- Publication Date
- 2024-10-09
- Estimated Expiration
- 2039-12-27
AI Technical Summary
Conventional methods for sealing dentinal tubules to prevent hypersensitivity have issues with adhesion and sustainability of effect.
Hydroxyapatite fine particles with a specific X-ray diffraction peak intensity ratio and aggregate structure, produced by mixing an aqueous alkali phosphate salt solution with calcium hydroxide slurry under controlled conditions, providing excellent adhesion within dentinal tubules.
The hydroxyapatite fine particles effectively seal and adhere within dentinal tubules, offering improved durability and adhesion properties for hypersensitivity relief.
Smart Images

Figure 0007564577000001 
Figure 0007564577000002 
Figure 0007564577000003
Abstract
Description
[Technical field]
[0001] The present invention relates to hydroxyapatite microparticles and the like. [Background technology]
[0002] Hypersensitivity develops when dentin becomes exposed due to physical abrasion such as brushing, chemical abrasion by acid, etc. When dentin is exposed, external stimuli stimulate the nerves in the dentinal tubules in the dentin, making it more likely to cause pain.
[0003] For hypersensitivity, for example, the dentinal tubules are blocked with particles of fluoride, aluminum salts (see Patent Document 1 for an example), etc., to prevent external stimuli from reaching the nerves. However, most of the conventional methods have insufficient adhesion after blocking, and there is a problem with the durability of the effect. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-222325 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide particles that have the ability to seal dentinal tubules and have excellent adhesion within the dentinal tubules. [Means for solving the problem]
[0006] In view of the above problems, the present inventors have conducted intensive research and found that the above problems can be solved by using hydroxyapatite microparticles that are particle aggregates and have a ratio of the diffraction peak intensity around 2θ=32° to the diffraction peak intensity around 2θ=26° in an X-ray diffraction pattern measured using CuKα radiation of 0.8 to 1.6. Further research was conducted based on this finding, and as a result, the present invention was completed.
[0007] That is, the present invention includes the following aspects.
[0008] Item 1. Hydroxyapatite microparticles which are particle aggregates and in which the ratio of the diffraction peak intensity at about 2θ=32° to the diffraction peak intensity at about 2θ=26° in an X-ray diffraction pattern measured using CuKα radiation is 0.8 to 1.6.
[0009] Item 2. The hydroxyapatite microparticles according to Item 1, having a Ca / P molar ratio of less than 1.67.
[0010] Item 3. Hydroxyapatite microparticles according to Item 1 or 2, having a Ca / P molar ratio of 1.60 or less.
[0011] Item 4. Hydroxyapatite microparticles according to any one of Items 1 to 3, having a median diameter of 5 μm or less.
[0012] Item 5. Specific surface area is 30 to 200 m 2 Item 5. The hydroxyapatite microparticles according to any one of Items 1 to 4, wherein the average particle size is 1 / g.
[0013] Item 6. Hydroxyapatite microparticles according to any one of Items 1 to 5, in which the ratio of the diffraction peak intensity at about 2θ=34° to the diffraction peak intensity at about 2θ=32° in an X-ray diffraction pattern measured using CuKα radiation is 1 or less.
[0014] Item 7. An additive for an oral composition, comprising the hydroxyapatite fine particles according to any one of Items 1 to 6.
[0015] Item 8. A dentinal tubule sealant comprising the hydroxyapatite microparticles according to any one of Items 1 to 6.
[0016] Item 9. A method for producing hydroxyapatite microparticles, comprising a step of mixing an aqueous solution of an alkali phosphate having a pH of 4 or more and less than 7 with a calcium hydroxide slurry and reacting the mixture at 35 to 85°C.
[0017] Item 10. The method according to Item 9, wherein the calcium hydroxide slurry is a milled calcium hydroxide slurry.
[0018] Item 11. The method according to item 9 or 10, wherein the oxalic acid reactivity of the calcium hydroxide slurry is 40 minutes or less (the time (minutes) required for the pH to reach 7.0 after the addition of 40 g of an aqueous oxalic acid solution having a concentration of 0.5 mol / L and kept at 25±1° C. to 50 g of calcium hydroxide slurry prepared to a concentration of 5% by mass and kept at 25±1° C.).
