Polyimide precursor resin composition

A polyimide precursor resin composition with tailored molecular weight, shear rate dependence, and solid content improves slit coating and mechanical/optical properties, addressing issues in flexible substrate applications.

JP7564621B2Active Publication Date: 2024-10-09ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2019566503
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-02-16
Filing Date
2019-01-17
Publication Date
2024-10-09
Estimated Expiration
2039-01-17

AI Technical Summary

Technical Problem

Existing polyimide precursor compositions used in flexible substrates exhibit inadequate slit coating properties and insufficient mechanical and optical properties, particularly for large displays, leading to issues such as nozzle damage and non-uniform film thickness.

Method used

A resin composition containing a polyimide precursor with a specific molecular weight range of 110,000 to 250,000, a shear rate dependence of 0.9 to 1.1, and a solid content of 10 to 25% by mass, along with a specific structural formula, enhances slit coating performance and mechanical and optical properties.

Benefits of technology

The composition achieves excellent coating uniformity, mechanical strength, and optical clarity, suitable for large flexible displays, reducing the risk of nozzle damage and ensuring high film thickness uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564621000026
    Figure 0007564621000026
  • Figure 0007564621000001
    Figure 0007564621000001
  • Figure 0007564621000002
    Figure 0007564621000002
Patent Text Reader

Abstract

The following formula (1): Provided is a resin composition comprising a polyimide precursor having a structure represented by the following formula: {wherein, when there are multiple R1, each independently represents a divalent organic group, when there are multiple R2, each independently represents a tetravalent organic group, and n is a positive integer} and a solvent, wherein the polyimide precursor has a weight-average molecular weight of 110,000 to 250,000, and the resin composition has a solids content of 10 to 25 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a polyimide precursor, and a polyimide film. The present invention further relates to a flexible device (e.g., a flexible display) and a laminate, and a method for producing the same. [Background technology]

[0002] Polyimide resin is an insoluble, infusible, and extremely heat-resistant resin with excellent heat resistance (e.g., thermal oxidation resistance), radiation resistance, low temperature resistance, chemical resistance, and other properties. For this reason, polyimide resin is used in a wide range of fields, including electronic materials. Examples of applications of polyimide resin in the electronic materials field include insulating coating materials, insulating films, semiconductors, and electrode protective films for thin film transistor liquid crystal displays (TFT-LCDs). Recently, in the field of display materials, the use of flexible substrates, taking advantage of their lightness and flexibility, has been considered in place of the glass substrates that have been conventionally used.

[0003] For example, Patent Document 1 describes a resin precursor (weight average molecular weight 30,000 to 90,000) polymerized from bis(diaminodiphenyl)sulfone (hereinafter also referred to as DAS) and having a siloxane unit, and describes that a polyimide obtained by curing the precursor has low residual stress between the support such as glass, has excellent chemical resistance, and has little effect on the yellowness index (YI) value and total light transmittance due to the oxygen concentration during the curing process. Patent Document 2 describes a resin composition characterized by containing a polyimide precursor with a specific absorbance and an alkoxysilane compound with a specific absorbance, and describes that a resin obtained by curing the resin composition has both sufficient adhesion to the support and releasability by laser peeling or the like. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 148441 [Patent Document 2] International Publication No. 2016 / 167296 Summary of the Invention [Problem to be solved by the invention]

[0005] When a transparent polyimide resin is to be applied to a flexible substrate, a resin composition containing a polyimide precursor is applied onto a substrate such as glass to form a coating film, which is then heated and dried, and the polyimide precursor is further imidized to form a polyimide film. After a device is formed on the film as required, the film is peeled off from the support such as a glass substrate to obtain the desired product.

[0006] In recent years, with the increasing size of displays and other applications of flexible substrates, a slit coater may be used to coat a composition containing a polyimide precursor onto a substrate such as glass. When a coating film is formed by coating a composition with a slit coater, a parameter that affects the coating film is the coater gap (a set value that defines the distance between the glass substrate and the slit nozzle). If the coater gap is small, the nozzle may come into contact with the substrate if the flatness of the glass substrate is poor, and the slit nozzle may be damaged. In particular, with the increasing size of displays and other applications in recent years, it has become necessary to make this coater gap sufficiently large. Furthermore, when a polyimide film is used as a material for the screen of a flexible display or the like, since the wavelength of visible light is from about 380 nm to about 700 nm, a particularly high degree of film thickness uniformity is required to obtain good optical performance.

[0007] The present inventors conducted a coating evaluation of a slit coat using a polyimide precursor having the same molecular weight and skeleton as those described in the above Patent Documents 1 and 2, and found that the above properties were insufficient. Therefore, an object of one aspect of the present invention is to provide a polyimide precursor-containing resin composition that has excellent slit coat coating properties, as well as excellent mechanical properties and optical properties required for applications such as flexible substrates. [Means for solving the problem]

[0008] As a result of extensive investigations, the present inventors have found that the use of a polyimide precursor having a specific structure leads to the realization of good coating properties in slit coating, as well as good mechanical properties and optical properties. That is, the present invention includes the following aspects. [1] The following formula (1): [ka] A resin composition comprising a polyimide precursor having a structure represented by the formula: {wherein, when there are more than one R1, each independently represents a divalent organic group, when there are more than one R2, each independently represents a tetravalent organic group, and n is a positive integer} and a solvent, The weight average molecular weight of the polyimide precursor is 110,000 to 250,000; The resin composition has a solid content of 10 to 25% by mass. [2] The resin composition according to embodiment 1, wherein the resin composition has a shear rate dependency (TI) of 0.9 to 1.1 when the viscosity of the resin composition is measured at 23° C. using a temperature-adjusted viscometer: TI=ηa / ηb {In the formula, ηa (mPa·s) is the viscosity of the resin composition at a measurement rotation speed a (rpm), and ηb (mPa·s) is the viscosity of the resin composition at a measurement rotation speed b (rpm), where a*10=b.} [3] The resin composition according to aspect 1 or 2, wherein the resin composition is a resin composition for slit coating. [4] At least one of R1 in the formula (1) is the following formula (2): [ka] The resin composition according to any one of the above aspects 1 to 3, wherein the group is represented by the following formula: [5] The polyimide precursor is represented by the following formula (3): [ka] The resin composition according to any one of Aspects 1 to 4 above, having a structure represented by the following formula: {wherein, when there are more than one R3 and R4, each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m is an integer of 1 to 200.} [6] The resin composition according to any one of the above aspects 1 to 5, wherein the polyimide precursor is a copolymer of a tetracarboxylic dianhydride, including pyromellitic dianhydride, and a diamine. [7] The resin composition according to any one of the above aspects 1 to 6, wherein the polyimide precursor is a copolymer of a tetracarboxylic dianhydride, including 3,3',4,4'-biphenyltetracarboxylic dianhydride, and a diamine. [8] The resin composition according to any one of the above aspects 1 to 7, wherein the polyimide precursor is a copolymer of a tetracarboxylic dianhydride and a diamine, and the tetracarboxylic dianhydride contains pyromellitic dianhydride and 3,3',4,4'-biphenyltetracarboxylic dianhydride in a molar ratio of the pyromellitic dianhydride to the 3,3',4,4'-biphenyltetracarboxylic dianhydride of 20:80 to 80:20. [9] The resin composition according to any one of Aspects 1 to 8, wherein the polyimide precursor is a copolymer of a tetracarboxylic dianhydride and one or more diamines selected from the group consisting of 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,2'-bis(trifluoromethyl)benzidine, and 9,9-bis(4-aminophenyl)fluorene.

