Laser chip and its manufacturing method

The laser chip manufacturing method addresses the complexity and cost of improving optical mirror damage threshold by using zinc diffusion through controlled window regions, enhancing the local bandgap and reducing light absorption, thus improving the chip's reliability and lifespan.

JP7564563B2Active Publication Date: 2024-10-09SHENZHEN RUBEUST TECHNOLOGY LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022521056
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-12
Filing Date
2021-02-26
Publication Date
2024-10-09
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

The process of improving the catastrophic damage threshold of optical mirrors in semiconductor lasers is complex and costly, and epitaxial regrowth methods can lead to connectivity issues.

Method used

A method for manufacturing a laser chip involving a series of mask layer openings and zinc diffusion through specific window regions to enhance the local bandgap width and reduce light absorption, using heat treatment to diffuse zinc into the active and covering layers.

Benefits of technology

Improves the catastrophic damage threshold of optical mirrors by reducing light absorption, enhances the service life and quality of the laser chip, and simplifies the manufacturing process while avoiding adverse effects on other layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564563000001
    Figure 0007564563000001
  • Figure 0007564563000002
    Figure 0007564563000002
  • Figure 0007564563000003
    Figure 0007564563000003
Patent Text Reader

Abstract

The present invention provides a laser chip and a method for manufacturing the same. The method includes the steps of: providing a laser epitaxial structure including an active layer, a cladding layer, and a contact layer stacked in sequence on the active layer; covering the contact layer with a first mask layer and opening a window in the first mask layer to form a first window region; primarily etching the contact layer through the first window region to form a second window region corresponding to the first window region and exposing the cladding layer; performing zinc diffusion into the cladding layer and the active layer through the first and second window regions; removing the first mask layer; covering the contact layer with a second mask layer and opening a window in the second mask layer to form a third window region; and secondary etching the contact layer through the third window region to expand the second window region to correspond to the third window region, the projection of the third window region on the contact layer being located around the second window region. This configuration can effectively improve the threshold for catastrophic optical mirror damage.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of lasers, and in particular to laser chips and methods for manufacturing same. [Background technology]

[0002] Increasing the optical output power and improving the reliability and service life have always been the research focus in the field of semiconductor lasers. Catastrophic optical mirror damage is a significant factor that cannot be ignored that affects the maximum output power and reliability of semiconductor lasers. Catastrophic optical mirror damage refers to the catastrophic destruction of the laser cavity facet, which occurs when the region of the laser cavity facet absorbs the high optical radiation inside the resonator cavity, causing the temperature of the region to exceed its melting point, resulting in the melting of the cavity facet. Summary of the Invention [Problem to be solved by the invention]

[0003] The method for improving the damage threshold of the catastrophic optical mirror is generally to reduce the light absorption of the cavity surface, and in the prior art, the epitaxial regrowth method is generally adopted to epitaxially grow wide band gap material on the additional region of the cavity surface, and then form a related transparent window for light output, thereby reducing the light absorption of the cavity surface. However, the epitaxial regrowth process is complicated and expensive, and may cause epitaxial region connection problems, which may affect the device performance. [Means for solving the problem]

[0004] The present invention provides a laser chip and its manufacturing method to solve the problem in the prior art that the process of improving the catastrophic optical mirror damage threshold is complicated.

[0005] In order to solve the above technical problems, the solution adopted by the present invention provides a method for manufacturing a laser chip, the method including the steps of: providing a laser epitaxial structure including an active layer, a covering layer and a contact layer sequentially stacked on the active layer; covering the contact layer with a first mask layer and opening a window in the first mask layer to form a first window region; primarily etching the contact layer through the first window region to form a second window region corresponding to the first window region and exposing the covering layer; performing zinc diffusion on the covering layer and the active layer through the first window region and the second window region; removing the first mask layer; covering the contact layer with a second mask layer and opening a window in the second mask layer to form a third window region; secondary etching the contact layer through the third window region to expand the second window region to correspond to the third window region, and the projection of the third window region on the contact layer is located around the second window region.

[0006] According to one embodiment of the present invention, the step of diffusing zinc into the coating layer and the active layer through the first window region and the second window region includes covering the first mask layer and the coating layer exposed through the first window region and the second window region with a zinc diffusion layer, and diffusing zinc in the zinc diffusion layer into the coating layer and the active layer by a heat treatment method.

[0007] According to one embodiment of the present invention, the method further includes covering the zinc diffusion layer with a silicon oxide layer before diffusing zinc in the zinc diffusion layer into the coating layer and the active layer by a heat treatment method.

