Surface coated cutting tools
A two-layer hard coating structure with AlTiN and AlTiBN layers addresses chipping and wear issues in coated tools during interrupted cutting of high-hardness steel, enhancing durability and wear resistance.
Patent Information
- Application Number
- JP2021553475
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-29
- Filing Date
- 2020-10-20
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-10-20
AI Technical Summary
Existing coated tools exhibit insufficient chipping resistance and wear resistance during interrupted cutting of high-hardness steel, leading to short tool life.
A surface-coated cutting tool with a two-layer hard coating structure, comprising a lower AlTiN layer and an upper AlTiBN layer with a compositionally modulated B component, applied using arc ion plating, to enhance adhesion, toughness, and thermal conductivity, and controlled residual stress to prevent chipping and wear.
The tool demonstrates excellent wear resistance and prevents chipping during interrupted cutting of high-hardness steel, extending tool life by suppressing crack growth and peeling.
Smart Images

Figure 0007564510000009 
Figure 0007564510000010 
Figure 0007564510000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-coated cutting tool (hereinafter, sometimes referred to as a coated tool). This application claims priority based on Japanese Patent Application No. 2019-195796, filed on October 29, 2019. All contents of said Japanese Patent Application are incorporated herein by reference. [Background technology]
[0002] Coated tools include inserts which are removably attached to the tip of a cutting tool for turning and flat cutting of workpieces such as various types of steel and cast iron, drills and miniature drills which are used for drilling holes in the workpiece, and solid-type end mills which are used for facing, grooving and shoulder machining of the workpiece. Also known are insert-type end mills which have removably attached inserts and perform cutting in the same way as solid-type end mills. Materials used as the tool base for coated tools include WC-based cemented carbide, TiCN-based cermet, cubic boron nitride-based sintered compact, and high-speed tool steel.
[0003] Conventionally, various proposals have been made to improve the performance of coated tools.
[0004] For example, in Patent Document 1, a tool substrate made of cemented carbide (Al x Ti 1-x )(B y N 1-y It has been proposed to improve the wear resistance of coated tools by forming a hard coating layer made of boron nitride having the composition shown by the following formula: (where 0.05≦x≦0.75, 0.02≦y≦0.12).
[0005] In addition, Patent Document 2 proposes a surface-coated cutting tool in which a hard coating layer composed of an upper layer and a lower layer made of a composite nitride of Ti, Al and B is formed on the surface of a tool substrate made of WC-based cemented carbide, TiCN-based cermet or high-speed tool steel. The upper layer has an alternating laminate structure of thin layer A and thin layer B, and thin layer A has a composition formula: [Ti1-(M+N) Al M B N ]N (wherein, in atomic ratio, M is 0.15 to 0.35, and N is 0.15 to 0.30), the thin layer B is a composite nitride layer of Ti, Al and B satisfying the composition formula: [Ti 1-(X+Y) Al X B Y ]N (wherein, in terms of atomic ratio, X is 0.50 to 0.60 and Y is 0.01 to 0.10), the lower layer has a single-phase structure and is represented by the composition formula: [Ti 1-(X+Y) Al X B Y ]N (wherein, in atomic ratio, X is 0.50 to 0.60 and Y is 0.01 to 0.10), and it is disclosed that the hard coating layer of the surface-coated cutting tool exhibits excellent wear resistance in high-speed cutting of heat-resistant alloys.
[0006] The proposals in Patent Documents 1 and 2 are directed to surface-coated cutting tools in which a hard coating layer is formed on the surface of a cemented carbide alloy. However, Patent Document 3, for example, also proposes a surface-coated cutting tool in which a cBN sintered body is used as a tool base and a hard coating layer is formed on the tool by vapor deposition.
[0007] In Patent Document 3, a hard coating layer is provided that is composed of a lower layer A directly on a cBN sintered body and an upper layer B formed thereon, and the lower layer A has a composition formula: Ti 1-a Al a N (where a is an atomic ratio of 0.3≦a≦0.7), and the upper layer B has a composition formula: Ti 1-x―y Al x S y N (where x and y are atomic ratios of 0.3≦x≦0.7, 0.01≦y≦0.1), and further, the residual stress in the lower layer A of the flank face is σ A (GPa), and the residual stress of the entire hard coating layer is σ T (GPa), σ A <σ T、 -7, 0≦σ A ≦-1.0, -4.0≦σ T ≦-0.5, |σ A -σ TA surface coated cutting tool is disclosed in which the surface roughness is |<4.0. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 4-26756 [Patent Document 2] JP 2006-334739 A [Patent Document 3] JP 2015-178171 A Summary of the Invention [Problem to be solved by the invention]
[0009] The inventors have studied the coated tools described in the above Patent Documents 1 to 3. As a result, they have come to the following realization.
[0010] The coated tool described in Patent Document 1 exhibits excellent wear resistance in continuous cutting of carbon steel, but when used in intermittent cutting of high-hardness steel, it cannot be said that either chipping resistance or wear resistance is sufficient.
