or higher, more preferably 100° C. or higher, and even more preferably 110° C. or higher. The upper limit of Tg of the (meth)acrylic resin (A-1) is usually 140° C. The glass transition temperature in the present invention can be measured by the method described in the Examples.
[0024] The content of the (meth)acrylic resin (A-1) is preferably 15 to 98 parts by mass, more preferably 20 to 75 parts by mass, even more preferably 25 to 65 parts by mass, and particularly preferably 45 to 55 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin (A), from the viewpoints of the complex viscosity of the (meth)acrylic resin composition and the physical properties of a film obtained from the (meth)acrylic resin composition.
[0025] [(Meth)acrylic resin (A-2)] The (meth)acrylic resin (A-2) is added mainly to act as a compatibilizer for enhancing the dispersibility of the (meth)acrylic crosslinked rubber particles (B) in the (meth)acrylic resin composition, and for example, in the case of the above purpose, the content of the methyl methacrylate unit in the (meth)acrylic resin (A-2) is preferably between (including the same) the content of the methyl methacrylate unit in the (meth)acrylic resin (A-1) and the content of the methyl methacrylate unit in the thermoplastic polymer (II) constituting the outermost layer of the (meth)acrylic crosslinked rubber particles (B), which will be described later. From the viewpoint of the heat resistance and moldability of the film of the present invention, the content of the methyl methacrylate unit in the (meth)acrylic resin (A-2) is preferably 80 to 97% by mass, more preferably 84 to 94% by mass, and even more preferably 88 to 92% by mass. As the copolymerizable monomer other than methyl methacrylate, methyl acrylate is preferred from the viewpoint of heat resistance and thermal stability.
[0026] The weight average molecular weight of the (meth)acrylic resin (A-2) is preferably lower than the weight average molecular weight of the (meth)acrylic resin (A-1). The weight average molecular weight of the (meth)acrylic resin (A-2) is preferably 40,000 to 65,000, more preferably 45,000 to 63,000, and even more preferably 50,000 to 62,000. When the weight average molecular weight of the (meth)acrylic resin (A-2) is 40,000 or more, the mechanical properties can be improved, and when the weight average molecular weight is 65,000 or less, the (meth)acrylic resin (A-2) can play a role like a compatibilizer.
[0027] The (meth)acrylic resin (A-2) preferably has an MFR of 20 g / 10 min or more, more preferably 23 g / 10 min or more, and even more preferably 25 g / 10 min or more, at a temperature of 230° C. and a load of 3.8 kg. The (meth)acrylic resin (A-2) has an MFR of 20 g / 10 min or more, which can provide compatibility and a low viscosity effect for the composition. The upper limit is not particularly limited, but is preferably 100 g / 10 min.
[0028] From the viewpoint of heat resistance of the composition, the Tg of the (meth)acrylic resin (A-2) is preferably 80° C. or higher, more preferably 90° C. or higher, and even more preferably 100° C. or higher. The upper limit of the Tg of the (meth)acrylic resin (A-2) is usually 130° C.
[0029] The content of the (meth)acrylic resin (A-2) may be 2 to 85 parts by mass, preferably 2 to 15 parts by mass, more preferably 5 to 15 parts by mass, and even more preferably 10 to 15 parts by mass, per 100 parts by mass of the (meth)acrylic resin (A), from the viewpoints of the complex viscosity of the (meth)acrylic resin composition and the physical properties of the resulting film.
[0030] [(Meth)acrylic resin (A-3)] The content of methyl methacrylate units in the (meth)acrylic resin (A-3) is preferably 95% by mass or more, more preferably 97% by mass or more, and even more preferably 99% by mass or more. By having the content of methyl methacrylate units in the (meth)acrylic resin (A-3) of 95% by mass or more, heat resistance can be improved.
[0031] The weight average molecular weight of the (meth)acrylic resin (A-3) is preferably 92,500 to 150,000, more preferably 93,000 to 120,000, and even more preferably 94,000 to 100,000. When the weight average molecular weight of the (meth)acrylic resin (A-3) is 92,500 or more, the heat resistance and mechanical properties can be improved, and when it is 150,000 or less, the complex viscosity can be prevented from becoming too high, and the processability can be improved.
[0032] The (meth)acrylic resin (A-3) preferably has an MFR of 5 g / 10 min or less, more preferably 4 g / 10 min or less, and even more preferably 3 g / 10 min or less, at a temperature of 230° C. and a load of 3.8 kg. The (meth)acrylic resin (A-3) has an MFR of 5 g / 10 min or less, which can improve mechanical properties. The lower limit is not particularly limited, but is preferably 0.1 g / 10 min.
[0033] From the viewpoint of heat resistance, the Tg of the (meth)acrylic resin (A-3) is preferably 100° C. or higher, more preferably 105° C. or higher, and even more preferably 110° C. or higher. The upper limit of the Tg of the (meth)acrylic resin (A-3) is usually 140° C.
[0034] The content of the (meth)acrylic resin (A-3) may be 0 to 85 parts by mass, preferably 0 to 70 parts by mass, more preferably 20 to 65 parts by mass, and even more preferably 30 to 40 parts by mass, per 100 parts by mass of the (meth)acrylic resin (A), from the viewpoints of the complex viscosity of the (meth)acrylic resin composition and the physical properties of the resulting film.
[0035] The molecular weight distribution of the (meth)acrylic resin (A) is represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by GPC, and is preferably from 1.05 to 3, and more preferably from 1.3 to 2.5. When the (meth)acrylic resin (A) contains two or more types of (meth)acrylic resins (A), it is preferable that at least one type of (meth)acrylic resin (A) satisfies the above range, it is more preferable that two or more types of (meth)acrylic resins (A) satisfy the above range, and it is even more preferable that all of the (meth)acrylic resins (A) satisfy the above range. A molecular weight distribution of 1.05 or more can improve moldability, and a molecular weight distribution of 3 or less can improve physical properties such as creep characteristics. The weight average molecular weight (Mw) can be measured by the method described later in the Examples section, and the number average molecular weight (Mn) can be measured at the same time. The molecular weight distribution (Mw / Mn) of the (meth)acrylic resin (A) can be adjusted by the amounts of the polymerization initiator and the chain transfer agent, the temperature, and the like.
[0036] The method for producing the (meth)acrylic resin (A) is not particularly limited, and for example, it can be obtained by polymerizing a monomer mainly composed of methyl methacrylate, and can be produced by a bulk polymerization method, a solution polymerization method, a suspension polymerization method, an emulsion polymerization method, etc. Among these, either the bulk polymerization method or the solution polymerization method is preferable. Among these, the bulk polymerization method is preferable, and among the bulk polymerization methods, the continuous bulk polymerization method is preferable.
