Welding wire capable of producing giga-class welds, welded structure manufactured using the same, and welding method thereof

The welding wire and method address the challenges of producing high-strength welds for galvanized Giga Steel by optimizing element ratios and welding parameters, achieving robust welds with reduced defects and improved corrosion resistance, enhancing durability and productivity in automotive applications.

JP7564227B2Active Publication Date: 2024-10-08CLEANSOLUTION CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022552279
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-08
Filing Date
2021-04-23
Publication Date
2024-10-08
Estimated Expiration
2041-04-23

AI Technical Summary

Technical Problem

Existing welding technologies struggle to produce high-strength welds for galvanized Giga Steel with a tensile strength of 1 GPa or more and a thickness of 6 mm or less, particularly in automotive applications, due to issues such as slag generation, blowholes, and reduced corrosion resistance, which compromise durability and productivity.

Method used

A welding wire composition with controlled contents of C, Si, Mn, Cr, Mo, and a Cu plating layer, along with specific welding parameters, including a relational expression to balance element ratios and welding heat input, to minimize slag and blowholes, ensuring a microstructure of 30-50% martensite, 50-70% bainite, and 5% retained austenite, with a high hard angle of 47° or more, and using a shielding gas mixture of Ar with 5-20% CO2.

Benefits of technology

The solution effectively reduces slag and blowhole ratios to less than 1%, maintains weld strength at 1 GPa or more, enhances corrosion resistance, and eliminates the need for post-treatment processes, improving the durability and quality of welded parts in automotive components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564227000005
    Figure 0007564227000005
  • Figure 0007564227000006
    Figure 0007564227000006
  • Figure 0007564227000007
    Figure 0007564227000007
Patent Text Reader

Abstract

A welding wire that can produce giga-class welds, a welded structure manufactured using the same, and a welding method for the same are provided. [Solution] The welding wire of the present invention is characterized in that, in total mass %, the wire contains C: 0.08 to 0.15%, Si: 0.001% to 0.1%, Mn: 1.6 to 1.9%, P: 0.015% or less, S: 0.015% or less, Cr: 4.0 to 5.2%, Mo: 0.4 to 0.65%, and the balance being Fe and inevitable impurities, and the value X defined by the following relational expression 1 satisfies the range of 0.7 to 1.1%. [Equation 1] X(%)=[Cr] / 10+[Mo]-4×[Si] / [Mn]
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a welding wire capable of obtaining giga-class welds, a welded structure manufactured using the same, and a welding method thereof, and more particularly to a welding wire applicable to gas shielded arc welding of galvanized gigasteel having a tensile strength of 1 GPa or more and a thickness of 6 mm or less, which is used in structural members of the underbody of an automobile, a welded structure manufactured using the same, and a welding method thereof. [Background technology]

[0002] In the automotive industry, research into weight reduction technology for car bodies and parts has emerged as a major issue due to fuel efficiency regulations associated with environmental protection such as global warming. Due to this trend, there is a need for the supply of high-strength steel materials to reduce the weight of chassis parts, which are important for the driving performance of automobiles. To achieve such lightweight components, it is essential to increase the strength of the material, and it can be said that an important factor is to guarantee the durability of components made from high-strength steel in an environment where they are subjected to repeated fatigue loads.

[0003] However, in the case of arc welding, which is mainly used to ensure strength when assembling chassis parts for automobiles, lap joints between parts are welded by the deposition of a welding wire, so it is inevitable to give the joint a geometric shape. This causes the problem that repeated fatigue stress acts on the concentrated part (notch effect) and becomes the fracture origin, resulting in a decrease in the durability of the part, and thus losing the advantage of applying high-strength steel.

[0004] Therefore, in order to improve the fatigue properties of welds, it is most important to reduce the angle (toe angle) of the end of the bead, which is the main stress concentration area, and in addition, it can be said that controlling the material and stress of the toe area is an important factor. Also, as described above, the trend toward high strength and light weight of parts has led to the thinning of materials, which has increased the demand for rust prevention to prevent penetration corrosion, and the use of plated steel has tended to increase. However, the weld metal of arc welds in particular has a problem that there is no plated layer, and the corrosion resistance after painting of the base material decreases. This causes a problem that early corrosion occurs in the welds of chassis parts made of plated steel sheets in a severe corrosive environment when the car is running, leading to a decrease in fatigue properties. On the other hand, when gas-shielded arc welding of plated steel is performed, a large number of pore defects in the form of pits and blowholes occur in the weld bead due to the generation of vapor such as zinc, which may reduce the strength of the weld, which is a problem of reduced welding productivity. In addition, even with ordinary uncoated steel, slag generated in the form of weld beads during gas shielded arc welding causes painting defects and reduces corrosion resistance after painting, so post-processing such as pickling or brushing to remove slag after welding is required during part manufacturing, which causes an increase in costs. Meanwhile, the application of Gigasteel, a steel material with a tensile strength of 1 GPa or more, is expected to expand for effective weight reduction in preparation for the age of electric vehicles, and ensuring the strength of welds is an important priority.

[0005] An example of a conventional technique for solving such problems is the invention described in Patent Document 1. Patent Document 1 discloses that the blowhole and slag area ratios of a welded part can be controlled to within 10% by appropriately controlling the contents of Si, Mn, Ti, and Al in a gas-shielded arc welding wire. However, in the case of actual high-strength steel, when the blowhole area ratio of a welded part exceeds 5%, there is a risk of a significant decrease in the tensile strength and fatigue strength of the weld metal. In particular, in the case of giga-class steel with a tensile strength of 1 GPa or more, a problem occurs in which the occurrence of blowholes makes the welded part more sensitive to a decrease in strength. Patent Document 2 discloses that the tensile strength of the weld metal can be ensured to be 800 MPa or more by controlling the carbon equivalent of the gas shielded arc welding wire to 0.8 to 0.9%, but does not present any method for reducing blowholes and slag in the weld.

