gasket

The gasket design with a low Kd/Kst ratio and rubber hardness of 90 or less addresses the issue of inadequate vibration damping in environmentally friendly vehicles, enhancing noise reduction and comfort by converting vibrations into thermal energy.

JP7564186B2Active Publication Date: 2024-10-08NOK CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022500347
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-12
Filing Date
2021-02-03
Publication Date
2024-10-08
Estimated Expiration
2041-02-03

AI Technical Summary

Technical Problem

Existing gaskets, particularly those used in environmentally friendly vehicles, lack sufficient vibration damping and isolation properties, leading to unwanted vibrations and noise.

Method used

A gasket design featuring an elastic portion with a dynamic spring constant to static spring constant ratio (Kd/Kst) of 2.5 or less, made from rubber with a hardness of 90 or less, and optionally with a metal plate, providing enhanced vibration damping and isolation.

Benefits of technology

The gasket effectively suppresses vibrations and noise transmission, improving the quietness and comfort of devices by converting vibrations into thermal energy within the elastic section.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564186000002
    Figure 0007564186000002
  • Figure 0007564186000001
    Figure 0007564186000001
Patent Text Reader

Abstract

The purpose of the present invention is to provide a gasket having excellent vibration-damping properties and vibration-isolating properties. A gasket which has an elastic part comprising a rubber having a dynamic multiplication Kd / Kst, which is a ratio of a dynamic spring constant Kd to a static spring constant Kst, of 2.5 or less. A dynamic spring constant Kd refers to a constant prescribed in JIS K6394:2007 and measured under the conditions of 23±2°C, 100 Hz and a strain amplitude of 0.1%, and a static spring constant Kst refers to a constant prescribed in JIS K6394:2007 and measured under the conditions of 23±2°C and a strain amplitude of 0.1%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gasket. [Background technology]

[0002] Currently, gaskets made of laminated rubber and metal are used in various fields such as automobiles. Gaskets are required to have high sealing properties, and therefore improvements in compression set resistance (CS), stress relaxation properties, and rubber hardness have been studied. Patent Document 1 (International Publication No. 2011 / 024812) discloses a metal gasket made of multiple laminated metal sheets and sealing materials made of elastomers (Claim 1, paragraph

[0044] ).

[0003] In recent years, automobiles have become more hybridized and electric, and environmentally friendly automobiles such as fuel cell vehicles are being developed. These automobiles use gaskets for motors, gaskets for batteries such as secondary batteries and fuel cells, and gaskets for power control units. Environmentally friendly automobiles such as hybrid automobiles, electric automobiles, and fuel cell vehicles use motors, which generate vibrations when the motors are driven. Therefore, there has been a demand for suppressing the vibrations generated in these environmentally friendly automobiles. In addition, there has been a demand for suppressing vibrations originating from vibration sources such as motors in devices other than environmentally friendly automobiles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2011 / 024812 Summary of the Invention [Problem to be solved by the invention]

[0005] Although the gasket of Patent Document 1 has high sealing properties, further improvement in vibration damping and vibration prevention properties is desired. The present invention has been made in consideration of the above circumstances, and provides a gasket with excellent vibration damping and vibration prevention properties. [Means for solving the problem]

[0006] The embodiments of the present invention are as follows. [1] A gasket having an elastic part containing rubber with a dynamic spring factor Kd / Kst, which is the ratio of the dynamic spring constant Kd to the static spring constant Kst, of 2.5 or less. (The dynamic spring constant Kd is the constant measured under the conditions of 23±2°C, 100Hz, and strain amplitude of 0.1% as specified in JIS K6394:2007. The static spring constant Kst is the constant measured under the conditions of 23±2°C and strain amplitude 0.1% as specified in JIS K6394:2007. [2] The gasket according to [1] above, wherein the hardness of the rubber is 90 or less. [3] A metal plate; The elastic portion is provided on one or both sides of the metal plate. The gasket according to the above [1] or [2], [4] A gasket according to any one of [1] to [3] above, wherein the rubber is a nitrile rubber. [5] A gasket according to any one of [1] to [4] above, which is a gasket for a motor. [6] A gasket according to any one of [1] to [4] above, which is a gasket for an inverter case. Effect of the Invention

[0007] A gasket having excellent vibration damping and vibration prevention properties can be provided. [Brief description of the drawings]