[0008] According to one embodiment of the present invention, the method further includes the steps of sequentially removing the silicon oxide layer and the zinc diffusion layer after diffusing zinc in the zinc diffusion layer into the coating layer and the active layer by a heat treatment method.

[0009] According to one embodiment of the present invention, the heat treatment method has a treatment temperature of 600° C. or higher.

[0010] According to one embodiment of the present invention, the manufacturing method further includes a step of providing an insulating layer on the contact layer and a step of covering the insulating layer and the contact layer with a contact metal layer, and the second window region is filled with the insulating layer.

[0011] According to one embodiment of the invention, the primary etch is a solution wet etch or a mechanical dry etch.

[0012] According to one embodiment of the present invention, the first window region has a dimension of not less than 5 μm and not more than 15 μm.

[0013] In order to solve the above technical problems, the present invention adopts another solution: Manufactured by the manufacturing method of the laser chip, A laser chip is provided. According to one embodiment of the present invention, The laser chip includes a laser epitaxial structure, which includes an active layer, a coating layer and a contact layer stacked in order on the active layer, a window region exposing the coating layer is formed in the contact layer, zinc diffusion regions are formed in the active layer and the coating layer, and a projection of the window region in the coating layer is located around the zinc diffusion region and is spaced a certain distance from the zinc diffusion region.

[0014] According to one embodiment of the present invention, the laser chip further includes an insulating layer and a contact metal layer sequentially stacked on the contact layer, and the window region is filled with the insulating layer. Effect of the Invention

[0015] The beneficial effects of the present invention are as follows: Different from the prior art, the present application first covers the contact layer with a first mask layer, opens a window in the first mask layer to form a first window region, and then etch the contact layer based on the first window region to form a second window region, thereby exposing the covering layer, and then covers the zinc diffusion layer, realizes zinc diffusion by heat treatment, and further forms zinc diffusion regions in the covering layer and the active layer, which can effectively make the atoms of the quantum well components in the local cavity surface diffuse into each other, further improve the band gap width in the local cavity surface, further reduce the absorption of light in the local cavity surface, improve the damage threshold of the catastrophic optical mirror, and further improve the service life and quality of the entire laser chip. Meanwhile, compared with directly diffusing the laser epitaxial structure, the present application can make the zinc diffusion layer closer to the quantum well by opening a window, thereby improving the diffusion efficiency and preventing the problem of doping in other layers of the laser chip caused by too long heat treatment time, so as not to adversely affect other layers of the laser chip. Meanwhile, instead of first opening a window in the contact layer and then covering the first mask layer, the first mask layer is first covered on the contact layer, so that the first mask layer can be prevented from being broken due to thermal stress in a heat treatment environment due to its high and low levels (part of it is located within the window region of the contact layer and part of it is located partially on the contact layer), and further the problem of the first mask layer becoming useless due to breaking of the first mask layer is solved. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic flowchart of a first embodiment of a method for manufacturing a laser chip according to the present application. [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of one embodiment of the laser epitaxial structure in FIG. [Diagram 3] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 4] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Diagram 5] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 6] 2 is a schematic flowchart of sub-steps of step S14 in FIG. 1. [Figure 7] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 8] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 9] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 10] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 11] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 12] 5 is a schematic flowchart of a second embodiment of the method for manufacturing a laser chip according to the present application. [Figure 13] 2 is a schematic diagram showing another embodiment of the laser epitaxial structure in FIG. 1. [Figure 14] 1 is a schematic diagram illustrating a configuration of an embodiment of a laser chip according to the present application. [Figure 15] 1 is a schematic diagram illustrating a configuration of another embodiment of a laser chip according to the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The solutions in the embodiments of the present invention will be described below clearly and completely with reference to the drawings in the embodiments of the present invention, and obviously, the described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, any other embodiments that a person skilled in the art can obtain without any creative efforts will fall within the scope of protection of the present invention.

[0018] In addition, if there are descriptions of "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are used for explanatory purposes only and cannot be understood as indicating or implying the relative importance or the quantity of the indicated technical features. Thus, the features defined by "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions in each embodiment may be combined with each other, but this must be based on what a person skilled in the art can realize. If the combination of technical solutions is contradictory to each other or cannot be realized, such combination of technical solutions does not exist and is not within the scope of protection sought by the present invention.

[0019] As shown in FIG. 1, FIG. 1 is a schematic flow chart of a first embodiment of a method for manufacturing a laser chip according to the present application, which specifically includes the following steps: In S11, a laser epitaxial structure is provided, the laser epitaxial structure including an active layer, and a cladding layer and a contact layer stacked in sequence on the active layer.