[10] The resin composition according to any one of the above aspects 1 to 9, wherein the polyimide precursor has a weight average molecular weight of 160,000 to 220,000.

[11] The resin composition according to any one of the above aspects 1 to 10, which is a resin composition for a flexible device.

[12] The resin composition according to any one of the above aspects 1 to 11, which is a resin composition for a flexible display.

[13] A polyimide film which is a cured product of the resin composition according to any one of the above embodiments 1 to 12.

[14] The polyimide film according to aspect 13, having a thickness direction retardation (Rth) of 300 or less when converted to a thickness of 10 μm and / or a yellowness index (YI) of 20 or less when converted to a thickness of 10 μm.

[15] A flexible device comprising the polyimide film according to aspect 13 or 14.

[16] A flexible display comprising the polyimide film according to embodiment 13 or 14.

[17] The flexible display described in claim 16, wherein the polyimide film is disposed in a location that is visible when the flexible display is observed from the outside.

[18] A coating step of coating a surface of a support with the resin composition according to any one of the above aspects 1 to 12; a film-forming step of heating the resin composition to form a polyimide film; and a peeling step of peeling the polyimide film from the support.

[19] The method for producing a polyimide film according to Aspect 18, wherein the coating step includes slit coating the resin composition.

[20] At least one of R1 in the formula (1) is the following formula (2): [ka] 20. The method for producing a polyimide film according to the above-mentioned embodiment 19, wherein the group is represented by the following formula:

[21] The polyimide precursor is represented by the following formula (3): [ka] {wherein, when there are more than one R3 and R4, each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m is an integer of 1 to 200.}

[22] The method for producing a polyimide film according to any one of the above aspects 18 to 21, further comprising, prior to the peeling step, an irradiation step of irradiating the polyimide film with a laser from the support side.

[23] A coating step of coating a surface of a support with the resin composition according to any one of the above aspects 1 to 12; a film-forming step of heating the resin composition to form a polyimide film; an element forming step of forming an element on the polyimide film; and peeling the polyimide film on which the elements are formed from the support.

[24] The method for producing a display according to the above-mentioned aspect 23, wherein the applying step includes slit coating the resin composition.

[25] The method for producing a display according to aspect 23 or 24, further comprising disposing the polyimide film at a location that is visible when the display is observed from the outside. Effect of the Invention

[0009] According to one aspect of the present invention, it is possible to provide a polyimide precursor-containing resin composition that has excellent coating properties in slit coating and also has excellent mechanical properties and optical properties required for applications such as flexible substrates. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a diagram showing the structure above a polyimide substrate of a top-emission type flexible organic EL display as an example of a display provided in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, exemplary embodiments of the present invention (hereinafter, abbreviated as "embodiments") will be described in detail. Note that the present invention is not limited to the following embodiments, and can be practiced with various modifications within the scope of the gist of the present invention. In addition, unless otherwise specified, the characteristic values ​​described in this disclosure are intended to be values ​​measured by the method described in the [Examples] section or a method that is understood to be equivalent to the method by a person skilled in the art.

[0012] In this embodiment, The following formula (1): [ka] {In the formula, when there is a plurality of R1, each independently represents a divalent organic group, when there is a plurality of R2, each independently represents a tetravalent organic group, and n is a positive integer.} The present invention provides a resin composition comprising a polyimide precursor having a structure represented by the following formula: In one embodiment, the resin composition comprises the polyimide precursor and a solvent.

[0013] In a preferred embodiment, at least one of R1 in formula (1) is the following formula (2): [ka] It is a group represented by the following formula:

[0014] At least one of R1 in formula (1) being a structure represented by formula (2) contributes to good optical properties (particularly Rth) and heat resistance of the polyimide, which is a cured product of the polyimide precursor. In one embodiment, all of the n R1 in formula (1) have a structure represented by formula (2). In one embodiment, the proportion of the structure represented by formula (2) among the n R1 in formula (1) may be 0% or more, 10% or more, or 20% or more, and may be 100% or less, or 90% or less.

[0015] The present embodiment also provides a resin composition containing a polyimide precursor having a structure represented by the above formula (1), wherein the polyimide, which is a cured product of the resin composition, has a retardation in the thickness direction (Rth) of 300 or less and / or a yellowness index (YI) of 20 or less. The low retardation in the thickness direction (Rth) indicates that the polyimide has low birefringence, and the low yellowness index (YI) indicates that the polyimide has a good color tone (i.e., is almost colorless).

[0016] The resin composition of the present embodiment has excellent slit coating performance and gives a polyimide film having excellent mechanical properties and optical properties, and is therefore preferably useful for flexible devices (e.g., flexible substrates), and particularly preferably useful for flexible displays.

[0017] (Weight average molecular weight of polyimide precursor) In one embodiment, the weight average molecular weight of the polyimide precursor is 110,000 or more and 250,000 or less. The present inventor found that when the resin composition of this embodiment is used for slit coating, the weight average molecular weight of the polyimide precursor greatly affects the coating performance, and conducted extensive research. As a result, it was found that when the weight average molecular weight of the polyimide precursor is 110,000 or more, the solid content of the resin composition can be adjusted to achieve good slit coating, while a polyimide precursor having a weight average molecular weight of 250,000 or less is easy to manufacture. That is, in this embodiment, the weight average molecular weight of the polyimide precursor is 110,000 or more from the viewpoint of coating performance, and 250,000 or less from the viewpoint of ease of manufacture.

