Aramid fiber composite paper and preparation method thereof
The problem of insufficient tensile strength of aramid fiber composite paper is solved by the coating of modified aramid fiber with hyperbranched copolymer and branched polybenzimidazole, and the cross-linking reaction of polyacrylamide nanomicrosphere emulsion, which is significantly Improves its mechanical properties.
Patent Information
- Application Number
- CN202411158766.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The mechanical properties of aramid fiber composite paper are insufficient, especially the tensile strength is low, making it difficult to meet the needs of high-performance applications.
Modified aramid fiber and homemade tackifier are used to coat branched polybenzimidazoles by reacting with hyperbranched copolymers, and polyacrylamide nanomicrosphere emulsion is used as tackifier. The combination reaction enhances the mechanical properties of composite paper.
The tensile strength and mechanical properties of aramid fiber composite paper are significantly improved, making it suitable for high-performance applications.
Smart Images

Figure BDA0005005835990000081 
Figure BDA0005005835990000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of papermaking industry, in particular to aramid fiber composite paper and a preparation method thereof. Background Art
[0002] Aramid fiber is a representative of high-performance synthetic fibers, with many advantages such as high strength, high modulus, high temperature resistance, low density, and low thermal shrinkage. Aramid paper made from aramid fiber through wet papermaking and hot pressing has the characteristics of light specific gravity, high specific strength, high specific stiffness, impact resistance, outstanding corrosion resistance, good high temperature stability, and electromagnetic wave permeability. As an advanced substrate composite material, it is widely used in high-temperature insulation materials, aerospace, and high-performance electronic equipment.
[0003] Aramid composite paper is a sheet-like composite material formed by wet-making aramid short fibers and aramid pure pulp and hot pressing to form a composite material with good strength, heat resistance and insulation properties. However, aramid fiber composite paper still has the disadvantage of insufficient strength, so the present invention studies and prepares an aramid fiber composite paper with excellent mechanical properties. Summary of the invention
[0004] The object of the present invention is to provide an aramid fiber composite paper and a preparation method thereof to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: an aramid fiber composite paper, the aramid fiber composite paper comprises modified aramid fiber and a homemade thickener; the homemade thickener is a polyacrylamide nanosphere emulsion.
[0006] Preferably, the modified aramid fiber is prepared by reacting aramid fiber with a hyperbranched copolymer and then coating the surface with branched polybenzimidazole.
[0007] Preferably, the hyperbranched copolymer is obtained by free polymerization of p-chloromethylstyrene and grafting methyl methacrylate on the surface; the branched polybenzimidazole is obtained by introducing a rigid triazine structure into an ether-bonded polybenzimidazole.
[0008] Preferably, the polyacrylamide nanosphere emulsion is prepared by mixing an oil phase and an aqueous phase and then performing a phase inversion treatment; the aqueous phase comprises acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent; and the oil phase comprises white oil, sorbitan monooleate and diethylene glycol maleate.
[0009] Preferably, the method for preparing the aramid fiber composite paper comprises the following specific steps:
[0010] S1. The aramid fiber was extracted with acetone for 24 hours, vacuum dried at 40-50°C, immersed in a hyperbranched copolymer, heated to 50-60°C, treated for 18-24 hours, removed, washed with deionized water 3-5 times, and vacuum dried at 40-50°C to obtain a modified aramid fiber matrix;
[0011] S2. The modified aramid fiber matrix is immersed in the branched polybenzimidazole, the temperature is raised to 80-90°C, the reaction is performed for 6-12 hours, the matrix is removed and washed with deionized water for 3-5 times and vacuum dried at 40-50°C to obtain the modified aramid fiber;
[0012] S3. In a nitrogen atmosphere, the oil phase and the water phase were mixed at a mass ratio of 1:0.6-0.8, stirred evenly, and nitrogen was passed through the plastic at 1-3 ml / min. After reacting for 30-50 minutes, 0.2-0.4 times the mass of the oil phase sodium bisulfite was added, and the nitrogen was continued to react for 6-8 hours, and then the homemade thickener was obtained after reverse treatment;
[0013] S4. The modified aramid fiber and the dispersant polyethylene oxide are mixed in a mass ratio of 100:0.5-1, and after stirring evenly, a homemade thickener in an amount of 0.05-0.1 times the mass of the modified aramid fiber is added, and the mixture is stirred and dispersed evenly to obtain a slurry, which is formed on a rotary screen paper machine, pressed by an oil press and dried, and impregnated with a polyimide resin with an impregnation amount of 10-30%, and then pre-pressed and hot-pressed on a roller hot press to obtain an aramid fiber composite paper.