[0006] Patent Document 3 discloses that the Si:Mn content ratio of gas shielded arc welding wire is controlled within an appropriate range to suppress the generation of Si-based slag in the weld bead and improve the paintability and porosity resistance of the weld. However, Patent Document 3 is aimed at general steel materials with a maximum weld strength of 540 MPa, and does not present a method for ensuring the strength of the weld of gigasteel, which has a tensile strength of 1 GPa or more. Patent Document 4 discloses that the slag area ratio of a weld can be controlled to within 5% by appropriately controlling the Si, Al, Ti, Al, Sb, and S contents of a gas-shielded arc welding wire, but does not provide a method for reducing pits and blowholes in a weld of a plated steel material. On the other hand, it does provide a method for improving the strength of a weld by adding an appropriate amount of B to the wire, but the strength does not reach 1 GPa or more.

[0007] Patent Document 5 discloses that the total amount of Cr and Ni in the welding wire is controlled to 1% to 24%, and the strength of the welded part of a steel material having a tensile strength of 980 MPa or more is 90% or more of that of the base material. However, it does not propose any method for reducing slag in the welded part or improving the porosity resistance. That is, the inventions disclosed in Patent Documents 1 to 5 are directed to steel sheets having a tensile strength of 1 GPa or more and a plating amount per side of 20 to 120 g / m 2 Sufficient consideration was not given to the welding of galvanized steel sheets, and it was unclear whether it was possible to simultaneously ensure sufficient strength of the Gigasteel welds while reducing slag and preventing porosity. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 2015-0108930 [Patent Document 2] Korean Patent Publication No. 2016-0080096 [Patent Document 3] Korean Patent Publication No. 2019-0047388 [Patent Document 4] International Publication No. 2019 / 124305 [Patent Document 5] Korean Patent Publication No. 2019-0134703 Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, an object of the present invention is to provide a welding wire that can be used for gas shielded arc welding of galvanized gigasteel having a tensile strength of 1 GPa or more and a thickness of 6 mm or less, which is used for structural members of the lower part of an automobile, a welded structure manufactured using the same, and a welding method thereof. The object of the present invention is not limited to the above. The object of the present invention can be understood from the general contents of this specification, and a person having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding further object of the present invention. [Means for solving the problem]

[0010] The gas shielded arc welding wire of the present invention is The wire is characterized in that the wire contains, in mass % relative to the entire wire, C: 0.08-0.15%, Si: 0.001%-0.1%, Mn: 1.6-1.9%, P: 0.015% or less, S: 0.015% or less, Cr: 4.0-5.2%, Mo: 0.4-0.65%, and the balance being Fe and unavoidable impurities, with a value X defined by the following relational expression 1 falling within the range of 0.7-1.1%. [Equation 1] X(%)=[Cr] / 10+[Mo]-4×[Si] / [Mn] In the relational formula 1, [Cr], [Mo], [Si] and [Mn] represent the mass percentage of each element.

[0011] It is preferable that a Cu plating layer is formed on the surface of the welding wire. The Cu constituting the Cu plating layer preferably has a Cu content of 0.4% or less (excluding 0%), more preferably in the range of 0.1 to 0.3%, in mass % based on the entire wire including the plating layer.

[0012] The welding wire preferably contains, by mass %, Cr: 4.2 to 4.9%, Mo: 0.45 to 0.48%, and Mn: 1.65 to 1.75%. The welding wire preferably has a Si content in the range of 0.04 to 0.08%. The welding wire may be a solid wire for gas shielded arc welding.

[0013] The welded structure of the present invention is A welded structure having a weld obtained by welding two or more welding base materials using the welding wire, wherein the weld has a microstructure consisting of, by area%, 30-50% martensite, 50-70% bainite, and the remainder being 5% or less of retained austenite, and the microstructure constituting the weld has an average effective crystal grain size of 1-3 μm and a crystal grain fraction of high hard angle of 47° or more of 35% or more.

[0014] At least one of the weld base materials may be a galvanized steel sheet. The galvanized steel sheet may be one of an electrolytic galvanized steel sheet, a hot-dip galvanized steel sheet, and a galvannealed hot-dip galvanized steel sheet. The base steel sheet constituting the above-mentioned galvanized steel sheet preferably contains, in mass %, one or more of Cr: 0.2 to 0.9% and Mo: 0.1 to 0.2%.

[0015] The gas shielded arc welding method of the present invention further comprises: The method for gas-shielded arc welding of a base metal using the above welding wire is characterized in that, when the thickness of the base metal is t (mm), a mixture of Ar and 5 to 20% CO2 is used as a protective gas during welding, and welding is performed such that the range of the welding heat input Q (kJ / cm) defined by the following relational expression 2 satisfies 1.15t≦Q≦1.6t. [Equation 2] Q = (I × E) × 0.048 / υ In the relational expression 2, I, E, and υ respectively represent the welding current (A), the welding voltage (V), and the welding speed (cm / min). The welding wire may be a solid wire having a diameter of 0.9 to 1.2 mm. Effect of the Invention

[0016] According to the present invention having the above configuration, the slag area ratio and blowhole area ratio of the gas shielded arc welded part of Gigasteel having a tensile strength of 1 GPa or more and a thickness of 6 mm or less are reduced to within 1%, respectively, so that post-treatment processes such as separate pickling or brushing for removing slag from the welded part can be omitted and excellent paintability can be secured, thereby reducing costs and improving quality at industrial manufacturing sites. In addition, when welding plated materials, not only can defects such as pits and blowholes be effectively prevented, but also a weld strength of 1 GPa or more can be ensured without fracture of the weld metal or fusion line. Therefore, by meeting the needs for improved rust resistance and durability associated with the high strength and thinning of parts such as automobile chassis components, Gigasteel can have industrial significance in expanding its adoption. [Brief description of the drawings]