[0008] [Figure 1] 1 is an exploded perspective view of a housing to which an example of a gasket according to an embodiment of the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The gasket of the present invention has an elastic part containing rubber with a dynamic ratio Kd / Kst, which is the ratio of the dynamic spring constant Kd to the static spring constant Kst, of 2.5 or less. Here, the dynamic spring constant Kd represents a constant measured under the conditions of 23±2°C, 100Hz, and strain amplitude 0.1% as described in JIS K6394:2007. The static spring constant Kst represents a constant measured under the conditions of 23±2°C and strain amplitude 0.1% as described in JIS K6394:2007. By making the dynamic ratio Kd / Kst of the rubber 2.5 or less, vibration from a vibration source is less likely to be transmitted to the gasket. Also, even if vibration is transmitted from the vibration source to the elastic part, the vibration is easily converted into thermal energy in the elastic part. As a result, the gasket can have excellent vibration-damping and vibration-proofing properties, and the gasket can effectively prevent vibration from being transmitted from the vibration source to other members. In addition, the gasket suppresses vibration from a vibration source, and therefore reduces noise caused by the vibration, thereby improving the quietness of the device having the gasket. Typically, the elastic part is made of rubber with a dynamic magnification Kd / Kst of 2.5 or less. For example, the gasket can be used for a motor or an inverter case, and can reduce vibration and noise generated from these devices. In addition, the gasket can be used inside machines and devices such as automobiles, robots, and home appliances equipped with motors and inverter cases. When the gasket of the present invention is used in an automobile, vibration and noise are reduced, allowing the automobile to drive in a comfortable condition.

[0010] The dynamic spring constant Kd and the static spring constant Kst of the rubber constituting the elastic portion are measured as follows. The vulcanization rate of the rubber composition for the elastic portion is measured in advance in accordance with JIS K6300-2, and the T c (90) (90% vulcanization time) is measured. Then, T cA rubber piece is prepared by pressurizing and vulcanizing the rubber composition for the elastic part under conditions exceeding (90). Thereafter, the dynamic spring constant is measured by a tensile method under conditions of 23±2°C, 100Hz, and strain amplitude of 0.1% in accordance with the forced vibration non-resonance method described in JIS K6394:2007. The static spring constant is measured by a tensile method under conditions of 23±2°C and strain amplitude of 0.1% as described in JIS K6394:2007. The dynamic spring constant Kd of the rubber measured in this manner is divided by the static spring constant Kst to obtain the dynamic ratio Kd / Kst. For example, Rheogel-E4000 manufactured by UBM can be used as a measuring device for the dynamic spring constant and the static spring constant. The dynamic ratio Kd / Kst is 2.5 or less, preferably 2.0 or less, and more preferably 1.8 or less. The dynamic ratio Kd / Kst is preferably 0.5 or more, and more preferably 1.0 or more. By having the dynamic magnification ratio within the above range, the gasket can have higher vibration damping and vibration prevention properties. The dynamic spring constant is preferably 1.5 g / μm or less, more preferably 1.2 g / μm or less, and even more preferably 0.8 g / μm or less. By having the dynamic spring constant within the above range, the gasket can achieve both excellent vibration damping and vibration prevention properties and sealing properties.

[0011] The hardness (Durometer A hardness) of the rubber contained in the elastic portion is preferably 90 or less, more preferably 85 or less, and even more preferably 80 or less. If the rubber hardness is within the above range, the gasket can have higher sealing performance and vibration damping and vibration prevention properties. The rubber hardness can be measured by a method conforming to JIS K6253.

[0012] The gasket according to one embodiment has a metal plate and an elastic part containing rubber having a dynamic magnification Kd / Kst of 2.5 or less on one or both sides of the metal plate. The material of the metal plate is not particularly limited, but iron, aluminum, copper, or alloys thereof can be used. For example, SPCC (cold rolled steel plate), SPFC (cold rolled high tensile steel plate), mild steel, stainless steel plate, aluminum, and aluminum die cast can be used. As the stainless steel plate, SUS301, SUS301H, SUS304, SUS430, etc. can be used. The thickness of the metal plate is not particularly limited, but is preferably 100 to 2000 μm, and more preferably 200 to 1000 μm. The metal plate can be used in a degreased state, and the metal surface can be roughened by shot blasting, Scotch bride, hairline, dull finishing, etc. as necessary. The elastic part may be bonded to the metal plate by containing an adhesive component or by providing an adhesive layer between the elastic part and the metal plate. The adhesive component and the adhesive layer component are not particularly limited as long as they can improve the adhesion between the metal plate and the elastic part, and for example, a resin-based vulcanizing adhesive such as a phenolic resin or an epoxy resin can be used. The phenolic resin can be any thermosetting phenolic resin such as a cresol novolac type phenolic resin, a cresol resol type phenolic resin, or an alkyl-modified type phenolic resin. The epoxy resin can be a cresol novolac type epoxy resin, in which case a bisphenol novolac type phenolic resin is used as a curing agent and an imidazole compound is used as a curing catalyst.