[0037] The content of the (meth)acrylic resin (A) in the (meth)acrylic resin composition is not particularly limited, but is preferably 60 to 95 mass%, more preferably 65 to 90 mass%, and even more preferably 70 to 85 mass%. By having the content of the (meth)acrylic resin (A) within the above range, a film with excellent strength can be obtained.
[0038] [(Meth)acrylic crosslinked rubber particles (B)] The (meth)acrylic resin composition used in the present invention preferably contains (meth)acrylic crosslinked rubber particles (B) from the viewpoint of mechanical properties such as improved toughness and impact resistance of the film. The (meth)acrylic crosslinked rubber particles (B) are rubber particles containing a polymer containing a structural unit derived from an acrylic acid alkyl ester (hereinafter, sometimes referred to as an acrylic acid alkyl ester unit), and may be particles made of a single polymer or particles in which polymers having different elastic moduli form at least two layers. The content of the acrylic acid alkyl ester unit in the (meth)acrylic crosslinked rubber particles (B) is preferably 20 to 98% by mass, more preferably 25 to 80% by mass, and even more preferably 30 to 60% by mass, from the viewpoint of the balance between impact resistance and dispersibility.
[0039] In addition, from the viewpoint of the impact resistance of the film of the present invention, the (meth)acrylic crosslinked rubber particles (B) are preferably core-shell type graft copolymers, which are crosslinked rubber particles having an outermost layer and an inner layer. Such crosslinked rubber particles are not particularly limited as long as they have an outermost layer and an inner layer, and can have various laminated structures such as, for example, two-layer polymer particles in which the core (inner layer) is a crosslinked rubber polymer (I) and the outer shell (outermost layer) is a thermoplastic polymer (II); three-layer polymer particles in which the core (inner layer) is a polymer (III) and the inner shell (inner layer) is a crosslinked rubber polymer (I) and the outer shell (outermost layer) is a thermoplastic polymer (II); four-layer polymer particles in which the core (inner layer) is a crosslinked rubber polymer (I) and the first inner shell (inner layer) is a polymer (III) and the second inner shell (inner layer) is a crosslinked rubber polymer (I) and the outer shell (outermost layer) is a thermoplastic polymer (II), but three-layer polymer particles are preferred. In the (meth)acrylic crosslinked rubber particles (B), when there is one crosslinked rubber layer, the crosslinked rubber layer alone or the crosslinked rubber layer and the layer inside it are collectively referred to as the "inner layer", and the layer outside the crosslinked rubber layer is referred to as the "outermost layer". On the other hand, when there are two or more crosslinked rubber layers, the outermost crosslinked rubber layer and the layer inside the crosslinked rubber layer are collectively referred to as the "inner layer", and the layer outside the crosslinked rubber layer is referred to as the "outermost layer". Hereinafter, the (meth)acrylic crosslinked rubber particles (B) will be described by taking three-layer polymer particles as an example.
[0040] The crosslinked rubber polymer (I) preferably contains 70 to 98 mass% of structural units derived from an acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms, more preferably 75 to 90 mass%, and even more preferably 80 to 85 mass%, based on the mass of the crosslinked rubber polymer (I). The above content makes it possible to obtain a flexible rubber material and effectively impart impact resistance. The crosslinked rubber polymer (I) preferably contains 2 to 30 mass%, more preferably 10 to 25 mass%, and even more preferably 15 to 20 mass%, of structural units derived from an aromatic vinyl monomer, based on the mass of the crosslinked rubber polymer (I). The above content allows the refractive index of the crosslinked rubber polymer (I) to be adjusted to match that of the (meth)acrylic resin (A), and a (meth)acrylic resin composition having high transparency can be obtained. The crosslinked rubber polymer (I) preferably contains 1 to 5 mass % of structural units derived from a crosslinkable monomer, more preferably 1 to 3 mass %, based on the mass of the crosslinked rubber polymer (I). The above content provides an appropriate crosslink density, and the rubber material behaves well.
[0041] The thermoplastic polymer (II) preferably contains 80 to 100 mass % of methyl methacrylate units, more preferably 85 to 97 mass %, and even more preferably 90 to 96 mass %, based on the mass of the thermoplastic polymer (II). The above content improves compatibility with the (meth)acrylic resin (A). The thermoplastic polymer (II) preferably contains 0 to 20 mass %, more preferably 3 to 15 mass %, and even more preferably 4 to 10 mass % of structural units derived from an alkyl acrylate ester having an alkyl group having 1 to 8 carbon atoms relative to the mass of the thermoplastic polymer (II). The above content improves compatibility with the (meth)acrylic resin (A).
[0042] The polymer (III) preferably contains 80 to 99.95% by mass, more preferably 85 to 98% by mass, and even more preferably 90 to 96% by mass of methyl methacrylate units relative to the mass of the polymer (III). The above content is preferable because it provides good hardness. The polymer (III) preferably contains 0 to 19.95% by mass of structural units derived from an acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms and 0.05 to 2% by mass of a crosslinkable monomer, more preferably 2 to 15% by mass of structural units derived from an acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms and 0.05 to 1.5% by mass of structural units derived from a crosslinkable monomer, and even more preferably 4 to 10% by mass of structural units derived from an acrylic acid alkyl ester monomer having an alkyl group with 1 to 8 carbon atoms and 0.1 to 1% by mass of structural units derived from a crosslinkable monomer, relative to the mass of the polymer (III). The above contents provide good hardness.
[0043] The content of each of the monomers is calculated for each layer. For example, in a four-layer polymer particle, when the core (inner layer) and the second inner shell (inner layer) are both composed of the crosslinked rubber polymer (I), the content of the structural unit derived from each monomer is calculated separately for the core (inner layer) and the second inner shell (inner layer).
[0044] From the viewpoint of transparency of the (meth)acrylic crosslinked rubber particles (B), it is preferable to select the polymers contained in each layer so that the difference in refractive index between adjacent layers is preferably less than 0.005, more preferably less than 0.004, and even more preferably less than 0.003.
[0045] The mass ratio of the inner layer to the outermost layer (inner layer / outermost layer) in the (meth)acrylic crosslinked rubber particles (B) is preferably 30 / 70 to 95 / 5, and more preferably 50 / 50 to 90 / 10. In the inner layer, the ratio of the layer containing the crosslinked rubber polymer (I) is preferably 20 to 70 mass %, more preferably 30 to 50 mass %. When the inner layer has two or more crosslinked rubber layers, the ratio of the layer containing the crosslinked rubber polymer (I) in the inner layer is a value calculated based on the total amount of each layer containing the crosslinked rubber polymer (I).
[0046] The method for producing the (meth)acrylic crosslinked rubber particles (B) is not particularly limited, and can be carried out by known methods, but emulsion polymerization method is preferred.Specifically, for example, the monomer constituting the core (inner layer) is emulsion-polymerized to obtain seed particles, and the monomers constituting each layer are successively added in the presence of this seed particle, and polymerization is carried out successively up to the outermost layer, thereby obtaining the particles.
