Process for preparing silicon oxide coated particles by flame spray pyrolysis

The flame spray pyrolysis method coats metal oxide particles with a silicon oxide layer, addressing stability and water resistance issues by forming a 'four-membered ring' structure, maintaining optical properties and enabling use in cosmetics and electronics.

JP7564214B2Active Publication Date: 2024-10-08LOREAL SA
View PDF 22 Cites 0 Cited by

Patent Information

Application Number
JP2022539238
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-24
Publication Date
2024-10-08
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Existing methods for coating metal oxide particles with silicon oxide to enhance their stability and water resistance, particularly in acidic environments, are inadequate, leading to degradation and loss of optical properties.

Method used

A flame spray pyrolysis method is used to coat metal oxide particles with a silicon oxide layer containing a specific 'four-membered ring' structure, formed by injecting elemental M precursors and silicon precursors with Si-carbon covalent bonds into a flame, ensuring a stable and protective coating.

Benefits of technology

The method produces metal oxide particles with enhanced water resistance and retention of optical properties, suitable for use in cosmetic and electronic applications without requiring hydrophobic coatings or surfactants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564214000005
    Figure 0007564214000005
  • Figure 0007564214000001
    Figure 0007564214000001
  • Figure 0007564214000002
    Figure 0007564214000002
Patent Text Reader

Abstract

The present invention relates to a method for preparing silicon oxide coated oxide particles, particularly metal oxide particles, by flame spray pyrolysis techniques, to silicon oxide coated oxide particles, particularly metal oxide particles, and compositions containing said particles. The present invention also relates to certain silicon oxide coated oxide particles, particularly metal oxide particles, derived from such methods, compositions containing such particles, and uses thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for preparing silicon oxide coated oxide particles, in particular metal oxide particles, by flame spray pyrolysis technique, to silicon oxide coated oxide particles, in particular metal oxide particles, and compositions comprising said particles.

[0002] The invention also relates to certain oxide particles, particularly metal oxide particles, coated with silicon oxide derived from such a process, compositions containing such particles and also uses thereof. [Background technology]

[0003] Inorganic compounds, also called oxides, such as zinc oxide, copper oxide or iron oxide, are used in many applications (cosmetics, paints, dyes, electronics, rubber, etc.) Zinc oxide, for example, is used in particular for its optical properties, in particular for its light absorbing and / or scattering properties that allow it to protect surfaces from UV rays and / or to convert ambient light into electricity.

[0004] However, some of these oxides have the drawback of being particularly unstable over time. They tend to decompose in the presence of water, especially coming from the composition containing them or from atmospheric moisture. Such decomposition has the effect of partially or even completely dissolving the oxide in water, greatly reducing or even eliminating the desired properties of said oxide.

[0005] These decompositions can be particularly problematic in certain circumstances, especially when the product is for public use, such as in the cosmetics, paint or food industries. As an example, as zinc oxide decomposes, the UV protection of the sunscreen composition decreases. To overcome these shortcomings, it is common practice to package these compounds in anhydrous media or even protect them with specific packaging, which has proven to be particularly restrictive.

[0006] Other approaches, such as preparing the mixture extemporaneously at the point of use or adding preservatives capable of stabilizing these compounds, have not provided a satisfactory solution either from the consumer's or the environmental point of view. However, reducing the preservative compounds leads to the use of more acidic formulations, which creates conditions that make the oxides used less stable. Magnesia or oxides of zinc, copper and iron are particularly susceptible to this acidity.

[0007] In certain applications, oxide compounds are intended to be used in particulate form, such as for example the application of a fluid formulation to a surface. In that case, there is a risk that the particles will generate CO2 and water forms in the surrounding air. Furthermore, if the surface to which the fluid formulation is applied contains water or may subsequently come into contact with water, the decomposition of the oxide compounds will be accelerated. As an example, sweating produces water, usually acidic water, which can decompose the oxide compounds present in the cosmetic composition. The same is true when desired or undesired water (rain, spray, etc.) is provided after the cosmetic product is applied to the skin or hair. Thus, the use of anhydrous products containing such oxides can cause the decomposition of the oxides after the product is applied to the skin or hair.

[0008] These drawbacks are exacerbated when using fine particles, which are commonly used in cosmetics because they are invisible and imperceptible to the touch.

[0009] To protect metal oxide particles, it is known to coat them with fat or polymer coatings. However, the use of fat coatings limits the use of the particles and requires the use of hydrophobic products or surfactants. Furthermore, the production of polymer coatings is also problematic due to the restrictions imposed on microplastics.

[0010] It has been envisaged to coat metal oxides with silica by a sol-gel method, but this solution is not entirely satisfactory: protection of metal oxides has proven to be particularly poor in acidic media.

[0011] It is also known to use flame spray pyrolysis (FSP) to prepare zinc oxide particles.

[0012] Flame spray pyrolysis or FSP is a well-known method nowadays, which has been essentially developed to synthesize ultrafine powders of single or mixed oxides of various metals (e.g. SiO2, Al2O3, BO3, ZrO2, GeO2, WO3, Nb2O5, SnO2, MgO, ZnO) with controlled morphology and / or deposit them on various substrates, starting from various metal precursors, usually in the form of organic or inorganic, preferably non-flammable, sprayable liquids. The liquid sprayed into the flame releases nanoparticles of the metal oxide that are sprayed onto these various substrates by the combustion, and in particular by the flame itself. This method has also been used for the production of oxide particles covered with a layer of silica. The principle of this method is recalled, for example, in a recent (2011) publication by Johnson Matthey entitled (J. Matthey, 2001). Numerous variants of FSP processes and reactors are also described, for example, in the following patents or patent applications: US Pat. No. 5,399,414, US Pat. No. 5,399,421, US Pat. No. 5,399,432, US Pat. No. 5,399,443, US Pat. No. 5,399,511, US Pat. No. 5,399,621, US Pat. No. 5,399,711, US Pat. No. 5,399,821, US Pat. No. 5,399,931, US Pat. No. 5,399,941, US Pat. No. 5,399,951, US Pat. No. 5,399,102, US Pat. No. 5,399,113, US Pat. No. 5,399,122, US Pat. No. 5,399,133, US Pat. No. 5,399,142, US Pat. No. 5,399,152, US Pat. No. 5,399,162, US Pat. No. 5,399,172.

[0013] However, the layer of silica thus formed nevertheless proved to be too thin and insufficient to protect the oxide from water. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] U.S. Pat. No. 5,958,361 [Patent Document 2] U.S. Patent No. 2,268,337 [Patent Document 3] International Publication No. 01 / 36332 Brochure [Patent Document 4] U.S. Patent No. 6,887,566 [Patent Document 5] International Publication No. 2004 / 005184 Brochure [Patent Document 6] U.S. Patent No. 7,211,236 [Patent Document 7] International Publication No. 2004 / 056927 Brochure [Patent Document 8] International Publication No. 2005 / 103900 Brochure [Patent Document 9] International Publication No. 2007 / 028267 Brochure [Patent Document 10] U.S. Patent No. 8,182,573 [Patent Document 11] International Publication No. 2008 / 049954 Brochure [Patent Document 12] U.S. Patent No. 8,231,369 [Patent Document 13] International Publication No. 2008 / 019905 Brochure [Patent Document 14] US Patent Application Publication No. 2009 / 0123357 [Patent Document 15] U.S. Patent Application Publication No. 2009 / 0126604 [Patent Document 16] US Patent Application Publication No. 2010 / 0055340 [Patent Document 17] International Publication No. 2011 / 020204 Brochure [Non-patent literature]

[0015] [Non-Patent Document 1] Flame Spray Pyrolysis: a Unique Facility for the Production of Nanopowders”,Platinum Metals Rev.,2011,55,(2),149-151 Summary of the Invention [Problem to be solved by the invention]

[0016] There is therefore a real need to develop a process for the preparation of oxide particles, in particular metal oxide particles, which makes it possible to endow said particles with good stability over time, in particular good water resistance, whilst preserving the properties of the oxides used, such as good optical properties in terms of absorption and / or scattering of light, and more particularly ultraviolet light. [Means for solving the problem]

[0017] These objects are achieved by the present invention, one subject of which is in particular a method for preparing coated particles of an oxide of the element M, comprising at least the following steps: a) preparing a composition (A) by adding one or more precursors of element M to one or more combustible solvents, and then b) forming a flame in a flame spray pyrolysis device by injecting composition (A) and an oxygen-containing gas until aggregates of oxides of element M are obtained; c) injecting a composition (B) comprising one or more silicon precursors and one or more polar protic solvents other than water into the flame until an inorganic coating layer containing silicon oxide is obtained on the surface of the aggregates of element M; Including, - said element M is selected from the alkali metals from the first column, the alkaline earth metals from the second column, the elements from the third to the sixteenth columns and the elements from the lanthanide group of the Periodic Table of the Elements, and - the silicon precursor contains at least two silicon atoms and some Si-carbon covalent bonds; This is a method by which the above-mentioned

[0018] It has been observed that the method according to the invention makes it possible to obtain particles of the oxide of the particular element M, which are covered with a layer of silicon oxide and which are particularly stable over time and have good water resistance, even at acidic pH.