[0011] Furthermore, the coated tool described in Patent Document 2 exhibits excellent wear resistance when used for high-speed cutting of heat-resistant alloys, such as Ni alloys, Co alloys, and Ti alloys, which generate high heat. However, when used for intermittent cutting of high-hardness steel, the coated tool does not have sufficient chipping resistance.
[0012] Furthermore, the coated tool described in Patent Document 3 exhibits excellent chipping resistance and wear resistance in high-speed continuous cutting of hardened steel as described in the document, but when subjected to intermittent cutting, the chipping resistance is still unsatisfactory.
[0013] In any case, the coated tools described in Patent Documents 1 to 3 cannot reduce the occurrence of chipping while simultaneously ensuring excellent wear resistance in the interrupted cutting of high-hardness steel, and therefore have a problem in that the tool life is short.
[0014] Here, high speed steel refers to an alloy steel having a surface hardness of HRC 35 to 65, the surface of which has been carburized and quenched. In addition, the intermittent cutting refers to a process in which the cutting edge rotates idly during cutting, and an example of this is the cutting of a workpiece exclusive of a slit. [Means for solving the problem]
[0015] The surface-coated cutting tool according to an embodiment of the present invention comprises: The tool has a tool base made of a cubic boron nitride sintered body and a hard coating layer on at least a cutting edge surface of the tool base, (a) the hard coating layer has a lower layer α immediately above the tool substrate and an upper layer β above the lower layer α, (b) the lower layer α has an average composition Composition formula: (Al 1-x Ti x )N (where x is an atomic ratio of 0.40≦x≦0.60), (c) the upper layer β has an average composition Composition formula: (Al 1-y-z Ti y B z )N (where y and z are atomic ratios, and 0.40≦y≦0.60, 0.01≦z≦0.10) are satisfied; (d) the upper layer β has a compositionally modulated structure in which the concentration of the B component changes repeatedly along the layer thickness direction, (e) the repeated change in the concentration of the B component in the compositionally modulated structure is repeated with an average interval between adjacent maximum and minimum values of the concentration of the B component of 1 to 100 nm, (f) When the average of the maximum values of the concentration of the B component is Bmaxav, z <Bmaxav≦2.0×zであり、 On the other hand, when the average of the minimum values of the concentration of the B component is Bminav, 0≦Bminav <zであり、 (g) the average thickness of the hard coating layer is 1.0 to 4.0 μm, and when the average thickness of the lower layer α is tα and the average thickness of the upper layer β is tβ, the relationship 2.0≦tβ / tα≦6.0 is satisfied; (h) The residual stress σ of the entire hard coating layer satisfies −2.0 GPa≦σ≦−0.5 GPa.
[0016] Furthermore, the surface-coated cutting tool according to the embodiment may satisfy one or more of the following requirements. (1) Regarding the upper layer β, average The plastic deformation work ratio W obtained by performing a nanoindentation test with an indentation depth of less than 1 / 10 of the layer thickness plast / (W plast +W elast ) is 0.42 to 0.47, and the nanoindentation hardness is 26 to 30 GPa. (2) The hard coating layer has a TiN layer as an upper layer thereof. Effect of the Invention
[0017] According to the above, even when used in the interrupted cutting of high-hardness steel, abnormal damage such as chipping, fracture, and peeling does not occur, and excellent wear resistance is exhibited over long-term use. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a cross-sectional schematic view showing a layer structure of a hard coating layer of the coated tool according to the embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a compositionally modulated structure of the B component along the layer thickness direction in the upper layer β of the coated tool according to the embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic explanatory view for measuring the residual stress σ of the entire hard coating layer. [Figure 4]FIG. 2 is a schematic diagram of a displacement-load load curve and a displacement-load unloading curve for determining a plastic deformation work ratio. [Diagram 5] FIG. 2 is a schematic diagram illustrating a test method for determining a plastic deformation work ratio. [Figure 6] FIG. 1 is a schematic plan view of an arc ion plating (AIP) device for depositing a hard coating layer of a coated tool according to an embodiment of the present invention. [Figure 7] FIG. 7 is a schematic side view of the arc ion plating (AIP) apparatus of FIG. 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] As a result of extensive investigations, the present inventors have obtained the following findings (1) to (4). (1) A hard coating layer having a two-layer structure consisting of a lower layer and an upper layer is vapor-deposited on at least the cutting edge surface of a tool base (hereinafter sometimes referred to as the "cBN base") made of sintered cBN. The lower layer of the hard coating layer is then formed as a buffer layer of a composite nitride of Al and Ti (hereinafter sometimes referred to as AlTiN), which has excellent deformation follow-up properties. This increases the adhesive strength between the tool base and the hard coating layer and makes it possible to suppress peeling of the hard coating layer at the cutting edge.
[0020] (2) As the upper layer on the lower layer of the hard coating layer, a composite nitride layer of Al, Ti and B (hereinafter, sometimes referred to as an AlTiBN layer) having a composition modulated structure in which the concentration of the B component changes repeatedly along the layer thickness direction (a cross section perpendicular to the surface of the tool base (longitudinal cross section, thickness direction of the hard coating layer)) is formed. This provides high hardness and high thermal conductivity as well as high toughness, and makes it possible to suppress the occurrence of chipping and breakage when intermittent high loads are applied to the cutting edge.