[0018] The desired weight average molecular weight of the polyimide precursor may vary depending on the desired application, the type of polyimide precursor, the solids content of the resin composition, the type of solvent that the resin composition may contain, and the like.

[0019] For example, preferred examples of the lower limit of the weight average molecular weight are 111,000, 112,000, 113,000, 114,000, 115,000, 116,000, 117,000, 118,000, 119,000, 120,000, 121,000, 122,000, 123,000, 124,000, 125,000, 126,000, 127,000, 128,000, 129,000, 130,000, 131,000, 132,000, 133,000, 134,000, 135,000, 136,000, 137,000, 138,000, and 139,000. 9,000, 140,000, 141,000, 142,000, 143,000, 144,000, 145,000, 146,000, 147,000, 148,000, 149,000, 150,000, 151,000, 152,000, 153,000, 154,000 0, 155,000, 156,000, 157,000, 158,000, 159,000, 160,000, 161,000, 162,000, 163,000, 164,000, 165,000, 166,000, 167,000, 168,000, 169,000, 170 ,000, 171,000, 172,000, 173,000, 174,000, 175,000, 176,000, 177,000, 178,000, 179,000, 180,000, 181,000, 182,000, 183,000, 184,000, 185,000 , 186,000, 187,000, 188,000, 189,000, 190,000, 191,000, 192,000, 193,000, 194,000, 195,000, 196,000, 197,000, 198,000, 199,000, 200,000, 201 ,000, 202,000, 203,000, 204,000, 205,000, 206,000, 207,000, 208,000, 209,000, 210,000, 211,000, 212,000, 213,000, 214,000, 215,000, 216,000 , 217,000, 218,000, 219,000, 220,000, 221,000, 222,000, 223,000, 224,000, 225,000, 226,000, 227,000, 228,000, 229,000, 230,000, 231,000, 232,000, 233,000, 234,000, 235,000, 236,000, 237,000, 238,000, 239,000, 240,000, 241,000, 242,000, 243,000, 244,000, 245,000, 246,000, 247,000, 248,000, or 249,000.

[0020] Preferred examples of the upper limit of the weight average molecular weight are 249,000, 248,000, 247,000, 246,000, 245,000, 244,000, 243,000, 242,000, 241,000, 240,000, 239,000, 238,000, 237,000, 236,000, 235,000, 234,000, 233,000, 232,000, 231,000, 230,000, 229,000, 228,000, 227,000, 226,000, 225,000, 224,000, 223,000, 222,000, 221,000, 223,000, 224,000, 225,000, 226,000, 227,000, 228,000, 229,000, 229,000, 230,000, 231,000, 232,000, 233,000, 234,000, 235,000, 236,000, 237,000, 238,000, 239,000, 239,000, 240,000, 241,000, 242,000, 243,000, 244,000, 245,000, 246,000, 24 00, 220,000, 219,000, 218,000, 217,000, 216,000, 215,000, 214,000, 213,000, 212,000, 211,000, 210,000, 209,000, 208,000, 207,000, 206,000, 20 5,000, 204,000, 203,000, 202,000, 201,000, 200,000, 199,000, 198,000, 197,000, 196,000, 195,000, 194,000, 193,000, 192,000, 191,000, 190,000 , 189,000, 188,000, 187,000, 186,000, 185,000, 184,000, 183,000, 182,000, 181,000, 180,000, 179,000, 178,000, 177,000, 176,000, 175,000, 174, 000, 173,000, 172,000, 171,000, 170,000, 169,000, 168,000, 167,000, 166,000, 165,000, 164,000, 163,000, 162,000, 161,000, 160,000, 159,000, 1 58,000, 157,000, 156,000, 155,000, 154,000, 153,000, 152,000, 151,000, 150,000, 149,000, 148,000, 147,000, 146,000, 145,000, 144,000, 143,000 0, 142,000, 141,000, 140,000, 139,000, 138,000, 137,000, 136,000, 135,000, 134,000, 133,000, 132,000, 131,000, 130,000, 129,000, 128,000, 127,000, 126,000, 125,000, 124,000, 123,000, 122,000, 121,000, 120,000, 119,000, 118,000, 117,000, 116,000, 115,000, 114,000, 113,000, 112,000, or 111,000.

[0021] For example, from the viewpoint of the elongation and yellowness index (YI) of a cured product (e.g., a polyimide film (also referred to as a cured film in the present disclosure)) of a resin composition containing a polyimide precursor, the weight average molecular weight is preferably 120,000 or more, more preferably 130,000 or more, and particularly preferably 160,000 or more. Furthermore, from the viewpoint of the haze of the cured product (e.g., a polyimide film), the weight average molecular weight is preferably 220,000 or less, and more preferably 200,000 or less. In a preferred embodiment, the weight average molecular weight of the polyimide precursor is 160,000 or more and 220,000 or less.

[0022] (Thickness retardation of polyimide film (Rth)) When a polyimide film is produced as a cured product (i.e., an imidized product) of a polyimide precursor, the thickness direction retardation (Rth) of the polyimide film at a film thickness of 10 μm varies depending on the monomer skeleton of the polyimide precursor, but for the same monomer skeleton, the higher the weight average molecular weight of the polyimide precursor, the smaller the Rth tends to be. When DAS is used as the polymer skeleton, the Rth tends to be lower. The mechanism of the above relationship between the weight average molecular weight of the polyimide precursor and the Rth of the polyimide film is unknown, but it is thought to be related to the molecular orientation and crystallinity of the polyimide film.

[0023] In a specific embodiment, Rth is 300nm or less from the viewpoint of obtaining a polyimide film with low birefringence. In particular, when the polyimide film is used as a display material, Rth is preferably 200nm or less, more preferably 100nm or less, more preferably 80nm or less, more preferably 50nm or less, and particularly preferably 30nm. If Rth is 300nm or less, it is easy to capture an image correctly, and in particular, if Rth is 200nm or less, the color reproducibility of the image is good.

[0024] In one embodiment, the polyimide film has a thickness direction retardation (Rth) of 300 nm or less when converted to a 10 μm film thickness, and / or a yellowness index (YI) of 20 or less when converted to a 10 μm film thickness. In one embodiment, the polyimide film has a thickness direction retardation (Rth) of 300 nm or less when converted to a 10 μm film thickness, and a yellowness index (YI) of 20 or less when converted to a 10 μm film thickness.