[0019] More specifically, the method of the invention makes it possible to form a layer of silicon dioxide having a specific "four-membered ring" structure. This specific assembly of silicon dioxide surrounds the oxide of element M and forms a protective layer around this compound.

[0020] Moreover, unlike conventional coating methods, the method according to the invention has the advantage of preserving good intrinsic properties of the core despite the presence of the coating: in fact, due to the particular nature of the coating layer, for a given particle mass it is possible to reduce the proportion of metal oxide without degrading and / or adversely affecting the properties of the metal oxide.

[0021] The method of the invention therefore makes it possible to produce stable metal oxide particles, whilst avoiding the drawbacks of the increased amounts of particles previously required to maintain good optical properties of said oxides.

[0022] Additionally, compositions containing coated metal oxide particles can protect fillers, pigments or other water sensitive inorganic active agents, such as magnesium oxide.

[0023] By varying the quality of the metal oxide, especially the silica, high but intermediate water protection can be obtained, which does not allow for complete protection, for example by allowing a more gradual or controlled release of the metal oxide from the core.

[0024] These particles of oxide of element M comprise a core (1) and one or more upper coating layers (2) covering said core (1), and (i) the core (1) consists of one or more oxides of element M, preferably in a crystalline state; (ii) the upper coating layer (2) covers at least 90% of the surface of the core (1), preferably covers the entire surface of the core (1), and comprises one or more silicon oxides; (iii) the element M is selected from magnesium, calcium, zinc, copper, iron, zirconium, aluminum, gallium, indium, tin, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium; (iv) (M / silicon) 粒子 The molar atomic ratio is within the range of 0.1 to 10, preferably 0.2 to 2, and more preferably 0.5 to 1.5. It is characterized by:

[0025] More specifically, the particles of the specific element M oxide according to the invention do not degrade significantly over time in the presence of water, even when they are formulated in an aqueous composition or even in an acid composition.

[0026] It has also been observed that the particles prepared according to the invention retain the properties inherent to the element M oxide used, such as good optical properties with respect to light absorption and / or light scattering. More specifically, they have high UV absorption and low or high visible light scattering, thus enabling applications such as sun protection and / or visual appearance modification, while benefiting from resistance in the presence of water.

[0027] Moreover, compositions containing such particles exhibited good screening power, especially with respect to long and short UV-A rays.

[0028] Furthermore, compositions comprising the particles of the invention have a particularly high transparency, which may prove to be advantageous when the composition is applied and then dried onto a coating, in particular onto the skin.

[0029] In addition, the particles of element M oxide coated with silicon oxide according to the invention do not require a hydrophobic coating, which allows them to be used over a wide range of formulations (e.g. in fully aqueous and / or surfactant-free formulations), further reducing the risk of inappropriate deposits (on the edges of the basin, on the walls of the pipes or on rocks) when the formulations thus obtained end up in water (basin drains, lakes or the sea).

[0030] The accompanying drawings are schematic diagrams, not necessarily to scale, and are intended to illustrate, among other things, the principles of the invention. [Brief description of the drawings]

[0031] [Figure 1] 1 depicts a cross-sectional view of a zinc oxide particle according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] Other objects, features, aspects and advantages of the present invention will become more apparent on reading the following description and examples.

[0033] As used herein, unless otherwise specified: - the term "at least one" is equivalent to and may be replaced with the term "one or more"; - the expression "to the extent of" is equivalent to and may be substituted for the expression "to the extent of" and indicates that a limit is included; - the expression "keratinous materials" denotes in particular human keratinous fibres such as skin and hair; - The core (1), also called the "center", - the upper coating layer (2), also called the "outer layer", "shell" or "coating"; - the expression "organic (inorganic) compound" is equivalent to "organic or inorganic compound"; - "Alkyl" means "alkyl group", i.e. C1-C 10, in particular a C1-C8, more particularly C1-C6 and preferentially C1-C4 linear or branched hydrocarbon-based radical, such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl or tert-butyl, an "aryl" group is understood to mean a monocyclic or fused or non-fused polycyclic carbon-based group containing 6 to 22 carbon atoms, at least one ring of which is aromatic, preferentially an aryl group is phenyl, biphenyl, naphthyl, indenyl, anthracenyl or tetrahydronaphthyl, preferably phenyl; - An "arylate" group is one or more -C(O)O groups, such as naphthalate or naphthenate. - is understood to mean an aryl group containing a carboxylate group, - "complexed zinc" is understood to mean that zinc forms a "metal complex" or "coordination compound" in which the metal ion corresponding to the central atom, i.e. zinc, is chemically bound to one or more electron donors (ligands); - "ligand" is understood to mean a coordinating organic chemical group or compound, i.e. which comprises at least one carbon atom and is capable of coordinating to a metal, in particular a Zn atom, preferably Zn(II), and which, when coordinated or complexed, results in a metal compound (unique complex or chelate) which corresponds to the principle of a coordination sphere with a given number of electrons - see Ullmann's Encyclopedia of Industrial Chemistry, "Metal complex dyes", 2005, p. 1-42. More specifically, the ligand is an organic group which comprises at least one group which is electron donating by inductive and / or mesomeric effect, more specifically it has at least one electron donating group which is amino, phosphino, hydroxy or thiol, or the ligand is a persistent carbene, in particular of the "argengo" type (imidazol-2-ylidene) or it comprises at least one carbonyl group. As ligands, more specifically, mention may be made of: i) those containing at least one phosphorus atom -P<, i.e. phosphines such as triphenylphosphine; ii) bidentate ligands of the formula RC(X)-CR'R''-C(X)-R''', such as acetylacetone or β-diketones, where R and R'' are the same or different and represent a linear or branched (C1-C6) alkyl group, R' and R'' are the same or different and represent a hydrogen atom or a linear or branched (C1-C6) alkyl group, preferentially R' and R'' represent a hydrogen atom and X represents an oxygen atom, a sulfur atom or an N(R) group, where R represents a hydrogen atom or a linear or branched (C1-C6) alkyl group; iii) lactic acid, glycolic acid, tartaric acid, citric acid and maleic acid as well as arylates, such as naphthalates, of the formula [HO-C(O)]. n-AC(O)-OH (poly)hydroxycarboxylic acid ligands and their deprotonated forms, in which A represents a monovalent group when the value of n is zero or a polyvalent group when n is 1 or more, which is a saturated or unsaturated, cyclic or acyclic, aromatic or non-aromatic, based on a hydrocarbon containing 1 to 20 carbon atoms, optionally interrupted by one or more heteroatoms and / or optionally substituted, in particular substituted by one or more hydroxyl groups, preferably A represents a monovalent (C1-C6) alkyl group or a polyvalent (C1-C6) alkylene group, optionally substituted by one or more hydroxyl groups, n represents an integer from 0 to 10 (both end values ​​inclusive), preferably n is from 0 to 5, e.g. from 0, 1 or 2, and iv) C2-C alkyl groups containing 2 to 5 hydroxyl groups. 10 polyol ligands, in particular ethylene glycol, glycerol, more particularly further ligands having carboxy, carboxylate or amino groups, in particular selected from acetate, (C1-C6)alkoxylate, (di)(C1-C6)alkylamino and arylate, such as naphthalate or naphthenate groups; The term "fuel" is understood to mean a liquid compound that burns in a chemical reaction that produces heat: combustion, using dioxygen and energy. In particular, liquid fuels are selected from aprotic solvents, in particular alcohols such as methanol, ethanol, isopropanol, n-butanol, esters such as those derived from methyl esters and acetates (such as 2-ethylhexyl acetate), acids (such as 2-ethylhexanoic acid (EHA)), acyclic ethers (such as ethyl ether, methyl tert-butyl ether (MTBE), methyl tert-amyl ether (TAME), methyl tert-hexyl ether (THEME), ethyl tert-butyl ether (ETBE), ether tert-amyl ether (TAEE), diisopropyl ether (DIPE)), cyclic ethers (such as tetrahydrofuran (THF)), aromatic hydrocarbons or arenes (such as xylene), aprotic solvents, in particular selected from non-aromatic hydrocarbons, and mixtures thereof. The fuel may optionally be selected from liquefied hydrocarbons such as acetylene, methane, propane or butane, and mixtures thereof.