[0021] (3) By imparting a predetermined residual stress to the hard coating layer, it is possible to suppress the propagation of interfacial cracks that occur at the interface between the lower layer and the cBN substrate, and it is also possible to suppress the propagation of cracks that occur on the surface of the upper layer into the interior of the upper layer during cutting. As a result, even when subjected to intermittent cutting of high-hardness steel, chipping and fracture can be prevented.
[0022] (4) When the lower layer and the AlTiBN layer having a compositionally modulated structure in which the concentration of the B component changes repeatedly are deposited by an arc ion plating apparatus (referred to as an "AIP apparatus"), which is a type of physical vapor deposition apparatus, the desired residual stress can be imparted to the hard coating layer by controlling the DC bias voltage applied to the cBN substrate, which is one of the deposition conditions.
[0023] Here, the inventors surmise that the AlTiN layer (lower layer) is able to ensure excellent strength and toughness due to its constituent Ti component, that Al improves high-temperature hardness and heat resistance, and that the coexistence of Al and Ti has the effect of further improving high-temperature oxidation resistance, and that the AlTiBN layer (upper layer) further contains the B component, thereby improving thermal conductivity, and as a result, the plastic deformation resistance and high-temperature hardness of the AlTiBN layer are improved.
[0024] Hereinafter, an embodiment of the present invention will be described in detail. In this specification and claims, when a numerical range is expressed as "A to B" (where A and B are both numerical values), the range includes an upper limit value (B) and a lower limit value (A), and the upper limit value (B) and the lower limit value (A) have the same units.
[0025] Hard coating layer: As shown in FIG. 1, the hard coating layer according to the embodiment of the present invention has a lower layer α of AlTiN on at least the cutting edge surface of a tool substrate, and an upper layer β of AlTiBN thereon.
[0026] Although not shown in Fig. 1, a TiN layer may be provided as an upper layer of the hard coating layer. As will be described later, this TiN layer can serve as, for example, a corner identification layer.
[0027] The lower layer α has excellent strength and toughness due to its Ti component, and the Al component improves high-temperature hardness and heat resistance, and the coexistence of the Al and Ti components improves high-temperature oxidation resistance and deformation followability. The lower layer α also enhances the buffering effect between the upper layer β and the tool base, improving the adhesive strength of the hard coating layer, which can suppress peeling of the hard coating layer when intermittent high loads are applied to the cutting edge.
[0028] Moreover, the upper layer β is a layer of the same composition as the lower layer α, but further contains the component B, and forms a composition-modulated structure of the component B, thereby increasing hardness and improving thermal conductivity. As a result, the hardness of the upper layer β does not decrease even when exposed to high heat during cutting, and it exhibits excellent wear resistance.
[0029] In particular, the upper layer β has a composition modulation structure in which a region with a relatively low concentration of the B component, which has excellent strength and toughness (a region where the concentration of the B component is approximately close to the minimum value Bmin) and a region with a relatively high concentration of the B component, which has high thermal conductivity and high hardness (a region where the concentration of the B component is approximately close to the maximum value Bmax), are repeatedly formed in the thickness direction of the upper layer β, thereby making it possible to suppress chipping and damage to the hard coating layer during intermittent cutting in which a high intermittent load acts on the cutting edge.
[0030] When the average thickness of the hard coating layer (the total thickness of the lower layer α and the upper layer β) is 1.0 to 4.0 μm, the above-mentioned effects are prominently exhibited. The reason is that if the average layer thickness is less than 1.0 μm, the thickness of the hard coating layer is thin compared to the surface roughness of the tool base, making it impossible to ensure sufficient wear resistance over long periods of use, while if the average layer thickness exceeds 4.0 μm, the crystal grains of the composite nitride constituting the hard coating layer tend to become coarse, making chipping and breakage more likely to occur.
[0031] The lower layer α constituting the hard coating layer: The lower layer α has a composition represented by the formula: (Al 1-x Ti x )N, the average content ratio x of Ti in the total amount of Al and Ti (where x is an atomic ratio) preferably satisfies 0.40≦x≦0.60. The reason for this is that if the Ti content is less than 0.40, the AlTiN layer cannot maintain the rock-salt crystal structure, resulting in a drastic reduction in hardness and a decrease in deformation compliance when a high load is applied to the cutting edge; on the other hand, if the Ti content exceeds 0.60, the Al content decreases relatively, making it impossible to obtain sufficient high-temperature hardness and heat resistance.
[0032] The upper layer β constituting the hard coating layer: The upper layer β is a layer having the same component system as the lower layer α and further containing a B component, and a compositionally modulated structure is formed in the upper layer β in which the concentration of the B component repeatedly changes along the layer thickness direction.