[0019] Item 12. The BET specific surface area of the calcium hydroxide slurry is 5 m 2 / g or more. Effect of the Invention
[0020] According to the present invention, it is possible to provide hydroxyapatite microparticles that have a dentinal tubule sealing property and excellent adhesion to the dentinal tubules. In addition, it is also possible to provide an additive for an oral composition, a dentinal tubule sealant, etc., by using the microparticles. [Brief description of the drawings]
[0021] [Figure 1] 1 shows X-ray diffraction peaks of the hydroxyapatite microparticles of Example 1. [Diagram 2] The X-ray diffraction peaks of commercially available reagent hydroxyapatite microparticles are shown. [Diagram 3] 1 shows an SEM photograph of the hydroxyapatite microparticles of Example 1. [Figure 4] 3 shows the X-ray diffraction peaks of the hydroxyapatite microparticles of Example 2. [Diagram 5] 3 shows an SEM photograph of the hydroxyapatite microparticles of Example 2. [Figure 6] 1 shows X-ray diffraction peaks of the hydroxyapatite microparticles of Example 3. [Figure 7] 1 shows an SEM photograph of the hydroxyapatite microparticles of Example 3. [Figure 8] 1 shows X-ray diffraction peaks of the hydroxyapatite microparticles of Example 4. [Figure 9] 1 shows an SEM photograph of the hydroxyapatite microparticles of Example 4. [Figure 10] 1 shows X-ray diffraction peaks of the hydroxyapatite microparticles of Example 5. [Figure 11] 1 shows an SEM photograph of the hydroxyapatite microparticles of Example 5. [Figure 12] 1 shows X-ray diffraction peaks of the hydroxyapatite microparticles of Example 6. [Figure 13] 1 shows an SEM photograph of the hydroxyapatite microparticles of Example 6. [Figure 14] 1 shows X-ray diffraction peaks of the hydroxyapatite microparticles of Example 7. [Figure 15] 1 shows the X-ray diffraction peaks of the hydroxyapatite microparticles of Example 8. [Figure 16] 1 shows an SEM photograph of the hydroxyapatite microparticles of Example 8. [Figure 17] 1 shows X-ray diffraction peaks of the hydroxyapatite fine particles of Comparative Example 1. [Figure 18] 1 shows an SEM photograph of the hydroxyapatite fine particles of Comparative Example 1. [Figure 19] This shows the X-ray diffraction peaks of the sample of Comparative Example 2. The peaks indicated by black circles are the diffraction peaks of monetite. [Figure 20] 3 shows an SEM photograph of the sample of Comparative Example 2. [Figure 21] 3 shows the X-ray diffraction peaks of the sample of Comparative Example 3. [Figure 22] 3 shows an SEM photograph of the sample of Comparative Example 3. [Figure 23] This shows the X-ray diffraction peaks of the sample of Comparative Example 4. The peaks indicated by black circles are the diffraction peaks of monetite. [Figure 24] 1 shows an SEM photograph of the sample of Comparative Example 4. [Diagram 25] 1 shows X-ray diffraction peaks (Test Example 1) of hydroxyapatite microparticles before and after immersion in artificial saliva. [Figure 26]4 shows SEM photographs of dentinal tubules before and after brushing (Test Example 2). [Figure 27] 4 shows SEM photographs of dentinal tubules before and after water pressure treatment (Test Example 3). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] In this specification, the expressions "contain" and "comprise" include the concepts of "contain", "include", "consist essentially of" and "consist only of".
[0023] 1. Hydroxyapatite microparticles In one aspect, the present invention relates to hydroxyapatite microparticles (also referred to as "microparticles of the present invention" in this specification) which are particle aggregates and have a ratio of a diffraction peak intensity around 2θ=32° to a diffraction peak intensity around 2θ=26° in an X-ray diffraction pattern measured using CuKα radiation of 0.8 to 1.6. This will be described below.
[0024] The diffraction peak near 2θ=26° is a peak of hydroxyapatite, specifically, a diffraction peak at 2θ=25.5 to 26.5°. When multiple diffraction peaks are present, the diffraction peak with the highest intensity is indicated.
[0025] The diffraction peak near 2θ=32° is a peak of hydroxyapatite, specifically, a diffraction peak at 2θ=31.5 to 32.5°. When multiple diffraction peaks are present, the diffraction peak with the highest intensity is the one with the highest intensity.
[0026] The method of acquiring the X-ray diffraction pattern is not particularly limited, and a method according to a known method can be adopted. As an example, it can be acquired under the following conditions: Apparatus: X-ray diffraction apparatus MultiFlex 2kW (manufactured by Rigaku Corporation), target: Cu, tube voltage: 40 kV, tube current: 30 mA, sampling width: 0.02°, scan speed: 2.00° / min, divergence slit: 1.0°, scattering slit: 1.0°, receiving slit: 0.3 mm. Alternatively, it can be acquired under the following conditions: Apparatus: X-ray diffraction apparatus Miniflex500 (manufactured by Rigaku Corporation), target: Cu, tube voltage: 40 kV, tube current: 15 mA, sampling width: 0.02°, scan speed: 2.00° / min, divergence slit: 1.25°, scattering slit: 1.25°, receiving slit: 0.3 mm.
[0027] The fine particles of the present invention have a ratio (32° / 26°) of the diffraction peak intensity at about 2θ=32° to the diffraction peak intensity at about 2θ=26° of 0.8 to 1.6. The peak intensity ratio is preferably 0.8 to 1.5, more preferably 0.9 to 1.3, even more preferably 1.0 to 1.25, still more preferably 1.05 to 1.2, and particularly preferably 1.05 to 1.15. The upper limit of the peak intensity ratio is preferably 1.60, 1.59, or 1.58.
[0028] Each of the microparticles of the present invention is an aggregate of particles. The particles constituting the microparticles of the present invention are particularly preferably plate-like particles. The shape of the plate-like particles constituting the microparticles of the present invention is not particularly limited, and may be a circular, polygonal, rod-like shape, or a combination of these shapes. In addition, the plate-like particles may be in either a state in which the surface is folded or a state in which the surface is not folded and the surface maintains a planar structure.