[0034] The term "pigment" is understood to mean any inorganic pigment of synthetic or natural origin that colours keratinous materials and has a solubility in water at 25° C. and atmospheric pressure (760 mmHg) of less than 0.05% by weight, preferably less than 0.01% by weight.

[0035] These are white or colored solid particles that are essentially insoluble in the hydrophilic and lipophilic liquid phases commonly used in cosmetics. More specifically, they are pigments that are poorly soluble or insoluble in aqueous-alcoholic media.

[0036] The pigments that can be used are selected from inorganic pigments known in the art, in particular those described in Kirk-Othmer's Encyclopedia of Chemical Technology and Ullmann's Encyclopedia of Industrial Chemistry.Pigments that may be mentioned in particular include inorganic pigments such as those defined and described in Ullmann's Encyclopedia of Industrial Chemistry "Pigment organics", 2005 Wiley-VCH Verlag GmbH&Co.KGaA, Weinheim and in the same book "Pigments, Inorganic, 1. General", 2009 Wiley-VCH Verlag GmbH&Co.KGaA, Weinheim.

[0037] These pigments may be in powder form. The pigments may be selected, for example, from inorganic pigments, pigments with special effects such as pearlescent or glitter flakes, and mixtures thereof.

[0038] The pigment may be an inorganic pigment. The term "inorganic pigment" is intended to mean any pigment that meets the definition in the chapter on inorganic pigments of Ullmann's encyclopaedia. Among the inorganic pigments useful in the present invention, mention may be made of iron oxide, chromium oxide, manganese violet, ultramarine blue, chromium hydrate, ferric blue and titanium dioxide. The pigment may be a special effect pigment.

[0039] The term "special effect pigments" refers to pigments that generally produce colored appearances (characterized by a particular hue, a particular sparkle, and a particular level of brightness) that are non-uniform and vary depending on the conditions of observation (light, temperature, angle of observation, etc.) Thus, they differ from colored pigments that exhibit standard uniform shades of opaque, translucent, or transparent.

[0040] Examples of special effect pigments which may be mentioned include pearlescent pigments, such as titanic mica coated with iron oxide, mica coated with iron oxide, mica coated with bismuth oxychloride, titanic mica coated with chromium oxide, in particular dye-coated titanic mica of the type mentioned above, and also pearlescent pigments based on bismuth oxyhalides, such as bismuth oxychloride.

[0041] The pearlescent agent may more particularly have a yellow, pink, red, bronze, orange, brown, gold and / or copper color or shade.

[0042] Examples of pearlescent agents which may be used in the context of the present invention include the gold pearlescent agents sold in particular under the names Gold 222C (Cloisonne), Sparkle gold (Timica), Gold 4504 (Chromalite) and Monarch gold 233X (Cloisonne) by the company Engelhard, the bronze pearlescent agents sold in particular under the names Bronze fine (17384) (Colorona) and Bronze (17353) (Colorona) by the company Merck, under the name Prestige Bronze by the company Eckart and under the name Super bronze (Cloisonne) by the company Engelhard, in particular under the names Orange 363C (Cloisonne) and Orange MCR 101 (Cosmica) by the company Engelhard and the names Passion orange (Colorona) and Matte orange (17449) (Microna), brown pearlescent agents sold in particular under the names Nu-antique copper 340XB (Cloisonne) and Brown CL4509 (Chromalite) by the company Engelhard, pearlescent agents with a coppery shade sold in particular under the name Copper 340A (Timica) by the company Engelhard and under the name Prestige Copper by the company Eckart, pearlescent agents with a red shade sold in particular under the name Sienna fine (17386) (Colorona) by the company Merck, pearlescent agents with a yellow shade sold in particular under the name Yellow (4502) (Chromalite) by the company Engelhard, red pearlescent agents with a golden shade sold in particular under the name Sunstone G012 (Gemtone) by the company Engelhard, in particular Nu antique bronze 240 A black pearlescent agent with a golden hue sold by AB (Timica), in particular the one sold by Merck under the name Matte blue (17433) (Microna), DarkMention may be made of the blue pearlescent agent sold in particular under the name Xirona Blue (117324) (Colorona), the white pearlescent agent having a silvery tinge, sold in particular under the name Xirona Silver by the company Merck, as well as the gold-green, pink-orange pearlescent agents sold in particular under the name Indian summer (Xirona) by the company Merck, and mixtures thereof.

[0043] In addition to pearlescent agents on mica carriers, multi-layer pigments based on synthetic substrates such as alumina, silica, sodium calcium or calcium aluminum borosilicate and aluminum may also be envisaged.

[0044] Method for preparing particles coated with silicon oxide The preparation method according to the invention comprises a step (a) of preparing a composition (A) containing one or more precursors of element M and one or more combustible solvents, said element M being selected from alkali metals from column 1, alkaline earth metals from column 2, elements from columns 3 to 16 and elements from the lanthanide group of the Periodic Table of the Elements.

[0045] Advantageously, the element M is selected from magnesium, calcium, zinc, copper, iron, titanium, zirconium, aluminum, gallium, indium, tin, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, preferably from magnesium, calcium, zinc, copper, iron, titanium, aluminum, tin, lanthanum, cerium and yttrium.

[0046] The precursor of element M preferably comprises one or more atoms of element M optionally complexed with one or more ligands containing at least one carbon atom, more preferentially with one or more ligands containing at least two carbon atoms.

[0047] Preferably, the ligands are selected from acetate, (C1-C6)alkoxylate, (di)(C1-C6)alkylamino and arylate, such as naphthalate or naphthenate groups.

[0048] The flammable solvents which can be used according to the invention can be selected from the flammable solvents conventionally used in flame spray pyrolysis.

[0049] Preferably, the flammable solvent is selected from protic flammable solvents, aprotic flammable solvents and mixtures thereof, more preferentially from alcohols, esters, acids, acyclic ethers, cyclic ethers, aromatic hydrocarbons or arenes, non-aromatic hydrocarbons and mixtures thereof, and even more preferably from 2-ethylhexyl acetate, 2-ethylhexanoic acid (EHA), ethyl ether, methyl tert-butyl ether (MTBE), methyl tert-amyl ether (TAME), methyl tert-hexyl ether (THEME), ethyl tert-butyl ether (ETBE), ether tert-amyl ether (TAEE), diisopropyl ether (DIPE), tetrahydrofuran (THF), xylene and mixtures thereof.

[0050] More preferentially, the flammable solvent is chosen from aprotic flammable solvents containing at least 3 carbon atoms, more preferentially from xylene, tetrahydrofuran, 2-ethylhexyl acetate, 2-ethylhexanoic acid (EHA) and mixtures thereof.

[0051] Advantageously, the content of element M precursor in composition (A) is between 1% and 60% by weight, preferably between 15% and 30% by weight, relative to the total weight of composition (A).

[0052] The preparation method according to the present invention further comprises a step (b) of injecting the composition (A) prepared in step (a) and an oxygen-containing gas into a flame spray pyrolysis (FSP) device to form a flame.