[0017] [Figure 1] Photographs showing the cross-sectional structure of a weld obtained from an example of the present invention [X(%)=0.85, Q(kJ / cm)=2.6] welded using Wire No. 7 in Table 2 in Example 1 of the present invention, the hardness distribution, and the cross-sectional structure of a fractured part after a static tensile test. [Diagram 2]FIG. 1 is a photograph showing the cross-sectional structure of a weld obtained from a comparative example [X(%)=0.55, Q(kJ / cm)=2.6] in which welding was performed using Wire No. 32 in Table 2 in Example 1 of the present invention, the hardness distribution, and the cross-sectional structure of a fractured part after a static tensile test. [Diagram 3] FIG. 1 shows radiographic test (RT) photographs of welds obtained in Example 1 of the present invention after lap joint welding of galvanized steel sheets and lap joint welding of alloyed galvanized steel sheets using wires Nos. 5, 7, 12, 34, and 36 in Table 2. [Figure 4] FIG. 6 is an EBSD micrograph and an inverse pole figure of a weld metal obtained from an invention example [X(%)=0.85, Q(kJ / cm)=3.2] in which No. 7 wire and No. 1 steel material in Table 4 were welded in combination in Example 2 of the present invention. [Diagram 5] FIG. 11 is an EBSD micrograph and an inverse pole figure of a weld metal obtained in a comparative example [X(%)=0.55, Q(kJ / cm)=3.2] in which a combination of No. 32 wire and No. 1 steel material in Table 4 were welded in Example 2 of the present invention. [Figure 6] FIG. 1 shows an external photograph of a weld bead obtained from an invention example [X(%)=0.85, Q(kJ / cm)=2.6] in which a combination of No. 7 wire and No. 1 steel material in Table 4 was welded in Example 2 of the present invention, and an external photograph after painting was applied without post-treatment steps such as pickling or brushing for removing slag from the welded part. [Figure 7a] FIG. 13 is a diagram showing a change in load on a steel material, which is a base material for welding, when a load is applied to a weld obtained from an example of the invention [X(%)=0.85, Q(kJ / cm)=2.6] in which No. 7 wire and No. 1 steel material in Table 4 are welded in combination in Example 2 of the present invention, and a high-speed tensile test (tensile speeds of 1 m / s and 15 m / s, respectively) is performed. [Figure 7b]FIG. 13 is a diagram showing a change in load on a welded portion when a load is applied to the welded portion obtained from an example of the invention [X(%)=0.85, Q(kJ / cm)=2.6] in which No. 7 wire and No. 1 steel material in Table 4 are welded in combination in Example 2 of the present invention to perform a high-speed tensile test (tensile speeds of 1 m / s and 15 m / s, respectively). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will now be described. The present invention is characterized in that, when gas-shielded arc welding is performed on gigasteel having a tensile strength of 1 GPa or more and a thickness of 6 mm or less, the slag area ratio and blowhole area ratio of the weld can be reduced to within 1%, respectively, and the weld strength of 1 GPa or more can be ensured without fracture of the weld metal or fusion line. As a result of various experiments and studies, the inventors have confirmed that it is effective to control the contents of Cr and Mo, which are strengthening elements for improving strength, and Si and Mn, which are deoxidizing elements, among the components of the welding wire used in gas-shielded arc welding, so that the X value defined by the above Relational Formula 1 falls within the range of 0.7 to 1.1%. The inventors have found that when the value of the above Relational Expression 1 is used as a parameter, the X value has a significant effect on the occurrence of slag and blowholes in the welded portion and the strength of the welded portion. In particular, the inventors have confirmed that the occurrence of slag and blowholes in the weld bead can be reliably suppressed and the strength of the welded portion can be secured to 1 GPa or more without fracture of the weld metal or fusion line by controlling not only the individual content of each element as a component contained in the welding wire but also the amount of each component so that the above X value is in the range of 0.7 to 1.1%, and have come to present the present invention.

[0019] A welding wire according to one aspect of the present invention contains, by mass%, C: 0.08-0.15%, Si: 0.001%-0.1%, Mn: 1.6-1.9%, P: 0.015% or less, S: 0.015% or less, Cr: 4.0-5.2%, Mo: 0.4-0.65%, with the balance being Fe and unavoidable impurities, and the value X defined by the above Relation 1 satisfies the range of 0.7-1.1%. The composition of the gas-shielded arc welding wire according to one aspect of the present invention and the reasons for its limitations will be described below. The percentages used herein are by mass unless otherwise specified. The welding wire according to the present invention is not limited to a specific type of wire, and may be a solid wire or a flux-cored wire, and is preferably used as a solid wire. It is preferable that a Cu plating layer is formed on the surface of the welding wire.

[0020] C: 0.08-0.15% C is a component that stabilizes the arc and atomizes the volume. However, if the C content is less than 0.08%, the volume becomes large, the arc becomes unstable, and not only does it increase the amount of spatter, but it may also be difficult to ensure sufficient strength of the weld metal of giga-class steel with a tensile strength of 1 GPa or more. On the other hand, if the C content exceeds 0.15%, not only does the viscosity of the molten metal decrease, resulting in poor bead shape, but it also causes the weld metal to become excessively hardened and increase brittleness. Therefore, in the present invention, it is preferable to limit the C content of the welding wire to the range of 0.08 to 0.15%.

[0021] Silicon: 0.001 to 0.1% Silicon is an element (deoxidizing element) that promotes deoxidation of molten metal during arc welding, and is effective in suppressing the occurrence of blowholes. On the other hand, when excessively contained, silicon is also an element that causes significant slag generation and causes poor coating of welded parts. If the silicon content is less than 0.001%, deoxidation is insufficient and blowholes are likely to occur, whereas if the silicon content exceeds 0.1%, slag increases significantly. Therefore, from the viewpoint of a balance between suppressing the occurrence of blowholes and suppressing the amount of slag, the silicon content of the welding solid wire is set to a range of 0.001 to 0.1%. Also, it is preferable to limit the Si content to the range of 0.04 to 0.08%, since this makes it possible to more effectively suppress both the blowholes and the amount of slag.