[0033] Here, the composition of the upper layer β is represented by the formula: (Al 1-y-z Ti y B z )N, the average content y of Ti in the total amount of Al and Ti (where y is an atomic ratio) is preferably 0.40≦y≦0.60 for the same reasons as for the content x of Ti in the lower layer α, but the content y of Ti does not necessarily have to be the same as the content x of Ti in the lower layer α (it may be different).
[0034] When the average content ratio z of B to the total amount of Al, Ti, and B in the upper layer β (where z is an atomic ratio) is less than 0.01, the effect of improving the hardness and thermal conductivity of the upper layer β is small. On the other hand, even if the average content ratio z exceeds 0.10, the effect of improving the hardness is small. Therefore, it is preferable that 0.01≦z≦0.10.
[0035] Here, the concentration of the B component in the upper layer β has a compositionally graded structure along the layer thickness direction. That is, it is preferable that the concentration of the B component in the upper layer β has a minimum value Bmin and a maximum value Bmax of the B component concentration repetitively present along the layer thickness direction.
[0036] Fig. 2 is a diagram showing an example of a repeated change in the concentration of the B component, with the concentration of the B component on the vertical axis and the position of the upper layer β on the horizontal axis. In Fig. 2, the maximum value Bmax and the minimum value Bmin are the same value, and the interval d between adjacent maximum values Bmax and minimum values Bmin is also the same, but the repeated change in the B concentration (composition modulation structure) referred to in this specification and claims is only required to change the B concentration to have the maximum value Bmax and the minimum value Bmin, and the maximum value Bmax and the minimum value Bmin may or may not be the same value, and the interval d between adjacent maximum values Bmax and minimum values Bmin may or may not be the same value.
[0037] Here, the average interval between the position giving the maximum value Bmax of B and the adjacent position giving the minimum value Bmin in the upper layer β having a repeated change in B concentration can be determined by measuring the B content in a cross section (longitudinal cross section) of the upper layer β perpendicular to the surface of the tool base in a direction perpendicular to the surface of the tool base (layer thickness direction), and graphing the result after performing known measurement noise removal.
[0038] That is, as shown in Figure 2, a straight line m is drawn across the curve showing the repeated change in B concentration. This straight line m is drawn so that the area of the region surrounded by the curve is equal on both sides of the line. Then, for each region where this straight line m crosses the curve showing the repeated change in B concentration, the maximum value Bmax or minimum value Bmin of the B component concentration is obtained, and the distance between the two is measured. The measured values at multiple points are averaged to obtain the average distance of the repeated change in B concentration in the upper layer β. The value of m can be regarded as the average B composition z.
[0039] When the concentration of the B component forms such a compositionally modulated structure, the upper layer β has excellent hardness and thermal conductivity in the region where the concentration of the B component is relatively high (region where the concentration of the B component is close to Bmax), and has excellent strength and toughness in the region where the concentration of the B component is relatively low (region where the concentration of the B component is close to Bmin). This increases the hardness, thermal conductivity, strength, and toughness of the upper layer β as a whole, and as a result, it is possible to suppress the occurrence of chipping and breakage even when intermittent high loads are applied to the cutting edge.
[0040] In the periodic change in the concentration of the B component in the compositionally modulated structure, it is preferable that the interval (the distance in the layer thickness direction of the upper layer β) between adjacent maximum value Bmax and minimum value Bmin of the B component concentration is repeated at an average interval of 1 to 100 nm.
[0041] The reason for this is that if the average distance between the maximum value Bmax and the minimum value Bmin of the B component is less than 1 nm, the maximum value Bmax and the minimum value Bmin of the B component concentration cannot be clearly distinguished from each other, and the upper layer β cannot ensure the strength, toughness, and high hardness properties as a whole. On the other hand, if the average distance between the maximum value and the minimum value of the B component exceeds 100 nm, the defects inherent to the respective maximum and minimum values of the B component concentration become clearly apparent, and the property of the upper layer β of suppressing the occurrence of chipping and defects is reduced.
[0042] In order to suppress the occurrence of chipping and defects, it is preferable that the average Bmaxav of the maximum value Bmax of the concentration of component B and the average Bminav of the minimum value Bmin of the concentration of component B satisfy z < Bmaxav ≤ 2.0×z and 0 ≤ Bminav < z, respectively.
[0043] Incidentally, as described above, the average composition z of the upper layer β is a value calculated as the average value of the maximum value Bmax and the minimum value Bmin of the concentration of component B in the compositional modulation of component B measured at at least five positions in the upper layer β.
[0044] In this embodiment, as already described, the average layer thickness of the hard coating layer is 1.0 to 4.0 μm. When the layer thickness of the lower layer α is tα and the average layer thickness of the upper layer β is tβ, it is more preferable that the average layer thickness ratio tβ / tα of the upper layer to the average layer thickness of the lower layer satisfies 2.0 ≤ tβ / tα ≤ 6.0.
[0045] The reason is that if the layer thickness ratio tβ / tα is between 2 and 6, the occurrence of chipping can be more reliably reduced and excellent wear resistance can be exhibited.