[0053] During this step (b), the composition (A) and the oxygen-containing gas are advantageously injected into the flame spray pyrolysis apparatus by two injections separated from each other, in other words, the composition (A) and the oxygen-containing gas are injected separately, i.e. the composition (A) and the oxygen-containing gas are not injected by a single nozzle.

[0054] More specifically, composition (A) is transported through one tube, while an oxygen-containing gas (also called "dispersed oxygen") is transported through another tube. The inlets of the two tubes are positioned such that the oxygen-containing gas creates a negative pressure, which draws up composition (A) by the Venturi effect and converts it into droplets.

[0055] Step (b) may optionally further comprise the additional injection of a "premix" mixture comprising oxygen and one or more combustible gases. This "premix" mixture, also called "flame support oxygen", allows the generation of a flame support intended to ignite and sustain the flame arising from composition (A) and the oxygen-containing gas (i.e., "dispersed oxygen").

[0056] Preferably, during step (b), composition (A), the oxygen-containing gas and optionally the "premix" mixture (if present) are injected into a reaction tube, also called "filling tube". Preferably, this reaction tube is made of metal or quartz. Advantageously, the reaction tube has a height of at least 30 cm, more preferentially at least 40 cm and even at least 50 cm. Advantageously, the length of said reaction tube is between 30 cm and 300 cm, preferably between 40 cm and 200 cm, more preferentially between 45 cm and 100 cm and even more preferably, this length is 50 cm.

[0057] The mass ratio between the mass of the solvent present in composition (A) on the one hand and the mass of the oxygen-containing gas on the other hand is defined as follows: first, the amount of oxygen-containing gas (also called oxidizer compound) is calculated for the aggregate formed by composition (A) (i.e. the combustible solvent and zinc precursor on the one hand and the oxygen-containing gas on the other hand) so that they can react together in a combustion reaction in stoichiometric ratio (thus without excess or deficiency of oxidizer compound).

[0058] Starting from this calculated amount of oxygen-containing gas, also called "calculated oxidant", a new calculation is carried out according to the following formula in order to derive from this the amount of oxygen-containing gas to be injected, also called "injected oxidant", where φ is preferably between 0.30 and 0.9, more preferentially between 0.4 and 0.65.

[0059] This method is defined, inter alia, by Turns, S. R. in An Introduction to Combustion: Concepts and Applications, 3rd ed.; McGraw-Hill: New York, 2012.

[0060] Step (b) of the preparation method according to the invention allows obtaining aggregates of element M oxide. Preferably, the element M oxide thus formed is stable. The term "stable" is understood to mean a higher oxide than the metal would assume in an oxidizing medium. By way of example, if an iron precursor is used, the oxide obtained is Fe2O3 and not Fe3O4. Similarly, if a copper precursor is used, the oxide obtained is CuO and not Cu2O.

[0061] More preferentially, the oxide of element M has the formula M x O y where x and y are such that 1≦y / x≦2.

[0062] According to one particular embodiment of the invention, the element M is selected from the alkaline earth metals from the second column of the periodic table of the elements, so that the M oxide formed has the formula MO. In other words, according to this embodiment, x=y=1.

[0063] According to yet another particular embodiment of the invention, the element M is selected from the elements from columns 3 to 16 and from the lanthanide group, more particularly from the elements from columns 3 and 4, from the lanthanide group, from column 8 and from columns 11 to 14 of the Periodic Table of the Elements.

[0064] According to this embodiment, the oxide of element M thus formed is preferably selected from zinc oxide ZnO, magnesium oxide MgO, calcium oxide CaO, copper oxide CuO, titanium oxide TiO2, iron oxide Fe2O3, aluminum oxide Al2O3, cerium oxide CeO2, lanthanum oxide La2O3 and yttrium oxide Y2O3, and more preferentially from zinc oxide ZnO, magnesium oxide MgO, calcium oxide CaO, copper oxide CuO, titanium oxide TiO2 and iron oxide Fe2O3.

[0065] The preparation method according to the present invention further comprises a step (c) of injecting into the flame formed during step (b) a composition (B) comprising one or more silicon precursors and one or more polar protic solvents other than water, the silicon precursors comprising at least two silicon atoms and several Si-carbon covalent bonds.

[0066] In other words, the method of the present invention is continuous and the flame formed in step (b) is maintained.

[0067] During step (c) of the preparation method of the present invention, compositions (A) and (B) are injected separately and simultaneously. In other words, composition (A) is transported by one tube, while composition (B) is transported by another tube. The distance between the outlets of the two tubes is preferably at least 30 cm, more preferentially at least 40 cm.

[0068] Preferably the flame formed during step (b) is at a temperature of 2000° C. or greater in at least a part of the flame.

[0069] At the site of injection of composition (B) into the flame formed in step (b) and maintained in step (c), i.e. during step (c), the temperature is preferably between 200°C and 600°C, more preferentially between 300°C and 400°C.

[0070] Advantageously, during step (c), composition (B) is injected through a spray ring placed above said reaction tube as described above, in which the injection of composition (A) in particular takes place.

[0071] The silicon precursor of composition (B) contains at least two silicon atoms and several Si-carbon covalent bonds, preferably at least three silicon atoms and several Si-carbon covalent bonds.

[0072] Advantageously, the silicon precursor is chosen from hexadimethyldisiloxane, 1,2-bis(triethoxysilyl)ethane, 1,2-bis(trimethoxysilyl)ethane and mixtures thereof.

[0073] Preferably, the silicon oxide thus formed is silicon dioxide SiO2, the latter more preferentially having a "four-membered ring" structure.

[0074] In the process according to the invention, (M / silicon) 注入 It is possible to calculate the molar atomic ratio, which corresponds to the molar amount of atoms of element M implanted in step (b) on the one hand, relative to the molar amount of silicon atoms implanted in step (c) on the other hand. Preferably, this (M / silicon) 注入 The molar atomic ratio is in the range from 0.1 to 10, more preferentially from 0.2 to 2, more preferentially from 0.5 to 1.5.

[0075] Preferably, nitrogen is bubbled through the composition (B) of the present invention before injection in step (c).The injection rate of the composition (B) can be controlled by pressure determinations known to those skilled in the art, such as the method prescribed by Scott, DW; Messerly, JF; Todd, SS; Guthrie, GB; Hossenlopp, IA; Moore, RT; Osborn, AG; Berg, WT; McCullough, JP, Hexamethyldisiloxane: chemical thermodynamic properties and internal rotation about the siloxane linkage, J.Phys.Chem., 1961, 65, 1320-6.

[0076] According to one particular embodiment of the invention, said composition (B) is brought to a temperature ranging from 25°C to 70°C, more preferentially from 30°C to 60°C, before its injection during step (c).

[0077] Preferably, the content of silicon precursor in composition (B) injected during step (c) of the method according to the invention is between 1% and 60% by weight, more preferably between 5% and 30% by weight, relative to the total weight of composition (B).

[0078] Advantageously, the polar protic solvent other than water present in composition (B) is chosen from (C1-C8) alkanols. More preferentially, composition (B) comprises ethanol.

[0079] Preferably, the polar protic solvent other than water present in composition (B) is selected from solvents which are flammable at the flame temperature of step (c) and are preferably flammable at temperatures between 200° C. and 600° C., more preferentially between 300° C. and 400° C. More preferably, the polar protic solvent other than water present in composition (B) has a boiling point above room temperature (25° C.), more preferentially between 50° C. and 120° C.

[0080] Preferably, the content of the polar protic solvent other than water present in composition (B) is from 40% to 99% by mass, more preferentially from 50% to 98% by mass, even more preferentially from 70% to 95% by mass, relative to the total mass of composition (B).

[0081] According to a preferred embodiment of the invention, the preparation process according to the invention comprises the steps of: - a treatment step (d1) comprising introducing the particles of oxide of element M obtained at the end of step (c) into an alkaline bath having a pH between 7 and 11, preferentially between 7.5 and 9, and / or - a step (d2) of calcining the particles of oxide of element M obtained at the end of step (c) or at the end of treatment step (d1); Further includes:

[0082] If the treatment step (d1) is present, (i) the treatment preferably lasts for between 10 and 600 minutes, more preferentially between 40 and 300 minutes, and / or (ii) the pH of the alkaline bath preferably varies between 7 and 11, more preferentially between 7.5 and 9, and / or (iii) the temperature is preferably room temperature, i.e. 25° C.; and / or (iv) The content of particles of oxide of element M obtained at the end of step (c) in the alkaline bath is preferably between 0.5 and 100 g of particles per liter of alkaline bath, more preferentially between 1 and 10 g of particles per liter of alkaline bath.