[0014] Preferably, in the above step S1., the preparation method of the hyperbranched copolymer is: under a nitrogen atmosphere, 2,2-bipyridine, cuprous chloride, p-chloromethylstyrene and chlorobenzene are mixed in a mass ratio of 1:0.3-0.4:20:8, the temperature is raised to 115-125° C., the reaction is carried out for 8-10 hours, and then 0.02-0.04 times the mass of p-chloromethylstyrene of 2,2-bipyridine, 0.1-0.2 times the mass of p-chloromethylstyrene of cuprous chloride, 0.8-0.9 times the mass of p-chloromethylstyrene of methyl methacrylate and 0.4-0.6 times the mass of p-chloromethylstyrene of toluene are added, and the reaction is continued for 8-12 hours to obtain a hyperbranched copolymer silicon.
[0015] Preferably, in the above step S2., the preparation method of the branched polybenzimidazole is: under a nitrogen atmosphere, the polyphosphoric acid is heated to 135-145° C., and after keeping warm for 1-3 hours, 0.4-0.6 times the mass of the polyphosphoric acid 3,3'4,4'-biphenyltetramine is added, and after stirring evenly, 0.25-0.35 times the mass of the polyphosphoric acid 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, 0.2-0.4 times the mass of the polyphosphoric acid 4,4-dicarboxy diphenyl ether and 0.1-0.3 times the mass of the polyphosphoric acid are added. After reacting for 6-8 hours, the mixture is transferred to sodium bicarbonate with a mass fraction of 8-12%, boiled, and the branched polybenzimidazole is obtained.
[0016] Preferably, in the above step S3., the oil phase is prepared by mixing white oil, sorbitan monooleate and diethylene glycol maleate in a mass ratio of 5:1 to 2:4.
[0017] Preferably, in the above step S3., the preparation method of the aqueous phase is: deionized water, acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent ethylenediaminetetraacetic acid are mixed in a mass ratio of 20-30:4-6:0.2:0.1, the pH is adjusted to 7.8-8.2 with sodium hydroxide, and then 0.04-0.06 times the mass of acrylamide ammonium persulfate is added to obtain an aqueous phase.
[0018] Preferably, in the above step S4., during pre-pressing, the time is 10 to 30 seconds, the temperature is 120 to 160°C, and the pressure is 8 to 10 MPa; during hot pressing, the time is 4 to 6 minutes, the temperature is 180 to 220°C, the pressure is 10 to 16 MPa, and the roller speed is 1 to 2 m / min.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The aramid fiber composite paper prepared by the present invention comprises modified aramid fiber and a self-made tackifier;
[0021] The modified aramid fiber is prepared by reacting aramid fiber with a hyperbranched copolymer and then coating the surface with branched polybenzimidazole. The hyperbranched copolymer is prepared by free polymerization of p-chloromethylstyrene and grafting methyl methacrylate on the surface. The branched polybenzimidazole is prepared by introducing a rigid triazine structure into ether-bonded polybenzimidazole. The hyperbranched copolymer has a multi-arm hyperbranched structure, reacts with the aramid fiber to crosslink on the surface, and then reacts with the hyperbranched copolymer to coat the surface of the aramid fiber to enhance the tensile strength.