[0046] Incidentally, the average composition of the lower layer α and the upper layer β, the average layer thickness of one layer, the average layer thickness of the hard coating layer, and further, the concentration change of component B in the upper layer β can be measured by cross-sectional measurement using secondary ion mass spectrometry (SIMS) in the depth direction of the hard coating layer from the surface of the coated tool (i.e., the thickness direction of the hard coating layer), and scanning electron microscopy (SEM), transmission electron microscopy (TEM), and energy dispersive X-ray spectroscopy (EDS) for a longitudinal section perpendicular to the surface of the tool substrate, respectively.
[0047] Residual stress σ of the entire hard coating layer: In this embodiment, in order to sufficiently suppress the progress of cracks occurring in the hard coating layer or cracks occurring at the interface between the cBN substrate and the lower layer α, it is preferable to impart a residual stress σ satisfying -2.0 (GPa) ≦ σ ≦ -0.5 (GPa) to the entire hard coating layer (note that the negative sign means that the residual stress σ is a compressive residual stress). In this way, it is possible to suppress the propagation and progress of cracks that propagate from the surface of the upper layer β into the hard coating layer during cutting, and to prevent peeling of the hard coating layer due to the propagation and progress of cracks at the interface between the lower layer α and the cBN substrate.
[0048] A specific method for measuring residual stress is, for example, the well-known 2θ-sin 2 It is performed by X-ray diffraction (XRD) using the ψ method. The measurement principle and method are described in detail in, for example, the Standard for X-Ray Stress Measurement Method (1997 edition) published by the X-Ray Materials Strength Division Committee of the Japan Society for Materials Science, Revised Edition of X-Ray Stress Measurement Method (Yokendo, 1990), and Fundamentals and Recent Developments of X-Ray Stress Measurement Method (Zaiyo Vol. 47, No. 11, 1998).
[0049] Here, the residual stress σ (GPa) of the hard coating layer as a whole refers to the residual stress calculated by treating the overlapping XRD peak intensity DI of the lower layer α ((Ti,Al)N layer) and the upper layer β ((Ti,Al,B)N layer) indicated by the downward arrow as one peak intensity when measuring the residual stress using XRD peaks, as shown in FIG. 3.
[0050] Plastic deformation work ratio and nanoindentation hardness of the upper layer β: When the plastic deformation work ratio and nanoindentation hardness were obtained by performing a nanoindentation test on the upper layer β at a depth of 1 / 10 or less of the layer thickness, the plastic deformation work ratio (= W plast / (W plast +W elast It is more preferable that the value of ) is 0.42 to 0.47 and the nanoindentation hardness is 26 GPa to 30 GPa.
[0051] Here, the indentation depth is 1 / 10 or less of the thickness of the upper layer β, and may be a depth at which nanoindentation hardness can be measured. An example of the load that gives this indentation depth is 1.96 N (200 mgf).
[0052] The reason why a nanoindentation hardness in the above range is more preferable is that if it is less than 26 GPa, the upper layer β may not be able to exhibit sufficient wear resistance, while if the nanoindentation hardness exceeds 30 GPa, chipping and damage may become more likely to occur.
[0053] The plastic deformation work ratio W plast / (W plast +W elast ) is calculated as follows. That is, a load is applied so that the indentation depth is 1 / 10 or less of the thickness of the upper layer β, and the surface of the upper layer β is displaced (see FIG. 5), a load curve of displacement-load is calculated (see FIG. 4), and then the load is removed to calculate an unloading curve of displacement-load (see FIG. 4). From the difference between the load curve and the unloading curve, the plastic deformation work ratio W plast and elastic deformation work W elast From these, the plastic deformation work ratio W plast / (W plast +W elast ) is calculated.
[0054] Here, the plastic deformation work ratio W plast / (W plast +W elast ) is more preferably 0.42 to 0.47.
[0055] The reason is that the plastic deformation work ratio W plast / (W plast +W elast If the ratio is less than 0.42, the impact relaxation properties are insufficient, and sufficient chipping resistance and fracture resistance may not be obtained when subjected to interrupted cutting conditions. On the other hand, if the ratio exceeds 0.47, the plastic deformation resistance decreases, and sufficient wear resistance may not be obtained.
[0056] The coated tool of this embodiment may further have a TiN layer on the upper layer β as an upper layer of the hard coating layer. When a TiN layer is formed as the upper layer, the TiN layer itself has a golden color tone, and therefore, can be used as an identification layer that can determine, for example, whether a cutting tool is unused or used based on a change in color tone of the upper layer. The average thickness of the TiN layer serving as the discrimination layer may be, for example, 0.1 to 1 μm.