[0047] Examples of emulsifiers used in emulsion polymerization include anionic emulsifiers such as dialkyl sulfosuccinates (e.g., sodium dioctyl sulfosuccinate, sodium dilauryl sulfosuccinate, etc.), alkyl benzene sulfonates (e.g., sodium dodecyl benzene sulfonate, etc.), and alkyl sulfates (e.g., sodium dodecyl sulfate, etc.); nonionic emulsifiers such as polyoxyethylene alkyl ethers and polyoxyethylene nonyl phenyl ethers; nonionic and anionic emulsifiers such as polyoxyethylene nonyl phenyl ether sulfates (e.g., sodium polyoxyethylene nonyl phenyl ether sulfate, etc.), polyoxyethylene alkyl ether sulfates (e.g., sodium polyoxyethylene alkyl ether sulfate, etc.), and alkyl ether carboxylates (e.g., sodium polyoxyethylene tridecyl ether acetate, etc.). These may be used alone or in combination of two or more. In addition, the average number of repeating ethylene oxide units in the example compounds of the nonionic emulsifiers and nonionic / anionic emulsifiers is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less, in order to prevent the foaming property of the emulsifier from becoming extremely high.
[0048] The polymerization initiator used in the emulsion polymerization is not particularly limited, and examples thereof include persulfate-based initiators such as potassium persulfate and ammonium persulfate; and redox-based initiators such as persulfoxylate / organic peroxide and persulfate / sulfite.
[0049] The (meth)acrylic crosslinked rubber particles (B) can be separated and obtained from the polymer latex obtained by emulsion polymerization by known methods such as salting-out coagulation, freeze-coagulation, and spray drying. Among these, the salting-out coagulation and freeze-coagulation methods are preferred, and the freeze-coagulation method is more preferred, since impurities can be easily removed by washing with water. The freeze-coagulation method does not use a flocculant, so a film with excellent water resistance is easily obtained. In order to remove foreign matter mixed into the polymer latex before the coagulation step, it is preferable to filter the polymer latex with a wire mesh having an opening of 50 μm or less. From the viewpoint of facilitating uniform dispersion in melt-kneading with the (meth)acrylic resin (A), it is preferable to take out the (meth)acrylic crosslinked rubber particles (B) as aggregated particles of 1,000 μm or less, and more preferably as aggregated particles of 500 μm or less. The form of the aggregated particles is not particularly limited, and may be, for example, a pellet-like form in which the particles are fused to each other at the outermost layer portion, or a powder-like or granular powder.
[0050] The average particle size of the (meth)acrylic crosslinked rubber particles (B) is preferably 0.05 to 1 μm, more preferably 0.07 to 0.5 μm, even more preferably 0.1 to 0.4 μm, and particularly preferably 0.15 to 0.3 μm. By using the (meth)acrylic crosslinked rubber particles (B) having an average particle size within the above range, toughness can be imparted to the film with a small amount of incorporation, and the possibility of impairing rigidity and surface hardness can be suppressed. The average particle size in this specification is an arithmetic mean value in a volume-based particle size distribution measured by a light scattering method, and specifically, can be determined by the method described in the Examples.
[0051] The content of the (meth)acrylic crosslinked rubber particles (B) in the (meth)acrylic resin composition is not particularly limited, but is preferably 5 to 40 mass%, more preferably 10 to 35 mass%, and even more preferably 15 to 30 mass%. By having the content of the (meth)acrylic crosslinked rubber particles (B) within the above range, a (meth)acrylic resin composition having an excellent balance between hardness and impact resistance can be obtained. In addition, when the (meth)acrylic resin (A) contains a plurality of types of resins (e.g., (A-1) and (A-2), or (A-1), (A-2) and (A-3)), the dispersibility of the (meth)acrylic crosslinked rubber particles (B) in the (meth)acrylic resin composition is further improved, and thickness unevenness due to aggregation of the (meth)acrylic rubber particles (B) is less likely to occur.
[0052] [Other additives] To the (meth)acrylic resin composition used in the present invention, various additives, such as a polymer processing aid (C), an ultraviolet absorber (D), an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a colorant, an impact resistance aid, etc., may be added as necessary within a range that does not impair the effects of the present invention. From the viewpoint of the mechanical properties and surface hardness of the (meth)acrylic resin film of the present invention, it is preferable not to add a large amount of a foaming agent, a filler, a matting agent, a light diffusing agent, a softener, or a plasticizer.
[0053] [Polymer processing aids (C)] The (meth)acrylic resin composition used in the present invention preferably further contains a polymer processing aid (C) as the other additives described above. The polymer processing aid (C) is a compound that is effective in terms of thickness accuracy, film formation stability, etc., when molding the (meth)acrylic resin composition. As the polymer processing aid (C), a methacrylic resin having an ultra-high molecular weight (weight average molecular weight of 500,000 or more) mainly composed of methyl methacrylate units (e.g., containing 50% by mass or more) that can be produced by emulsion polymerization can be used.
[0054] Commercially available products can be used as the polymer processing aid (C), and specific examples include "Kane Ace (registered trademark)" PA series (manufactured by Kaneka Corporation), "Metablen (registered trademark)" P series (manufactured by Mitsubishi Rayon Co., Ltd.), "Paraloid (registered trademark)" K series (manufactured by Dow Co., Ltd.), etc. Among them, "Paraloid (registered trademark)" K125P is preferred from the viewpoint of compatibility with resins.
[0055] The content of the polymer processing aid (C) in the (meth)acrylic resin composition is preferably 0.1 to 3.0% by mass. The content of the polymer processing aid (C) varies depending on the application, but from the viewpoint of further reducing fisheye defects and improving thickness accuracy during film production, it is more preferably 1.0% by mass or more, and even more preferably 1.3% by mass or more. In addition, from the viewpoints of reducing costs and reducing melt viscosity, it is more preferably 2.5% by mass or less, and even more preferably 2.0% by mass or less. In the present invention, the polymer processing aid (C) is not included in the (meth)acrylic resin (A) and the (meth)acrylic crosslinked rubber particles (B).
[0056] [Ultraviolet absorber (D)] The (meth)acrylic resin composition used in the present invention preferably further contains an ultraviolet absorber (D) from the viewpoint of blocking ultraviolet rays and improving weather resistance. The ultraviolet absorber (D) is a compound capable of absorbing ultraviolet rays, and mainly has the function of converting light energy into heat energy.
[0057] Examples of the ultraviolet absorber (D) include benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalic anilides, malonic acid esters, and formamidines. These may be used alone or in combination of two or more. Among these, benzotriazoles and triazines are preferred because they have a high ability to inhibit resin deterioration when irradiated with ultraviolet light and are highly compatible with resins.