[0025] (Yellowness index (YI) of polyimide film) In a specific embodiment, when a polyimide film is produced as a cured product (i.e., an imidized product) of the polyimide precursor, from the viewpoint of obtaining good optical properties, the yellowness index (YI) of the polyimide film at a thickness of 10 μm is 20 or less, preferably 18 or less, more preferably 16 or less, even more preferably 14 or less, even more preferably 13 or less, still more preferably 10 or less, and particularly preferably 7 or less. The YI of the polyimide film at a thickness of 10 μm varies depending on the monomer skeleton of the polyimide precursor, but when the monomer skeleton is the same, the larger the weight average molecular weight of the polyimide precursor, the smaller the YI tends to be.

[0026] (Other desirable properties of polyimide film) When a polyimide film is produced on an inorganic support substrate such as a glass substrate as a cured product of a polyimide precursor (i.e., an imidized product), the residual stress generated between the polyimide film having a thickness of 10 μm and the glass substrate is preferably 25 MPa or less, more preferably 23 MPa or less, even more preferably 20 MPa or less, still more preferably 18 MPa or less, and particularly preferably 16 MPa or less, from the viewpoint of reducing the amount of warping of the glass substrate with the polyimide in production for display applications, for example.

[0027] In addition, the tensile elongation of the polyimide film at a thickness of 10 μm is preferably 15% or more. From the viewpoint of the mechanical strength of a flexible display, the tensile elongation is more preferably 20% or more, even more preferably 25% or more, even more preferably 30% or more, even more preferably 35% or more, and particularly preferably 40% or more. The tensile elongation of the polyimide film varies depending on the monomer skeleton of the polyimide precursor, but if the monomer skeleton is the same, the tensile elongation tends to be greater as the weight average molecular weight of the polyimide precursor increases.

[0028] The glass transition temperature Tg of the polyimide film is preferably 360°C or higher, more preferably 400°C or higher, and even more preferably 470°C or higher, from the viewpoint of being able to increase the process temperature when forming an inorganic film such as silicon nitride on the polyimide by a CVD process.

[0029] The polyimide film preferably has a uniform thickness. In particular, when the polyimide film is used as a material for a screen such as a flexible display, the wavelength of visible light is about 380 nm to about 700 nm, so that a particularly high thickness uniformity is required from the viewpoint of obtaining good display performance and from the viewpoint of the display manufacturing process. The thickness uniformity (standard deviation of thickness at multiple points) of the polyimide film is preferably 10 μm or less, preferably 8 μm or less, preferably 5 μm or less, preferably 3 μm or less, preferably 2 μm or less, particularly preferably 1 μm or less, particularly preferably 500 nm or less, and particularly preferably 300 nm or less. The smaller the thickness uniformity, the more preferable it is, but from the viewpoint of improving the yield of display manufacturing, it may be, for example, 50 nm or more, or 100 nm or more. The above thickness uniformity means a 3σ value calculated from the thickness at multiple points as measured, for example, by the method described in the [Example] section of this disclosure.

[0030] (Shear rate dependence of resin composition) The shear rate dependency (TI) (hereinafter, simply referred to as TI) of the resin composition of the present embodiment is preferably 0.9 or more and 1.1 or less. In the present disclosure, TI is calculated by the following formula, from the viscosity ηa (mPa·s) at the measurement rotation speed a (rpm) and the viscosity ηb (mPa·s) at the measurement rotation speed b (rpm) (where a*10=b), when the viscosity of the resin composition is measured at 23° C. with a temperature-controlled viscometer (TVE-35H manufactured by Toki Sangyo Kikai Co., Ltd.): TI=ηa / ηb The details of the measurement conditions will be explained in the examples.

[0031] The shear rate dependency (TI) is preferably 0.9 or more, or 0.95 or more, or 1.0 or more, and preferably 1.1 or less, or 1.05 or less, or 1.0 or less. When the TI is in this range, the resin composition is called a Newtonian fluid, and is preferable because the film thickness uniformity is good when the resin composition is slit-coated. A polyimide film obtained by curing a resin composition with good film thickness uniformity has good film thickness uniformity, and can be suitably used as a material for a screen such as a flexible display.

[0032] The detailed reason why the film thickness uniformity becomes good when the shear rate dependency of the resin composition is 0.9 or more and 1.1 or less is unclear, but is thought to be as follows. In slit coating, the shear rate given to the resin composition immediately after the start of coating is small, and the shear rate given to the resin composition when coating is continued is large. When the shear rate dependency is small (specifically, TI is 0.9 or more and 1.1 or less), the difference in viscosity of the resin composition immediately after coating is started and when coating is continued is small, so the film thickness variation in the coating direction (MD (Machine direction)) is small (i.e., the film thickness uniformity in the coating direction is good). In addition, when the slit coating nozzle is designed to inject the resin composition from only one end of the width direction (TD (Transverse direction)), the shear rate of the resin composition is high near the injection port during slit coating, but the shear rate of the resin composition is low on the opposite side to the injection port (i.e., the deadlock side of the nozzle). Even in such a case, the shear rate dependency is small (specifically, TI is 0.9 or more and 1.1 or less), so that the film thickness variation in the width direction can be reduced. In this way, the small shear rate dependency (specifically, TI is 0.9 or more and 1.1 or less) reduces the effect of shear on the viscosity, and provides the advantage of small film thickness variation in both MD and TD (i.e., good film thickness uniformity).

[0033] The shear rate dependency of the resin composition is considered to be correlated with the synthesis method of the resin composition. For example, when comparing the case where all of the acid dianhydride, diamine, and silicone oil, which may be an acid dianhydride or diamine depending on the structure, are added to a reaction vessel and heated to react with the case where the acid dianhydride dissolved in a solvent and the silicone oil dissolved in a solvent are dropped into the diamine at room temperature over time and reacted little by little, in the former case, the monomers (i.e., the acid dianhydride, diamine, and silicone oil) that are more reactive (highly acidic or basic, low steric hindrance, etc.) react first, and the polyimide precursor tends to become a block polymer. On the other hand, in the latter case, the acid dianhydride and silicone oil are dissolved in a solvent and dropped in small amounts, so that each monomer can react regardless of reactivity, etc., and the polyimide precursor tends to become a random polymer. Thus, the polymer composition of the product is thought to be different between the former and the latter. And in the case of a block polymer (the former case), since specific monomers are gathered in the polymer, it is thought that intermolecular interactions are more likely to occur between polymer chains, or the flexibility of the polymer is impaired, so that the polymer chains tend to stack with each other. As a result, it is considered that the shear rate dependency of the resin composition becomes large. On the other hand, in the latter case, each monomer is bonded in an orderly manner, and intermolecular interactions are unlikely to occur, so that it is considered that the shear rate dependency is small.