[0022] Mn: 1.6-1.9% Mn is also a deoxidizing element, and has the effect of promoting deoxidation of the molten metal during arc welding and suppressing the occurrence of blowholes, but on the other hand, it is also an element that increases the viscosity of the molten metal. If the Mn content is less than 1.6%, deoxidation is insufficient within the above-mentioned appropriate range of the Si content, and blowholes are likely to occur. On the other hand, if the Mn content exceeds 1.9%, the viscosity of the molten metal becomes excessively high, and when the welding speed is fast, the molten metal cannot flow properly into the welded part, resulting in a humping bead, which is likely to cause a defective bead shape. Therefore, the Mn content of the welding wire is set to a range of 1.6 to 1.9%. In order to reliably suppress the occurrence of blowholes, it is preferable to limit the Mn content to a range of 1.65 to 1.75%.

[0023] Cr: 4.0~5.2% Cr is a ferrite stabilizing element and a hardening element that improves the strength of the weld metal. In particular, in order to ensure sufficient strength of giga-class steel weld metal with a tensile strength of 1 GPa or more, the Cr content must be limited to the range of 4.0 to 5.2%. If the Cr content is less than 4.0%, the strength of the giga-class steel weld metal is likely to be insufficient. On the other hand, if the Cr content exceeds 5.2%, the formation of a δ ferrite structure and the precipitation of chromium carbide in the structure increase the risk of embrittlement of the weld metal, that is, a decrease in toughness. In addition, it is preferable to limit the Cr content to the range of 4.2 to 4.9%, in that it is possible to more effectively ensure sufficient strength of the weld metal and suppress embrittlement.

[0024] Mo: 0.4-0.65% Mo is also a ferrite stabilizing element and a hardening element that improves the strength of the weld metal. In particular, in order to ensure sufficient strength of the weld metal of giga-class steel with a tensile strength of 1 GPa or more, the Mo content must be limited to the range of 0.4 to 0.65%. If the Mo content is less than 0.4%, it becomes difficult to obtain sufficient strength of the weld metal of giga-class steel with a tensile strength of 1 GPa or more within the above-mentioned appropriate composition range, and if the Mo content exceeds 0.65%, there is a high risk of the toughness of the weld metal decreasing. In addition, it is preferable to limit the Mo content to the range of 0.45 to 0.48%, in that it is possible to more effectively ensure sufficient strength of the weld metal and suppress embrittlement.

[0025] P:0.015% or less P is an element that is generally mixed as an inevitable impurity in steel, and is usually also contained as an impurity in arc welding wire. Here, P is one of the main elements that cause hot cracking in weld metal, and it is preferable to suppress it as much as possible. If the P content exceeds 0.015%, hot cracking in the weld metal becomes significant. Therefore, in the present invention, it is preferable to limit the P content of the welding wire to 0.015% or less.

[0026] S: 0.015% or less S is also an element that is generally mixed in steel as an inevitable impurity, and is usually also contained as an impurity in solid wire for arc welding. Here, S is an element that impairs the toughness of the weld metal, and it is preferable to suppress it as much as possible. If the S content exceeds 0.015%, the toughness of the weld metal deteriorates. Therefore, in the present invention, it is preferable to limit the S content of the welding wire to 0.015% or less.

[0027] [Equation 1] In the gas-shielded arc welding wire of the present invention, it is important to control the contents of Cr, Mo, Si and Mn so that the X value defined by the following relational expression 1 falls within the range of 0.7 to 1.1%. [Equation 1] X(%)=[Cr] / 10+[Mo]-4×[Si] / [Mn] In the relational formula 1, [Cr], [Mo], [Si] and [Mn] represent the mass percentage of each element.

[0028] That is, according to the research results of the present inventors, it was found that the contents of Cr, Mo, Si and Mn contained in the wire are strongly correlated not only with the strength of the welded portion but also with the occurrence of blowholes and slag, and the inventors devised Relational Formula 1. Specifically, by controlling the contents of Cr, Mo, Si and Mn so that the X value defined by the above Relational Formula 1 is in the range of 0.7 to 1.1%, it is possible to ensure sufficient strength of the welded portion of giga-class steel material having a tensile strength of 1 GPa or more, and to reliably obtain improved porosity resistance and reduced slag. That is, by applying the parameters of the above Relational Formula 1, it is possible to reliably suppress the occurrence of slag and blowholes in the weld bead and to ensure a welded portion strength of 1 GPa or more without the occurrence of fracture of the weld metal or fusion line. If the X value is less than 0.7%, it is difficult to secure sufficient strength of the weld metal as well as the porosity resistance and slag reduction effects of the welded portion of the giga-class steel material. Conversely, if the X value exceeds 1.1%, even if the porosity resistance and slag reduction effects of the welded portion are satisfied, the weld metal may become too brittle, and the weld metal or fusion line fracture may become sensitive, resulting in a problem of poor physical properties of the welded portion.

[0029] [impurities] Impurities refer to components contained in raw materials or components mixed in during the manufacturing process, and are not intentionally contained in the welding wire. On the other hand, it is preferable that a Cu plating layer is formed on the surface of the welding wire of the present invention. Cu is generally an impurity in the steel constituting the wire and is usually contained at about 0.02%, but in the case of the arc welding wire of the present invention, it is mainly derived from the copper plating applied to the wire surface. In the case of arc welding wire, copper plating is an important surface treatment method for stabilizing wire feedability and electrical conductivity, and when copper plating is applied, a certain amount of Cu will inevitably be contained.

[0030] In the present invention, the Cu content in the plating layer is preferably controlled to 0.4% or less (excluding 0%) in mass % based on the entire wire including the Cu plating layer. If the Cu content exceeds 0.4%, there is a risk that the crack susceptibility of the weld metal will increase. A more preferable Cu content range is 0.1 to 0.3%, which can more effectively reduce the crack susceptibility of the weld metal while stabilizing the wire feedability and electrical conductivity. If the Cu content is too low, there is a risk that the required wire feedability and electrical conductivity will not be obtained.

[0031] Next, a welded structure manufactured using the above welding wire, which is another aspect of the present invention, will be described. The welded structure of the present invention is a welded structure having a weld obtained by welding two or more welding base materials with the above welding wire, and the weld has a microstructure consisting of, by area %, 30-50% martensite, 50-70% bainite, and the balance 5% or less of retained austenite. The microstructure constituting the weld has an average effective grain size of 1-3 μm, and a grain fraction of high hard angle of 47° or more is 35% or more.