[0022] The homemade thickener is polyacrylamide nanosphere emulsion, which is prepared by mixing the oil phase and the water phase and then performing a reverse treatment. The water phase includes acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinker and a chelating agent, and the oil phase includes white oil, sorbitan monooleate and diethylene glycol maleate. Ester groups are introduced into the polyacrylamide nanospheres, which are slowly hydrolyzed in an alkaline environment to release carboxyl groups, which crosslink with modified aramid fibers to enhance viscosity, thereby enhancing the mechanical properties of the composite paper. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods of various indicators of the aramid fiber composite paper prepared in the examples and comparative examples as follows:
[0025] Tensile strength: The aramid fiber composite papers prepared in the examples and comparative examples were subjected to a tensile index test according to GB / T12914.
[0026] Tensile strength: The aramid fiber composite papers prepared in the embodiment and the comparative example were cut into the same size, and subjected to a tensile test on a universal material testing machine. The test was repeated 5 times and the average value was taken.
[0027] Example 1
[0028] S1. Under a nitrogen atmosphere, 2,2-bipyridine, cuprous chloride, p-chloromethylstyrene and chlorobenzene were mixed in a mass ratio of 1:0.3:20:8, heated to 115°C, reacted for 8 hours, and then 0.02 times the mass of p-chloromethylstyrene of 2,2-bipyridine, 0.1 times the mass of p-chloromethylstyrene of cuprous chloride, 0.8 times the mass of p-chloromethylstyrene of methyl methacrylate and 0.4 times the mass of p-chloromethylstyrene of toluene were added, and the reaction was continued for 8 hours to obtain a hyperbranched copolymer; the aramid fiber was extracted with acetone for 24 hours, vacuum dried at 40°C, immersed in the hyperbranched copolymer, heated to 50°C, treated for 18 hours, fished out, washed 3 times with deionized water and vacuum dried at 40°C to obtain a modified aramid fiber matrix;
[0029] S2. In a nitrogen atmosphere, the polyphosphoric acid was heated to 135°C, kept warm for 1 hour, and then 0.4 times the mass of the polyphosphoric acid was added with 3,3'4,4'-diphenyltetramine, stirred evenly, and then 0.25 times the mass of the polyphosphoric acid was added with 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, 0.2 times the mass of the polyphosphoric acid was 4,4-dicarboxy diphenyl ether, and 0.1 times the mass of the polyphosphoric acid was phosphorus pentoxide. After reacting for 6 hours, the mixture was transferred to 8% sodium bicarbonate by mass, boiled, and branched polybenzimidazole was obtained; the modified aramid fiber matrix was immersed in the branched polybenzimidazole, heated to 80°C, reacted for 6 hours, removed, washed with deionized water 3 times, and vacuum dried at 40°C to obtain modified aramid fiber;
[0030] S3. White oil, sorbitol monooleate and diethylene glycol maleate were mixed in a mass ratio of 5:1:4 to prepare an oil phase; deionized water, acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent ethylenediaminetetraacetic acid were mixed in a mass ratio of 20:4:0.2:0.1, the pH was adjusted to 7.8 with sodium hydroxide, and then 0.04 times the mass of ammonium persulfate of acrylamide was added to prepare an aqueous phase; under a nitrogen atmosphere, the oil phase and the aqueous phase were mixed in a mass ratio of 1:0.6, stirred evenly and nitrogen was passed through a plastic at 1 ml / min. After reacting for 30 minutes, 0.2 times the mass of sodium bisulfite of the oil phase was added, and the nitrogen reaction was continued for 6 hours, and then the homemade tackifier was prepared after reverse treatment;
[0031] S4. The modified aramid fiber and the dispersant polyethylene oxide are mixed in a mass ratio of 100:0.5, and after stirring evenly, a homemade thickener in an amount of 0.05 times the mass of the modified aramid fiber is added, and the mixture is stirred and dispersed evenly to obtain a slurry. The slurry is formed on a rotary screen paper machine, pressed by an oil press, and dried. The slurry is impregnated with a polyimide resin with an impregnation amount of 10%, and then pre-pressed and hot-pressed on a roller hot press. The pre-pressing time is 10 seconds, the temperature is 120°C, and the pressure is 8 MPa. The hot pressing time is 4 minutes, the temperature is 180°C, the pressure is 10 MPa, and the roller speed is 1 m / min to obtain aramid fiber composite paper.