[0057] Although there are no particular limitations on the composition and structure of the cBN substrate, which is the tool substrate of the coated tool of the present invention, it is preferable that the average particle size of the cBN particles is 0.5-4.0 μm and the volume ratio of the cBN particles in the cBN sintered compact is in the range of 40-70 volume %. In addition, it is preferable to use particles containing at least one selected from the group consisting of Ti nitrides, carbides, carbonitrides, and borides, and Al nitrides and oxides, as the binder phase forming component particles in the cBN sintered compact. EXAMPLES
[0058] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0059] Preparation of the tool substrate: As the raw material powders, cBN particles having an average particle size of 0.5 to 4.0 μm were prepared as the raw material powder for forming the hard phase, and TiN powder, TiC powder, TiCN powder, Al powder, AlN powder, and Al2O3 powder, all of which had average particle sizes within the range of 0.3 to 0.9 μm, were prepared as the raw material powder for forming the binder phase.
[0060] Some of these binder phase forming raw material powders were mixed with the cBN particle powder and blended in the blending ratios shown in Table 1 so that the cBN particle content in the cBN sintered body would be 40 to 70 volume %. In Table 1, "-" indicates that no cBN particles were included.
[0061] Here, the content (volume%) of cBN particles in the cBN sintered body was calculated as follows. That is, the cross-sectional structure of the prepared cBN sintered body was observed at a magnification of 5,000 times using a scanning electron microscope (SEM), the cBN particle part in the obtained secondary electron image was extracted by image processing, the area occupied by the cBN particles was calculated by image analysis using image analysis software (ImageJ), and the area was divided by the total area of the image to calculate the area ratio, which was regarded as the content (volume%). The content (volume%) was measured using the secondary electron image obtained by this SEM for at least three observation areas, and the average of the calculated volume% was regarded as the content (volume%, vol%) of cBN particles. Note that an area of 20 μm × 20 μm was used as the observation area used for image processing.
[0062] Next, the blended powder was wet mixed in a ball mill for 72 hours, dried, and then molded in a hydraulic press at a molding pressure of 1 MPa to obtain a press-molded body with dimensions of diameter: 50 mm × thickness: 1.5 mm. Then, this press-molded body was subjected to a pressure of 1 × 10 -4 The mixture was pre-sintered at 900-1300°C in a vacuum atmosphere of 0.1 Pa or less, and then loaded into an ultra-high pressure sintering apparatus and held at a pressure of 5 GPa and a temperature of 1200-1400°C for 30 minutes to produce a cBN sintered body.
[0063] The cBN sintered body was cut to a predetermined size by a wire electric discharge machine. Then, a WC-based cemented carbide insert body having a composition of 5 mass% Co, 5 mass% TaC, and the remainder of WC and an insert shape of ISO standard CNGA120408 was prepared, and the cut sintered body was brazed to the brazing part (corner part) using Ag-based brazing material (having a composition of Cu: 26%, Ti: 5%, and Ag: the remainder in mass%), and the upper and lower surfaces and the outer circumference were polished and honed to produce cBN bases 1 to 3 for the example having an insert shape of ISO standard CNGA120408.
[0064] [Table 1]
[0065] Film forming process: A hard coating layer was formed on the cBN substrates (tool substrates) 1 to 3 by the following steps using an arc ion plating apparatus shown in FIGS. 6 and 7, to obtain coated tools of the example (also referred to as Examples) 1 to 10.
[0066] (a) The cBN substrates 1 to 3 were ultrasonically cleaned in acetone and, in a dried state, mounted along the outer periphery at a predetermined distance in the radial direction from the central axis on a rotating table in an arc ion plating apparatus. In addition, an Al-Ti alloy for forming the lower layer α, an Al-Ti-B alloy for forming the upper layer β, and an Al-Ti alloy for forming the upper layer β, each having a predetermined composition, were placed in the apparatus as cathode electrodes (evaporation sources).
[0067] Although this did not apply to Examples 1 to 3, if the Ti content x in the lower layer α and the Ti content y in the upper layer β are the same, a single Al-Ti alloy may be used to form both the lower layer α and the upper layer β.
[0068] (b) Evacuate the inside of the device for 10 -2 While maintaining a vacuum of 0.1 Pa or less, the inside of the apparatus was heated to 500° C. with a heater, and then the pressure was set to 2 Pa of Ar gas atmosphere. A DC bias voltage of −200 to −600 V was applied to the cBN substrates 1 to 3 rotating on the rotating table, whereby the surfaces were bombarded and cleaned with argon ions.
[0069] (c) Nitrogen gas was introduced into the apparatus as a reactive gas, and the film formation atmosphere temperature was set to 400 to 550°C and the nitrogen gas pressure was set to a predetermined value of 2 to 8 Pa as shown in Table 2. A DC bias voltage of -20 to -100 V as shown in Table 2 was applied to the cBN substrates 1 to 3 rotating on the turntable, and a current of 100 to 200 A as shown in Table 2 was applied between the cathode electrode (evaporation source) made of the Al-Ti alloy and the anode electrode to generate an arc discharge, and the lower layer α was formed by vapor deposition on the surface of the cBN substrates 1 to 3 so as to become an (Al, Ti)N layer having the average composition and average layer thickness as shown in Table 2.