[0058] Benzotriazole ultraviolet absorbers are highly effective in suppressing the deterioration of optical properties such as coloration caused by ultraviolet irradiation. Examples of benzotriazole ultraviolet absorbers include 2-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "Tinuvin (registered trademark)" 329), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (BASF's "Tinuvin (registered trademark)" 234), and 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-tert-octylphenol] (ADEKA CORPORATION's "ADEKA STAB (registered trademark)" LA-31). Among these, from the viewpoint of compatibility with the (meth)acrylic resin composition, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol] ("ADEKA STAB (registered trademark)" LA-31, manufactured by ADEKA CORPORATION) is preferred.
[0059] Examples of the triazine ultraviolet absorbers include hydroxyphenyltriazine ultraviolet absorbers. More specifically, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-butyloxyphenyl)-1,3,5-triazine ("Tinuvin (registered trademark)" 460, manufactured by BASF), 2-(4-(2-hydroxy-3-(2-ethylhexyloxy)propyloxy)-2-hydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine ("Tinuvin (registered trademark)" 405, manufactured by BASF), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine ("Tinuvin (registered trademark)" 479, manufactured by BASF), Tinuvin (registered trademark) 1477, 400, 477, 1600; 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(2-(2-ethylhexanoyloxy)ethoxy)phenol ("ADEKA STAB (registered trademark)" LA-46 manufactured by ADEKA Corporation), 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenoxy)-1,3,5-triazine ("ADEKA STAB (registered trademark)" manufactured by ADEKA Corporation) (registered trademark)" LA-F70; 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and the like.
[0060] The content of the ultraviolet absorber (D) in the (meth)acrylic resin composition is preferably 0.1 to 4.0% by mass. The content of the ultraviolet absorber (D) varies depending on the type and application of the ultraviolet absorber (D), but is more preferably 0.2% by mass or more, and even more preferably 0.4% by mass or more. From the viewpoint of cost reduction, it is more preferably 3.8% by mass or less, and even more preferably 3.5% by mass or less.
[0061] [Other polymers] The (meth)acrylic resin composition used in the present invention may further contain other polymers other than the (meth)acrylic resin (A), the (meth)acrylic crosslinked rubber particles (B), and the polymer processing aid (C), which may be a polymer, within a range that does not impair the effects of the present invention. Examples of other polymers include polyolefin resins such as polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; ethylene-based ionomers; polystyrene, styrene-maleic anhydride copolymers, high-impact polystyrene, acrylonitrile copolymer-styrene (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylonitrile-ethylene propylene-styrene copolymer (AES resin), acrylonitrile-acrylic elastomer-styrene copolymer (AAS resin), acrylonitrile-chlorinated polyethylene-styrene copolymer (ACS resin), and methyl methacrylate-butadiene-styrene copolymer (MBS resin); methyl methacrylate-styrene copolymer; polyethylene terephthalate, polybutylene terephthalate, and other styrene-based resins. Examples of suitable thermoplastic elastomers include polyester resins such as polystyrene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, polyacetal, polyvinylidene fluoride, polyurethane, modified polyphenylene ether, polyphenylene sulfide, and silicone-modified resins; acrylic rubber, silicone rubber; styrene-ethylene / propylene-styrene copolymer (SEPS), styrene-ethylene / butylene-styrene copolymer (SEBS), and styrene-isoprene-styrene copolymer (SIS); and olefin-based rubbers such as isoprene rubber (IR), ethylene-propylene copolymer (EPR), and ethylene-propylene-diene terpolymer (EPDM).
[0062] The (meth)acrylic resin composition used in the present invention contains a (meth)acrylic resin (A) and (meth)acrylic crosslinked rubber particles (B), and has a complex viscosity of preferably 500 to 1300 Pa·s, more preferably 600 to 1200 Pa·s, and even more preferably 700 to 1200 Pa·s, measured under conditions of 265°C, 10 rad / sec, and 1% strain. When the complex viscosity is 500 Pa·s or more, the mechanical properties of the film can be kept high, and when the complex viscosity is 1300 Pa·s or less, a high discharge rate (e.g., 150 to 500 kg / h) can be achieved, thereby increasing productivity. The complex viscosity can be adjusted by the composition of the (meth)acrylic resin (A), and when the (meth)acrylic resin composition contains two or more kinds of (meth)acrylic resins (A), the weight average molecular weight of each of them, the composition ratio, the mass ratio of the (meth)acrylic resin (A) to the (meth)acrylic crosslinked rubber particles (B), the content of other additives, etc. Specifically, the complex viscosity can be measured by the method described in the Examples.
[0063] The method for preparing the (meth)acrylic resin composition used in the present invention is not particularly limited, but a method of mixing by melt kneading is preferred. Specifically, a method is generally used in which the (meth)acrylic resin (A), the (meth)acrylic crosslinked rubber particles (B), and other additives such as the polymer processing aid (C) and the ultraviolet absorber (D) as required, and other polymers are dry blended in advance and melt kneaded. The mixing operation can be performed using a known mixing or kneading device such as a kneader-ruder, an extruder, a mixing roll, or a Banbury mixer. In particular, from the viewpoint of kneading property and productivity, it is preferable to use a twin-screw extruder. The shear rate during melt kneading is preferably 10 to 1,000 / sec. The temperature during mixing and kneading is usually 150 to 320°C, and preferably 200 to 300°C. When melt kneading using a twin-screw extruder, it is preferable to use a vent and perform melt kneading under reduced pressure or under a nitrogen gas flow from the viewpoint of suppressing coloring. The (meth)acrylic resin composition obtained in this manner can be in the form of, for example, pellets.
[0064] The lower limit of the total content of the (meth)acrylic resin (A) and the (meth)acrylic crosslinked rubber particles (B) in the (meth)acrylic resin composition used in the present invention is usually 50% by mass, preferably 70% by mass, more preferably 80% by mass, and even more preferably 85% by mass. The upper limit may be preferably 99.5% by mass, 99% by mass, or 98% by mass.
[0065] <Method of Manufacturing (Meth)acrylic Resin Film> The method for producing the (meth)acrylic resin film of the present invention can be carried out using known methods such as a T-die method, an inflation method, a melt casting method, and a calendar method. Among them, the T-die method is preferred from the viewpoint of obtaining a film with good surface smoothness and low haze, and it is more preferred to have a melt extrusion step of melt-extruding the (meth)acrylic resin composition from a T-die and a holding step of holding the melt extruded molten material between a pair of mirror rolls or mirror belts. The rolls or belts used in this case are preferably made of metal. In addition, the pair of mirror rolls or mirror belts that hold the molten material are preferably a pair of mirror rolls from the viewpoint of producing a film with good surface properties, and the pair of mirror rolls are more preferably a combination of a mirror elastic roll and a mirror rigid roll from the viewpoint of obtaining a film with good surface properties and low haze.