[0020] 2, a laser epitaxial structure 10 is provided, which includes an active layer 100, a covering layer 200, and a contact layer 300. Here, the covering layer 200 and the contact layer 300 are stacked on the active layer 100 in order.

[0021] In S12, a first mask layer is applied to cover the contact layer, and a window is opened in the first mask layer to form a first window region.

[0022] As shown in Figures 3 and 4, a first mask layer 310 is covered on the contact layer 300, and a window is opened in the first mask layer 310 to form a first window region 311 in the first mask layer 310, and the contact layer 300 can be exposed through the first window region 311.

[0023] Optionally, the first mask layer 310 may specifically be a SiNx layer.

[0024] Optionally, the size of the first window region 311 can be preset based on the size of the specifically required resonant cavity, and may be 5 μm to 15 μm, for example, 5 μm, 10 μm, or 15 μm.

[0025] In S13, the contact layer is primarily etched through the first window region to form a second window region that corresponds to the first window region and exposes the coating layer.

[0026] As shown in FIG. 5 , a second window region 320 can be formed in the contact layer 300 by first etching the contact layer 300 through the first window region 311, and the covering layer 200 can be exposed through the second window region 320.

[0027] Here, the second window area 320 corresponds to the first window area 311 and has a size equal to that of the first window area 311 , that is, the projections of the first window area 311 and the second window area 320 on the covering layer 200 overlap.

[0028] Optionally, the primary etching may be specifically solution wet etching or mechanical dry etching. Since the contact layer 300 has different components from the covering layer 200, the contact layer 300 may be etched using a solution with a preset ratio without affecting the covering layer 200, or mechanical dry etching may be performed on the contact layer 300 using an etching knife according to the thickness of the contact layer 300.

[0029] In S14, zinc is diffused into the coating layer and the active layer through the first and second window regions.

[0030] Zinc diffusion is performed into the coating layer 200 and the active layer 100 through the first window region 311 and the second window region 320 .

[0031] Referring to FIG. 6, FIG. 6 shows sub-steps of step S14 shown in FIG. 1, specifically including the following steps:

[0032] In S141, the first mask layer and the coating layer exposed through the first window region and the second window region are covered with a zinc diffusion layer.

[0033] As shown in FIG. 7, the first mask layer 310 and the covering layer 200 exposed through the first window region 311 and the second window region 320 are covered with a zinc diffusion layer 330 .

[0034] Optionally, the zinc diffusion layer 330 is specifically ZnO:SiO 2 Specifically, the zinc diffusion layer 330 may be formed on the first mask layer 310 and the exposed coating layer 200 by using a sputtering method.

[0035] In S142, the zinc diffusion layer is covered with a silicon oxide layer.

[0036] In an optional embodiment, the zinc diffusion layer 330 may be further covered with a silicon oxide layer 340. By further covering with the silicon oxide layer 340, the zinc diffusion layer 330 and the coating layer 200 can have a better adhesion effect, and the zinc diffusion effect can be further enhanced.

[0037] In S143, the zinc in the zinc diffusion layer is diffused into the coating layer and the active layer by a heat treatment method.

[0038] Through the heat treatment, the zinc in the zinc diffusion layer 330 can diffuse into the coating layer 200 and the active layer 100 .

[0039] As shown in Figures 7 and 8, in the heat treatment environment, the zinc in the zinc diffusion layer 330 begins to diffuse toward the coating layer 200 and further into the active layer 100, thereby realizing atomic diffusion of the coating layer 200 and the active layer 100, and forming a zinc diffusion region 110 in the coating layer 200 and the active layer 100.

[0040] Optionally, because each layer of the laser epitaxial structure 10 is a metastable interface and zinc atoms have strong diffusivity, zinc diffusion into the covering layer 200 and the active layer 100 can cause atoms of the quantum well components of the local cavity surface of the laser epitaxial structure 10 to diffuse into each other, thereby improving the local band gap width of the cavity surface, reducing the local light absorption of the cavity surface, improving the catastrophic optical mirror damage threshold, and improving the service life and quality of the entire laser chip.

[0041] Optionally, the processing temperature of the heat treatment method may specifically be 600° C. or higher.

[0042] In step S141 of the above embodiment, the zinc diffusion layer 330 is not only covered on the coating layer 200 exposed to the first window region 311 and the second window region 320, but also covered on the first mask layer 310. Therefore, in the subsequent zinc diffusion process, the zinc diffusion layer 330 located on the first mask layer 310 can constantly provide zinc atoms to the second mask layer 330 located on the first window region 311 and the second window region 320, so that the zinc atom concentration in the coating layer 200 can be maintained at a high level, and the overall effect of zinc diffusion can be further improved.