[0032] First, the welded portion of the present invention has a microstructure consisting of, by area%, 30-50% martensite, 50-70% bainite, and the balance 5% or less of retained austenite. In the present invention, if the martensite fraction is too high, the welded metal may become too hard and sensitive to brittleness, whereas if the martensite fraction is too low, the welded metal may have insufficient strength. Meanwhile, bainite forming a weld zone, which is generally formed by low-temperature transformation at a temperature of 550°C or less, can include both upper bainite and lower bainite, but in particular, lower bainite, which develops by transformation in the range of 250 to 400°C, has many high-hardness grains interlocking with each other within the prior austenite grains. Therefore, when such lower bainite is mixed with martensite, it has the effect of improving toughness compared to when martensite exists alone.

[0033] Considering these points, in the present invention, the microstructure forming the weld has an average effective grain size of 1 to 3 μm, and the grain fraction of high hard angles of 47° or more is controlled to 35% or more. If the average effective grain size of the microstructure forming the weld is less than 1 μm, the toughness of the weld metal may be insufficient, and conversely, if it exceeds 3 μm, the strength of the weld metal relative to the giga-class steel base material may be insufficient. Also, if the grain fraction of high hard angles of 47° or more is less than 35%, the strength and toughness of the weld metal may be reduced. Furthermore, the welded portion may have an average hardness of 370 to 400 Hv and a tensile strength of 940 MPa or more, preferably 1 GPa or more, which is 95% or more of the welded base metal.

[0034] In addition, the microstructural characteristics of the weld metal improve the mechanical properties of the welded joint, and not only does it prevent the welded metal or fusion line fracture when a tensile load is applied as described above, but in the case of subframes, which are front collision members, it is possible to ensure sufficient strength and toughness to prevent fracture of the welded metal joint even in a high-speed collision (application of high-speed tensile load) situation in which the automobile is traveling at a speed of 3.6 to 54 km / h. In the present invention, the welded portion can have a high-speed tensile strength of 95% or more and 80% or more of that of the base material at tensile speeds of 3.6 km / h and 54 km / h, respectively. On the other hand, the welded portion of the present invention can be obtained by welding two or more base materials with the above welding wire.

[0035] On the other hand, in the present invention, the type and composition of the steel sheet to be gas-shielded arc-welded using the welding wire are not particularly limited. For example, it is preferable that at least one of the above-mentioned welding base materials is a zinc-plated steel sheet, because the effect becomes remarkable when the zinc-plated steel sheet is gas-shielded arc-welded using the welding wire of the present invention. Specifically, the coating weight on one side is 20 to 120 g / m 2When a zinc or zinc alloy plated steel sheet having the above formula (I) is used as a base steel sheet, particularly when there is no gap at the lap joint during welding and the joint is in close contact, blowholes can be reliably reduced by using the gas-shielded arc welding wire of the present invention even in a situation where a large amount of zinc vapor generated is not sufficiently discharged before the molten pool solidifies.

[0036] The galvanized steel sheet may be one of an electrolytic galvanized steel sheet, a hot-dip galvanized steel sheet, and a galvannealed hot-dip galvanized steel sheet. Furthermore, the base steel sheet constituting the above-mentioned galvanized steel sheet preferably contains, in mass %, one or more of Cr: 0.2 to 0.9% and Mo: 0.1 to 0.2%.

[0037] Next, a method for welding gigasteel or the like using the above welding wire of the present invention will be described. The present invention uses the above welding wire to gas-shielded arc-weld a base metal, and uses a protective gas, Ar, mixed with 5-20% CO2, during the welding. When the thickness of the base metal is t (mm), welding can be performed such that the range of the welding heat input Q (kJ / cm) defined by the following relational expression 2 satisfies 1.15t≦Q≦1.6t. [Equation 2] Q = (I × E) × 0.048 / υ In the relational expression 2, I, E, and υ respectively represent the welding current (A), the welding voltage (V), and the welding speed (cm / min). In the present invention, the specific form of welding (welding position) is not particularly limited, and the present invention is applicable to, for example, lap fillet welding, which is a form of lap joint, and fillet welding of a T-joint.

[0038] The type of shielding gas used is not particularly limited, and 100% CO2 gas, Ar+20% CO2 gas, Ar+10% CO2 gas, Ar+5% CO2 gas, Ar+2% O2 gas, etc. can be used as the shielding gas, but the present invention can exhibit remarkable effects when Ar+5-20% CO2 is used as the shielding gas. That is, in the present invention, in order to ensure a tensile strength of 1 GPa or more at the weld without causing fracture of the weld metal or fusion line, it is preferable to use a mixture of Ar and 5-20% CO2 as the protective gas during the above welding. In addition, when the thickness of the weld base metal is t (mm), the range of the welding heat input Q (kJ / cm) defined by the above Relational Formula 2 is required to satisfy 1.15t≦Q≦1.6t. If the welding heat input Q value is less than 1.15t, the strength and toughness of the weld metal and the coarse grained heat affected zone of the giga-class steel may be insufficient, while if it exceeds 1.6t, not only will the strength of the weld metal be insufficient and the strength of the welded heat affected zone be excessively reduced, but backbeads and meltdowns will easily occur in the welded part, resulting in a defective product.