[0013] The rubber constituting the elastic portion is preferably nitrile rubber (NBR). Nitrile rubber is a copolymer of butadiene and acrylonitrile. The nitrile rubber (NBR) may be hydrogenated or not. As the nitrile rubber, various types of NBR with very high nitrile content (nitrile content of 43% or more), high nitrile content (36 to 42%), medium-high nitrile content (31 to 35%), medium nitrile content (25 to 30%) and low nitrile content (24% or less) can be used.

[0014] The rubber may further contain carbon black, silica, a filler, a plasticizer, an additive, an antioxidant, a vulcanizing agent, a vulcanization accelerator, a vulcanization aid, etc. The type of carbon black may be appropriately selected depending on the application of the gasket, and for example, SAF carbon black, ISAF carbon black, HAF carbon black, EPC carbon black, XCF carbon black, FEF carbon black, GPF carbon black, HMF carbon black, SR carbon black, FT carbon black, MT carbon black, etc. may be used. Examples of additives include calcium metasilicate, calcium carbonate, zinc oxide, stearic acid, and wax. In addition, the vulcanizing agent is not particularly limited as long as it is used as a vulcanizing agent for rubber, and examples of the vulcanizing agent include sulfur-based vulcanizing agents and organic peroxide-based vulcanizing agents.

[0015] Examples of sulfur-based vulcanizing agents include powdered sulfur, sulfur flowers, precipitated sulfur, colloidal sulfur, highly dispersible sulfur, and insoluble sulfur; sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, dibenzothiazyl disulfide, N,N'-dithio-bis(hexahydro-2H-azenopine-2), phosphorus-containing polysulfide, and polymeric polysulfide-containing sulfur-containing compounds. Examples of organic peroxide-based vulcanizing agents include ketone peroxides, peroxy esters, diacyl peroxides, and dialkyl peroxides. Also, vulcanization accelerators and vulcanization assistants can be used as necessary.

[0016] FIG. 1 shows an exploded perspective view of a housing to which an example of a gasket according to an embodiment is applied. The housing 100 shown in FIG. 1 is composed of two members, a case member 200 and a cover member 300. The case member 200 and the cover member 300 have flanges 201, 301 integrally formed around the periphery of their respective openings. One gasket 1 is disposed between the opposing butt surfaces 202, 302 of the flanges 201, 301. The butt surfaces 202, 302 of the flanges 201, 301 are formed so as to surround the outer periphery of the openings of the case member 200 and the cover member 300 in a band shape of a certain width. The portions where the bolt holes 203, 303 are formed partially protrude to the side.

[0017] The gasket 1 has an annular portion 1a and a protruding portion 1b. The annular portion 1a is formed with a constant width similar to that of the butting surfaces 202, 302 of the flange portions 201, 301 of the case member 200 and the cover member 300. The protruding portion 1b partially protrudes laterally from the annular portion 1a at positions corresponding to the bolt holes 203, 303 of the flange portions 201, 301 so as to be connected by a smooth curve. Each protruding portion 1b has a bolt hole 11 formed therein corresponding to the bolt hole 203, 303 of the flange portions 201, 301.

[0018] The housing 100 has the case member 200, the cover member 300, and the gasket 1 fastened together by inserting bolts 400 through the bolt holes 203, 303, 11. The gasket 1 sandwiched between the flange portions 201, 301 provides a seal between the mating surfaces 202, 302 of the flange portions 201, 301.

[0019] The gasket 1 is not particularly limited as long as it has the above configuration. In the above description, an example has been shown in which the gasket 1 according to one embodiment is applied as a sealing member between the flanges 201, 301 of the case member 200 and the cover member 300 of the housing 100. However, the gasket 1 according to one embodiment is not limited to applications to such a housing 100, and can be widely applied to cases in which the butted surfaces between two members are sealed.

