Manufacturing method of high density carbon fiber nonwoven fabric

The wet papermaking process with stable fiber dispersion addresses the challenges of producing high-density carbon fiber nonwoven fabrics, achieving improved performance and cost-effectiveness without specialized equipment.

JP7564415B2Active Publication Date: 2024-10-09ORIBESUTO
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020115221
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-09
Publication Date
2024-10-09
Estimated Expiration
2040-06-09

AI Technical Summary

Technical Problem

Existing methods for producing high-density carbon fiber nonwoven fabrics face issues such as fiber breakage, reduced strength, and increased manufacturing costs due to the use of special equipment like water jet punching, which affects their performance in various applications, especially in CC composite base materials.

Method used

A method involving a wet papermaking process that includes preparing a liquid with a thickener and water, adding highly fibrillated fibers, dispersing carbon fibers, and using a conventional wet papermaking method to produce a carbon fiber nonwoven fabric with a high density by ensuring stable fiber dispersion and agglomeration.

Benefits of technology

The method enables the production of a high-density carbon fiber nonwoven fabric with stable density and improved performance, using conventional equipment, allowing for efficient resin impregnation and reduced manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564415000001
    Figure 0007564415000001
  • Figure 0007564415000002
    Figure 0007564415000002
Patent Text Reader

Abstract

To provide a novel high-density carbon fiber non-woven fabric which is obtained by using a conventional wet papermaking method, and a method of manufacturing the same.SOLUTION: There are provided a high-density carbon fiber non-woven fabric which has been difficult to get in the past, and a method of manufacturing the same. When a carbon fiber is manufactured by a wet papermaking method, manufacture can be performed by the manufacturing method consisting of first to fourth steps of: preparing a liquid made by mixing at least a thickener and water as the first step; dispersing a highly fibrillated fiber in the liquid so as to be 0.001 to 0.1 mass% (dry mass) based on the total mass of the liquid as the second step; dispersing the carbon fiber in the liquid obtained in the second step as the third step; and wet papermaking the liquid obtained in the third step as the fourth step.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An object of the present invention is to provide a carbon fiber nonwoven fabric and a manufacturing method thereof that uses a conventional wet papermaking method while not relying on special equipment or methods, and that has a higher density by dispersing highly fibrillated fibers in a liquid prepared for dispersing carbon fibers during the production of the carbon fiber nonwoven fabric, and a manufacturing method thereof. [Background technology]

[0002] Recently, density control is required as one of the issues related to the quality of paper and nonwoven fabric. The present invention is a technology for increasing the density of carbon fiber nonwoven fabric in particular. In the conventional papermaking industry, the high density of carbon fiber nonwoven fabric is realized by integrating carbonized polymer fibers and nonwoven fabric by needle punching and sintering them in the dry papermaking method (see Patent Document 1). Also, when a wet papermaking method is used, a multilayered papermaking web is manufactured by repeating the process of forming a papermaking web from a papermaking slurry containing short carbon fibers and ultrafine acrylonitrile fibers, and the multilayered papermaking web is further entangled and integrated by water jet punching to manufacture a high density carbon fiber nonwoven fabric (see Patent Document 2).

[0003] However, the nonwoven fabrics that have been successfully densified as described above have various problems and are not satisfactory as high-density carbon fiber nonwoven fabrics for use in a wide variety of applications, and in particular cannot be said to have sufficient performance in CC composite substrate applications. For example, in the dry carbon nonwoven fabrics of Patent Document 1, if stiff fibers such as PAN-based carbon fibers are used, the carbon fibers are broken or scratched during needle punching, resulting in a problem of reduced physical strength of the nonwoven fabric. In order to prevent the strength of the nonwoven fabric from decreasing, it is possible to use cotton-like pitch-based carbon fibers, but if cotton-like pitch-based carbon fibers are used, the mesh size of the carbon fiber nonwoven fabric becomes small, and in applications where resin impregnation processing is performed, such as CC composite substrates, the resin impregnation speed becomes slow, resulting in poor processing efficiency. In addition, the manufacturing method of water jet punching a multilayered wet web produced by a wet papermaking method is advantageous for the above-mentioned resin impregnation process because it allows the use of rigid PAN-based carbon fibers and produces a large mesh size and high density. However, it is necessary to install the wet web multilayering process and the water jet punching process separately in a wet papermaking machine, which increases the manufacturing cost. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 05-033249 [Patent Document 2] JP 2012-162835 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has an object to provide a carbon fiber nonwoven fabric having a high density that has sufficient performance as a high-density carbon fiber nonwoven fabric used for various applications and that is densified using a normal wet papermaking method without using special equipment such as water jet punching, in order to solve the problems specific to the densification papermaking method of carbon fiber nonwoven fabric described in paragraphs "0002" and "0003". The object of the present invention is to provide a carbon fiber nonwoven fabric having a high density that has not been achieved before and a method for producing the same, using a normal wet papermaking method, without using special equipment such as water jet punching. [Means for solving the problem]