[0032] Example 2
[0033] S1. Under a nitrogen atmosphere, 2,2-bipyridine, cuprous chloride, p-chloromethylstyrene and chlorobenzene were mixed in a mass ratio of 1:0.35:20:8, heated to 120°C, reacted for 9 hours, and then 0.03 times the mass of p-chloromethylstyrene of 2,2-bipyridine, 0.15 times the mass of p-chloromethylstyrene of cuprous chloride, 0.85 times the mass of p-chloromethylstyrene of methyl methacrylate and 0.5 times the mass of p-chloromethylstyrene of toluene were added, and the reaction was continued for 10 hours to obtain a hyperbranched copolymer; the aramid fiber was extracted with acetone for 24 hours, vacuum dried at 45°C, immersed in the hyperbranched copolymer, heated to 55°C, treated for 22 hours, removed, washed 4 times with deionized water and vacuum dried at 45°C to obtain a modified aramid fiber matrix;
[0034] S2. In a nitrogen atmosphere, the polyphosphoric acid was heated to 140°C, kept warm for 2 hours, and then 0.5 times the mass of the polyphosphoric acid was added with 3,3'4,4'-diphenyltetramine, and stirred evenly. Then, 0.30 times the mass of the polyphosphoric acid was added with 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, 0.3 times the mass of the polyphosphoric acid was added with 4,4-dicarboxy diphenyl ether, and 0.2 times the mass of the polyphosphoric acid was added with phosphorus pentoxide. After reacting for 7 hours, the mixture was transferred to 10% sodium bicarbonate by mass, boiled, and branched polybenzimidazole was obtained; the modified aramid fiber matrix was immersed in the branched polybenzimidazole, heated to 85°C, reacted for 9 hours, removed, washed with deionized water 4 times, and vacuum dried at 45°C to obtain modified aramid fiber;
[0035] S3. White oil, sorbitol monooleate and diethylene glycol maleate were mixed in a mass ratio of 5:1.5:4 to prepare an oil phase; deionized water, acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent ethylenediaminetetraacetic acid were mixed in a mass ratio of 25:5:0.2:0.1, the pH was adjusted to 8.0 with sodium hydroxide, and then 0.05 times the mass of ammonium persulfate of acrylamide was added to prepare an aqueous phase; under a nitrogen atmosphere, the oil phase and the aqueous phase were mixed in a mass ratio of 1:0.7, stirred evenly and nitrogen was passed through a plastic at 2 ml / min. After reacting for 40 minutes, 0.3 times the mass of sodium bisulfite of the oil phase was added, and the nitrogen reaction was continued for 7 hours, and then the homemade tackifier was prepared after reverse treatment;
[0036] S4. The modified aramid fiber and the dispersant polyethylene oxide are mixed in a mass ratio of 100:0.8, and after stirring evenly, a homemade thickener in an amount of 0.08 times the mass of the modified aramid fiber is added, and the mixture is stirred and dispersed evenly to obtain a slurry. The slurry is formed on a rotary screen paper machine, pressed by an oil press, and dried. The slurry is impregnated with a polyimide resin with an impregnation amount of 20%, and then pre-pressed and hot-pressed on a roller hot press. The pre-pressing time is 20 seconds, the temperature is 140°C, and the pressure is 9 MPa. The hot pressing time is 5 minutes, the temperature is 200°C, the pressure is 14 MPa, and the roller speed is 1.5 m / min to obtain aramid fiber composite paper.