[0066] The thickness of at least one of the outer cylinders of the pair of mirror rolls and the thickness of at least one of the pair of mirror belts are preferably more than 3 mm, more preferably 6 mm or more. When the pair of mirror rolls is a combination of a mirror elastic roll and a mirror rigid roll, from the viewpoint of exerting the effects of the present invention, the thickness of the outer cylinder of the mirror elastic roll is preferably more than 3 mm, more preferably 6 mm or more. The upper limit of the thickness of the outer cylinder of the mirror elastic roll is not particularly limited as long as it has elastic performance, but is preferably 20 mm, more preferably 15 mm. By making the thickness of the outer cylinder of the mirror roll and the thickness of the mirror belt more than 3 mm and using the above-mentioned (meth)acrylic resin composition, it becomes easier to suppress the number of protruding defects having a height of 1 μm or more, and by using the (meth)acrylic resin film obtained in this way, it becomes easier to produce a laminated film with fewer harmful defects.
[0067] When forming a film by contacting both sides of the extruded molten material (molten resin) with mirror surfaces, it is preferable to pressurize and sandwich the molten material (the molten resin may be in the form of a film) between mirror rolls or mirror belts. The higher the sandwiching pressure by the mirror rolls or mirror belts, the better, and the linear pressure is preferably 15 N / mm or more, and more preferably 20 N / mm or more. There is no particular limit to the upper limit of the linear pressure, but it is usually 50 N / mm. By having a linear pressure of 15 N / mm or more, the number of protruding defects having a height of 1 μm or more is reduced to 1 per 10 m. 2 When the film is used to produce a laminate film such as a polarizing plate, practical defects can be reduced.
[0068] The surface temperatures of the pair of mirror-finished rolls or mirror-finished belts that sandwich the molten material are both preferably 60° C. or higher, and more preferably 70° C. or higher. Also, they are preferably 130° C. or lower, and more preferably 100° C. or lower. If the surface temperatures of the mirror-finished rolls or mirror-finished belts that sandwich the molten material are both less than 60° C., it tends to be difficult to suppress the number of protruding defects having a height of 1 μm or more, and the number of protruding defects having a height of 1 μm or more per 10 m tends to be 1. 2 The film is likely to have the above-mentioned properties, and when the film is used to manufacture a laminate film such as a polarizing plate, there is a risk of many practical defects. In addition, there is a risk that it is difficult to obtain the effect of reducing haze. On the other hand, by keeping the surface temperature at 130°C or less, the film and the mirror-finished roll or belt do not come into too close contact with each other, and surface roughness and lateral wrinkles are suppressed when the film is peeled off from the mirror-finished roll or belt, and the appearance of the film tends to be good.
[0069] From the viewpoint of a balance between productivity and production of a high-quality film, the take-up speed is preferably from 10 to 50 m / min, and more preferably from 15 to 35 m / min.
[0070] In the case of a manufacturing method using the T-die method, an extruder-type melt extrusion device equipped with a single-screw or twin-screw extrusion screw can be used. The melt extrusion temperature for manufacturing the film of the present invention is preferably 230° C. or higher, more preferably 240° C. or higher. The melt extrusion temperature is preferably 290° C. or lower, more preferably 280° C. or lower. When using a melt extrusion device, melt extrusion is performed under reduced pressure using a vent from the viewpoint of suppressing coloration, a gear pump is attached from the viewpoint of manufacturing a film with a uniform thickness, and further, protruding defects having a height of 1 μm or more are reduced to 1 / 10 m. 2 In order to keep the melt extrusion temperature below 100° C., it is preferable to perform the melt extrusion using a polymer filter. Furthermore, in order to suppress oxidative deterioration, it is preferable to perform the melt extrusion under a nitrogen gas flow.
[0071] When the (meth)acrylic resin film of the present invention is produced using an extrusion device equipped with a vent, a gear pump, a polymer filter and a T-die in this order, it is preferable to control the temperature from the vent to the T-die, including the gear pump and the polymer filter, in the range of 230 to 290° C. By producing the film within such a temperature range, deterioration is reduced and the number of protruding defects having a height of 1 μm or more is reduced to 1 per 10 m. 2 Therefore, it is easy to obtain a film having excellent mechanical properties and optical properties.
[0072] In the method for producing the (meth)acrylic resin film of the present invention, it is very important to use the above-mentioned (meth)acrylic resin composition and to suppress the variation in temperature (temperature of the molten resin) in the width direction. Variation in the temperature of the molten resin in the width direction causes variation in the linear pressure in the width direction, and the variation in the linear pressure may result in a problem with the smoothness of the surface, particularly in the case where locally gelled resin is present, in which case the surface cannot be made sufficiently smooth, which may lead to protruding defects. In the method for producing a (meth)acrylic resin film of the present invention, the temperature of the die end is set to be 1° C. or more higher than that of the die center, thereby suppressing the variation in linear pressure and suppressing the number of protruding defects, particularly protruding defects having a height of 1 μm or more, at any position in the width direction. 2 It is now easier to obtain films of less than this size. The temperature of the die edge is preferably at least 1° C. higher than that of the die center, more preferably at least 3° C. higher, and even more preferably at least 5° C. The upper limit of the die edge temperature is usually 15° C. higher than the temperature of the die center. The above conditions are effective in the production of films having a width perpendicular to the machine direction of the film of, for example, 1 m or more, more effective in the case of films of 1.3 m or more, even more effective in the case of films of 1.5 m or more, and particularly effective in the case of films of 2 m or more.
[0073] Furthermore, in the method for producing a (meth)acrylic resin film of the present invention, it is preferable to use a crown roll as the mirror roll that presses the extruded molten resin. At least one of the pair of mirror rolls may be a crown roll, and in the case of a combination of a mirror elastic roll and a mirror rigid roll, it is preferable that the mirror elastic roll is a crown roll. By using a crown roll, the number of protruding defects with a height of 1 μm or more is reduced to 1 per 10 m. 2 It is now easier to obtain films of less than this size.
[0074] The thickness of the (meth)acrylic resin film of the present invention is preferably 20 μm or more, and preferably 500 μm or less. By having a thickness of 20 μm or more, the film becomes stiff and the handling property is improved, and by having a thickness of 500 μm or less, the secondary processability such as lamination property, handling property, cutting property, punching property, etc. is improved. The thickness of the (meth)acrylic resin film of the present invention is more preferably 30 μm or more, and even more preferably 50 μm or more. Also, it is more preferably 300 μm or less, even more preferably 200 μm or less, and particularly preferably 100 μm or less. The thickness of the film can be measured with a micrometer, specifically, by the method described in the examples. The effects of the present invention are particularly easily obtained in a film having a thickness within the above range.