[0029] The microparticles of the present invention are particles containing hydroxyapatite as a main component. In the X-ray diffraction pattern of the microparticles of the present invention, the peaks of other substances (such as monetite) are not observed separately, or the peak intensities are relatively low. Therefore, the microparticles of the present invention are distinguished from microparticles in which the peak intensities of these peaks are high.
[0030] Although not wishing to be limited in any way, it is believed that the microparticles of the present invention exhibit excellent sealing properties for dentinal tubules and excellent adhesion within the dentinal tubules due in part to the fact that they have a shape and structure represented by a specific X-ray diffraction pattern and are composed of aggregated particles, which in combination with each other.
[0031] In a preferred embodiment of the fine particles of the present invention, the ratio (34° / 32°) of the diffraction peak intensity around 2θ=34° to the diffraction peak intensity around 2θ=32° in the X-ray diffraction pattern is 1 or less. Specifically, the diffraction peak around 2θ=34° is a diffraction peak at 2θ=33.5 to 34.5°. When there are multiple diffraction peaks, the peak intensity ratio refers to the diffraction peak with the highest intensity. The peak intensity ratio is preferably 0.1 to 1, more preferably 0.2 to 0.9, even more preferably 0.3 to 0.8, even more preferably 0.4 to 0.7, and particularly preferably 0.4 to 0.6.
[0032] In a preferred embodiment of the microparticles of the present invention, the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the area of all diffraction peaks in the range of 31.5°≦2θ≦32.5° is 30-45% relative to the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° being 100%. This value is preferably 33-42%, more preferably 35-40%. In addition, in a preferred embodiment of the microparticles of the present invention, the crystallite size calculated from the diffraction peak of the (130) plane near 2θ=40° is 12nm or less, preferably 10nm or less. Although not intended to be limited, it is believed that the crystal growth in the dentinal tubules is enhanced after sealing due to the relatively low crystallinity, which leads to improved fixation in the tubules. The lower limit of the crystallite size is not particularly limited, but is, for example, 1nm, 2nm, 3nm, 4nm, or 5nm.
[0033] The Ca / P molar ratio of the microparticles of the present invention is not particularly limited as long as it is a value that hydroxyapatite can take.In the microparticles of the present invention, it is considered that a part of calcium is replaced with other elements (sodium, etc.), and therefore the Ca / P molar ratio can be a relatively low value.From this viewpoint, the Ca / P molar ratio of the microparticles of the present invention is preferably less than 1.67, more preferably 1.60 or less, even more preferably 1.5 or less, and even more preferably 1.4 or less.The lower limit of the Ca / P molar ratio of the microparticles of the present invention is not particularly limited, and is, for example, 1.0, 1.1, or 1.2.
[0034] The median diameter (Dx(50)) of the microparticles of the present invention is not particularly limited, but is preferably 5 μm or less, more preferably 4.5 μm or less, from the viewpoint of dentinal tubule sealing property, adhesion, etc. The lower limit of the median diameter is not particularly limited, but is, for example, 1 μm, 2 μm, or 3 μm.
[0035] The specific surface area of the fine particles of the present invention is not particularly limited, but from the viewpoints of dentinal tubule sealing ability, adhesion ability, etc., it is preferably 30 m 2 / g or more, more preferably 40m 2 / g or more, more preferably 55m 2 / g or more, and even more preferably 55m 2 The upper limit of the specific surface area is not particularly limited, but is, for example, 200 m 2 / g, 150m 2 / g, 120m 2 / g, 100m 2 / g, 90m 2 / g.
[0036] 2. Manufacturing method One aspect of the present invention relates to a method for producing hydroxyapatite microparticles, which comprises a step of mixing an aqueous solution of an alkali phosphate having a pH of 4 or more and less than 7 with a calcium hydroxide slurry and reacting them at 35 to 85° C. The microparticles of the present invention can be produced, for example, by this method.
[0037] The alkali phosphate salt is not particularly limited and includes hydrates and anhydrides. Examples of the alkali phosphate salt include sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, tetrasodium pyrophosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, etc., preferably sodium phosphate salts such as sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, etc., more preferably sodium dihydrogen phosphate.
[0038] The concentration of the alkali phosphate in the aqueous alkali phosphate solution is not particularly limited and is, for example, 3 to 50% by mass, preferably 3 to 30% by mass, more preferably 5 to 20% by mass, and further preferably 7 to 15% by mass.
[0039] The pH of the aqueous solution of alkali phosphate is preferably 4 or more and less than 7. The pH is more preferably 5 to 6.5. As described later, when the pH of the aqueous solution of alkali phosphate is relatively low (for example, pH 4 or more and less than 5), it is desirable to use an anhydride as the alkali phosphate and set the reaction temperature to a relatively high temperature, for example, 65 to 85°C, preferably 70 to 85°C, more preferably 75 to 85°C.
[0040] The calcium hydroxide slurry is not particularly limited as long as it is a slurry of calcium hydroxide that is reactive with oxalic acid.
[0041] The reactivity towards oxalic acid can be expressed, for example, by the following definition: Oxalic acid reactivity: 40 g of 0.5 mol / L oxalic acid aqueous solution kept at 25±1°C is added all at once to 50 g of calcium hydroxide slurry prepared to a concentration of 5% by mass and kept at 25±1°C, and the time (minutes) until the pH reaches 7.0 after the addition.