[0037] Example 3
[0038] S1. Under a nitrogen atmosphere, 2,2-bipyridine, cuprous chloride, p-chloromethylstyrene and chlorobenzene were mixed in a mass ratio of 1:0.4:20:8, heated to 125°C, reacted for 10 hours, and then 0.04 times the mass of p-chloromethylstyrene of 2,2-bipyridine, 0.2 times the mass of p-chloromethylstyrene of cuprous chloride, 0.9 times the mass of p-chloromethylstyrene of methyl methacrylate and 0.6 times the mass of p-chloromethylstyrene of toluene were added, and the reaction was continued for 12 hours to obtain a hyperbranched copolymer; the aramid fiber was extracted with acetone for 24 hours, vacuum dried at 50°C, immersed in the hyperbranched copolymer, heated to 60°C, treated for 24 hours, fished out, washed with deionized water 5 times and vacuum dried at 50°C to obtain a modified aramid fiber matrix;
[0039] S2. In a nitrogen atmosphere, the polyphosphoric acid was heated to 145°C, kept warm for 3 hours, and then 0.6 times the mass of the polyphosphoric acid was added with 3,3'4,4'-diphenyltetramine, and stirred evenly. Then, 0.35 times the mass of the polyphosphoric acid was added with 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, 0.4 times the mass of the polyphosphoric acid was 4,4-dicarboxy diphenyl ether, and 0.3 times the mass of the polyphosphoric acid was phosphorus pentoxide. After reacting for 8 hours, the mixture was transferred to 12% sodium bicarbonate by mass, boiled, and branched polybenzimidazole was obtained; the modified aramid fiber matrix was immersed in the branched polybenzimidazole, heated to 90°C, reacted for 12 hours, removed, washed with deionized water 5 times, and vacuum dried at 50°C to obtain modified aramid fiber;
[0040] S3. white oil, sorbitol monooleate and diethylene glycol maleate were mixed in a mass ratio of 5:2:4 to prepare an oil phase; deionized water, acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent ethylenediaminetetraacetic acid were mixed in a mass ratio of 30:6:0.2:0.1, the pH was adjusted to 8.2 with sodium hydroxide, and then 0.06 times the mass of ammonium persulfate of acrylamide was added to prepare an aqueous phase; under a nitrogen atmosphere, the oil phase and the aqueous phase were mixed in a mass ratio of 1:0.8, stirred evenly and nitrogen was passed through a plastic at 3 ml / min. After reacting for 50 minutes, 0.4 times the mass of sodium bisulfite of the oil phase was added, and the nitrogen reaction was continued for 8 hours, and then the homemade tackifier was prepared after reverse treatment;
[0041] S4. The modified aramid fiber and the dispersant polyethylene oxide are mixed in a mass ratio of 100:1, and after stirring evenly, a homemade thickener in an amount of 0.1 times the mass of the modified aramid fiber is added, and the mixture is stirred and dispersed evenly to obtain a slurry. The slurry is formed on a rotary screen paper machine, pressed by an oil press, and dried. The slurry is impregnated with a polyimide resin with an impregnation amount of 30%, and then pre-pressed and hot-pressed on a roller hot press. The pre-pressing time is 30 seconds, the temperature is 160°C, and the pressure is 10 MPa. The hot pressing time is 6 minutes, the temperature is 220°C, the pressure is 16 MPa, and the roller speed is 2 m / min to obtain aramid fiber composite paper.
[0042] Comparative Example 1
[0043] The composition of Comparative Example 1 is the same as that of Example 2. The difference between the preparation method of the aramid fiber composite paper and that of Example 2 is that the modified aramid fiber is prepared by reacting aramid fiber with a hyperbranched copolymer.
[0044] Comparative Example 2
[0045] The composition of Comparative Example 2 is the same as that of Example 2. The difference between the preparation method of the aramid fiber composite paper and that of Example 2 is that the prepared aramid fiber composite paper includes aramid fiber and a homemade tackifier.
[0046] Comparative Example 3
[0047] The composition of Comparative Example 3 is the same as that of Example 2. The difference between the preparation method of the aramid fiber composite paper and that of Example 2 is that the homemade tackifier is polyacrylamide emulsion.