[0034] In the former case, since all the monomers are added and heated, it is believed that the acid dianhydride group, especially in some acid dianhydrides, opens the ring due to heat before reacting with the polymer chain. When the acid dianhydride group opens the ring to become a dicarboxyl group, the reactivity decreases compared to the acid dianhydride group, so the molecular weight of the polyimide precursor is thought to decrease. On the other hand, in the latter case, the acid dianhydride is dissolved in a solvent and dropped in small amounts at room temperature, so that the acid dianhydride group can react with the polymer chain without opening the ring, and it is thought that the molecular weight increases.

[0035] (Slit Coating Properties of Resin Composition) The coating characteristics (slit coating characteristics) of a resin composition containing a polyimide precursor by a slit nozzle are correlated with the weight average molecular weight of the polyimide precursor and the solid content of the resin composition. When the polyimide precursor has a low molecular weight and / or the resin composition has a low solid content, liquid leakage from the nozzle is likely to occur, while when the polyimide precursor has a high molecular weight and / or the resin composition has a high solid content, clogging of the nozzle tip with varnish is likely to occur. Therefore, it is preferable to control the weight average molecular weight of the polyimide precursor within a range in which the desired slit coating characteristics can be obtained by controlling the solid content.

[0036] (Edge characteristics of coating film) When a resin composition containing a polyimide precursor is slit-coated to form a dry coating film, if the polyimide precursor has a low molecular weight and / or the resin composition has a low solid content, edge sagging is likely to occur, whereas if the polyimide precursor has a high molecular weight and / or the resin composition has a high solid content, edge beads (i.e., raised edges) are likely to occur. Therefore, it is preferable to control the weight-average molecular weight of the polyimide precursor within a range in which the desired edge characteristics can be obtained by controlling the solid content.

[0037] In one embodiment, the solid content of the resin composition is 10% by mass to 25% by mass. The coat gap that can be set when slit-coating the resin composition (i.e., the gap between the tip of the slit coat nozzle and the substrate) correlates with the solid content of the resin composition, and if the type of solid content contained in the resin composition is the same, the coat gap tends to be larger as the solid content of the resin composition is smaller. From the viewpoint of good coating, a larger coat gap is preferable, and for example, if the coat gap is 50 μm or more, collision between the slit nozzle and the substrate can be avoided even when the substrate size is relatively large. When the solid content of the resin composition is 10% by mass to 25% by mass, the desired coat gap can be achieved by selecting the type and molecular weight of the polyimide precursor. The preferred solid content of the resin composition may vary depending on the desired application, the type and molecular weight of the polyimide precursor, the type of solvent that the resin composition may contain, and the like.

[0038] Preferred examples of the lower limit of the solid content are 11 mass%, 12 mass%, 13 mass%, 14 mass%, 15 mass%, 16 mass%, 17 mass%, 18 mass%, 19 mass%, 20 mass%, 21 mass%, 22 mass%, 23 mass%, or 24 mass%.

[0039] Preferred examples of the upper limit of the solid content are 24 mass%, 23 mass%, 22 mass%, 21 mass%, 20 mass%, 19 mass%, 18 mass%, 17 mass%, 16 mass%, 15 mass%, 14 mass%, 13 mass%, 12 mass%, or 11 mass%.

[0040] In a preferred embodiment, the solid content is 10 to 20% by mass, and more preferably 10 to 15% by mass.

[0041] In a preferred embodiment, the polyimide precursor has the formula (3): [ka] {wherein, when there are more than one R3 and R4, each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m is an integer of 1 to 200.} It is advantageous for R3 and R4 to be a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms in terms of obtaining a polyimide capable of reducing Rth and the residual stress generated between the support. Preferred structures of R3 and R4 include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. From the viewpoint of obtaining a polyimide capable of reducing the residual stress generated between the support and Rth, m is 1 to 200, and is preferably 1 or more, or 3 or more, or 5 or more, and is preferably 200 or less, or 180 or less, or 160 or less.

[0042] The polyimide precursor may have the structure of formula (3) at any site in the molecule, but from the viewpoints of the type of siloxane monomer and cost, the structure of formula (3) is preferably derived from a diamine component. The ratio of the structural site represented by formula (3) to the total mass of the polyimide precursor is preferably 5 mass% or more, more preferably 6 mass% or more, and even more preferably 7 mass% or more from the viewpoints of reducing the residual stress and Rth generated between the support and the polyimide precursor, and is preferably 40 mass% or less, more preferably 30 mass% or less, and even more preferably 25 mass% or less from the viewpoints of the transparency and heat resistance of the obtained cured product (e.g., polyimide film).

[0043] In a typical embodiment, the polyimide precursor having the structure represented by the above formula (1) is a polymer of a diamine component containing an R1 group and an acid dianhydride component containing an R2 group.

[0044] Examples of acid dianhydrides containing the R2 group include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2 dicarboxylic anhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxlic dianhydride, and 1,2,3,4-benzenetetracarboxylic dianhydride. diphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethylidene-4,4'-diphthalic dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, p-phenylenebis(trimethylsilyl) mellitate anhydride), thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene dianhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene dianhydride, bis[3-(3,4-dicarboxy 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, bis(3,4-dicarboxyphenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,Examples of the dianhydride include 8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, and 1,2,7,8-phenanthrenetetracarboxylic dianhydride.

[0045] Among them, pyromellitic dianhydride (PMDA) and biphenyltetracarboxylic dianhydride (BPDA) are preferred from the viewpoint of easily obtaining good slit coating performance, as well as good mechanical properties, optical properties, and a high glass transition temperature of a cured product (e.g., a polyimide film) when the solid content of the resin composition is controlled within a predetermined range of the weight average molecular weight of the polyimide precursor. In one embodiment, the polyimide precursor having a structure represented by formula (1) is a copolymer of a tetracarboxylic dianhydride and a diamine. In one embodiment, the polyimide precursor is a copolymer of a tetracarboxylic dianhydride containing pyromellitic dianhydride (PMDA) and a diamine. In another embodiment, the polyimide precursor is a copolymer of a tetracarboxylic dianhydride containing 3,3',4,4'-biphenyltetracarboxylic dianhydride and a diamine.