[0083] If the calcination step (d2) is present, (i) the calcination is preferably continued for 60 to 400 minutes, more preferentially for 60 to 180 minutes, and / or (ii) The temperature range is preferably from 100°C to 600°C, more preferentially from 100°C to 300°C, and even more preferentially from 130°C to 250°C.

[0084] According to one particular embodiment of the invention, the manufacturing process further comprises, at the end of step (c), a treatment step (d1) followed by a calcination step (d2).

[0085] According to one particular embodiment of the invention, the particles of oxide of element M obtained by the preparation method according to the invention are doped. According to this embodiment of the invention, composition (A) further comprises one or more precursors of an element D different from element M, D being selected from fluorine, yttrium, vanadium, scandium, zirconium, hafnium, iron, copper and tungsten.

[0086] Particles of element M oxide Another subject of the invention is a particle of oxide of element M comprising a core (1) and one or more upper coating layers (2) covering said core (1), (i) the core (1) consists of one or more oxides of element M, preferably in a crystalline state; (ii) the upper coating layer (2) comprises one or more silicon oxides SiO2 and covers at least 90% of the surface of the core (1), preferably covering the entire surface of the core (1); (iii) the element M is selected from magnesium, calcium, zinc, copper, iron, zirconium, aluminum, gallium, indium, tin, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium; and (iv) (M / silicon) 粒子 The molar atomic ratio is in the range of 0.1 to 10, preferably 0.2 to 2, and more preferably 0.5 to 1.5. The particles are characterized by the above.

[0087] Preferably, the particles according to the invention comprise a core 1 consisting of an oxide of element M in a crystalline state. The crystalline state of core 1 and its composition can be determined, for example, by conventional X-ray diffraction methods.

[0088] Advantageously, the core 1 of the particle according to the invention consists of one or more aggregates of crystalline primary particles of an oxide of element M. In other words, the core 1 consists of several crystallites of an oxide of element M.

[0089] Preferably, the particles of oxide of element M are obtained by the preparation process of the invention as defined above.

[0090] The particles of the oxide of the element M according to FIG. 1 consist of the oxide of the element M in a crystalline state and contain one or more aggregates of primary particles of the oxide of the element M and have a diameter D m Includes Core 1.

[0091] The particles of oxide of element M according to FIG. 1 completely cover the surface of the core 1 and have a thickness d m It also includes an upper coating layer 2 having

[0092] Number average diameter D of core 1 m can be determined, for example, by transmission electron microscopy (abbreviated as TEM). Preferably, the number-average diameter D of the core 1 of the particles according to the invention m is in the range of 3 to 1000 nm, more preferentially 6 to 50 nm, and even more preferentially 10 to 30 nm.

[0093] The particles of oxide of element M according to the invention comprise one or more upper coating layers covering at least 90% of the surface of the core 1, and preferably covering the entire surface of the core.

[0094] The degree of coverage of the core by the upper coating layer can be determined, for example, by visual analysis of the TEM-BF or STEM-HAADF type combined with a SEM-EDX analysis.

[0095] Each analysis is carried out on a statistical number of particles, in particular at least 20 particles. The particles are deposited on a metal grid made of a metal different from element M and from other metals forming part of the particle (core or upper coating layer). For example, the grid is made of copper (unless it is desired to use copper in the manufacture of the particles).

[0096] Visual analysis of the TEM-BF and STEM-HAADF images allows one to infer, based on contrast, whether the coating completely surrounds the core of the particle. Each of the 20 (or more) images can be analyzed to estimate the degree of coverage of the core, and then averaged to determine the average degree of coverage.

[0097] By STEM-EDX analysis it is possible to verify that the coating indeed contains mainly or only silicon. For this purpose, measurements must be made at the edge of the particles (for at least 20 particles). These measurements then reveal silicon.

[0098] STEM-EDX analysis also makes it possible to verify that the core does indeed not contain the element M. For this, measurements must be made in the center of the particles (for at least 20 particles). These measurements then reveal the elements M and silicon.

[0099] Preferably, the upper coating layer completely covers the surface of the core.

[0100] Number average thickness of the upper coating layer d m The number average thickness d can also be determined by transmission electron microscopy. m is in the range of 1 to 30 nm, more preferentially 1 to 15 nm, and even more preferentially 1 to 6 nm.

[0101] Advantageously, the upper coating layer is amorphous.

[0102] The core consists of one or more oxides of element M.

[0103] Advantageously, the element M is selected from magnesium, calcium, zinc, copper, iron, zirconium, aluminum, gallium, indium, tin, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, preferably from magnesium, calcium, zinc, copper, iron, aluminum, tin, lanthanum, cerium and yttrium.

[0104] Preferably, the oxide of element M thus formed is stable and advantageously has the formula M x O y where x and y are such that 1≦y / x≦2.

[0105] According to one particular embodiment of the invention, the element M is selected from magnesium and calcium, so that the oxide of element M formed has the formula MO, in other words, according to this embodiment, x=y=1.

[0106] According to another particular embodiment of the invention, the element M is selected from zinc, copper, iron, zirconium, aluminum, gallium, indium, tin, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and more particularly from zinc, copper, iron, aluminum, tin, lanthanum, cerium and yttrium.

[0107] According to these embodiments, the oxide of element M thus formed is preferably selected from zinc oxide ZnO, magnesium oxide MgO, calcium oxide CaO, copper oxide CuO, iron oxide Fe2O3, aluminum oxide Al2O3, cerium oxide CeO2, lanthanum oxide La2O3 and yttrium oxide Y2O3, and more preferentially from zinc oxide ZnO, magnesium oxide MgO, calcium oxide CaO, copper oxide CuO and iron oxide Fe2O3.

[0108] The particles of the oxide of element M according to the invention are characterized in that the (M / silicon) of the particles according to the invention 粒子 It contains, in molar atomic ratio, the element M and silicon.

[0109] This ratio corresponds, on the one hand, to the molar amount of silicon atoms present in the particles according to the invention, and, on the other hand, to the molar amount of atoms of the element M present in the particles according to the invention.

[0110] This ratio can be determined by spectroscopic analysis according to one of the following two methods: According to the first method, the powder is spread and an X-ray fluorescence measurement study is carried out using an X-ray spectrometer, from which the metal ratio is deduced; According to another method, the particles of the invention are dissolved beforehand in acid. Then, the material obtained is subjected to an elemental analysis by ICP-MS (Inductively Coupled Plasma Mass Spectroscopy), from which the metal ratio is deduced.

[0111] Preferably, this (M / silicon) 粒子 The molar atomic ratio is in the range of 0.1 to 10, preferably 0.2 to 2, and more preferentially 0.5 to 1.5.

[0112] The number average diameter of the particles according to the invention can also be determined by transmission electron microscopy. Preferably, the number average diameter of the particles according to the invention is in the range of 3 to 1000 nm, more preferentially 10 to 100 nm and even more preferentially 15 to 70 nm.

[0113] Preferably, the particles according to the invention have a BET specific surface area of ​​1 m 2 / g~350m 2 / g, more preferentially 1m 2 / g~200m 2 / g, and more preferentially 30-100m 2 / g.

[0114] Preferably, the sum of the content of element M oxide and the content of silicon oxide is at least equal to 99% by weight relative to the total weight of the core 1 and of the upper coating layer 2 .

[0115] The particles of element M oxide may optionally further comprise an additional coating layer overlying the upper coating layer and comprising at least one hydrophobic organic compound.

[0116] The hydrophobic organic compound contained in the additional coating layer is more preferentially chosen from silicones, in particular silicones containing at least one fatty chain, carbon-based derivatives containing at least 6 carbon atoms, in particular fatty acid esters, and mixtures thereof.