[0006] A carbon fiber nonwoven fabric produced by a wet papermaking method, the first step being a step of preparing a liquid obtained by mixing at least a thickener and water, the second step being a step of dispersing highly fibrillated fibers in the liquid so that the amount of the highly fibrillated fibers is 0.001 to 0.1 mass% based on the total mass of the liquid, the third step being a step of dispersing carbon fibers in the liquid obtained in the second step, and the fourth step being a step of wet papermaking the liquid obtained in the third step, the highly densified carbon fiber nonwoven fabric produced by a production method consisting of the first to fourth steps (claim 1). The carbon fiber nonwoven fabric according to claim 1, the highly fibrillated fibers being organic fibers and / or inorganic fibers that have been mechanically and / or chemically fibrillated (claim 2). The carbon fiber nonwoven fabric according to any one of claims 1 to 2, the highly densified carbon fiber nonwoven fabric, the composition ratio of the dry mass of the carbon fibers to the dry mass of the entire carbon fiber nonwoven fabric being 10 to 98 mass% (claim 3). A densified carbon fiber nonwoven fabric according to any one of claims 1 to 3, characterized in that it contains highly fibrillated fibers and fibers other than carbon fibers (claim 4).A method for producing a carbon fiber nonwoven fabric by a wet papermaking process, comprising the first step of preparing a liquid obtained by mixing at least a thickener and water, the second step of dispersing highly fibrillated fibers in the liquid so that the highly fibrillated fibers are present in an amount of 0.001 to 0.1 mass% based on the total mass of the liquid, the third step of dispersing carbon fibers in the liquid obtained in the second step, and the fourth step of wet papermaking the liquid obtained in the third step, the method for producing a densified carbon fiber nonwoven fabric comprising the first to fourth steps (claim 5).A method for producing a carbon fiber nonwoven fabric according to claim 5, characterized in that the highly fibrillated fibers are organic fibers and / or inorganic fibers that are mechanically and / or chemically fibrillated (claim 6). 7. The method for producing a densified carbon fiber nonwoven fabric according to claim 5, wherein the composition ratio of the dry mass of the carbon fibers to the dry mass of the entire carbon fiber nonwoven fabric is 10 to 98 mass % (Claim 7).A method for producing a densified carbon fiber nonwoven fabric according to any one of claims 5 to 7, characterized in that the densified carbon fiber nonwoven fabric contains highly fibrillated fibers and fibers other than carbon fibers (claim 8). Effect of the Invention

[0007] The present invention provides a carbon fiber nonwoven fabric and a manufacturing method thereof, which can be easily manufactured by a normal wet papermaking method by wet papermaking a dispersion of carbon fibers in a liquid in which highly fibrillated fibers are dispersed within a certain range, thereby realizing a carbon fiber nonwoven fabric and a manufacturing method thereof that have a high density that has not been achieved in the past. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The details are explained below. As a result of studying the problem described in paragraph "0005", the present inventors have found that the first step is a step of preparing a liquid obtained by mixing at least a thickener and water, the second step is a step of dispersing highly fibrillated fibers in the liquid so that the amount of the highly fibrillated fibers is 0.001 to 0.1 mass% relative to the total mass of the liquid, the third step is a step of dispersing carbon fibers in the liquid obtained in the second step, and the fourth step is a step of producing the liquid obtained in the third step by a wet papermaking method, and that the carbon fiber nonwoven fabric produced by the first to fourth steps has a higher density than a nonwoven fabric produced by a normal wet papermaking method, and that a carbon fiber nonwoven fabric with a higher density than that obtained by the conventional method can be produced. Note that in the densified carbon fiber nonwoven fabric and the method for producing the same in the present invention, the definition of the densified carbon fiber nonwoven fabric is that the density measured by the measurement method described in the present invention is 0.1 g / cm. 3 The above applies.