[0046] In a specific embodiment, the total content of pyromellitic dianhydride (PMDA) and biphenyltetracarboxylic dianhydride (BPDA) in the total acid dianhydrides is preferably 60 mol % or more, more preferably 80 mol % or more, and particularly preferably 100 mol %, from the viewpoint of obtaining good slit coating performance, and good thickness direction retardation (Rth), yellowness index (YI), glass transition temperature Tg, and elongation of a cured product (e.g., a polyimide film).

[0047] In a specific embodiment, the content of pyromellitic dianhydride (PMDA) in the total acid dianhydrides is preferably 0 mol% or more, more preferably 10 mol% or more, more preferably 20 mol% or more, more preferably 100 mol% or less, and more preferably 90 mol% or less, from the viewpoint of obtaining good slit coating performance and a good glass transition temperature Tg of a cured product (e.g., a polyimide film).

[0048] In a specific embodiment, the content of biphenyltetracarboxylic dianhydride (BPDA) in the total acid dianhydrides is preferably 0 mol% or more, more preferably 10 mol% or more, and more preferably 20 mol% or more, and is preferably 100 mol% or less, and more preferably 90 mol% or less, from the viewpoint of obtaining good slit coating performance, and good retardation through thickness (Rth), yellowness index (YI), and elongation of a cured product (e.g., a polyimide film).

[0049] In a specific embodiment, the content ratio of pyromellitic dianhydride (PMDA):biphenyltetracarboxylic dianhydride (BPDA) in the acid dianhydride is preferably 20:80 to 80:20, more preferably 30:70 to 70:30, from the viewpoint of achieving good thickness direction retardation (Rth), yellowness index (YI) and heat resistance represented by glass transition temperature of the cured product (e.g., polyimide film). In a specific embodiment, the polyimide precursor is a copolymer of tetracarboxylic dianhydride and diamine, and the tetracarboxylic dianhydride contains pyromellitic dianhydride and 3,3',4,4'-biphenyltetracarboxylic dianhydride in a molar ratio of pyromellitic dianhydride:3,3',4,4'-biphenyltetracarboxylic dianhydride of 20:80 to 80:20, more preferably 30:70 to 70:30.

[0050] Diamines containing the R group in formula (1) include diaminodiphenylsulfone (e.g., 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone), p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylsulfide, 3,4'-diaminodiphenylsulfide, 3,3'-diaminodiphenylsulfide, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminodiphenylmethane), bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, and the like.

[0051] The diamine used to form the polyimide precursor having the structure represented by formula (1) preferably includes diaminodiphenylsulfone (eg, 4,4'-diaminodiphenylsulfone and / or 3,3'-diaminodiphenylsulfone).

[0052] The content of diaminodiphenyl sulfone in all diamines is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and may be 95 mol% or more. The larger the amount of diaminodiphenyl sulfone, the more preferable it is in terms of the yellowness index (YI), glass transition temperature Tg, and thickness direction retardation Rth of the cured product (e.g., polyimide film). As the diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone is particularly preferable in terms of low yellowness index (YI).

[0053] In a preferred embodiment, the diamine to be copolymerized with diaminodiphenylsulfone preferably includes diamide biphenyls, more preferably diaminobis(trifluoromethyl)biphenyl (TFMB), from the viewpoint of the heat resistance and yellowness index (YI) of the cured product (e.g., polyimide film). The content of diaminobis(trifluoromethyl)biphenyl (TFMB) in all diamines is preferably 20 mol% or more, more preferably 30 mol% or more, from the viewpoint of the yellowness index (YI) of the cured product (e.g., polyimide film), and is preferably 80 mol% or less, more preferably 70 mol% or less, from the viewpoint of allowing the diamine to contain other advantageous components such as diaminodiphenylsulfone.

[0054] In a preferred embodiment, the diamine includes a silicon-containing diamine. In a more preferred embodiment, the diamine includes a silicon-containing diamine including a structure represented by the above formula (3). Examples of the silicon-containing diamine include those represented by the following formula (3a): [ka] {wherein R5 represents a divalent hydrocarbon group and may be the same or different, each of the multiple R3 and R4 is as defined in formula (3), and l represents an integer of 1 to 200.} can be suitably used.

[0055] Preferred structures of R5 in the above general formula (3a) include a methylene group, an ethylene group, a propylene group, a butylene group, a phenylene group, etc. Preferred structures of R3 and R4 in the formula (3a) include a methyl group, an ethyl group, a propyl group, a butyl group, a phenyl group, etc.

[0056] The number average molecular weight of the compound represented by the above formula (3a) is preferably 500 or more, more preferably 1,000 or more, and even more preferably 2,000 or more, from the viewpoint of reducing residual stress generated between the obtained cured product (e.g., polyimide film) and the support, and is preferably 12,000 or less, more preferably 10,000 or less, and even more preferably 8,000 or less, from the viewpoint of transparency (particularly low haze) of the obtained cured product (e.g., polyimide film).

[0057] Specific examples of the compound represented by the above formula (3a) include methylphenyl silicone oil modified with amines at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-1660B-3 (number average molecular weight 4400), X22-9409 (number average molecular weight 1300)), dimethyl silicone modified with amino at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X22-161A (number average molecular weight 1600), X22-161B (number average molecular weight 3000), KF8012 (number average molecular weight 4400), Toray Dow Corning Co., Ltd.: BY16-835U (number average molecular weight 900), Chisso Corporation: Silaplane FM3311 (number average molecular weight 1000)), and the like. Among these, methylphenyl silicone oil modified with amines at both ends is preferred from the viewpoint of improving chemical resistance and improving Tg.

[0058] The copolymerization ratio of the silicon-containing diamine is preferably in the range of 0.5 to 30 mass% based on the mass of the total polyimide precursor, more preferably 1.0 to 25 mass%, and even more preferably 1.5 to 20 mass%. When it is 0.5 mass% or more, the effect of reducing the stress generated between the support is good. When it is 30 mass% or less, the transparency (e.g., low haze) of the obtained cured product (e.g., polyimide film) is good, and it is preferable in terms of realizing high total light transmittance and preventing a decrease in Tg.