[0043] In S144, the silicon oxide layer and the zinc diffusion layer are removed in that order.

[0044] After the zinc diffusion is completed, the silicon oxide layer 340 and the zinc diffusion layer 330 may be removed in sequence.

[0045] In the above embodiment, the contact layer 300 is first covered with the first mask layer 310, a window is opened in the first mask layer 310 to form the first window region 311, the contact layer 300 is then etched based on the first window region 311 to form the second window region 320, so as to expose the coating layer 200, and then the zinc diffusion layer 330 is covered and zinc diffusion is realized by a heat treatment method, and the zinc diffusion region 110 is formed in the coating layer 200 and the active layer 100, so that the atoms of the quantum well components in the local area of ​​the cavity surface can effectively diffuse into each other, and the band gap width in the local area of ​​the cavity surface can be improved, and the local light absorption in the cavity surface can be reduced, and the catastrophic damage threshold of the optical mirror can be improved, so as to improve the service life and quality of the entire laser chip. Meanwhile, compared with directly diffusing the laser epitaxial structure 10, the present invention can make the zinc diffusion layer 330 closer to the quantum well by opening a window, thereby improving the diffusion efficiency and preventing the problem of doping in other layers of the laser chip due to too long heat treatment time, so that other layers of the laser chip are not adversely affected. Meanwhile, instead of opening a window in the contact layer 300 and then covering the first mask layer 310, the first mask layer 310 is first covered on the contact layer 300, thereby preventing the first mask layer 310 from being broken by thermal stress in the heat treatment environment due to its high and low levels (a part of it is located in the window region of the contact layer 300 and a part of it is partially located on the contact layer 300), and further solving the problem of the first mask layer 310 being broken and becoming useless.

[0046] In S15, the first mask layer is removed.

[0047] After the zinc diffusion is completed, the first mask layer 310 may be removed.

[0048] In S16, a second mask layer is applied to the contact layer, and a window is opened in the second mask layer to form a third window region, the projection of the third window region on the contact layer being located at the periphery of the second window region.

[0049] 9 , after removing the first mask layer 310, the contact layer 300 may be further covered with a second mask layer 370. Alternatively, a window may be opened in the second mask layer 370 to form a third window region 371 in the second mask layer 370, and the projection of the third window region 371 on the contact layer 300 is located around the second window region 320. That is, the projection of the second window region 320 on the contact layer 300 is located in the inner peripheral region of the projection of the third window region 371 on the contact layer 300.

[0050] Optionally, the second mask layer 370 may specifically be a photolithography mask.

[0051] In S17, the contact layer is secondarily etched through the third window region to expand the second window region to correspond to the third window region.

[0052] 10 and 11, the contact layer 300 is secondarily etched through the third window region 371 to expand the second window region 320 to correspond to the third window region 371. Optionally, the contact layer 300 may be wet-etched using solutions with other preset ratios.

[0053] After the etch is completed, the second mask layer 370 may be removed.

[0054] In the above embodiment, the contact layer 300 is covered with the second mask layer 370, and in addition to the second window region 320, a window is opened in the second mask layer 370, and the contact layer 300 is etched to expand the second window region 320, so that the zinc diffusion region can be directly positioned. Compared with the conventional method of achieving zinc diffusion by some ion injection or other methods, there is no need to reposition the zinc diffusion region, and the zinc diffusion region can be directly used as the laser resonant cavity region, which can effectively simplify the process and reduce the manufacturing cost.

[0055] As described above, the present application first covers the contact layer 300 with the first mask layer 310, opens a window in the first mask layer 310 to form a first window region 311, and then etches the contact layer 300 based on the first window region 311 to form a second window region 320, thereby exposing the coating layer 200, and then covers the zinc diffusion layer 330, and realizes zinc diffusion by heat treatment, and further forms a zinc diffusion region 110 in the coating layer 200 and the active layer 100, which can effectively make the atoms of the quantum well components in the local cavity surface diffuse into each other, and further improve the local band gap width of the cavity surface, and further reduce the local light absorption of the cavity surface, improve the catastrophic damage threshold of the optical mirror, and improve the service life and quality of the entire laser chip. Furthermore, by covering the contact layer 300 with the second mask layer 370, and opening a window in the second mask layer 370 in addition to the second window region 320, and etching the contact layer 300 to enlarge the second window region 320, the zinc diffusion region can be directly positioned. Compared with the conventional methods of achieving zinc diffusion by ion injection or the like, there is no need to position the zinc diffusion region again, and the zinc diffusion region can be directly made into the laser resonant cavity region, which can effectively simplify the process and reduce the manufacturing cost.