[0009] The reasons for the high density are as follows: first, the highly fibrillated fibers have many fiber fibrils on the surface, which are physically entangled with the carbon fibers in the liquid, forming a dense aggregate state between the fibers, thereby densifying the carbon fiber nonwoven fabric. Second, in the conventional wet papermaking manufacturing method, the carbon fibers and the highly fibrillated fibers are simultaneously dispersed in a liquid obtained by mixing a thickener and water, so the amount of highly fibrillated fibers in the carbon fiber nonwoven fabric is often not stable. That is, in the wet papermaking method, when forming a wet paper in the meshmaking process (wet paper means a wet nonwoven fabric sheet), the dehydrated liquid flows down through the mesh of the mesh, is collected, and becomes a carbon fiber dispersion liquid again, but at this time, some of the highly fibrillated fibers flow down through the mesh together with the liquid. The amount of highly fibrillated fibers that flows down together with the liquid usually varies depending on the influence of the time elapsed since the start of production and the change in mesh size due to deterioration of the mesh. For this reason, the amount of highly fibrillated fibers in the produced carbon fiber nonwoven fabric also fluctuates, making it difficult to stabilize the density and to obtain a desired high-density carbon fiber nonwoven fabric. However, as in the present invention, if the liquid prepared for dispersing the carbon fibers is in a state in which the highly fibrillated fibers are dispersed within a certain range, the amount of highly fibrillated fibers flowing down from the mesh with the liquid during the formation of a wet paper in the mesh-making process does not fluctuate, and the amount of highly fibrillated fibers remaining in the wet paper formed in the mesh-making process is stable. For this reason, the carbon fiber nonwoven fabric and its manufacturing method of the present invention can provide a nonwoven fabric with a stable high density.

[0010] In the high density carbon fiber nonwoven fabric and its manufacturing method described in the present invention, all of the conventionally known carbon fibers can be used for the carbon nonwoven fabric. That is, both PAN-based carbon fibers made from polyacrylonitrile and pitch-based carbon fibers made from pitch can be used, and recycled carbon fibers can also be used. The recycled carbon fibers are carbon fibers obtained by removing resin from carbon fiber reinforced resin composites by a regeneration treatment method such as a heat treatment method, a sintering method, a superheating method, or a superheated steam method. In addition, the fiber diameter and fiber length are not limited as long as they can be used in a wet papermaking method, but the fiber diameter is preferably in the range of 3 to 20 μm, and the fiber length is preferably in the range of 1 to 30 mm. In particular, in consideration of dispersibility and re-aggregation in liquid, the fiber diameter is more preferably 5 to 10 μm, and the fiber length is more preferably 3 to 12 mm. Furthermore, two or more of the carbon fibers listed above may be mixed and used at any desired mixing ratio, but it goes without saying that this does not impair the performance of the high density carbon fiber nonwoven fabric of the present invention.

[0011] Regarding the content of carbon fibers in the carbon fiber nonwoven fabric, if the dry mass ratio of the carbon fibers to the dry mass of the entire carbon fiber nonwoven fabric is in the range of 10 to 98 mass%, densification can be performed without any problem. In the present invention, a carbon fiber nonwoven fabric having a content in the range of 80 to 90 mass% can be particularly preferably produced.

[0012] The highly fibrillated fibers used in the high density carbon fiber nonwoven fabric and its manufacturing method described in the present invention can be any fiber that can be used in a wet papermaking process, regardless of whether it is an organic fiber or an inorganic fiber. Examples of organic fibers include cellulose fibers such as natural pulp fibers and rayon, as well as synthetic fibers such as aramid, polyester, acrylic, polyethylene, and polypropylene. Examples of inorganic fibers include cotton-like artificial inorganic fibers such as glass wool, micro glass wool, silica wool, rock wool, and ceramic wool, which are produced by dissolving and blowing away minerals. Note that two or more of the organic fibers and inorganic fibers listed above can be used as the highly fibrillated fibers, and a mixture of organic and inorganic fibers can also be used.