[0039] In addition, in the present invention, the welding wire may be a solid wire having a diameter of 0.9 to 1.2 mm, and the description of the welding base metal is as above. As described above, in the present invention, the contents of Cr, Mo, Si and Mn are controlled so as to satisfy the above Relational Formula 1. In addition, by suppressing the Cr content in the welding wire to a relatively high value within the range of 4.0 to 5.2% and suppressing the Si content to a low value of 0.001 to 0.1%, it is possible to simultaneously secure sufficient strength of the weld, reduce slag and improve porosity resistance. EXAMPLES

[0040] The present invention will now be described in detail with reference to examples. Example 1 An ingot having the composition shown in Table 2 below was vacuum melted, and then hot-rolled at room temperature to draw the wire, followed by annealing to produce a wire. Next, a Cu plating layer was formed on the surface of the wire, and the copper content was plated to be in the range of 0.15 to 0.36% by mass based on the entire wire including the plating layer. The copper-plated wire was then drawn to produce a welding solid wire having a diameter of 0.9 to 1.2 mm. Using the solid wires manufactured as described above, lap joint welding was performed by gas shielded arc welding to galvanized steel sheets having a tensile strength of 1050MP using steel material No. 1, which is the welding base material in Table 1 below, as the base steel sheet. For comparison, lap joint welding was performed using the above galvanized steel sheets as the welding base material and lap joint welding was performed using wires Nos. 5, 7, 12, 34 and 36 in Table 2 below, and lap joint welding was also performed using alloyed galvanized steel sheets as the welding base material.

[0041] On the other hand, the zinc or zinc alloy plated steel sheets used here were base steel sheets plated on both sides with zinc, the base steel sheets had a thickness of 2.0 mm, and the plating amount was 100 g / m2 per side for the zinc and zinc alloy plated steel sheets. 2 and 45 g / m 2 It was decided. The standard conditions for welding were as follows: Ar+20% CO2 mixed shielding gas (flow rate 20 l / min) was applied, two identical steel plates were welded as lap joints without a gap, with a wire projection length of 15 mm, pulse MAG, and a welding speed of 80 cm / min. At this time, the Q (kJ / cm) value defined by the above Relational Formula 2 was set to 1.5 to 3.4.

[0042] After the weld metal obtained by the above lap joint welding was solidified, the bead appearance of the weld was observed, and an RT test was performed to investigate the occurrence of blowholes, and hardness measurements and static / dynamic tensile tests were performed. The evaluation results are shown in Tables 2 and 3 below and in FIG. 3. At this time, the average hardness of the weld metal was rated as ○ (pass) when it was 370 to 400 in Vickers hardness (Hv, load 500gf, measured at 0.2mm intervals), △ when it was 330 to 370, and × (fail) when it was over 400 or less than 330. After a static tensile test of the weld (speed 10mm / min), cases where the tensile strength was 1GPa or more and cases where the fracture position was not the weld metal or fusion line were rated as ○ (pass), and other cases were rated as × (fail).

[0043] In the case of the RT test for observing the bead appearance of the welded part and for irradiation of blowholes, images were taken of the bead surface and RT photography of the central 50 mm long part of the bead, excluding the beginning and end 50 mm parts of the 150 mm weld bead. Then, the slag and blowhole parts were marked, the total area of ​​the marked parts was calculated, and the slag area ratio was calculated from the total image area using the following relational formula 3. [Equation 3] Slag (or blowhole) area ratio (%) = [total of slag (or blowhole) area / total image area] x 100

[0044] In addition, when evaluating the slag generation status shown in Table 2 below, the standard value for the slag area rate was set to 1%, with slag area rates of 1% or less being evaluated as ○ (pass) and the rest being evaluated as × (fail). This is a target standard set to completely omit the post-processing process of removing slag from welded parts, such as separate pickling or mechanical abrasive brushing (both pickling and brushing are performed as necessary) that is performed after welding to improve the paint adhesion of the welded parts and the corrosion resistance after painting when manufacturing parts.

[0045] Also, when evaluating the occurrence of blowholes, the standard value for the blowhole area ratio based on the ISO 5817 standard was rated as ○ (pass) if it was 1% or less, and as × (fail) if it was anything else. This is because in the case of high-strength steel with a tensile strength of 590 MPa or more, if the blowhole area ratio of the normal weld bead exceeds 5%, there is concern that the static strength and fatigue strength of the weld will rapidly decrease, and in particular in the case of giga-class steel with a tensile strength of 1 GPa or more, the decrease in strength of the weld metal due to the increase in the blowhole area ratio of the weld bead is even more sensitive, so this target standard was set to completely prevent this. Furthermore, in order to evaluate the brittleness of the weld metal obtained using the above wire and to evaluate the simulation of a high-speed collision situation of a front part, a high-speed tensile test was performed on a test piece of the weld at low speed (3.6 km / h) and high speed (54 km / h) conditions, i.e., tensile speeds of 1 m / s and 15 m / s, to confirm the fracture position. The maximum load value at this time was compared with the physical properties of the steel. In this case, if no fracture occurred in the weld metal and the maximum load value of the weld under high-speed conditions was 80% or more of the base metal, it was evaluated as ○ (pass), and otherwise as × (fail). It was determined that when these criteria were met, the robustness of the weld can be sufficiently ensured in a high-speed collision situation of a front part of an automobile.

[0046] [Table 1]

[0047] [Table 2] *In Table 1, the balance consists of Fe and unavoidable impurities.

[0048] [Table 3]

[0049] As can be seen from Tables 2 and 3 above, it can be confirmed that wires No. 1 to 18, which satisfy not only the solid wire composition but also the X value defined by Relational Formula 1 in the range of 0.7 to 1.1%, all meet the standards in terms of average hardness of the weld, tensile strength of the weld, and fracture location. Figure 1 is a photograph showing the cross-sectional structure of the weld obtained from an example of the invention [X(%)=0.85, Q(kJ / cm)=2.6] welded using wire No. 7 in Table 2 above, hardness distribution, and cross-sectional structure of the fractured part after static tensile testing.

[0050] In contrast, in the case of Wire Nos. 19 to 23, the Si content was controlled to 0.001 to 0.1% or less, and as shown in Table 3, the blowholes and slag area ratios were at the acceptable level, but the above-mentioned X value was outside the required range, so the average hardness, tensile strength, fracture location, and high-speed tensile properties of the weld metal were poor. In particular, Wire Nos. 21 to 23 had an average hardness of the weld metal part exceeding 400, and as a result, fracture occurred in the weld metal during static or high-speed tensile testing. This was determined to be the result of the martensite fraction of the weld metal exceeding 50%, resulting in excessive increase in brittleness. In addition, the values ​​of X in Wire Nos. 24 to 31 were far outside the range of 0.7 to 1.1%. As a result, as shown in Tables 2 and 3, Wire No. 31 did not meet the criteria in any of the items except for the average hardness of the weld metal part, which was judged as △.