[0117] The additional coating layer can be produced by liquid or solid methods. Through liquid methods, the hydroxyl functional groups on the surface of the particles react with reactive functional groups of the compound that forms the coating (typically silanol functional groups of silicones or acid functional groups of carbon-based fatty materials). Through solid methods, the particles are contacted with a liquid or paste-like compound that contains a hydrophobic material. The mixture is then dried after contact, and the mixture is pulverized, for example, by milling.

[0118] Another subject of the invention relates to a composition, preferably a cosmetic composition, comprising one or more particles of an oxide of element M as defined above and preferably obtained by a preparation process according to the invention.

[0119] The composition according to the invention is advantageously an aqueous composition.

[0120] The coated particles of the oxide of element M of the present invention may be present in dry form (powder, flakes, plates), as a dispersion, or as a liquid suspension, or even as an aerosol. The coated particles of the oxide of element M of the present invention may be used as such or in admixture with other components.

[0121] The composition of the invention may be in various galenic forms: it may thus be in the form of a powder (pulverulent) composition or a liquid composition or in the form of a milk, cream, paste or aerosol composition.

[0122] The composition according to the invention is in particular a cosmetic composition. That is to say, the multi-layer material according to the invention is a cosmetic medium. The term "cosmetic medium" means a medium suitable for application to keratinous materials, in particular human keratinous materials such as the skin, said cosmetic medium generally consisting of water or a mixture of water and one or more organic solvents or a mixture of organic solvents. Preferably, the composition comprises water, in particular in a content of 5% to 95% by weight relative to the total weight of the composition.

[0123] The term "organic solvent" refers to an organic substance that can dissolve another substance without chemically modifying it. Examples of organic solvents that can be used in the composition of the present invention include lower C2-C6 alkanols, such as ethanol and isopropanol, polyols and polyol ethers, such as 2-butoxyethanol, propylene glycol, propylene glycol monomethyl ether, and diethylene glycol monoethyl ether and monomethyl ether, and aromatic alcohols, such as benzyl alcohol or phenoxyethanol, and mixtures thereof.

[0124] When present, the organic solvent is preferably present in a proportion of from about 0.1% to 40% by weight, more preferentially from about 1% to 30% by weight, and even more preferentially from 5% to 25% by weight, relative to the total weight of the composition.

[0125] The compositions of the invention may contain a fatty phase and may be in the form of a direct or inverse emulsion.

[0126] The content of particles of oxide of element M present in the composition of the invention is preferably in the range of 0.1% by weight to 40% by weight, more preferentially 0.5% by weight to 20% by weight, even more preferentially 1% by weight to 10% by weight and more preferentially 1.5% by weight to 5% by weight, relative to the total weight of the composition.

[0127] According to a particular embodiment of the present invention, the composition according to the present invention can be in the form of anhydrous composition, for example in the form of oil.The term "anhydrous composition" is intended to mean a composition that contains less than 2% by weight of water, preferably less than 1% by weight of water, and even more preferentially less than 0.5% by weight of water relative to the total weight of the composition, or even a composition that does not contain water.In this type of composition, the water that may be present corresponds to the residual water that is not added during the preparation of the composition, but is carried over from the mixed raw materials.

[0128] The compositions according to the invention can be prepared according to techniques known to those skilled in the art, and may in particular be in the form of simple or multiple emulsions (abbreviated as oil-in-water or O / W, water-in-oil or W / O, oil-in-water-in-oil or O / W / O or water-in-oil-in-water or W / O / W), such as creams, milky or creamy gels, or in the form of powders or aerosol compositions.

[0129] Another subject of the invention is a composition according to the invention, preferably a cosmetic composition, for use in protecting the skin, in particular human skin, against visible radiation (i.e. wavelengths between 400 nm and 800 nm) and / or ultraviolet radiation (i.e. wavelengths between 100 nm and 400 nm), UV-A radiation (i.e. wavelengths between 320 nm and 400 nm) and / or UV-B radiation (i.e. wavelengths between 280 nm and 320 nm). The compositions according to the invention make it possible to efficiently screen solar radiation, which are broad-spectrum, in particular against UV-A radiation (including long-wave UV-A radiation), whilst being particularly stable over time under UV exposure.

[0130] The composition according to the invention may optionally comprise, besides the particles of element oxide M according to the invention, one or more additional UV filters chosen from hydrophilic, lipophilic or insoluble organic UV filters and / or one or more inorganic pigments. It will preferentially be composed of at least one hydrophilic, lipophilic or insoluble organic UV filter.

[0131] Another subject of the invention is the use of particles of oxide of element M as defined above, preferably obtained by the process according to the invention, in - formulating cosmetic or pharmaceutical compositions intended in particular to protect the skin, in particular human skin, against visible and / or ultraviolet radiation or to modify the appearance of the skin, in particular human skin, - Formulating paints, varnishes and / or stains; or - Producing coatings for electronic devices or products, in particular to obtain moisture-resistant electronic components For use.

[0132] How to apply Another subject of the invention is a method for treating keratinous materials, in particular human keratinous materials such as the skin, by applying a composition as defined above to the material, preferably by 1 to 5 successive applications, with drying between the layers, the application being by spraying or in other manner.

[0133] The composition of the present invention can be used for single application or multiple applications. When the composition of the present invention is intended for multiple applications, the content of particles of the oxide of element M of the present invention is usually lower than that in the composition intended for single application.

[0134] For the purposes of the present invention, the term "single application" means a single application of the composition, which application is optionally repeated several times a day, each application being separated from the next by one or more hours, if desired, or a single application per day.

[0135] For purposes of the present invention, the term "multiple applications" refers to the application of the composition multiple times, usually 2 to 5 times, with each application separated by a few seconds to a few minutes from the next application. Each multiple application can be repeated multiple times a day, or once a day, if desired, separated by an hour or more from the next application.

[0136] They may be connected application methods such as a saturated single application, i.e. a single application of a cosmetic composition comprising a high concentration of particles of element M oxide coated with silicon oxide according to the present invention, or multiple applications of (less concentrated) cosmetic compositions comprising one or more particles of element M oxide coated with silicon oxide according to the present invention. In the case of multiple applications, multiple successive applications of a cosmetic composition comprising one or more particles of element M oxide coated with silicon oxide according to the present invention may be repeated with or without a delay between applications.

[0137] According to one embodiment of the present invention, multiple applications are performed on the keratinous material with a drying step between successive applications of the cosmetic composition comprising particles of element M oxide coated with silicon oxide according to the present invention. The drying step between successive applications of the cosmetic composition comprising one or more particles of element M oxide coated with silicon oxide according to the present invention can be carried out outdoors or artificially, for example using a hot air drying system such as a hair dryer.

[0138] Another subject of the present invention is the use of one or more particles of oxide of element M coated with silicon oxide according to the invention as defined above as a UVA and UVB screening agent for protecting keratinous materials, in particular human keratinous materials such as the skin.

[0139] The following examples serve to illustrate the invention without being limiting in nature. EXAMPLES

[0140] Example 1: 1.1. First, a composition (A) of zinc naphthenate (500 mM) in xylene was prepared. Then, zinc oxide particles P1 coated with silicon dioxide were prepared using an FSP method according to the invention, which involves the injection of composition (A) with composition (B) comprising hexadimethyldisiloxane and ethanol in a ratio of 3:1.

[0141] The preparation method parameters are as follows: - Ratio (composition (A) / O2) = 5 / 7, i.e. 5 mL / min liquid and 7 L / min gas (O2). To adjust the oxygen flow rate, φ = 0.48 is used.

[0142] In this method, a quartz tube with a height of 40 cm is used. Furthermore, nitrogen is first blown into the composition (B). When the composition (B) is injected, the flow of nitrogen heated to 25°C allows the evaporation of hexadimethyldisiloxane (HMDSO) and the ratio (Zn / Si) 注入 The ratio is adjusted to be 1.

[0143] 1.2. The Raman spectrum of these particles showed that the coating has a specific structure, with silicon atoms mainly in the form of "four-membered rings". The peaks of the "three-membered rings" of Si-O are also present, but are less intense and have a smaller peak area.

[0144] 1.3 Water resistance rating: An aqueous suspension S1 was prepared from particles P1 and water at a content of 100 mg of P1 per liter of water. The suspension S1 thus obtained was then placed in an ultrasonic bath at a power of 20 W for 10 minutes.