[0070] (d) Nitrogen gas is introduced into the apparatus as a reactive gas, and the film formation atmosphere temperature is set to 400 to 550°C and the nitrogen gas pressure is set to a predetermined value of 3 to 10 Pa as shown in Table 3. A DC bias voltage of -30 to -100 V as shown in Table 3 is applied to the cBN substrates 1 to 3 rotating on the rotating table, and a current of 90 to 180 A as shown in Table 3 is applied between the cathode electrode (evaporation source) made of the Al-Ti-B alloy and the anode electrode to generate an arc discharge. At the same time, a predetermined DC bias voltage of -30 to -100 V shown in Table 3 was applied, and a predetermined current of 90 to 180 A shown in Table 3 was passed between the cathode electrode (evaporation source) made of the Al-Ti alloy and the anode electrode to generate an arc discharge and perform simultaneous deposition, thereby forming the upper layer β, which is an (Al, Ti, B)N layer having the average composition and average layer thickness shown in Table 3 on the surface of the lower layer α, and has a composition modulation structure of the B component within the (Al, Ti, B)N layer. The lower layer α and the upper layer β are shown in Table 6.
[0071] Here, the maximum value Bmax of the B component concentration in the upper layer β, the minimum value Bmin of the B component concentration, the average interval between the adjacent maximum value Bmax and minimum value Bmin, etc. can be adjusted by the rotation speed of the turntable of the cBN substrate on the turntable in step (d), the B content in the Al-Ti-B alloy, the strength of the arc discharge between the cathode electrode (evaporation source) made of the Al-Ti-B alloy and the anode electrode, etc., and the residual stress σ of the entire hard coating layer can be controlled by adjusting the bias voltage.
[0072] In the step (c), the film was formed at a lower gas pressure and a higher arc current than in the step (d), so that the lower layer α formed a fine structure, while in the step (d), the film was formed at a higher gas pressure and a lower arc current than in the step (c), and the film formation time was adjusted so that the thickness of the upper layer β was thicker than that of the lower layer α.
[0073] For comparison, the conditions in steps (c) and (d) of the cBN substrates 1 to 3 were changed to the values shown in Tables 4 and 5, respectively, to produce comparative coated tools (also referred to as comparative examples) 1 to 6 having the component composition ratios, layer thickness ratios of the lower layer α and the upper layer β, and residual stress σ shown in Table 7.
[0074] In some of the examples and comparative examples, a cathode electrode (evaporation source) made of metal Ti was added to the apparatus (not shown in Figs. 6 and 7), and a TiN layer having a thickness of 0.1 to 1 µm was further vapor-deposited as an upper layer of the hard coating layer.
[0075] For Examples 1 to 10 and Comparative Examples 1 to 6, the composition of the lower layer α and the composition of the upper layer β, as well as the maximum value Bmax and minimum value Bmin of the concentration of the B component in the composition-modulated structure of the upper layer β, were measured at least at five locations by Secondary Ion Mass Spectrometry (SIMS), and x, y, z, Bmaxav, and Bminav were calculated by averaging these measured values.
[0076] The average composition z of the B component in the upper layer β having a compositionally modulated structure of the B component was calculated as the average value of (Bmax+Bmin) / 2 measured at at least five locations.
[0077] The thickness of the lower layer α and the thickness of the upper layer β were measured in longitudinal section using a scanning electron microscope (SEM), and the thicknesses in the direction perpendicular to the cBN substrate surface were measured at any five points within the field of view. The average thickness was calculated from the average value of the measurements, and the average thickness of the hard coating layer and the thickness ratio tβ / tα of the lower layer α and the upper layer β were calculated based on this.
[0078] Furthermore, the distance between the maximum value Bmax and the minimum value Bmin of the B component concentration was measured at least five points from the position where the maximum value Bmax of the B component concentration in the upper layer β was detected and the adjacent position where the minimum value Bmin of the B component concentration was detected, and the measurement values were averaged to calculate the average distance between the maximum value and the minimum value of the B component concentration.
[0079] Moreover, for the above-prepared Examples 1 to 10 and Comparative Examples 1 to 6, the residual stress σ (GPa) of the entire hard coating layer was measured. The residual stress σ (GPa) was measured on the flank of the cemented carbide. The cutting edge of the cBN coated tool is brazed to the brazing part (corner part) of the WC-based cemented carbide insert body, so the residual stress of the coating on the cutting edge used for cutting is equivalent to the residual stress measured in this specification.
[0080] That is, the residual stress σ (GPa) of the entire hard coating layer is a residual stress value calculated by evaluating the overlapping XRD peaks of the lower layer α and the upper layer β as one peak as shown in FIG. 3, as described above.
[0081] In addition, a nanoindentation test was performed on the upper layer β of Examples 1 to 10 and Comparative Examples 1 to 6, and the plastic deformation work ratio and hardness were measured at at least five locations as described above, and the average of the measured values was taken as the nanoindentation hardness.
[0082] Tables 2 to 7 show the results of the measurements and calculations.