[0056] As shown in FIG. 12, FIG. 12 is a schematic flow chart of a second embodiment of the method for manufacturing a laser chip according to the present application, which specifically includes the following steps:

[0057] In S21, an insulating layer is provided on the contact layer.

[0058] 13 , the contact layer 300 is further provided with an insulating layer 400. And the second window region 320 is filled with the insulating layer 400. Optionally, the projection of the insulating layer 400 on the contact layer 300 is located around the second window region 320.

[0059] As shown in FIG. 13, the insulating layer 400 is provided mainly to surround the second window region 320 and does not completely cover the entire contact layer 300.

[0060] In S22, a contact metal layer is deposited on the insulating layer and the contact layer.

[0061] Thereafter, the insulating layer 400 and the contact layer 300 are further covered with a contact metal layer 500 .

[0062] In the above embodiment, the contact layer 300 is further provided with an insulating layer 400, and the insulating layer 400 and the contact layer 300 are covered with a contact metal layer 500 to complete the fabrication of the laser chip.

[0063] As shown in FIG. 14, the present application further provides a laser chip 1, which includes a substrate 20 and a laser epitaxial structure 10 provided on the substrate 20, and the laser epitaxial structure 10 includes an active layer 100, a coating layer 200 and a contact layer 300 sequentially stacked on the active layer 100, a window region 350 exposing the coating layer 200 is formed in the contact layer 300, and a zinc diffusion region 110 is formed in the active layer 100 and the coating layer 200, and the projection of the window region 350 on the coating layer 200 is located around the zinc diffusion region 110 and is spaced a certain distance from the zinc diffusion region 110.

[0064] As shown in FIG. 15, the laser chip 1 further includes an insulating layer 400 and a contact metal layer 500 which are stacked in this order on the contact layer 300, and the window region 350 is filled with the insulating layer 400.

[0065] The above are merely examples of the present invention, and are not intended to limit the scope of the patent of the present invention. Any equivalent result or equivalent flow transformation made by utilizing the contents of the specification and drawings of the present invention, or any direct or indirect application in other related technical fields, are also within the scope of patent protection of the present invention.

Claims

1. A method for manufacturing a laser chip, comprising the steps of: providing a laser epitaxial structure including an active layer and a cladding layer and a contact layer stacked in sequence on the active layer; covering the contact layer with a first mask layer and opening a window in the first mask layer to form a first window region; forming a second window region corresponding to the first window region and exposing the covering layer by primarily etching the contact layer through the first window region; performing zinc diffusion into the coating layer and the active layer through the first window region and the second window region; removing the first mask layer; covering the contact layer with a second mask layer and opening a window in the second mask layer to form a third window region; and performing a second etching of the contact layer through the third window region to expand the second window region to correspond to the third window region.

4. A method for manufacturing a laser chip, comprising: a projection of the third window region on the contact layer located at a periphery of the second window region.

2. The step of diffusing zinc into the coating layer and the active layer through the first window region and the second window region includes: covering the first mask layer and the coating layer exposed through the first window region and the second window region with a zinc diffusion layer; 2. The method according to claim 1, further comprising diffusing zinc in the zinc diffusion layer into the coating layer and the active layer by a heat treatment method.

3. Before diffusing zinc in the zinc diffusion layer into the coating layer and the active layer by a heat treatment method, The method of claim 2 further comprising the step of covering the zinc diffusion layer with a silicon oxide layer.

4. After diffusing zinc in the zinc diffusion layer into the coating layer and the active layer by a heat treatment method, The method of claim 3 further comprising the steps of sequentially removing the silicon oxide layer and the zinc diffusion layer.

5. 3. The method according to claim 2, wherein the heat treatment is performed at a temperature of 600° C. or higher.

6. The manufacturing method includes: providing an insulating layer on the contact layer; and covering the insulating layer and the contact layer with a contact metal layer; The method of claim 1 , wherein the second window area is filled with the insulating layer.

7. The method of claim 1 , wherein the primary etch is a solution wet etch or a mechanical dry etch.

8. The method according to claim 1 , wherein the first window region has a dimension of 5 μm or more and 15 μm or less.

9. A laser chip, characterized by being manufactured by the laser chip manufacturing method described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Edge-emitting semiconductor laser having a phase structure

    CN102113187A

  • High-power semiconductor laser with non-absorbing windows

    CN102891435A

  • Method of fabricating vertical cavity surface emitting laser, and vertical cavity surface emitting laser

    CN108736316A

  • Avalanche photodiode and manufacturing method thereof

    CN110323284A

  • Manufacture of photoelectron semiconductor device

    JP1993102611A