[0048] Comparative Example 4
[0049] The composition of Comparative Example 4 is the same as that of Example 2. The difference between the preparation method of the aramid fiber composite paper and that of Example 2 is that the oil phase is only white oil.
[0050] Effect example
[0051] Table 1 below shows the performance analysis results of the aramid fiber composite papers prepared using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4:
[0052] Table 1
[0053]
[0054]
[0055] By comparing the experimental data of the examples and the comparative examples in Table 1, it can be clearly found that the aramid fiber composite paper prepared by using Examples 1, 2 and 3 has excellent tensile strength and mechanical properties.
[0056] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, it can be found that after the aramid fiber reacts with the hyperbranched copolymer, the modified aramid fiber prepared by coating the surface with branched polybenzimidazole, the hyperbranched copolymer having a multi-arm hyperbranched structure, reacts with the aramid fiber to crosslink on the surface, and then reacts with the hyperbranched copolymer and is coated on the surface of the aramid fiber to enhance the tensile strength.
[0057] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, Comparative Example 4, it can be found that the polyacrylamide nanosphere emulsion is prepared by mixing an oil phase and an aqueous phase and then performing a reverse phase treatment, the aqueous phase includes acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent, the oil phase includes white oil, sorbitan monooleate and diethylene glycol maleate, and an ester group is introduced into the polyacrylamide nanosphere, which is slowly hydrolyzed in an alkaline environment to release a carboxyl group, which is crosslinked with the modified aramid fiber to enhance the viscosity, thereby enhancing the mechanical properties of the composite paper.
[0058] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.
Claims
1. A aramid fiber composite paper, characterized in that: The aramid fiber composite paper comprises modified aramid fiber and a self-made tackifier; the self-made tackifier is polyacrylamide nano-microsphere emulsion.
2. The aramid fiber composite paper according to claim 1, characterized in that: The modified aramid fiber is prepared by reacting aramid fiber with a hyperbranched copolymer and then coating the surface with branched polybenzimidazole.
3. The aramid fiber composite paper according to claim 2, characterized in that: The hyperbranched copolymer is prepared by free polymerization of p-chloromethylstyrene and grafting methyl methacrylate on the surface; the branched polybenzimidazole is prepared by introducing a rigid triazine structure into an ether-bonded polybenzimidazole.
4. The aramid fiber composite paper according to claim 1, characterized in that: The polyacrylamide nano-microsphere emulsion is prepared by mixing an oil phase and a water phase and then performing a reverse phase treatment; the water phase comprises acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent; the oil phase comprises white oil, sorbitol monooleate and diethylene glycol maleic acid diester.
5. A method for preparing the aramid fiber composite paper according to claim 1, characterized in that: The specific steps include: S1. The aramid fiber was extracted with acetone for 24 hours, vacuum dried at 40-50°C, immersed in a hyperbranched copolymer, heated to 50-60°C, treated for 18-24 hours, removed, washed with deionized water 3-5 times, and vacuum dried at 40-50°C to obtain a modified aramid fiber matrix; S2. The modified aramid fiber matrix is immersed in the branched polybenzimidazole, the temperature is raised to 80-90°C, the reaction is performed for 6-12 hours, the matrix is removed and washed with deionized water for 3-5 times and vacuum dried at 40-50°C to obtain the modified aramid fiber; S3. In a nitrogen atmosphere, the oil phase and the water phase were mixed at a mass ratio of 1:0.6-0.8, stirred evenly, and nitrogen was passed through the plastic at 1-3 ml / min. After reacting for 30-50 minutes, 0.2-0.4 times the mass of the oil phase sodium bisulfite was added, and the nitrogen was continued to react for 6-8 hours, and then the homemade thickener was obtained after reverse treatment; S4. The modified aramid fiber and the dispersant polyethylene oxide are mixed in a mass ratio of 100:0.5-1, and after stirring evenly, a homemade thickener in an amount of 0.05-0.1 times the mass of the modified aramid fiber is added, and the mixture is stirred and dispersed evenly to obtain a slurry, which is formed on a rotary screen paper machine, pressed by an oil press and dried, and impregnated with a polyimide resin with an impregnation amount of 10-30%, and then pre-pressed and hot-pressed on a roller hot press to obtain an aramid fiber composite paper.