[0145] A portion of suspension S1 was then brought to pH=5 with a nitric acid solution. The Zn present in the suspension was then measured as a function of time and in comparison with the amount of zinc introduced. 2+ The ionic content was measured by conventional anodic stripping voltammetry.

[0146] The results are listed in the table below.

[0147] [Table 1]

[0148] t0 corresponds to the first measurement taken less than 10 minutes after the end of the ultrasonic bath.

[0149] It should be noted that the coated zinc oxide particles P1 obtained according to the preparation method of the invention have good water resistance, even at acidic pH.

[0150] Example 2: 2.1. Zinc oxide particles P2 coated with silicon dioxide were prepared according to the method described in Example 1. The particles P2 thus obtained were then divided into two groups P2a and P2b. The particles P2a were post-treated according to the following protocol, whereas the particles P2b were not.

[0151] Protocol for post-processing of P2a particles: After collecting the particles obtained by the method, two processes are performed: a treatment step (d1) consisting in introducing the particles of oxide of element M obtained at the end of step (c) into an alkaline bath (a mixture of sodium hydroxide and water) at a pH of 7.5, a temperature of 25° C. and a ratio of 5 g of particles per liter of alkaline bath, for 120 minutes, - a step (d2) of calcining the particles of oxide of element M obtained at the end of step (d1) at 200°C for 120 minutes.

[0152] 2.2. The zinc oxide particles P2a and P2b thus obtained were observed to be crystalline and coated with silicon dioxide. (Zn / Si) 粒子 The atomic ratio is 1, and the BET specific surface area of ​​the particles is 116 m for particle P2a. 2 / g, 74m for particle P2b 2 / g. Furthermore, the particles have a number average diameter of 40 nm.

[0153] When a water resistance test equivalent to that of Example 1 was carried out, it was shown that the particles that had been subjected to the FSP treatment and post-treatment (P2a) had even higher water resistance.

[0154] An aqueous suspension S1' was prepared from particles P2a and water at a content of 100 mg of P2a per liter of water. The suspension S1' thus obtained was then placed in an ultrasonic bath at a power of 20 W for 10 minutes.

[0155] A portion of suspension S'1 was then brought to pH=5 with a nitric acid solution. The Zn present in the suspension was then measured as a function of time and in comparison with the amount of zinc introduced. 2+ The ionic content was measured by conventional anodic stripping voltammetry.

[0156] The results are listed in the table below.

[0157] [Table 2]

[0158] 2.3 Water resistance rating: Two aqueous suspensions S2a and S2b were prepared from particles P2a and P2b and water at a content of 100 mg of particles per liter of water at pH 8.2.

[0159] Furthermore, an aqueous suspension S3 was prepared from zinc oxide particles sold by BASF under the standard Z-COTE HP1 (zinc oxide and triethoxycaprylylsilane) and water at a content of 100 mg of commercial particles per liter of water. In other words, the particles Z-COTE HP1 are coated with a layer of triethoxycaprylylsilane, which provides hydrophobicity and protection from water. The BET specific surface area of ​​these particles is 15.8 m 2 / g.

[0160] The suspensions S2a, S2b and S3 thus obtained were then placed in an ultrasonic bath for 10 minutes at a power of 20 W.

[0161] Thereafter, the Zn present in each of the suspensions S2a, S2b and S3 as a function of time 2+ The ionic content was measured at various time points for each suspension by conventional anodic stripping voltammetry.

[0162] The results are listed in the table below.

[0163] [Table 3]

[0164] t0 corresponds to the first measurement taken less than 10 minutes after the end of the ultrasonic bath.

[0165] The Raman spectrum of S2a is similar to that of S1, i.e., peaks corresponding to silicon atoms in the form of "four-membered rings" are present. Peaks corresponding to the Si-O "three-membered rings" are also present, but with lower intensity and smaller peak area.

[0166] The coated zinc oxide particles P2a and P2b obtained according to the method of the invention have a particularly high BET specific surface area (15.8 m2 compared to the commercial compound). 2 / g, 116m for particles P2a and P2b 2 / g and 74m 2 It should be noted that, despite the high water resistance (P2 / g), the particles have better water resistance than commercial zinc oxide particles. This resistance is further improved since the particles formed at the end of the process were subjected to an alkaline post-treatment (P2b).

[0167] It should further be noted that the coated zinc oxide particles P2a and P2b according to the invention have the same shielding power as commercially available zinc oxide particles. The zinc oxide particles according to the invention make it possible to obtain better water resistance, better transparency in the visible spectrum while retaining good UVA shielding properties.

[0168] Example 3: Magnesium naphthanate (C) in xylene 22 H 14 A composition (C) of 0.1% 0.4% Mg (500 mM) was prepared.

[0169] The previously prepared composition (C) was then used to prepare uncoated magnesium oxide particles P4 (outside the present invention) using a conventional FSP preparation method, Prep 1.

[0170] Next, the same composition (C) and a composition (B) containing hexadimethyldisiloxane and ethanol in a ratio of 3:1 were used to prepare magnesium oxide particles P5 coated with silicon dioxide using the preparation method Prep 2 according to the present invention (present invention).

[0171] The parameters for the Prep 1 method are as follows: - Ratio (Composition (C) / O2) = 5 mL / min liquid and 7 L / min gas (O2). To adjust the oxygen flow rate, use φ = 0.48.

[0172] The parameters for the Prep 2 method are as follows: - Ratio (Composition (C) / O2) = 5 / 7, i.e. 5 mL / min liquid and 7 L / min gas (O2). To adjust the oxygen flow rate, use φ = 0.48.

[0173] In this Prep 2 method, a quartz tube with a height of 40 cm is used. In addition, nitrogen is first blown into composition (B). When composition (B) is injected, the flow of nitrogen heated to 25°C allows the evaporation of hexadimethyldisiloxane (HMDSO), ( Mg / Si) 注入 The ratio is adjusted to be 1.

[0174] The particles P5 thus obtained were then divided into two groups P5a and P5b, the latter of which was subjected to a post-treatment according to the following protocol, whereas the latter was not.

[0175] Protocol for post-processing of particles P5a: After collecting the particles obtained by the method, two processes are performed: a treatment step (d3) consisting in introducing the particles of oxide of element M obtained at the end of step (c) into an alkaline bath (a mixture of sodium hydroxide and water) at a pH of 8.5, a temperature of 25° C. and a ratio of 5 g of particles per liter of alkaline bath, for 120 minutes, - a step (d4) of calcining the particles of oxide of element M obtained at the end of step (d3) at 200°C for 120 minutes.

[0176] After the particles were prepared, it was observed that the resulting magnesium oxide particles were crystalline.

[0177] Furthermore, the particles obtained according to the method Prep 2 according to the invention are coated with silicon dioxide and have a (Mg / Si) 粒子 The atomic ratio is 1.

[0178] The BET specific surface area of ​​the particles by method Prep 2 is 24 m 2 / g.

[0179] The particles have a size of 40 to 90 nm.

[0180] Next, the resistance of the three P4, P5a and P5b particle samples is evaluated.

[0181] For this purpose, - 0.1 g of P4 sample is placed in a 2.5 L water bath acidified with hydrochloric acid (pH=5) (i.e. 1 mM MgO equivalent); - 0.2 g of each P5a and P5b sample is placed in a 2.5 L water bath acidified with hydrochloric acid (pH=5) (i.e. 1 mM as MgO equivalent).

[0182] After stirring with a magnetic stirrer for 30 min, the amount of recovered solids is filtered and weighed, and the "recovered solids" content (filtered mass / initial mass) is then deduced therefrom.

[0183] In the case of P4 (uncoated MgO particles), no solids are recovered.

[0184] In the case of P5a, the solids recovery is 93%.

[0185] In the case of P5b, the solids recovered is 78%.

[0186] Example 4: A composition (D) of titanium naphthenate (500 mM) in xylene was prepared.

[0187] Next, titanium oxide particles P6 coated with silicon dioxide were prepared using an FSP method according to the present invention, which includes the injection of composition (D) and composition (B) containing hexadimethyldisiloxane and ethanol in a ratio of 3:1 (particles P6).