[0075] The (meth)acrylic resin film of the present invention may be colored. Examples of the coloring method include a method in which a pigment or dye is added to the (meth)acrylic resin composition itself before it is made into a film, and a dyeing method in which the (meth)acrylic resin film is immersed in a liquid in which a dye is dispersed to color it, but the coloring method is not particularly limited to these.
[0076] The (meth)acrylic resin film of the present invention may be printed on at least one surface. Patterns such as pictures, characters, and figures, and colors can be imparted by printing. The patterns may be chromatic or achromatic.
[0077] The (meth)acrylic resin film of the present invention may be used alone, may be used as an inner layer or a part thereof of a laminate film, or may be used as the outermost layer of a laminate film. From the viewpoint of the design of the film, the other resin used in the laminate film is preferably a transparent resin such as a methacrylic resin. From the viewpoint of the film being less susceptible to scratches and the design lasting for a long time, the film forming the outermost layer is preferably one having high surface hardness and weather resistance, and is preferably the (meth)acrylic resin film of the present invention. The surface of the laminated film may further include a functional layer, such as a hard coat layer, an antiglare layer, an antireflection layer, an antisticking layer, a diffusion layer, an antiglare layer, an antistatic layer, an antifouling layer, and a slippery layer containing fine particles.
[0078] The (meth)acrylic resin film of the present invention has high productivity and has a protruding defect having a height of 1 μm or more of 1 / 10 m. 2 The film has a thickness of less than 100 nm, and when a laminate film such as a polarizing plate is manufactured using the film, the number of practical defects can be reduced. Taking advantage of such excellent characteristics, the (meth)acrylic resin film of the present invention is suitably used as a decorative film, an optical film, and the like. A specific example of an optical film is a polarizer protective film. The polarizer protective film can be used in a polarizing plate containing the film, and further in an image display device such as a liquid crystal display device, an organic EL display device, or a PDP containing at least one of the polarizing plates. The (meth)acrylic resin film of the present invention can be suitably used as an optical base film such as a light guide film, a moth-eye film, a Fresnel lens, a lenticular lens, a front film for various displays, a diffusion film, a glass shatterproof film, a liquid crystal ASF film, a transparent conductive film, a heat shielding film, and various barrier films.
[0079] More specifically, the (meth)acrylic resin film of the present invention has low haze, good optical properties, and high surface hardness, and furthermore, when the film is used to manufacture a laminate film such as a polarizing plate, the number of harmful defects can be reduced. By utilizing these properties, the film can be used in a variety of applications, including molded products that require design or molded products that require high optical properties, such as signboard parts such as advertising towers, stand signs, side signs, transom signs, and rooftop signs; display parts such as showcases, partition boards, and store displays; lighting parts such as fluorescent light covers, mood lighting covers, lampshades, lighted ceilings, lighted walls, and chandeliers; interior parts such as furniture, pendants, and mirrors; architectural parts such as doors, domes, safety window glass, partitions, staircase wainscoting, balcony wainscoting, and roofs of leisure buildings; aircraft windshields, pilot visors, etc. Parts related to transportation vehicles such as motorcycles, motorboats, sunshades for buses, side visors for automobiles, rear visors, head wings, headlight covers, automobile interior parts, automobile exterior parts such as bumpers; electronic equipment parts such as audiovisual nameplates, stereo covers, television protective masks, vending machines, mobile phones, personal computers; medical equipment parts such as incubators and X-ray parts; equipment parts such as machine covers, instrument covers, laboratory equipment, rulers, dials, observation windows; traffic-related parts such as road signs, guide boards, convex mirrors, soundproof walls; and decorative and protective films for the surfaces of greenhouses, large aquariums, box aquariums, bathroom parts, clock panels, bathtubs, sanitary products, desk mats, game parts, toys, face protection masks during welding, etc., wallpaper, marking films, etc. EXAMPLES
[0080] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the following examples. The present invention includes all aspects in which the above-mentioned technical features such as characteristic values, forms, manufacturing methods, and uses are combined in any manner. The physical properties in the examples and comparative examples were measured by the following methods.
[0081] (Weight average molecular weight (Mw), number average molecular weight (Mn)) The weight average molecular weight (Mw) and number average molecular weight (Mn) were determined by GPC (gel permeation chromatography) in terms of standard polystyrene. The molecular weight distribution (Mw / Mn) was calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) values. The measuring device and conditions are as follows: · Apparatus: Tosoh Corporation GPC device "HLC-8320" Separation column: Tosoh Corporation's "TSKgel SuperMultipore HZM-M" and "SuperHZ4000" are directly connected. Detector: Tosoh Corporation "RI-8020" Eluent: Tetrahydrofuran ·Eluent flow rate: 0.35mL / min Sample concentration: 8mg / 10mL Column temperature: 40℃
[0082] (Methyl methacrylate unit content (%)) 1 g of resin pellets was dissolved in 40 mL of dichloromethane. 25 μL of the resulting solution was collected on a platinum board. Dichloromethane was removed, and measurements were performed using pyrolysis gas chromatography under the following conditions. The proportion of methyl methacrylate units was calculated based on the measurement results. Equipment: Shimadzu GC-14A ·Pyrolysis furnace temperature: 500℃ Column: SGE BPX-5 Temperature conditions: 40°C for 5 minutes, then increase to 280°C at 5°C / min.
[0083] (Glass transition temperature (Tg)) The glass transition temperature was measured according to JIS K7121:2012. Using a differential scanning calorimeter (Shimadzu Corporation, "DSC-50"), the sample was heated to 230°C, cooled to room temperature (30°C or less), and then heated again from room temperature to 230°C at a heating rate of 10°C / min to measure the DSC curve. The midpoint glass transition temperature determined from the obtained DSC curve was taken as the glass transition temperature.
[0084] (Complex viscosity) Using a hydraulic molding machine (manufactured by Toho Machinery Co., Ltd.), a sheet having a thickness of 1 mm was produced from the (meth)acrylic resin composition at a set temperature of 250° C. The storage modulus (G') and loss modulus (G'') of the obtained sheet were measured under the following conditions, and the complex viscosity at 10 rad / sec was calculated. Measurement device: Dynamic viscoelasticity measuring device ARES (manufactured by TA Instruments) Measurement tool: Parallel plates with a diameter of 8 mm on both sides, with a gap of 1 mm between the top and bottom Measurement conditions: 265℃, angular frequency (ω) 0.1~100rad / sec, strain 1% ·Complex viscosity calculation method: η*={(G'(ω))2+(G''(ω))2}1 / 2 / ω (In the formula, G' is the storage modulus, and G is the loss modulus.)
[0085] (Melt Flow Rate: MFR) The melt flow rate was measured at 230°C under a load of 3.8 kg in accordance with JIS K7210-1:2014.