[0051] In the case of Wire No. 32, the Si content was controlled to 0.001 to 0.1% or less, and the blowhole and slag area ratios were excellent as shown in Table 3, but as shown in Table 2, the average hardness of the weld metal was 320 in Vickers hardness, which was too low compared to the base metal of the steel, so the tensile strength of the weld was even lower than that of the base metal, and the fracture position was also in the weld metal, which did not meet the standards. Figure 2 is a photograph showing the cross-sectional structure and hardness distribution of the weld obtained from the comparative example [X(%)=0.55, Q(kJ / cm)=2.6] welded using Wire No. 32 in Table 2, and the cross-sectional structure of the fractured part after a static tensile test. In addition, Wire Nos. 33 to 37 have X values ​​that do not satisfy the above-mentioned appropriate range, and the average hardness of the weld metal exceeds 400, and the Si content also exceeds 0.1%, which means that they do not meet all the criteria for the tensile properties of the weld, blowholes, and slag area ratio. In particular, some of these are broken at the fusion line when pulled, which confirms that the brittleness of the weld metal increases.

[0052] On the other hand, FIG. 3 shows RT (Radiographic Test) photographs of the weld metal parts obtained after lap joint welding was performed on the above-mentioned zinc-plated steel sheet and after lap joint welding was performed on an alloyed zinc-plated steel sheet using wires Nos. 5, 7, 12, 34, and 36 in Table 2 as described above. 3, in the case of welds obtained using wires No. 34 and No. 36, in which the Si content is outside the range of 0.001-0.1% and the above-mentioned X value is also outside the range of 0.7-1.1%, the blowhole area ratio increased significantly, as can be confirmed from the RT results. On the other hand, in the case of welds obtained using wires No. 5, 7 and No. 12, in which the Si and X values ​​fall within the appropriate ranges of the present invention, it can be confirmed that very good results were obtained, with the blowhole area ratio being within 1%.

[0053] Example 2 [Table 4] *In Table 4, M indicates martensite, B indicates bainite, and γ indicates retained austenite. In Table 4, the steel number indicates the steel number in Table 1, and the wire number indicates the wire number in Table 2.

[0054] As shown in Table 4 above, the steel materials in Table 4 were lap-welded using a solid wire to obtain weld metals. At this time, the steel materials were zinc-plated steel sheets with a thickness of 2.0 mm. The specific welding conditions for this welding were the same as those in Example 1, and only the welding heat input was changed for each combination of wire and steel material as shown in Table 4 above. The tensile strength of each weld metal obtained by applying different welding heat inputs as described above was measured, and the results are shown in Table 4 above, together with the microstructural characteristics of the weld metal.

[0055] On the other hand, in the present invention, the above tensile strength was measured by processing three tensile test pieces of JIS No. 5 standard tensile test pieces at the center of the bead as welded test pieces of the lap joint, attaching an extensometer and conducting a tensile test at a tension speed of 10 mm / min, and then calculating the average of the obtained measured values. The microstructure of the weld was measured by taking an optical photograph after Lepera etching of the weld metal, and analyzing the low-temperature transformation phases classified by color difference. The average effective grain size and the grain fraction with a high hard angle of 47° or more were also measured by EBSD analysis.

[0056] As shown in Table 4 above, in the examples of the invention in which the Q value according to Relation 2 was in the range of 2.3 to 3.2 kJ / cm based on a steel plate base material thickness of 2.0 mm, the tensile strength of the weld exceeded 1 GPa, and the tensile strength ratio of the weld to the steel plate base material was also 95 to 96%. In contrast, in the comparative examples in which the Q value is less than 2.3 kJ / cm, it can be confirmed that the tensile strength of the weld is less than 1 GPa. And, in the case where the Q value exceeds 3.2 kJ / cm, backbeads are formed or melt-down occurs due to excessive welding heat input relative to the steel plate thickness, so these were excluded from this analysis.

[0057] On the other hand, when the X value defined by the above Relational Formula 1 is in the range of 0.7 to 1.1%, the low-temperature transformation start temperature becomes lower, and therefore upper and lower bainite can develop in the temperature range of about 400 to 250°C. In particular, it has been determined that this is effective in improving strength and toughness because a large number of high-hardness grains develop in an interlocking structure intertwined with the prior austenite grains, as opposed to martensite alone, and are mixed with martensite.

[0058] Fig. 4 is an EBSD micrograph and an inverse pole figure of the weld metal obtained from an example of the invention [X(%)=0.85, Q(kJ / cm)=3.2] in which No. 7 wire and No. 1 steel material in Table 4 were welded together, and explains this point in detail. In contrast, Fig. 5 is an EBSD micrograph and an inverse pole figure of the weld metal obtained from a comparative example [X(%)=0.55, Q(kJ / cm)=3.2] in which No. 32 wire and No. 1 steel material in Table 4 were welded together, and it can be seen that although the welding heat input is within the range of the present invention, the X value is outside the range of the present invention and the desired microstructure is not obtained.

[0059] Meanwhile, Figure 6 shows a photograph of the appearance of the weld bead obtained from an example of the invention [X(%)=0.85, Q(kJ / cm)=2.6] in which No. 7 wire and No. 1 steel material in Table 4 were combined for welding, and a photograph of the appearance after painting was applied without post-treatment processes such as pickling or brushing to remove slag from the weld. In particular, it can be confirmed that the slag area ratio of the weld bead was extremely reduced to within 1%, despite the use of a mixture of 20% carbon dioxide gas in the shielding gas, and this confirms that it is possible to improve the paintability of the weld and the corrosion resistance after painting.