[0042] The oxalic acid reactivity, as defined above, is preferably 40 minutes or less, more preferably 30 minutes or less, and even more preferably 20 minutes or less.
[0043] The BET specific surface area of the calcium hydroxide slurry is preferably 5 m 2 / g or more, more preferably 6m 2 The upper limit of the BET specific surface area is not particularly limited, but is, for example, 20 m 2 / g, 15m 2 / g, 10m 2 / g.
[0044] A calcium hydroxide slurry having high oxalic acid reactivity can typically be obtained by grinding a calcium hydroxide slurry. The grinding process can further increase the oxalic acid reactivity (shorten the time defined above). The grinding process is performed, for example, using a bead mill. The conditions for the grinding process are not particularly limited, and for example, the conditions according to the method described in JP 2017-036176 A can be adopted.
[0045] Calcium hydroxide slurry can be prepared, for example, by reacting water with quicklime (calcium oxide) obtained by calcining limestone. For example, limestone is calcined in a kiln at about 1000°C to generate quicklime, and about 10 times the amount of hot water is added to the quicklime and stirred for 30 minutes to prepare calcium hydroxide slurry.
[0046] The solid content concentration of the calcium hydroxide slurry is not particularly limited, but is, for example, 1 to 30 mass %, preferably 3 to 20 mass %, more preferably 5 to 15 mass %, and further preferably 6 to 12 mass %.
[0047] The ratio of the amount of the aqueous alkali phosphate solution to the amount of the calcium hydroxide slurry is not particularly limited as long as it is a ratio that allows the production of hydroxyapatite microparticles. It is desirable to adjust the ratio so that the Ca / P molar ratio is preferably 0.3 to 0.7, more preferably 0.4 to 0.6, and even more preferably 0.45 to 0.55.
[0048] The mode of mixing the aqueous alkali phosphate solution and the calcium hydroxide slurry is not particularly limited. For example, the mode of adding the calcium hydroxide slurry to a reaction vessel containing the aqueous alkali phosphate solution (mode 1), the mode of adding the aqueous alkali phosphate solution to a reaction vessel containing the calcium hydroxide slurry (mode 2), and the mode of adding the aqueous alkali phosphate solution and the calcium hydroxide slurry to the reaction vessel simultaneously (mode 3) can be mentioned. Among these, mode 1 is preferable. During the above-mentioned addition to the reaction vessel, the liquid in the reaction vessel is usually stirred.
[0049] The addition to the reaction vessel is desirably carried out over a certain period of time, for example, 10 to 90 minutes, preferably 20 to 60 minutes, and more preferably 20 to 40 minutes.
[0050] The reaction is usually carried out under stirring. The reaction temperature is 35 to 85°C. The reaction temperature is preferably 40 to 75°C, more preferably 45 to 70°C, even more preferably 50 to 70°C, and even more preferably 55 to 65°C. When the pH of the aqueous solution of alkali phosphate is relatively low (for example, when the pH is 4 or more and less than 5), it is desirable to use an anhydride as the alkali phosphate and set the reaction temperature to a relatively high temperature, for example, 65 to 85°C, preferably 70 to 85°C, and more preferably 75 to 85°C. The reaction time (the time starting from when the aqueous solution of alkali phosphate and the calcium hydroxide slurry are completely mixed, and in the above-mentioned aspects 1 to 3, the time starting from the time when the addition of the aqueous solution of alkali phosphate and the calcium hydroxide slurry is completed) is, for example, 10 to 180 minutes, preferably 20 to 120 minutes, more preferably 40 to 90 minutes, and even more preferably 50 to 70 minutes.
[0051] The microparticles of the present invention produced by the above steps may be subjected to a purification treatment, such as filtration or washing, if necessary. If necessary, the microparticles may be subjected to a drying treatment.
[0052] 3.Applications The microparticles of the present invention have a dentinal tubule sealing property and are excellent in adhesion within the dentinal tubules. Therefore, the microparticles of the present invention can be used as an additive for an oral composition, a dentinal tubule sealant, etc. From this viewpoint, one embodiment of the present invention relates to an additive for an oral composition containing the microparticles of the present invention, a dentinal tubule sealant comprising the microparticles of the present invention, etc. EXAMPLES
[0053] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0054] Example 1 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry (BET specific surface area: 6.7 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 15 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 60°C while stirring, and maintained at this temperature until the stirring was stopped. A 10% aqueous solution of NaOH was added to adjust the pH to 5.5. The calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed and the mixture was stirred for another hour, it was filtered, washed with water, and dried at 80°C to obtain hydroxyapatite fine particles (powder).
[0055] The obtained hydroxyapatite particles were subjected to X-ray crystal diffraction, specific surface area measurement, particle size distribution measurement, Ca / P molar ratio measurement, and morphology observation.