[0086] (Average particle size) The average particle diameter was measured by diluting the latex containing the sample particles 200 times with water and analyzing the diluted solution at 25° C. using a laser diffraction scattering type particle size distribution measuring device (manufactured by Horiba, Ltd., device name "LA-950V2") In this case, the absolute refractive indexes of the (meth)acrylic crosslinked rubber particles (B) and water were set to 1.4900 and 1.3333, respectively.
[0087] (Thickness) The thickness of the film produced in each Example or Comparative Example was measured at the center and 100 mm from both ends with a micrometer (manufactured by Mitutoyo Corporation, model number: MDH-25), and the average value was regarded as the film thickness.
[0088] (Haze) The films produced in each of the Examples and Comparative Examples were cut into test pieces of 50 mm x 50 mm, and the haze was measured at 23°C in accordance with JIS K7136:2000.
[0089] (Pencil hardness) The films produced in each Example or Comparative Example were cut into test pieces measuring 10 cm x 10 cm, and the pencil hardness of both sides of the film was measured in accordance with JIS-K5600-5-4:1999. The higher pencil hardness was recorded as the pencil hardness of the film.
[0090] (Fisheye defect) The films produced in each Example or Comparative Example were cut into a size of 1.5 m wide x 0.67 m long, placed on black flannel cloth, and visually inspected for defects under fluorescent lighting. Of the defects detected, those for which the size of the fisheye nucleus could be identified (colored fisheye defects, transfer defects with clearly defined outlines) were checked for their size using a scale loupe, and the number of foreign objects with a diameter of 50 μm or more was counted. In addition, defects that were visible to the naked eye as Newton rings but could not be seen with the scale loupe were all counted as the number of foreign objects. This inspection was carried out at 10 different locations (a total of 10 m 2 ), and the total was taken as the number of fisheye defects.
[0091] (Protruding defects with a height of 1 μm or more) Fisheye defect detection (total 10m 2 The defective areas obtained by the measurement (measurement of 10 min) were observed with a laser microscope (Olympus Corporation, model number: OLS4100, magnification: 400x), the shape of each defective area (whether it was a protrusion or not) and its protruding height above the surface were measured, and the number of protrusion-like defects with a height of 1 μm or more was calculated.
[0092] (Actual damage and shortcomings) The film on which the fisheye defects had been measured was attached to a polarizer using a UV adhesive to create a polarizing plate (laminated film), and the number of visible defects was counted, which was taken as the number of actual harmful defects.
[0093] [Production Example 1: Production of (meth)acrylic resin (A-1)] To 95 parts by mass of methyl methacrylate and 5 parts by mass of methyl acrylate, 0.1 part by mass of a polymerization initiator (2,2'-azobis(2-methylpropionitrile), hydrogen abstraction ability: 1%, 1-hour half-life temperature: 83°C) and 0.27 part by mass of a chain transfer agent (n-octyl mercaptan) were added and dissolved to obtain a raw material liquid. A mixture was obtained by mixing 100 parts by mass of ion-exchanged water, 0.03 parts by mass of sodium sulfate, and 0.45 parts by mass of a suspension dispersant. 420 parts by mass of the mixture and 210 parts by mass of the raw material liquid were charged into a pressure-resistant polymerization tank, and the temperature was raised to 70°C while stirring under a nitrogen atmosphere to start the polymerization reaction. After 3 hours had elapsed since the start of the polymerization reaction, the temperature was raised to 90°C, and stirring was continued for 1 hour to obtain a liquid in which a bead-like copolymer was dispersed. Although some polymer adhered to the walls of the polymerization tank or the stirring blades, there was no foaming, and the polymerization reaction proceeded smoothly. The obtained copolymer dispersion was washed with an appropriate amount of ion-exchanged water, and the bead-like copolymer was taken out using a bucket centrifuge and dried for 12 hours in a hot air dryer at 80°C to obtain bead-like (meth)acrylic resin (A-1). The obtained (meth)acrylic resin (A-1) had a methyl methacrylate unit content of 95 mass%, a methyl acrylate unit content of 5 mass%, a weight average molecular weight (Mw) of 73,000, a molecular weight distribution (Mw / Mn) of 2.0, an MFR of 10.2 g / 10 min, and a Tg of 115°C.
[0094] [Production Example 2: Production of (meth)acrylic resin (A-2)] A (meth)acrylic resin (A-2) was obtained in the same manner as in Production Example 1, except that the monomers used were changed to 90 parts by mass of methyl methacrylate and 10 parts by mass of methyl acrylate, and the amount of the chain transfer agent was changed to 0.39 parts by mass. The obtained (meth)acrylic resin (A-2) had a methyl methacrylate unit content of 90 mass%, a methyl acrylate unit content of 10 mass%, a weight average molecular weight (Mw) of 60,000, a molecular weight distribution (Mw / Mn) of 2.1, an MFR of 30.0 g / 10 min, and a Tg of 110°C.
[0095] [Production Example 3: Production of (meth)acrylic resin (A-3)] A (meth)acrylic resin (A-3) was obtained in the same manner as in Production Example 1, except that the monomers used were changed to 99 parts by mass of methyl methacrylate and 1 part by mass of methyl acrylate, and the amount of the chain transfer agent was changed to 0.24 parts by mass. The obtained (meth)acrylic resin (A-3) had a methyl methacrylate unit content of 99 mass%, a methyl acrylate unit content of 1 mass%, a weight average molecular weight (Mw) of 95,000, a molecular weight distribution (Mw / Mn) of 2.0, an MFR of 2.4 g / 10 min, and a Tg of 119°C.
[0096] [Production Example 4: Production of (meth)acrylic crosslinked rubber particles (B)] (1) In a reactor equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a monomer inlet tube and a reflux condenser, 1050 parts by mass of ion-exchanged water, 0.3 parts by mass of sodium polyoxyethylene tridecyl ether acetate and 0.7 parts by mass of sodium carbonate were charged, and the inside of the reactor was fully replaced with nitrogen gas. The inside temperature was then set to 80°C. 0.25 parts by mass of potassium persulfate was added thereto and stirred for 5 minutes. 245 parts by mass of a monomer mixture consisting of 95.4% by mass of methyl methacrylate, 4.4% by mass of methyl acrylate and 0.2% by mass of allyl methacrylate was continuously dropped into the mixture over a period of 60 minutes. After the dropwise addition, the polymerization reaction was continued for another 30 minutes so that the polymerization conversion rate was 98% or more. (2) Next, 0.32 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 315 parts by mass of a monomer mixture consisting of 80.5% by mass of butyl acrylate, 17.5% by mass of styrene, and 2% by mass of allyl methacrylate was continuously added dropwise over 60 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 30 minutes so that the polymerization conversion rate was 98% or more. (3) Next, 0.14 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 140 parts by mass of a monomer mixture consisting of 95.2% by mass of methyl methacrylate, 4.4% by mass of methyl acrylate, and 0.4% by mass of n-octyl mercaptan was continuously added dropwise over 30 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 60 minutes until the polymerization conversion rate reached 98% or more. By the above operations, a latex containing (meth)acrylic crosslinked rubber particles (B) was obtained. The latex containing (meth)acrylic crosslinked rubber particles (B) was frozen and coagulated. It was then washed with water and dried to obtain particulate (meth)acrylic crosslinked rubber particles (B). The average particle size of the particles was 0.23 μm.