[0060] 7a and 7b are diagrams showing the load change of the weld (FIG. 7b) compared with the load change of the steel material (FIG. 7a), which is the base material for welding, when a load is applied to the weld obtained from the example of the invention [X(%)=0.85, Q(kJ / cm)=2.6] obtained by combining and welding No. 7 wire and No. 1 steel material in Table 4 and a high-speed tensile test (tensile speeds of 1 m / s and 15 m / s, respectively) is performed. Specifically, in a relatively low-speed collision (3.6 km / h), the maximum load ratio of the weld to the base steel material is 95%, which is very excellent, and no fracture occurs in the weld metal or fusion line. Even in a high-speed collision (54 km / h), the maximum load ratio of the weld to the base steel material is 82%, and it is confirmed that even in this case, the load ratio of the weld can be maintained at 80% or more without fracture of the weld metal. This confirms the above-mentioned characteristics of the microstructure of the weld metal, and shows that gas-shielded arc welds of giga-class steels with tensile strengths of 1 GPa or more can be effectively obtained.

[0061] As described above, the detailed description of the present invention has been given of the preferred embodiment of the present invention, but it is obvious that those skilled in the art can make various modifications without departing from the scope of the present invention. Therefore, the scope of the present invention should not be limited to the described embodiment, but should be determined by the claims below as well as equivalents thereto.

Claims

1. A gas-shielded arc welding wire comprising, in total mass %, C: 0.08-0.15%, Si: 0.001%-0.1%, Mn: 1.6-1.9%, P: 0.015% or less, S: 0.015% or less, Cr: 4.0-5.2%, Mo: 0.4-0.65%, with the balance being Fe and inevitable impurities, wherein a value X defined by the following relational expression 1 satisfies the range of 0.7-1.1%. [Relationship 1] X (%)=[Cr] / 10+[Mo]-4×[Si] / [Mn] In the relational formula 1, [Cr], [Mo], [Si] and [Mn] represent the mass percentage of each element.

2. 2. The wire for gas-shielded arc welding according to claim 1, wherein a Cu plating layer is formed on a surface of the welding wire.

3. 3. The wire for gas-shielded arc welding according to claim 2, characterized in that the Cu constituting the Cu plating layer has a Cu content of 0.4% or less (excluding 0%) in mass % with respect to the entire wire including the plating layer.

4. The wire for gas-shielded arc welding according to claim 3, characterized in that the Cu plating layer has a Cu content in the range of 0.1 to 0.3% by mass based on the entire wire including the plating layer.

5. 2. The wire for gas shielded arc welding according to claim 1, characterized in that the welding wire contains Cr: 4.2 to 4.9%, Mo: 0.45 to 0.48%, and Mn: 1.65 to 1.75%, respectively.

6. 2. The wire for gas-shielded arc welding according to claim 1, wherein the welding wire has a Si content in the range of 0.04 to 0.08%.

7. 2. The wire for gas-shielded arc welding according to claim 1, wherein the welding wire is a solid wire for gas-shielded arc welding.

8. A welded structure having a welded portion obtained by welding two or more weld base materials using the welding wire according to any one of claims 1 to 7, The welded portion has a microstructure consisting of, by area%, 30-50% martensite, 50-70% bainite, and the remainder being 5% or less of retained austenite, and the microstructure constituting the welded portion has an average effective crystal grain size of 1-3 μm and a crystal grain fraction with a high tilt angle of 47° or more of 35% or more.

9. The welded structure according to claim 8, wherein at least one of the weld base materials is a galvanized steel sheet.

10. The welded structure according to claim 9, wherein the galvanized steel sheet is one of an electrogalvanized steel sheet, a hot-dip galvanized steel sheet, and an alloyed hot-dip galvanized steel sheet.

11. The welded structure according to claim 10, characterized in that the base steel sheet constituting the galvanized steel sheet contains, by mass%, one or more of Cr: 0.2 to 0.9% and Mo: 0.1 to 0.2%.

12. 9. The welded structure according to claim 8, wherein the weld has an average hardness of 370 to 400 Hv and a tensile strength of 1 GPa or more, which is 95% or more of the weld base material.

13. 9. The welded structure according to claim 8, wherein the high-speed tensile strength of the welded portion is 95% or more and 80% or more of that of the base material at tensile speeds of 3.6 km / h and 54 km / h, respectively.

14. A method for gas-shielded arc welding of a weld base metal using the welding wire according to any one of claims 1 to 7, comprising the steps of: The protective gas during welding is 5 to 20% CO in Ar. 2 A mixture of A gas shielded arc welding method, characterized in that welding is performed so that the range of the welding heat input Q (kJ / cm) defined by the following relational expression 2 satisfies 1.15t≦Q≦1.6t, where t (mm) is the thickness of the weld base metal. [Relationship 2] Q=(I×E)×0.048 / υ In the relational expression 2, I, E, and υ respectively represent the welding current [A], the welding voltage [V], and the welding speed (cm / min).

15. The gas shielded arc welding method according to claim 14, wherein the welding wire is a solid wire having a diameter of 0.9 to 1.2 mm.

16. The gas shielded arc welding method according to claim 14, characterized in that the weld base metal contains, by mass%, one or more of Cr: 0.2 to 0.9% and Mo: 0.1 to 0.2%.

17. The gas shielded arc welding method according to claim 14, wherein the welding base material is a zinc-plated steel sheet.

18. The gas shielded arc welding method according to claim 17, wherein the galvanized steel sheet is one of an electrogalvanized steel sheet, a hot-dip galvanized steel sheet, and an alloyed hot-dip galvanized steel sheet.

Citation Information

Patent Citations

  • Method for welding rail by gas shielded arc welding method

    JP1996108281A

  • Ultrahigh strength steel sheet and ultrahigh strength steel tube having excellent high speed ductile fracture property, and their production method

    JP2005146407A

  • Gas-shielded arc welding solid wire for weather resistant steel and gas-shielded arc welding method using the same

    JP2007296541A

  • Arc welding method and solid wire

    JP2019000882A

  • Cold rolled steel sheet having excellent spot welding property and delayed fracture resistance and method for manufacturing the same

    KR101115790B1