[0188] The preparation method parameters are as follows: - Ratio (composition (D) / O2) = 5 / 7, i.e. 5 mL / min liquid and 7 L / min gas (O2). To adjust the oxygen flow rate, φ = 0.48 is used.

[0189] In this method, a quartz tube with a height of 40 cm is used. Furthermore, nitrogen is first blown into the composition (B). When the composition (B) is injected, the flow of nitrogen heated to 25°C allows the evaporation of hexadimethyldisiloxane (HMDSO), ( Ti / Si) 注入 The ratio is adjusted to 1.

[0190] Example 5: 5.1. Zinc oxide particles coated with silicon dioxide P1 (invention) were prepared according to the method described in Example 1.

[0191] Zinc oxide particles coated with silicon dioxide P7 (comparison) were prepared simultaneously using the same method, which involved the injection of composition (A) described in Example 1 and composition (B1) containing tetraethoxysilane and ethanol in a ratio of 3:1.

[0192] Zinc oxide particles coated with silicon dioxide P8 (comparison) were also prepared using the same method, which involved the injection of composition (A) described in Example 1 and composition (B2) containing only hexadimethyldisiloxane.

[0193] The preparation method parameters are as follows: - Ratio (composition (A) / O2) = 5 / 7, i.e. 5 mL / min liquid and 7 L / min gas (O2). To adjust the oxygen flow rate, φ = 0.48 is used.

[0194] In this method, a quartz tube 40 cm in height is used. In addition, nitrogen is first blown into the compositions (B), (B1) and (B2). When these compositions (B), (B1) and (B2) are injected, the flow of nitrogen heated to 25° C. allows the evaporation of hexadimethyldisiloxane (HMDSO) or tetraethoxysilane, and (Zn / Si) 注入 The ratio is adjusted to be 1.

[0195] 5.2. The Raman spectra of particles P7 and P8, unlike that of particle P1, show that the peaks corresponding to the specific structure in which the silicon atom is in the "four-membered ring" form are low intensity (P7) or too broad (P8). These results indicate that the "four-membered ring" form is only moderately formed in the case of P7, but not in the comparative particle P8.

[0196] 5.3 Water resistance rating: Aqueous suspensions S1, S7 and S8 were prepared from particles P1, P7 and P8 and water at a content of 100 mg of particles per liter of water. The suspensions S1, S7 and S8 thus obtained were then placed in an ultrasonic bath for 10 minutes at a power of 20 W.

[0197] A portion of suspensions S1, S7 and S8 were then brought to pH=5 with nitric acid.

[0198] Thereafter, the Z present in each of the suspensions S1, S7 and S8 as a function of time is 2+ The ionic content was measured by conventional anodic stripping voltammetry for each suspension.

[0199] The results are listed in the table below.

[0200] [Table 4]

[0201] t0 corresponds to the first measurement taken less than 10 minutes after the end of the ultrasonic bath.

[0202] It should be noted that the coated zinc oxide particles P1 obtained according to the preparation method of the present invention using a silicon precursor containing at least two silicon atoms and a Si-carbon covalent bond in a specific solvent have excellent water resistance.

[0203] Coated particles P7 obtained using a specific silicon precursor not containing two silicon atoms in a specific solvent provide good water resistance.

[0204] Conversely, particles P8 obtained using a specific silicon precursor containing two silicon atoms but without a specific solvent do not provide good water resistance.

[0205] It is therefore concluded that producing a silica-based coating to obtain a water protection effect is not sufficient.

Claims

1. A method for preparing coated particles of an oxide of element M, said method comprising at least the following steps: a) preparing a composition (A) by adding one or more precursors of element M to one or more combustible solvents, thereafter b) forming a flame in a flame spray pyrolysis device by injecting said composition (A) and an oxygen-containing gas until aggregates of oxides of element M are obtained; and c) injecting a composition (B) comprising one or more silicon precursors and one or more polar protic solvents other than water into said flame until an inorganic coating layer containing silicon oxide is obtained on the surface of said aggregates of element M; The present invention is characterized in that it comprises said element M is selected from magnesium, calcium, zinc and titanium; - said precursor of element M comprises one or more atoms of element M complexed with one or more naphthalate or naphthenate groups; and said silicon precursor is selected from hexadimethyldisiloxane, 1,2-bis(triethoxysilyl)ethane, 1,2-bis(trimethoxysilyl)ethane and mixtures thereof; is understood, the way.

2. The oxide of element M is represented by the formula M x O y 2. The method of claim 1, wherein x and y are such that 1≦y / x≦2.

3. 3. The method according to claim 1, wherein the content of element M precursor in composition (A) is from 1% by weight to 60% by weight relative to the total weight of composition (A).

4. 4. The method according to claim 1, wherein the flame formed in step (b) and maintained in step (c) is at a temperature of between 200° C. and 600° C. at the outlet of the tube transporting the composition (B).

5. (M / Silicon) 注入 5. The process according to claim 1, wherein the molar atomic ratio is in the range of 0.1 to 10.

6. The polar protic solvent other than water in the composition (B) is 1 ~C 8 6. The process according to claim 1, wherein the alcohol is selected from the group consisting of ethyl alcohol, ...

7. The method according to any one of claims 1 to 6, characterized in that the content of silicon precursor in composition (B) is 1% by weight to 60% by weight, based on the total weight of composition (B).

8. The process further comprises a treatment step (d) which comprises introducing the particles of oxide of element M obtained at the end of step (c) into a neutral or alkaline bath having a pH between 7 and 11. 1 ), and / or at the end of step (c) or said treatment step (d 1 step (d) of calcining the particles of oxide of element M obtained at the end of 2 The method according to any one of claims 1 to 7, further comprising:

9. Spherical particles of oxide of element M comprising a core (1) and one or more upper coating layers (2) covering said core (1), (i) the core (1) consists of one or more oxides of element M; (ii) the upper coating layer (2) comprises one or more silicon oxides and covers at least 90% of the surface of the core (1); (iii) the element M is selected from magnesium, calcium, zinc, and titanium; (iv) (M / silicon) 粒子 the molar atomic ratio is within the range of 0.2 to 1.5, as determined by X-ray fluorescence; and (v) the number average diameter D of the core (1) m is in the range of 3 nm to 1000 nm, and the number average thickness d mis in the range of 1 nm to 30 nm, both determined by transmission electron microscopy. The spherical particles are characterized by:

10. 10. Particles according to claim 9, characterized in that the oxides of element M constituting the core (1) are selected from zinc oxide ZnO, magnesium oxide MgO and calcium oxide CaO.

11. 11. Particle according to claim 9 or 10, characterized in that the sum of the content of element M oxide and the content of silicon oxide is at least equal to 99% by weight, relative to the combined weight of the core (1) and the upper coating layer (2).

12. The number average diameter D of the core (1) determined by transmission electron microscopy (TEM) m Particles according to any one of claims 9 to 11, characterized in that the diameter of the particles is in the range of 6 to 50 nm.

13. The number average thickness d of the upper coating layer (2) measured by transmission electron microscopy (TEM) m Particles according to any one of claims 9 to 12, characterized in that the diameter of the particles is in the range of 1 to 15 nm.

14. Particles according to any one of claims 9 to 13, characterized in that the number average diameter of the particles, determined by transmission electron microscopy (TEM), is in the range of 10 to 100 nm.

15. A composition comprising one or more particles of element M oxide according to any one of claims 9 to 14.

16. 16. The composition according to claim 15, for use in protecting human skin against visible and / or UV-A and / or UV-B ultraviolet radiation.

17. Use of particles of oxide of element M according to any one of claims 9 to 14, - formulating cosmetic or pharmaceutical compositions, - Formulating paints, varnishes and / or stains, or - Producing coatings for electronic devices or products For, use.

Citation Information

Patent Citations

  • Cosmetic including spherical fine particles of silica- including compound oxide

    JP2003081770A

  • Silica-coated zinc oxide particles obtained by flame pyrolysis

    JP2009545509A

  • Method for coating core ceramic particle by emulsion flame spray pyrolysis method

    JP2010053019A

  • embolization particles

    JP2018514525A

  • Method for making silica nanoparticles by flame spray pyrolysis adopting two-fluid nozzle

    US20090123357A1