[0059] In the present embodiment, the acid component for forming the polyimide precursor may be a dicarboxylic acid in addition to an acid dianhydride (for example, the tetracarboxylic dianhydride exemplified above) within a range that does not impair the performance. That is, the polyimide precursor of the present disclosure may be a polyamideimide precursor. A film obtained from such a polyimide precursor can have good performance such as mechanical elongation, glass transition temperature Tg, and yellowness index (YI). Examples of the dicarboxylic acid used include dicarboxylic acids having an aromatic ring and alicyclic dicarboxylic acids. In particular, at least one compound selected from the group consisting of aromatic dicarboxylic acids having 8 to 36 carbon atoms and alicyclic dicarboxylic acids having 6 to 34 carbon atoms is preferable. The number of carbon atoms referred to here includes the number of carbon atoms contained in the carboxyl group. Among these, dicarboxylic acids having an aromatic ring are preferable.

[0060] Specifically, for example, isophthalic acid, terephthalic acid, 4,4'-biphenyldicarboxylic acid, 3,4'-biphenyldicarboxylic acid, 3,3'-biphenyldicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-sulfonylbisbenzoic acid, 3,4'-sulfonylbisbenzoic acid, 3,3'-sulfonylbisbenzoic acid, 4,4'-oxybisbenzoic acid, 3,4'-oxybisbenzoic acid, 3,3'-oxybisbenzoic acid, 2,2-bis(4-carbo 2,2-bis(3-carboxyphenyl)propane, 2,2'-dimethyl-4,4'-biphenyldicarboxylic acid, 3,3'-dimethyl-4,4'-biphenyldicarboxylic acid, 2,2'-dimethyl-3,3'-biphenyldicarboxylic acid, 9,9-bis(4-(4-carboxyphenoxy)phenyl)fluorene, 9,9-bis(4-(3-carboxyphenoxy)phenyl)fluorene, 4,4'-bis(4-carboxyphenoxy)biphenyl, 4,4'-bis(3-carboxyphenoxy)biphenyl, 3,4'-bis (4-carboxyphenoxy)biphenyl, 3,4'-bis(3-carboxyphenoxy)biphenyl, 3,3'-bis(4-carboxyphenoxy)biphenyl, 3,3'-bis(3-carboxyphenoxy)biphenyl, 4,4'-bis(4-carboxyphenoxy)-p-terphenyl, 4,4'-bis(4-carboxyphenoxy)-m-terphenyl, 3,4'-bis(4-carboxyphenoxy)-p-terphenyl, 3,3'-bis(4-carboxyphenoxy)-p-terphenyl, 3,4'-bis(4-carboxyphenoxy) -m-terphenyl, 3,3'-bis(4-carboxyphenoxy)-m-terphenyl, 4,4'-bis(3-carboxyphenoxy)-p-terphenyl, 4,4'-bis(3-carboxyphenoxy)-m-terphenyl, 3,4'-bis(3-carboxyphenoxy)-p-terphenyl, 3,3'-bis(3-carboxyphenoxy)-p-terphenyl, 3,4'-bis(3-carboxyphenoxy)-m-terphenyl, 3,3'-bis(3-carboxyphenoxy)-m-terphenyl, 1,1-cyclobutanedicarboxylic acid, 1,Examples of the dicarboxylic acids include 4-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 1,3-phenylenediacetic acid, 1,4-phenylenediacetic acid, and the like; and 5-aminoisophthalic acid derivatives described in International Publication WO 2005 / 068535. When these dicarboxylic acids are actually copolymerized into a polymer, they may be used in the form of an acid chloride derived from thionyl chloride or an active ester.

[0061] In a preferred embodiment, the polyimide precursor is a copolymer of a tetracarboxylic dianhydride and one or more diamines selected from the group consisting of 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 2,2'-bis(trifluoromethyl)benzidine, and 9,9-bis(4-aminophenyl)fluorene.

[0062] Particularly preferred polyimide precursors include the following: (1) A polycondensate of material components in which the acid dianhydride component is pyromellitic dianhydride (PMDA) and biphenyltetracarboxylic dianhydride (BPDA) and the diamine component is diaminodiphenylsulfone (DAS) (more preferably, a weight average molecular weight of 110,000 to 130,000 and a solid content of 12 to 25% by mass). (2) A polycondensate of material components in which the acid dianhydride components are pyromellitic dianhydride (PMDA) and biphenyltetracarboxylic dianhydride (BPDA) and the diamine components are diaminodiphenylsulfone (DAS) and silicon-containing diamine (more preferably, a weight average molecular weight of 110,000 to 210,000 and a solid content of 10 to 25% by mass). (3) A polycondensate of material components in which the acid dianhydride components are pyromellitic dianhydride (PMDA) and biphenyltetracarboxylic dianhydride (BPDA), and the diamine components are diaminodiphenylsulfone (DAS), diaminobis(trifluoromethyl)biphenyl (TFMB), and silicon-containing diamine (more preferably, a weight average molecular weight of 110,000 to 250,000 and a solid content of 10 to 25% by mass).

[0063] (4) A polycondensate of material components in which the acid dianhydride component is pyromellitic dianhydride (PMDA) and the diamine component is diaminodiphenyl sulfone (DAS) (more preferably, a weight average molecular weight of 110,000 to 140,000 and a solid content of 10 to 25% by mass). (5) A polycondensate of material components in which the acid dianhydride component is pyromellitic dianhydride (PMDA) and the diamine component is diaminodiphenylsulfone (DAS) and a silicon-containing diamine (more preferably, a weight average molecular weight of 110,000 to 230,000 and a solid content of 10 to 25% by mass). (6) A polycondensate of material components in which the acid dianhydride component is pyromellitic dianhydride (PMDA) and the diamine component is diaminodiphenylsulfone (DAS), diaminobis(trifluoromethyl)biphenyl (TFMB) and a silicon-containing diamine (more preferably, a weight average molecular weight of 110,000 to 250,000 and a solid content of 10 to 25% by mass).

[0064] (7) A polycondensate of material components in which the acid dianhydride component is biphenyltetracarboxylic dianhydride (BPDA) and the diamine component is diaminodiphenylsulfone (DAS) (more preferably, a weight average molecular weight of 110,000 to 120,000 and a solid content of 20 to 25% by mass). (8) A polycondensate of material components in which the acid dianhydride component is biphenyltetracarboxylic dianhydride (BPDA) and the diamine component is diaminodiphenylsulfone (DAS) and a silicon-containing diamine (more preferably, a weight average molecular weight of 110,000 to 160,000 and a solid content of 10 to 25% by mass). (9) A polycondensate of material components in which the acid dianhydride component is biphenyltetracarboxylic dianhydride (BPDA) and the diamine component is diaminodiphenylsulfone (DAS), diaminobis(trifluoromethyl)biphenyl (TFMB) and a silicon-containing diamine (more preferably, a weight average molecular weight of 110,000 to 240,000 and a solid content of 10 to 25% by mass).