[0020] The gasket is preferably a gasket for a motor. The gasket is preferably a gasket for an inverter case.

[0021] In one embodiment of the method for producing a gasket, for example, a solution containing a rubber composition for the elastic portion is dropped and applied onto a substrate such as a metal plate, and then the solution is heated and dried while vulcanizing the rubber composition to produce the elastic portion. The solution containing the rubber composition for the elastic portion is not particularly limited, and methyl ethyl ketone, toluene, ethyl acetate, etc. can be used. EXAMPLES

[0022] Preferred embodiments of the present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to these examples.

[0023] (Examples 1 to 14 and Comparative Examples 1 to 5) A pressure kneader (manufactured by Nippon Spindle Co., Ltd.) and an open roll (manufactured by Kansai Roll Co., Ltd.) were used to mix the materials in the formulation shown in Table 1 below, thereby preparing a rubber composition. (evaluation) The rubber compositions obtained as described above were used to carry out the following measurements. (a) Measurement of hardness, tensile strength, and elongation of the elastic part The vulcanization rate of the rubber composition was measured in advance in accordance with JIS K6300-2. c (90) (90% vulcanization time) was measured. Then, T c The rubber composition was pressurized and vulcanized under conditions exceeding (90) to prepare a test specimen. The test specimen was subjected to measurement of hardness (Durometer A hardness) in accordance with JIS K6253, and measurement of tensile strength and elongation in accordance with JIS K6251. (b) Measurement of dynamic spring constant Kd A test piece having a thickness of 2 mm, a width of 4 mm, and a length of 20 mm was prepared by pressurizing and vulcanizing the rubber composition under the same conditions as in (a) above. Next, the dynamic spring constant of the test piece was measured by a tensile method under the conditions of 23±2°C, 100 Hz, and strain amplitude of 0.1%, using Rheogel-E4000 manufactured by UBM Co., Ltd., in accordance with the forced vibration non-resonance method described in JIS K6394:2007. (c) Measurement of static spring constant Kst The rubber composition was pressurized and vulcanized under the same conditions as in (a) above to prepare a test piece having a thickness of 2 mm, a width of 4 mm, and a length of 20 mm. The static spring constant of the test piece was then measured by a tensile method under conditions of 23±2°C and a strain amplitude of 0.1% using a Rheogel-E4000 manufactured by UBM in accordance with JIS K6394:2007.

[0024] (d) Calculation of dynamic magnification Kd / Kst Based on the dynamic spring constant Kd and the static spring constant Kst measured in the above (b) and (c), the dynamic magnification ratio Kd / Kst was calculated according to the following formula. Dynamic ratio Kd / Kst = (dynamic spring constant Kd) / (static spring constant Kst) (e) Measurement of gasket loss factor The surface of a 400 μm thick SPCC steel plate was treated with zinc phosphate. After that, methyl ethyl ketone (MEK) in which a phenolic resin (Sixon 715 (trade name)) was dissolved was applied onto the SPCC steel plate, and then dried. Next, the rubber composition prepared in each example was dissolved in methyl ethyl ketone (MEK). After that, MEK in which a rubber composition was dissolved was applied onto the SPCC steel plate after the MEK solution containing the phenolic resin was applied, and the rubber composition was vulcanized in an oven at 200 ° C. for 3 minutes to form an elastic part with a thickness of 120 μm on the SPCC steel plate (metal plate). As a result, a gasket with a width of 17 mm and a length of 250 mm having an elastic part on the SPCC steel plate (metal plate) was obtained. The gasket obtained in this way was attached to a SUS301 plate with a thickness of 250 μm, a width of 17 mm, and a length of 250 mm via a cyanoacrylate adhesive to obtain a sample for loss factor measurement. Furthermore, preliminary experiments confirmed that, as long as the gasket can be attached to the SUS301 plate, the type of adhesive does not affect the loss factor. Next, using Rion AS14PA5 (cantilever type), the loss factor was measured in accordance with JIS K7391:2008 using the half-width method, a measurement temperature of 23±2°C, and a second-order resonance frequency within the measurement range of 0 to 1 kHz. When the loss factor was 0.03 or more, the vibration damping and vibration-proof properties were judged to be good and rated as "○", and when the loss factor was less than 0.03, the vibration damping and vibration-proof properties were judged to be poor and rated as "×". The composition of the rubber composition and the evaluation results of the vibration damping and vibration-proof properties are shown in Table 1 below.