[0013] Furthermore, as a method of fibrillation, all of those produced by conventionally known methods such as mechanical production and chemical production can be used. In terms of mechanical production, natural pulp fibers are preferably beaten with a refiner, ball mill, homogenizer, underwater counter collision method device, ultrasonic crusher, etc., and in terms of chemical production, synthetic pulps such as aramid, polyethylene, polypropylene, etc. produced by shear coagulation method or jet coagulation method can be preferably used. Furthermore, those produced by chemical production and subjected to mechanical production may be able to achieve appropriate fibrillation, and those produced by chemical production and subjected to mechanical production can also be used.

[0014] In the densified carbon fiber nonwoven fabric and its manufacturing method of the present invention, the highly fibrillated fibers described in paragraphs "0012" and "0013" are dispersed in a range of 0.001 to 0.1 mass% in terms of dry mass with respect to the total mass of the liquid prepared in step 1, which is a mixture of at least a thickener and water. From the viewpoint of wet papermaking, if the amount of highly fibrillated fibers is large, it becomes difficult to dehydrate and flow down the liquid from the papermaking mesh during the formation of wet paper in the papermaking process, which leads to a decrease in production efficiency such as a decrease in papermaking speed, so that the highly fibrillated fibers are preferably dispersed in a range of 0.001 to 0.08 mass%, more preferably 0.001 to 0.007 mass%.

[0015] In the densified carbon fiber nonwoven fabric and the manufacturing method thereof described in the present invention, inorganic fibers and organic fibers that can be used in a wet papermaking method can be contained as fibers other than the highly fibrillated fibers and carbon fibers. Examples of inorganic fibers include glass fibers, mineral fibers (sepiolite, rock wool, etc.), and biosoluble fibers. Examples of organic fibers include natural cellulose fibers (wood pulp, cotton, etc.) and synthetic fibers (polyester fibers, polypropylene fibers, aramid fibers, vinylon fibers, etc.). Needless to say, two or more types of the inorganic fibers and organic fibers can be contained, and a mixture of inorganic fibers and organic fibers can also be contained. The content of the inorganic fibers and organic fibers can be contained as long as it does not impair the performance, quality, and production efficiency of the densified carbon fiber nonwoven fabric, but is preferably in the range of 0 to 20% by mass in terms of dry mass ratio with respect to the dry mass of the entire carbon fiber nonwoven fabric.

[0016] In the high density carbon fiber nonwoven fabric and the manufacturing method thereof described in the present invention, a binder can be used as a component that fixes the fibers of the carbon fiber nonwoven fabric together. All binders that can be used in wet papermaking methods can be used. The state of the binder is not limited to solid or liquid, and as a solid, granular or fibrous binders can be used. As a liquid, aqueous solutions, dispersions, and emulsions can be used. As the material of the binder, various natural and synthetic resins as well as inorganic binders can be used. For example, natural binders include starch, and synthetic resins include polyvinyl alcohol resins, vinyl acetate resins, acrylic resins, epoxy resins, and urethane resins. Furthermore, inorganic binders include colloidal dispersions of alumina, silica, and the like. In the high density carbon fiber nonwoven fabric and the manufacturing method thereof described in the present invention, a fibrous binder made of polyvinyl alcohol resin is less likely to cause migration, and can easily fix the inside of the layer of the carbon fiber nonwoven fabric uniformly, thereby promoting densification, which is a preferred embodiment.

[0017] In the densified carbon fiber nonwoven fabric and the manufacturing method thereof described in the present invention, any thickener that has been publicly known and used in the wet papermaking method can be used as the thickener to be mixed with water in the first step. Examples of thickeners include synthetic resin types such as acrylic acid, acrylamide, ethylene oxide, and polyethylene glycol, as well as natural polymer types such as cellulose and alfalfa.