6. The method for preparing aramid fiber composite paper according to claim 5, characterized in that: In the above step S1., the preparation method of the hyperbranched copolymer is: under a nitrogen atmosphere, 2,2-bipyridine, cuprous chloride, p-chloromethylstyrene and chlorobenzene are mixed in a mass ratio of 1:0.3-0.4:20:8, the temperature is raised to 115-125° C., the reaction is performed for 8-10 hours, and then 0.02-0.04 times the mass of p-chloromethylstyrene of 2,2-bipyridine, 0.1-0.2 times the mass of p-chloromethylstyrene of cuprous chloride, 0.8-0.9 times the mass of p-chloromethylstyrene of methyl methacrylate and 0.4-0.6 times the mass of p-chloromethylstyrene of toluene are added, and the reaction is continued for 8-12 hours to obtain a hyperbranched copolymer.
7. The method for preparing aramid fiber composite paper according to claim 5, characterized in that: In the above step S2., the preparation method of the branched polybenzimidazole is as follows: in a nitrogen atmosphere, the polyphosphoric acid is heated to 135-145° C., and after keeping warm for 1-3 hours, 0.4-0.6 times the mass of the polyphosphoric acid is added with 3,3'4,4'-biphenyltetramine, and after stirring evenly, 0.25-0.35 times the mass of the polyphosphoric acid is added with 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, 0.2-0.4 times the mass of the polyphosphoric acid, 4,4-dicarboxy diphenyl ether, and 0.1-0.3 times the mass of the polyphosphoric acid are added with phosphorus pentoxide, and after reacting for 6-8 hours, the mixture is transferred to sodium bicarbonate with a mass fraction of 8-12%, and boiled to obtain the branched polybenzimidazole.
8. The method for preparing aramid fiber composite paper according to claim 5, characterized in that: In the above step S3., the oil phase is prepared by mixing white oil, sorbitol monooleate and diethylene glycol maleate in a mass ratio of 5:1 to 2:
4.
9. The method for preparing aramid fiber composite paper according to claim 5, characterized in that: In the above step S3., the method for preparing the aqueous phase is: deionized water, acrylamide, a crosslinking agent N,N-methylenebisacrylamide crosslinking agent and a chelating agent ethylenediaminetetraacetic acid are mixed in a mass ratio of 20-30:4-6:0.2:0.1, the pH is adjusted to 7.8-8.2 with sodium hydroxide, and then 0.04-0.06 times the mass of acrylamide ammonium persulfate is added to obtain an aqueous phase.
10. The method for preparing aramid fiber composite paper according to claim 5, characterized in that: In the above step S4., during pre-pressing, the time is 10 to 30 seconds, the temperature is 120 to 160°C, and the pressure is 8 to 10 MPa; during hot pressing, the time is 4 to 6 minutes, the temperature is 180 to 220°C, the pressure is 10 to 16 MPa, and the roller speed is 1 to 2 m / min.
Citation Information
Patent Citations
Surface modification aramid fiber and preparation method thereof
CN105803789A
Aramid fiber-base insulation paper with high breakdown strength for transformer and preparation method of aramid fiber-base insulation paper
CN106758460A
Copolyacrylamide composite microsphere as well as preparation method and application thereof
CN112708083A
Glass fiber filter material with positive Zeta potential and preparation method and application thereof
CN113737570A
Preparation method of branched / cross-linked membrane applied to high-temperature proton exchange membrane fuel cell
CN116632302A
Cited By
High-voltage flexible cable for shield tunneling machine and preparation process of high-voltage flexible cable
CN120108830A
Aramid fiber coated diaphragm as well as preparation method and application thereof
CN122436664A