[0025] [Table 1]

[0026] The names of the materials in Table 1 are as follows: Nitrile rubber A: Nipol (registered trademark) DN3350 (Zeon Corporation) Nitrile rubber B: JSR N237 (JSR Corporation) Nitrile rubber C: JSR N220S (JSR Corporation) Carbon black A (MT carbon black): THERMAX (registered trademark) N990 LSR (Cancarb) Carbon black B (SRF carbon black): HTC#SS (Shin-Nichika Carbon Co., Ltd.) Carbon black C (SRF carbon black): ASAHI#50HG (Asahi Carbon Co., Ltd.) Carbon Black D (FEF Carbon Black): Seast (registered trademark) SO (Tokai Carbon Co., Ltd.) Carbon black E (HAF carbon black): Show Black (registered trademark) N330L (Cabot Japan Co., Ltd.) Silica: Nipsil (registered trademark) LP (Tosoh Corporation) Filler A: Actidil VM56 (Hoffman Minerals) Filler B: Nyad® 400 (NYCO Minerals, Inc.) Filler C: Hakuenka (registered trademark) CC (Shiraishi Kogyo Co., Ltd.) Plasticizer: Adeka Cizer (registered trademark) RS107 (ADEKA Corporation) Additive A: Zinc oxide (Seido Chemical Industry Co., Ltd.) Additive B: DTST (Miyoshi Oil Co., Ltd.) Additive C: NOCRAC 810-NA (Ouchi Shinko Chemical Industry Co., Ltd.) Additive D: SUNTIGHT® R (Seiko Chemical Co., Ltd.) Vulcanizing agent A: Colloidal sulfur A (Tsurumi Chemical Industry Co., Ltd.) Vulcanizing agent B: Valnoc (registered trademark) R (Ouchi Shinko Chemical Industry Co., Ltd.) Vulcanizing agent C: Peroximon (registered trademark) F-40 (NOF Corporation) Vulcanization accelerator A: Noccela (registered trademark) TBZTD (Ouchi Shinko Chemical Industry Co., Ltd.) Vulcanization accelerator B: Noccela (registered trademark)-CZ-P (Ouchi Shinko Chemical Industry Co., Ltd.) Vulcanization aid: TAIC (registered trademark) M60S (Mitsubishi Chemical Corporation)

[0027] The results in Table 1 show that by keeping the dynamic magnification Kd / Kst of the rubber that makes up the elastic portion at 2.5 or less, the loss factor becomes 0.03 or more, resulting in a gasket with excellent vibration damping and vibration isolation properties. [Explanation of symbols]

[0028] 1 Gasket 1a Annular part 1b Protruding part 11 Bolt holes 100 Case 200 Case material 201, 301 Flange part 202, 302 butt surface 203, 303 Bolt holes 300 Lid member 400 volts

Claims

1. The elastic portion includes a nitrile rubber having a dynamic spring constant Kd / Kst of 1.8 or less, the dynamic spring constant Kd being a ratio of the static spring constant Kst to the dynamic spring constant Kd. The dynamic spring constant Kd is 0.208 to 1.437 g / μm; The static spring constant Ks of the gasket is 0.148 to 0.584 g / μm. (The dynamic spring constant Kd is a constant measured under the conditions of 23±2°C, 100 Hz, and strain amplitude of 0.1% as described in JIS K6394:2007. The static spring constant Kst is a constant measured under the conditions of 23±2°C and strain amplitude of 0.1% as described in JIS K6394:2007.

2. 2. The gasket of claim 1, wherein the rubber has a hardness of 90 or less.

3. A metal plate; The elastic portion is provided on one or both sides of the metal plate. The gasket of claim 1 or 2, having

4. 4. The gasket according to claim 1, which is a gasket for a motor.

5. The gasket according to claim 1 , which is a gasket for an inverter case.

6. A gasket described in any one of claims 1 to 5, having a loss coefficient of 0.03 or more.

Citation Information

Patent Citations

  • Rubber vibration isolator

    JP1992246439A

  • Metal-rubber composite and manufacture thereof

    JP1999207859A

  • Heat-resistant damping rubber composition and method for producing heat-resistant damping rubber composition

    JP2005126473A

  • Silica treated with silane coupling agent, its preparation method, rubber composition for vibration proof and earthquake isolation, its production method, rubber product for vibration proof or earthquake isolation and its forming method

    JP2006052105A

  • Gasket

    JP2012255515A