[0018] In the high density carbon fiber nonwoven fabric and the method for producing the same described in the present invention, the water mixed with the thickener in the first step is water normally used in the wet papermaking method, "water having the molecular formula H 2 O" and examples of such substances include well water, industrial water, tap water, ion-exchanged water, and distilled water.

[0019] As the manufacturing method for the densified carbon fiber nonwoven fabric and the manufacturing method thereof described in the present invention, a conventionally known papermaking method generally called a wet papermaking method is adopted. In the present invention, as described in the first to third steps in paragraph "0006", carbon fibers, fibers other than carbon fibers, and a solid binder are added as necessary, and highly fibrillated fibers are dispersed in a liquid, and the liquid is made to be uniformly dispersed in the liquid, which is then poured onto a wire mesh and dehydrated to obtain a wet paper. The obtained wet paper is dried to obtain a nonwoven fabric. In some cases, a liquid binder may be imparted (impregnated or applied) to the wet paper, and then the wet paper may be dried to obtain a nonwoven fabric. In addition, for the liquid consisting of each of the above-mentioned fibers and a solid binder added as necessary, the liquid binder may be added, and then the binder portion may be fixed to each fiber by a fixing agent to form flocks, and the flock dispersion liquid may be poured onto a wire mesh, dehydrated, and dried to obtain a nonwoven fabric.

[0020] In the densified carbon fiber nonwoven fabric and the manufacturing method thereof of the present invention, chemicals such as dispersants, defoamers, fixing agents, coagulants, etc. can be added to improve the productivity, performance, and quality of the carbon fiber nonwoven fabric. As the chemicals, those conventionally known in the wet papermaking method can be used.

[0021] In the densified carbon fiber nonwoven fabric and the manufacturing method thereof of the present invention, a wet papermaking method is adopted as described in paragraphs "0006" and "0019," and any conventionally known wet papermaking machine can be used. For example, a Fourdrinier papermaking machine, a twin-wire papermaking machine, a hybrid papermaking machine, a cylinder papermaking machine, a Yankee papermaking machine, or any combination papermaking machine can be used.

[0022] Furthermore, in the description of paragraph "0019", the method for drying the wet paper obtained by flowing a liquid consisting of each fiber and a solid binder added as necessary onto a wire net and dehydrating it is described. Any of the devices equipped in conventionally known wet papermaking machines can be used. For example, air-through dryers, Yankee dryers, multi-cylinder cylinder dryers, suction drum dryers, far-infrared dryers, etc. can be mentioned. In addition, in the case of a manufacturing method in which a liquid binder is applied to a wet paper, an air-through dryer is preferred because the moisture content of the wet paper entering the dryer is large. In the case of a wet paper formed from flocks formed by fixing a liquid binder to each fiber, a Yankee dryer or a multi-cylinder cylinder dryer is preferred because the wet paper is pressurized and dehydrated by a press roll or the like, and the moisture content is relatively small. EXAMPLES

[0023] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following examples and comparative examples, the mass% and basis weight are all based on the dry mass, and the mass% indicates the dry mass ratio to the total dry mass of the carbon fiber nonwoven fabric. The viscosity was measured using a BL type viscometer in accordance with the Japanese Industrial Standard JIS8803:2011. (Measurement conditions: Rotating rotor: No. 1; Rotation speed: 60 rpm; Liquid temperature: 25°C) EXAMPLES

[0024] Sodium polyacrylate (AQUALIC® H-IH-G, Nippon Shokubai Co., Ltd.) was dissolved in well water as a thickener to prepare a liquid with a viscosity in the range of 3 to 4 mPa·s, and microfibrous cellulose fiber (Cerish® KY-100G, Daizel Finechem Co., Ltd.) was dispersed in the prepared liquid as a highly fibrillated fiber to a concentration of 0.001 mass% (dry mass relative to the total liquid). 85 mass% of PAN-based carbon fiber and 5 mass% of thermoplastic resin fiber were uniformly dispersed in the liquid in which the highly fibrillated fiber was dispersed. The liquid obtained by dispersing each of the fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper. After that, 10 mass% of an acrylic resin emulsion was applied as a binder to the wet paper, and the wet paper was dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2 and the density is 0.160 g / cm 3 The result was a high-density carbon fiber nonwoven fabric. EXAMPLES