[0083] [Table 2]
[0084] [Table 3]
[0085] [Table 4]
[0086] [Table 5]
[0087] [Table 6]
[0088] [Table 7]
[0089] Next, for Examples 1 to 10 and Comparative Examples 1 to 6, the maximum cutting length was set to 1200 m under the following dry intermittent cutting conditions, and the occurrence of chipping, breakage, peeling, etc. of the cutting edge and the amount of flank wear were evaluated every 100 m of cutting length. Cutting conditions: Workpiece: Chromium steel (JIS SCr420) carburized and hardened (HRC60) round bar with four longitudinal grooves spaced equally along the length. Cutting speed: 120 m / min. Cutting depth: 0.2 mm Feed: 0.15 mm / rev
[0090] The occurrence of chipping, fracture, and peeling was evaluated by observing the cutting edge surface of the coated tool with a SEM. The results are shown in Table 8. The tool was judged to have reached the end of its service life when the flank wear reached 0.25 mm or more before reaching the maximum cutting length, or when the cutting edge experienced chipping, breakage, or peeling.
[0091] [Table 8]
[0092] In Table 8, "*" indicates that the tool reached the end of its service life before reaching the maximum cutting length, and indicates the time (seconds) until the tool reached its service life.
[0093] From the results shown in Table 8, it can be seen that in the examples, the average compositions of the lower layer α and the upper layer β on the cBN substrate surface are set within a predetermined range, a composition modulated structure of the B component is formed in the upper layer β, the layer thickness ratio of the lower layer α to the upper layer β is set within a predetermined range, and further, the residual stress σ (GPa) of the entire hard coating layer is controlled within a predetermined range. Therefore, even when used in intermittent cutting of high-hardness steel in which intermittent and impactful high loads act on the cutting edge, no chipping, fracture, or peeling occurs, and excellent wear resistance is exhibited over long periods of use.
[0094] In contrast, all of the comparative examples were prone to chipping, breakage, and peeling, and were poor in wear resistance, clearly reaching the end of their service life in a relatively short period of time.
[0095] The above-disclosed embodiments are merely illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not by the above-disclosed embodiments, and is intended to include the equivalent meanings of the claims and all modifications within the scope of the claims. [Explanation of symbols]
[0096] 1 Tool base (cBN base) 2 cBN particles 3 Bonded phase 4 Hard coating layer 5 Lower layer α 6 Upper layer β 7 Indenter 8 Load 9 Displacement 11. Heater 12 Rotating table 13 Al-Ti alloy target (evaporation source) for forming upper layer β 14 Ai-Ti-B alloy target (evaporation source) 15 Ai-Ti alloy target for forming lower layer α (evaporation source) 16 Anode electrode 17 Tool base (cBN base) 18 Reaction gas inlet 19 Exhaust gas outlet 20 Arc Power Supply 21 Bias power supply
Claims
1. A surface-coated cutting tool having a tool base made of a cubic boron nitride sintered body and a hard coating layer on at least a cutting edge surface of the tool base, (a) the hard coating layer has a lower layer α immediately on the tool substrate and an upper layer β on the lower layer α, (b) the lower layer α has an average composition Composition formula: (Al 1-x Ti x )N (wherein x is an atomic ratio of 0.40≦x≦0.60); (c) the upper layer β has an average composition Composition formula: (Al 1-y-z Ti y B z )N (where y and z are atomic ratios, and 0.40≦y≦0.60, 0.01≦z≦0.10 are satisfied); (d) the upper layer β has a compositionally modulated structure in which the concentration of the B component changes repeatedly along the layer thickness direction, (e) the repeated change in the concentration of the B component in the composition modulation structure is repeated with an average interval between adjacent maximum and minimum values of the concentration of the B component of 1 to 100 nm; (f) When the average of the maximum values of the concentration of the B component is Bmaxav, z<Bmaxav≦2.0×z; On the other hand, when the average of the minimum values of the concentration of the B component is Bminav, 0≦Bminav<z, (g) the average thickness of the hard coating layer is 1.0 to 4.0 μm, and when the average thickness of the lower layer α is tα and the average thickness of the upper layer β is tβ, the relationship 2.0≦tβ / tα≦6.0 is satisfied; (h) the residual stress σ of the entire hard coating layer satisfies −2.0 GPa≦σ≦−0.5 GPa; A surface-coated cutting tool comprising:
2. The plastic deformation work ratio W obtained by performing a nanoindentation test on the upper layer β at a depth of 1 / 10 or less of the average layer thickness plast / (W plast +W elast 2. The surface-coated cutting tool according to claim 1, wherein the value of (a) is 0.42 to 0.47, and the nanoindentation hardness is 26 GPa to 30 GPa.
3. 3. The surface-coated cutting tool according to claim 1, further comprising a TiN layer as an upper layer on the hard coating layer.
Citation Information
Patent Citations
Cubic boron nitride sintered material and cutting tool using the same
CN101031525A
Wear resistant coating film
JP1992026756A
Composite high hardness material for tool
JP1996104583A
Surface coated cutting tool
JP2006082209A
Surface coated cermet cutting tool whose hard coating layer exhibits excellent wear resistance in high-speed cutting of heat resistant alloy
JP2006334739A