[0097] The other materials used were as follows: [Polymer processing aids (C)] Dow Chemical Company "Paraloid (registered trademark)" K125P [UV inhibitor (D)] ADEKA "ADEKA STAB (registered trademark)" LA31RG
[0098] [Example 1] 42 parts by mass of (meth)acrylic resin (A-1), 10 parts by mass of (meth)acrylic resin (A-2), 28 parts by mass of (meth)acrylic resin (A-3), 20 parts by mass of (meth)acrylic crosslinked rubber particles (B), 1.5 parts by mass of polymer processing aid (C), and 2.0 parts by mass of ultraviolet absorber (D) were fed into the hopper of a 41 mmφ twin-screw kneading extruder (Toshiba Machine Co., Ltd., TEM41-SS) while controlling with a weight feeder, and the temperature under the hopper was set to 150°C, and the barrel temperature was set to 230°C, respectively, to extrude the (meth)acrylic resin composition into a strand shape, which was then cut with a pelletizer to produce pellets of the (meth)acrylic resin composition. The obtained pellets were extruded at a melt extrusion temperature (film-forming temperature including the temperature from the vent to the T-die (center)) of 270 ° C., the temperature at the end of the T-die only was 275 ° C., and the extrusion rate was 180 kg / h. The pellets were sandwiched between an 80 ° C. metal mirror elastic roll (outer cylinder thickness 8 mm, crown roll) and an 80 ° C. metal mirror rigid roll at a linear pressure of 30 N / mm to form a film, and taken up at 18 m / min. The end was slit to form a film with a width of 1.5 m and a thickness of 80 μm. The evaluation results of the film obtained on the second day after the start of film formation are shown in Table 1.
[0099] [Example 2] The film was produced in the same manner as in Example 1, and the evaluation results are shown in Table 1 on the fifth day after the start of film production.
[0100] [Example 3] A film was formed in the same manner as in Example 1, except that the take-up speed was changed to 24 m / min and the film thickness was changed to 60 μm, and various physical properties were evaluated. The evaluation results are shown in Table 1.
[0101] [Example 4] The film was produced in the same manner as in Example 3, and the evaluation results are shown in Table 1 on the fifth day after the start of film production.
[0102] [Comparative Example 1] A film was formed in the same manner as in Example 1, except that the thickness of the outer cylinder of the metal mirror-surface elastic roll used was changed to 3 mm and the linear pressure was changed to 10 N / mm, and various physical properties were evaluated. The evaluation results are shown in Table 1.
[0103] [Comparative Example 2] The film obtained on the fifth day after the start of film production was evaluated in the same manner as in Comparative Example 1, and the results are shown in Table 1.
[0104] [Comparative Example 3] A film was produced in the same manner as in Example 1, except that the temperatures of the specular elastic metal roll and the specular rigid metal roll were changed to 50° C., and various physical properties were evaluated. The evaluation results are shown in Table 1.
[0105] [Comparative Example 4] The film obtained on the fifth day after the start of film production was evaluated in the same manner as in Comparative Example 3, and the results are shown in Table 1.
[0106] [Table 1]
Claims
1. a melt extrusion step of melt extruding the (meth)acrylic resin composition through a T-die; a clamping step of clamping the melt-extruded molten material between a pair of mirror-surface rolls consisting of a mirror-surface elastic roll and a mirror-surface rigid roll, The (meth)acrylic resin composition is 70 to 85% by mass of a (meth)acrylic resin (A) containing 90% by mass or more of a structural unit derived from methyl methacrylate; 15 to 30% by mass of (meth)acrylic crosslinked rubber particles (B) which are a core-shell type graft copolymer having an average particle size of 0.15 to 0.3 μm and which have a crosslinked rubber layer containing structural units derived from an acrylic acid alkyl ester; Including; The (meth)acrylic resin (A) contains, relative to 100 parts by mass of the (meth)acrylic resin (A), 45 to 55 parts by mass of a (meth)acrylic resin (A-1) having an MFR of 9 g / 10 min or more and 16 g / 10 min or less; 10 to 15 parts by mass of a (meth)acrylic resin (A-2) having an MFR of 25 g / 10 min or more and 100 g / 10 min or less; 30 to 40 parts by mass of a (meth)acrylic resin (A-3) having an MFR of 0.1 g / 10 min or more and 3 g / 10 min or less; Including; The surface temperatures of the specular elastic roll and the specular rigid roll are both 70° C. or higher and 100° C. or lower, and the thickness of the outer cylinder of the specular elastic roll is 6 mm or higher and 15 mm or lower; The (meth)acrylic resin film obtained by the above production method has less than 1 protruding defect having a height of 1 μm or more per 10 m 2 , and has 10 or less fish-eye defects per 10 m 2 . A method for producing a (meth)acrylic resin film.
2. The method for producing a (meth)acrylic resin film as described in claim 1, wherein the (meth)acrylic resin film has a film thickness of 20 to 500 μm.
3. A method for producing a (meth)acrylic resin film as described in claim 1 or 2, wherein the pencil hardness of at least one surface of the (meth)acrylic resin film is HB or higher.
4. A method for producing a (meth)acrylic resin film described in any one of claims 1 to 3, wherein the haze of the (meth)acrylic resin film is 1.5% or less.
5. A method for producing a (meth)acrylic resin film described in any one of claims 1 to 4, wherein the (meth)acrylic resin composition has a complex viscosity of 500 to 1300 Pa·s measured under conditions of 265°C, 10 rad / sec, and 1% strain.
6. The method includes a step of drawing off the molten material sandwiched between the pair of mirror-surface rolls, The method for producing a (meth)acrylic resin film according to any one of claims 1 to 5, wherein a take-up speed when the molten material is taken up is 10 to 50 m / min.
7. A method for producing the (meth)acrylic resin film described in claim 1, further comprising a step of laminating another layer.
8. A method for producing a (meth)acrylic resin film as described in claim 7, wherein the other layer is a functional layer.
9. The manufacturing method described in claim 1, wherein the (meth)acrylic resin film is a polarizer protective film.
Citation Information
Patent Citations
Optical film and method of manufacturing the same
JP2009039935A
Optical laminate, manufacturing method therefor, and polarizer protection film
JP2017068227A
Acrylic resin film and method for producing the same
JP2017078168A
Resin composition and production method therefor, molded body, film, and article
WO2016157908A1
Thermoplastic resin multilayer film, method for manufacturing same, and laminate
WO2018199161A1