[0025] Sodium polyacrylate (AQUALIC® H-IH-G, Nippon Shokubai Co., Ltd.) was dissolved in well water as a thickener to prepare a liquid with a viscosity in the range of 3 to 4 mPa·s. Microfibrous cellulose fiber (Cerish® KY-100G, Daizel Finechem Co., Ltd.) was dispersed in the prepared liquid as a highly fibrillated fiber to a concentration of 0.050 mass% (dry mass relative to the total liquid). 85 mass% of PAN-based carbon fiber and 5 mass% of thermoplastic resin fiber were uniformly dispersed in the liquid in which the highly fibrillated fiber was dispersed. The liquid obtained by dispersing each of the fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper. After that, 10 mass% of an acrylic resin emulsion was applied as a binder to the wet paper, and the wet paper was dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2 and its density is 0.184 g / cm 3 The result was a high-density carbon fiber nonwoven fabric. EXAMPLES

[0026] Sodium polyacrylate (AQUALIC® H-IH-G, Nippon Shokubai Co., Ltd.) was dissolved in well water as a thickener to prepare a liquid with a viscosity in the range of 3 to 4 mPa·s. Microfibrous cellulose fiber (Cerish® KY-100G, Daizel Finechem Co., Ltd.) was dispersed in the prepared liquid as a highly fibrillated fiber to a concentration of 0.1 mass% (dry mass relative to the total liquid). 85 mass% of PAN-based carbon fiber and 5 mass% of thermoplastic resin fiber were uniformly dispersed in the liquid in which the highly fibrillated fiber was dispersed. The liquid obtained by dispersing each of the fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper. After that, 10 mass% of an acrylic resin emulsion was applied as a binder to the wet paper, and the wet paper was dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2 and its density is 0.211 g / cm 3 The result was a high-density carbon fiber nonwoven fabric. EXAMPLES

[0027] Sodium polyacrylate (AQUALIC® H-IH-G, Nippon Shokubai Co., Ltd.) was dissolved in well water as a thickener to prepare a liquid with a viscosity in the range of 3 to 4 mPa·s, and microfibrous aramid fiber (TIARA® KY-400S, Daizel Finechem Co., Ltd.) was dispersed in the prepared liquid as a highly fibrillated fiber to a concentration of 0.005 mass% (dry mass relative to the total amount of liquid). 85 mass% of PAN-based carbon fiber and 5 mass% of thermoplastic resin fiber were uniformly dispersed in the liquid in which the highly fibrillated fiber was dispersed. The liquid obtained by dispersing each of the fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper, after which 10 mass% of acrylic resin emulsion was applied as a binder to the wet paper and dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2 and its density is 0.145 g / cm 3 The result was a high-density carbon fiber nonwoven fabric. EXAMPLES

[0028] Sodium polyacrylate (AQUALIC® H-IH-G, Nippon Shokubai Co., Ltd.) was dissolved in well water as a thickener to prepare a liquid with a viscosity in the range of 3 to 4 mPa·s. Polyolefin hyperbranched fiber (Mitsui Chemicals SWP® EST-8) was dispersed in the prepared liquid as a highly fibrillated fiber to a concentration of 0.003 mass% (dry mass relative to the total liquid). 85 mass% of PAN-based carbon fiber and 5 mass% of thermoplastic resin fiber were uniformly dispersed in the liquid in which the highly fibrillated fiber was dispersed. The liquid obtained by dispersing each of the fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper. After that, 10 mass% of an acrylic resin emulsion was applied as a binder to the wet paper, and the wet paper was dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2 and its density is 0.151 g / cm 3 The carbon fiber nonwoven fabric had a high density.