[0056] Measurements were performed in the range of 2θ=25-45° using an X-ray diffraction device MultiFlex 2kW (manufactured by Rigaku Corporation). The measurement conditions were as follows: target: Cu, tube voltage: 40 kV, tube current: 30 mA, sampling width: 0.02°, scan speed: 2.00° / min, divergence slit: 1.0°, scattering slit: 1.0°, receiving slit: 0.3 mm. The results are shown in FIG. 1. FIG. 2 shows the X-ray diffraction pattern of hydroxyapatite, a commercially available reagent product. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity ratio due to the (002) plane near 2θ=26° was 1.1, which was clearly lower than the peak intensity ratio of 2.7 for the reagent HAp. This revealed that the hydroxyapatite microparticles of Example 1 were plate-like microparticles with many exposed c-planes. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, while the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the range of 31.5°≦2θ≦32.5° was 37.2%. This is clearly lower than the 52.1% shown by the reagent HAp, and the X-ray diffraction pattern is relatively broad, which indicates low crystallinity. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 7 nm, which is clearly smaller than the 52 nm shown by the reagent HAp, and this also indicates low crystallinity.
[0057] The specific surface area was measured by nitrogen gas adsorption using a fully automatic specific surface area measuring device, Macsorb HM model-1208 (manufactured by Mountec Co., Ltd.). The specific surface area was 61.9 m 2 / g.
[0058] The particle size distribution was measured by dry particle size distribution measurement using a laser diffraction particle size distribution measuring device MASTER SIZER 3000. As a result, Dx(50) was 3.76 μm.
[0059] The Ca / P molar ratio was calculated from the measured values of Ca and P contents by inductively coupled plasma optical emission spectrometry using an iCAP 6000 ICP-OES (manufactured by ThermoFisher). As a result, the Ca / P molar ratio was 1.33.
[0060] The shape was observed using a scanning electron microscope (manufactured by JEOL Ltd.: hereinafter referred to as SEM). The results are shown in Figure 3. The results show that the hydroxyapatite obtained in the present invention forms aggregates of plate-like fine particles.
[0061] Example 2 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry (BET specific surface area: 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 60°C while stirring, and maintained at this temperature until the stirring was stopped. A 10% aqueous solution of NaOH was added to adjust the pH to 6.0. Calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed and the mixture was stirred for another hour, it was filtered, washed with water, and dried at 80°C to obtain hydroxyapatite fine particles (powder).
[0062] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0063] The results of X-ray crystal diffraction are shown in FIG. 4. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.1, which was the same value as in Example 1. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, and the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the sum of the areas of all diffraction peaks in the range of 31.5°≦2θ≦32.5° was 38.6%. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 7 nm.
[0064] The specific surface area is 75.4 m 2 / g.
[0065] The results of the shape observation are shown in Figure 5. As in Example 1, it was confirmed that the particles were aggregates of plate-like fine particles.
[0066] Example 3 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry (BET specific surface area 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 40°C while stirring, and maintained at this temperature until the stirring was stopped. A 10% aqueous solution of NaOH was added to adjust the pH to 5.5. The calcium hydroxide slurry was added thereto over a period of 50 minutes. After the addition was completed and the mixture was stirred for another hour, it was filtered, washed with water, and dried at 80°C to obtain hydroxyapatite fine particles (powder).
[0067] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0068] The results of X-ray crystal diffraction are shown in FIG. 6. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.2, which was the same value as in Example 1. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, and the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the sum of the areas of all diffraction peaks in the range of 31.5°≦2θ≦32.5° was 36.0%. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 6 nm.
[0069] The specific surface area is 81.5 m 2 / g.
[0070] The results of the shape observation are shown in Fig. 7. As in Example 1, it was confirmed that the particles were aggregates of plate-like fine particles.
[0071] Example 4 A 10.7% by mass anhydrous aqueous solution of sodium dihydrogen phosphate and a ground calcium hydroxide slurry (BET specific surface area 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate anhydride was placed in a stainless steel beaker and heated to 80°C while stirring. The pH was left at 4.2 without adjustment. The calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed, the mixture was stirred for another hour, filtered, washed with water, and dried at 80°C to obtain hydroxyapatite microparticles (powder).
[0072] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0073] The results of X-ray crystal diffraction are shown in FIG. 8. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.4, which was the same value as in Example 1. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, and the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the sum of the areas of all diffraction peaks in the range of 31.5°≦2θ≦32.5° was 37.8%. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 9 nm.
[0074] The specific surface area is 163.4 m 2 / g.
[0075] The results of the shape observation are shown in Fig. 9. As in Example 1, it was confirmed that the particles were aggregates of plate-like fine particles.
[0076] Example 5 A 10.7% by mass anhydrous aqueous solution of sodium dihydrogen phosphate and a ground calcium hydroxide slurry (BET specific surface area 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate anhydride was placed in a stainless steel beaker and heated to 60°C while stirring. The pH was left at 4.2 without adjustment. The calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed, the mixture was stirred for another hour, filtered, washed with water, and dried at 80°C to obtain hydroxyapatite microparticles (powder).
[0077] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0078] The results of X-ray crystal diffraction are shown in FIG. 10. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.1, which was the same value as in Example 1. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, and the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the sum of the areas of all diffraction peaks in the range of 31.5°≦2θ≦32.5° was 31.6%. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 7 nm.
[0079] The specific surface area is 94.7m 2 / g.
[0080] The results of the shape observation are shown in Figure 11. As in Example 1, it was confirmed that the particles were aggregates of plate-like fine particles.
[0081] Example 6 A 10.7% by mass anhydrous aqueous solution of sodium dihydrogen phosphate and a ground calcium hydroxide slurry (BET specific surface area 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate anhydride was placed in a stainless steel beaker and heated to 80°C while stirring. The pH was left at 4.2 without adjustment. The calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed, the mixture was stirred for another hour, filtered, washed with water, and dried at 80°C to obtain hydroxyapatite microparticles (powder).
[0082] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0083] The results of X-ray crystal diffraction are shown in FIG. 12. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.58. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, while the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the sum of the areas of all diffraction peaks in the range of 31.5°≦2θ≦32.5° was 40.9%. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 7 nm.
[0084] The specific surface area is 105.0 m 2 / g.
[0085] The results of the shape observation are shown in Fig. 13. As in Example 1, it was confirmed that the particles were aggregates of plate-like fine particles.
[0086] Example 7 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry (BET specific surface area: 6.7 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 15 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. An aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 60°C while stirring, and maintained at this temperature until the stirring was stopped. A 10% aqueous solution of NaOH was added to adjust the pH to 5.5. Calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed, the mixture was stirred for another hour, filtered, washed with water, and dried at 80°C, and then left to stand for 6 months at 40°C and 75% RH to obtain hydroxyapatite fine particles (powder).
[0087] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0088] The results of X-ray crystal diffraction are shown in FIG. 14. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.21. In addition, the sum of the areas of all diffraction peaks in the range of 25°≦2θ≦35° was 100%, while the sum of the areas of all diffraction peaks in the range of 25.5°≦2θ≦26.5° and the sum of the areas of all diffraction peaks in the range of 31.5°≦2θ≦32.5° was 39.4%. In addition, the crystallite size calculated from the diffraction peak due to the (130) plane near 2θ=40° was 8 nm.
[0089] The specific surface area is 34.8m 2 / g.
[0090] Example 8 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry (BET specific surface area 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. The sodium dihydrogen phosphate dihydrate aqueous solution was placed in a stainless steel beaker, and a 10% NaOH aqueous solution was added to adjust the pH to 5.5. The calcium hydroxide slurry was added thereto over 50 minutes. After the addition was completed, the mixture was stirred for another hour, then stopped and allowed to stand at room temperature for 9 days. It was then filtered, washed with water, and dried at 80°C to obtain hydroxyapatite fine particles (powder).
[0091] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction and shape observation in the same manner as in Example 1.
[0092] The results of X-ray crystal diffraction are shown in Figure 15. The ratio of the diffraction peak intensity due to the (211) plane near 2θ=32° to the diffraction peak intensity due to the (002) plane near 2θ=26° was 1.3.
[0093] The results of the shape observation are shown in Figure 16. It was confirmed that the particles were shaped like aggregates of minute spindle-shaped particles.
[0094] Comparative Example 1 A 10.7% by mass anhydrous aqueous solution of sodium dihydrogen phosphate and a ground calcium hydroxide slurry (BET specific surface area 7.9 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g Oxalic acid reactivity: 12 minutes 30 seconds (JP Patent Publication No. 2017-036176) was prepared. The calcium hydroxide slurry was placed in a stainless steel beaker and heated to 40°C while stirring. An aqueous solution of anhydrous sodium dihydrogen phosphate (pH: 4.2) was added thereto over 30 minutes. After the addition was completed, the mixture was stirred for another hour, filtered, washed with water, and dried at 80°C to obtain hydroxyapatite fine particles (powder).
[0095] The obtained hydroxyapatite microparticles were subjected to X-ray crystal diffraction, specific surface area measurement, and shape observation in the same manner as in Example 1.
[0096] The results of X-ray crystal diffraction are shown in Figure 17. The ratio of the diffraction peak intensity due to the (211) plane near 2θ = 32° to the diffraction peak intensity due to the (002) plane near 2θ = 26° was 1.7, which was clearly higher than that of Example 1. In addition, the diffraction peak due to the (300) plane near 2θ = 33° appeared separately.
[0097] The specific surface area is 50.9 m 2 / g.
[0098] The results of the shape observation are shown in Figure 18. The particle shape was shown to be an aggregation of spindle-shaped fine particles.
[0099] Comparative Example 2 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry with a solid content of 8.6% by mass (JP Patent Publication No. 2017-036176) were prepared so that the Ca / P molar ratio was 0.5. The aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 60°C while stirring, and maintained at this temperature until the stirring was stopped. The pH was left at 4.2 without adjustment. The calcium hydroxide slurry was added thereto over a period of 45 minutes. After the addition was completed, the mixture was stirred for another hour, then filtered, washed with water, and dried at 80°C to obtain a sample.
[0100] The obtained sample was subjected to X-ray crystal diffraction and shape observation in the same manner as in Example 1.
[0101] The results of X-ray crystal diffraction are shown in Figure 19. In addition to the diffraction peaks of hydroxyapatite, diffraction peaks of other substances were confirmed. The peaks indicated by black circles in the figure are the diffraction peaks of monetite, a calcium phosphate that is easily formed under acidic conditions.