[0029] Sodium polyacrylate (AQUALIC (registered trademark) H-IH-G, Nippon Shokubai Co., Ltd.) was dissolved in well water as a thickener to prepare a liquid with a viscosity of 3 to 4 mPa s. 85% by mass of PAN-based carbon fiber and 5% by mass of thermoplastic resin fiber were uniformly dispersed in the prepared liquid. The liquid obtained by dispersing each of the above fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper. After that, 10% by mass of acrylic resin emulsion was applied as a binder to the wet paper and dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2 and its density is 0.096 g / cm 3 Comparative Example 2

[0030] Polyethylene oxide (Meisei Chemical Industry Co., Ltd., Alcox (registered trademark) E-45) was dissolved in well water as a thickener to prepare a liquid with a viscosity of 3 to 4 mPa s. 85% by mass of PAN-based carbon fiber and 5% by mass of thermoplastic resin fiber were uniformly dispersed in the prepared liquid. The liquid obtained by dispersing each of the above fibers was passed through a mesh of a wet mesh machine and dehydrated to form a wet paper. After that, 10% by mass of acrylic resin emulsion was applied as a binder to the wet paper and dried to obtain a carbon fiber nonwoven fabric. The target basis weight was 100 g / m 2and its density is 0.092 g / cm 3 It became.

[0031] The densification evaluation carried out in the examples and comparative examples was carried out by the following test method. <Evaluation of high density> For the carbon fiber nonwoven fabric obtained in paragraphs "0024" to "0030", the basis weight and thickness were measured and the density was obtained in accordance with the Japanese Industrial Standard "Paper and Paperboard-Test Method for Thickness and Density P-8118:2014". The measurement conditions for basis weight and thickness are as follows. Thickness: 1 / 10m 2 Four sheets of carbon fiber nonwoven fabric of the same size were measured at six points on each sheet using a digital thickness gauge, DG-925, manufactured by Ono Sokki Co., Ltd. (load 110 g, surface diameter 10 mm Φ, surface pressure 13.7 KPa, thickness readable to within 0.001 mm), and the average value of the four sheets was calculated. Basis weight: 1 / 10m 2 Four sheets of carbon fiber nonwoven fabric of this size were weighed using a digital weighing scale (capable of measuring to the nearest 0.01 g), and the weight was multiplied by 10 to obtain the basis weight, which was then averaged over the four sheets. Density: The measured thickness (mm) is converted into basis weight (g / m 2 ) and then divided by 1000 to get the density (g / cm 3 ) was decided. The density values ​​obtained for the fiber papers produced in the above examples and comparative examples are shown in Table 1 below.

[0032] [Table 1] [Table 2] [Industrial Applicability]

[0033] The present invention will have a significant impact on various fields in which carbon nonwoven fabrics are used (electronic device materials, electrical device materials, building materials, automotive materials, aircraft materials, and space development materials). By increasing the density, it is possible to more efficiently combine resins and carbon nonwoven fabrics, such as in CC composites.

Claims

1. A method for producing a carbon fiber nonwoven fabric by a wet papermaking method, comprising the first step of preparing a liquid comprising at least a thickener and water, the second step of dispersing fibrillated organic fibers and / or inorganic fibers produced by a conventionally known method, such as a mechanical method and / or a chemical method, in the liquid so that the fibrillated organic fibers and / or inorganic fibers are dispersed in the liquid to a concentration of 0.001 to 0.1 mass % relative to the total mass of the liquid, the third step of dispersing carbon fibers in the liquid obtained in the second step, and the fourth step of wet papermaking the liquid obtained in the third step, said method for producing a densified carbon fiber nonwoven fabric comprising the first step to the fourth step.

2. A method for producing a densified carbon fiber nonwoven fabric as described in claim 1, characterized in that the composition ratio of the dry mass of the carbon fiber to the dry mass of the entire carbon fiber nonwoven fabric is 10 to 98 mass%.

3. A method for producing a densified carbon fiber nonwoven fabric as described in any one of claims 1 and 2, characterized in that the densified carbon fiber nonwoven fabric contains fibrillated organic fibers and / or inorganic fibers and fibers other than carbon fibers, the fibrillation method being produced by a conventionally known method, namely a mechanical method and / or a chemical method.

Citation Information

Patent Citations

  • High-density felt of carbon fiber and production thereof

    JP1993033249A

  • Nonwoven fabric of carbon fiber and method for producing the same

    JP2004353124A

  • Method for producing carbon fiber-containing nonwoven fabric

    JP2012162835A

  • Carbon short fiber wet type nonwoven fabric and carbon short fiber-reinforced resin composition

    JP2019031749A