[0102] The results of the morphology observation are shown in Figure 20. Large plate-like particles of monetite were confirmed.
[0103] Comparative Example 3 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a high-purity calcium hydroxide slurry (BET specific surface area: 2.4 m) with a solid content of 8.6% by mass were mixed so that the Ca / P molar ratio was 0.5. 2 / g, oxalic acid reactivity: 25 seconds (JP Patent Publication No. 2011-126772) was prepared. An aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 60°C with stirring, and maintained at this temperature until the stirring was stopped. A 10% aqueous solution of NaOH was added to adjust the pH to 5.5. The calcium hydroxide slurry was added thereto over 30 minutes. After the addition was completed and the mixture was stirred for another hour, it was filtered, washed with water, and dried at 80°C to obtain a sample.
[0104] The obtained sample was subjected to X-ray crystal diffraction in the same manner as in Example 1.
[0105] The results of X-ray crystal diffraction are shown in Figure 21. In addition to the diffraction peaks of hydroxyapatite, diffraction peaks of calcium hydroxide were confirmed near 2θ = 28° and 34°.
[0106] The results of the shape observation are shown in Figure 22. Large plate-like particles of calcium hydroxide were confirmed. The difference from Example 1 was thought to be due to the physical properties of the raw material calcium hydroxide.
[0107] Comparative Example 4 A 10.7% by mass aqueous solution of sodium dihydrogen phosphate dihydrate and a ground calcium hydroxide slurry with a solid content of 8.6% by mass (JP Patent Publication No. 2017-036176) were prepared so that the Ca / P molar ratio was 0.5. The aqueous solution of sodium dihydrogen phosphate dihydrate was placed in a stainless steel beaker and heated to 80°C while stirring, and maintained at this temperature until the stirring was stopped. The pH was left at 4.2 without adjustment. The calcium hydroxide slurry was added thereto over a period of 50 minutes. After the addition was completed, the mixture was stirred for another hour, then filtered, washed with water, and dried at 80°C to obtain a sample.
[0108] The obtained sample was subjected to X-ray crystal diffraction and shape observation in the same manner as in Example 1.
[0109] The results of X-ray crystal diffraction are shown in Figure 23. In addition to the diffraction peaks of hydroxyapatite, diffraction peaks of other substances were confirmed. The peaks indicated by black circles in the figure are the diffraction peaks of monetite, a calcium phosphate that is easily formed under acidic conditions.
[0110] The results of the morphology observation are shown in Figure 24. Large plate-like particles of monetite were confirmed.
[0111] Test Example 1. Crystallinity Change Confirmation Test [Test Purpose] To evaluate the reactivity of hydroxyapatite nanoparticles in the oral cavity, the change in crystallinity before and after immersion in artificial saliva was measured using a powder X-ray diffraction apparatus.
[0112] [Test Method] 0.5 g of hydroxyapatite microparticles obtained in the same manner as in Example 1 was immersed in 200 mL of artificial saliva (CaCl2: 1.5 mM, KH2PO4: 0.9 mM, KCl: 130 mM, HEPES: 20 mM, pH 7.0 (KOH)) for 7 days. The powder separated by suction filtration was measured using a powder X-ray diffractometer to observe the change in crystallinity before and after immersion in artificial saliva.
[0113] [Measurement conditions] -Model used: Miniflex II (Rigaku Corporation) ·Starting angle: 20° End angle: 40° Sampling width: 0.02° Scan speed: 4.0° / min Voltage: 30kV ·Current: 15mA Divergence slit: 1.25° Scattering slit: 8.0mm Receiving slit: 0.3mm.
[0114] The results are shown in Figure 25. It was confirmed that immersion in artificial saliva improved crystallinity (= increased sharpness of peaks, appearance of broad and hidden peaks). This confirmed that the hydroxyapatite microparticles of the present invention are particles that change (have reactivity) in the oral cavity.
[0115] Test Example 2. Dentinal tubule sealing test of hydroxyapatite microparticles [Test Purpose] To evaluate the ability of hydroxyapatite microparticles to seal dentinal tubules, bovine dentin surfaces were brushed with a solution of hydroxyapatite microparticles, and the degree of sealing of dentinal tubules was examined by scanning electron microscopy (SEM).
[0116] [Test Method] Preparation of dentin block (sample) 1. Dentin from the root surface of an extracted bovine tooth was cut into pieces measuring 5 x 5 mm. 2. The cut tooth pieces were embedded in resin (polymethyl methacrylate), blocks were created, and the blocks were polished with waterproof abrasive paper to bring out the surface. 3. The dentin block was immersed in a 5% w / w EDTA aqueous solution (pH 7.0) for 2 minutes. 4. Sonicate in distilled water for 5 minutes.
[0117] Preparation of hydroxyapatite microparticles 5. 0.3 g of the hydroxyapatite microparticles obtained in the same manner as in Example 1 was suspended in 39.7 g of the viscous diluent.
[0118] Brushing process 6. The dentin block was brushed with a toothbrush (GUM #211) in hydroxyapatite microparticle liquid (40 g) for 30 seconds (stroke: 150 rpm, load: 160 g). 7. The dentin block was rinsed with water and then immersed in artificial saliva (CaCl2: 1.5 mM, KH2PO4: 0.9 mM, KCl: 130 mM, HEPES: 20 mM, pH 7.0 (KOH)) for 5 minutes. 8. The above steps 1 and 2 were repeated six times.
[0119] SEM observation 9. After the surface was subjected to deposition treatment, it was observed under an electron microscope.
[0120] [Observation and measurement conditions] {Vapor deposition processing} -Model used: MCI1000 (Hitachi High-Technologies Corporation) ·Current: 20mA Processing time: 120 seconds {SEM observation} -Model used: S-3400N (Hitachi High-Technologies Corporation) Detector: SE (secondary electron image) Applied voltage: 5kV Probe current: 50mA ·Magnification: 25000x.
[0121] The results are shown in Figure 26. It was confirmed that the dentinal tubules were blocked by brushing in the hydroxyapatite microparticle liquid. This confirmed that the hydroxyapatite microparticles are particles that block the dentinal tubules present on the dentin surface.
[0122] Test Example 3: Adhesion test [Test Purpose] To evaluate the ability of hydroxyapatite microparticles to adhere within dentinal tubules, the surface of bovine dentin was brushed with a solution of hydroxyapatite microparticles, and then water pressure was applied from the back side of the dentin. The ability of the hydroxyapatite microparticles to withstand the water pressure was examined using a scanning electron microscope (SEM).
[0123] [Test Method] Preparation of dentin discs (samples) 1. Dentin from the root surface of an extracted bovine tooth was cut into pieces measuring 5 x 5 mm. 2. The cut tooth pieces were polished with waterproof abrasive paper. 3. The dentin disk was immersed in a 5% w / w aqueous solution of EDTA (pH 7.0) for 2 minutes. 4. Sonicate in distilled water for 5 minutes.
[0124] Preparation of hydroxyapatite microparticles 5. 1 g of the hydroxyapatite microparticles obtained in the same manner as in Example 1 was suspended in 39 g of the viscous diluent.
[0125] Brushing process 6. The dentin disk was brushed with a toothbrush (GUM #211) in hydroxyapatite microparticle liquid (40 g) for 30 seconds (stroke: 150 rpm, load: 160 g). 7. After rinsing the disk with water, it was immersed in artificial saliva (CaCl2: 1.5 mM, KH2PO4: 0.9 mM, KCl: 130 mM, HEPES: 20 mM, pH 7.0 (KOH)) for 5 minutes. 8. The above steps 1 and 2 were repeated six times. 9. Immersed in artificial saliva for 7 days.
[0126] Water Pressure Treatment 10. After brushing, the dentin disks were pressurized at 0.1 MPa for 30 minutes using an apparatus based on the report by Pashley et al. (Pashley DH, Galloway SE. The effects of oxalate treatment on the smear layer of ground surfaces of human dentin. Arch Oral Biol 1983; 30: 731-737.).
[0127] SEM observation 11. After the surface was subjected to deposition treatment, it was observed under an electron microscope.
[0128] [Observation and measurement conditions] {Vapor deposition processing} -Model used: MCI1000 (Hitachi High-Technologies Corporation) ·Current: 20mA Processing time: 120 seconds {SEM observation} -Model used: S-3400N (Hitachi High-Technologies Corporation) Detector: SE (secondary electron image) Applied voltage: 5kV Probe current: 50mA ·Magnification: 25000x.
[0129] The results are shown in Figure 27. It was confirmed that the dentinal tubules remained sealed even after the water pressure treatment. This confirmed that the hydroxyapatite microparticles were fixed inside the dentinal tubules and maintained a sealed state.
Claims
1. The method includes a step of mixing an aqueous solution of an alkali phosphate salt having a pH of 4 or more and less than 7 with a calcium hydroxide slurry having a BET specific surface area of 5 m 2 / g or more, and reacting the mixture at 35 to 85° C., When the alkali phosphate is a hydrate, the pH is 5 or more and less than 7; When the alkali phosphate is an anhydride, the pH is 4 or more and less than 5, and the reaction temperature is 60 to 85° C.; A method for producing hydroxyapatite microparticles.
2. 2. The method of claim 1, wherein the calcium hydroxide slurry is a ground calcium hydroxide slurry.
3. 3. The method according to claim 1, wherein the oxalic acid reactivity of the calcium hydroxide slurry is 40 minutes or less (the time (minutes) required for the pH to reach 7.0 after the addition of 40 g of an aqueous oxalic acid solution having a concentration of 0.5 mol / L and kept at 25±1° C. to 50 g of calcium hydroxide slurry prepared to a concentration of 5% by mass and kept at 25±1° C.).
Citation Information
Patent Citations
Spherical nano-porous hydroxylapatite prepared through shells and preparation method thereof
CN105347322A
Micro-nano structure hydroxyapatite and preparing method and application thereof
CN105502323A
Hydroxyapatite to be formulated to tooth paste and its production
JP1997020508A
Non-crystalline calcium phosphate slurry, its preparation and non-crystalline calcium phosphate particle
JP1999292524A
Method for producing apatite powder
JP2005075722A