[0065] In the material components of the polycondensates (1) to (9) above, the silicon-containing diamine is preferably a diamino(poly)siloxane represented by the above formula (3a) (preferably one having a number average molecular weight of 500 to 12,000), and more preferably a methylphenylsilicone oil modified with amines at both ends.

[0066] [Production of polyimide precursor] The polyimide precursor of the present embodiment can be synthesized by polycondensation reaction of a polycondensation component containing an acid dianhydride component and a diamine component. In a preferred embodiment, the polycondensation component is composed of an acid dianhydride component and a diamine component. The polycondensation reaction is preferably carried out in a suitable solvent. Specifically, for example, a method can be mentioned in which a predetermined amount of the diamine component is dissolved in a solvent, and then a predetermined amount of the acid dianhydride is added to the obtained diamine solution and stirred.

[0067] From the viewpoint of increasing the molecular weight of the polyimide precursor resin and the slit coating properties of the resin composition, the molar ratio of the acid dianhydride component to the diamine component when synthesizing the polyimide precursor is preferably in the range of 100:90 to 100:110 (0.90 to 1.10 molar parts of diamine per 1 molar part of acid dianhydride), and more preferably in the range of 100:95 to 100:105 (0.95 to 1.05 molar parts of diamine per 1 molar part of acid dianhydride).

[0068] The molecular weight of the polyimide precursor can be controlled by adjusting the type of the acid dianhydride component and the diamine component, adjusting the ratio of the acid dianhydride component and the diamine component, adding a terminal blocking agent, adjusting the reaction conditions, and the like. The closer the ratio of the acid dianhydride component and the diamine component is to 1:1, and the smaller the amount of the terminal blocking agent used, the higher the molecular weight of the polyimide precursor can be. It is recommended to use high-purity products as the acid dianhydride component and the diamine component. The purity is preferably 98% by mass or more, more preferably 99% by mass or more, and even more preferably 99.5% by mass or more. In addition, the purity can be increased by reducing the water content in the acid dianhydride component and the diamine component. When multiple types of acid dianhydride components or diamine components are used in combination, it is sufficient that the acid dianhydride components or diamine components as a whole have the above-mentioned purity, but it is preferable that all types of acid dianhydride components and diamine components used have the above-mentioned purity.

[0069] The reaction solvent is not particularly limited as long as it can dissolve the acid dianhydride component, the diamine component, and the resulting polyimide precursor, and can produce a high molecular weight polymer. Specific examples of such solvents include aprotic solvents, phenolic solvents, ether and glycol solvents. Specific examples of these solvents include aprotic solvents such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), N-methylcaprolactam, 1,3-dimethylimidazolidinone, tetramethylurea, and the following general formula (4): [ka] In the formula, R 12 = Equamide M100 (trade name: manufactured by Idemitsu Kosan Co., Ltd.), which is represented by a methyl group, and R 12= Amide-based solvents such as Equamide B100 (trade name: manufactured by Idemitsu Kosan Co., Ltd.) represented by an n-butyl group; lactone-based solvents such as γ-butyrolactone and γ-valerolactone; phosphorus-containing amide-based solvents such as hexamethylphosphoric amide and hexamethylphosphine triamide; sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide and sulfolane; ketone-based solvents such as cyclohexanone and methylcyclohexanone; tertiary amine-based solvents such as picoline and pyridine; ester-based solvents such as (2-methoxy-1-methylethyl) acetate; and the above-mentioned phenol-based solvents. Examples of the ether and glycol solvents include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, 1,4-dioxane, etc. These solvents may be used alone or in combination of two or more.

[0070] The boiling point of the solvent used in the synthesis of the polyimide precursor at normal pressure is preferably 60 to 300°C, more preferably 140 to 280°C, and particularly preferably 170 to 270°C. If the boiling point of the solvent is higher than 300°C, a long drying process is required. On the other hand, if the boiling point of the solvent is lower than 60°C, the surface of the resin film may become rough during the drying process, and air bubbles may be mixed into the resin film, making it difficult to obtain a uniform film. In particular, it is preferable to use a solvent having a boiling point of 170 to 270°C and / or a vapor pressure of 250 Pa or less at 20°C from the viewpoint of solubility and edge repellency during coating. More specifically, one or more selected from the group consisting of N-methyl-2-pyrrolidone (NMP), γ-butyrolactone (GBL), and the compound represented by the general formula (4) are preferred.

[0071] The water content in the solvent is preferably, for example, 3,000 ppm by mass or less from the viewpoint of good progress of the polycondensation reaction. In addition, the content of molecules having a molecular weight of less than 1,000 in the resin composition in this embodiment is preferably less than 5% by mass. The presence of molecules having a molecular weight of less than 1,000 in the resin composition is considered to be due to the water content of the solvent and raw materials (acid dianhydride, diamine) used during synthesis. That is, it is considered to be due to the fact that the acid anhydride group of some acid dianhydride monomers is hydrolyzed by water to become a carboxyl group, and remains in a low molecular weight state without being made into a high molecular weight. Therefore, the water content of the solvent used in the polycondensation reaction is preferably as low as possible. The water content of the solvent is preferably 3,000 ppm by mass or less, more preferably 1,000 ppm by mass or less. Similarly, the water content of the raw materials is preferably 3,000 ppm by mass or less, more preferably 1,000 ppm by mass or less.

[0072] The moisture content of the solvent is considered to be affected by the grade of the solvent used (dehydrating grade, general-purpose grade, etc.), the solvent container (bottle, 18L can, canister, etc.), the storage condition of the solvent (whether rare gas is enclosed, etc.), the time from opening to use (whether it is used immediately after opening, or after aging after opening, etc.), etc. It is also considered to be affected by the rare gas replacement of the reactor before synthesis, the presence or absence of rare gas circulation during synthesis, etc. Therefore, when synthesizing polyimide precursors, it is recommended to use high-purity products as raw materials, use solvents with low moisture content, and take measures to prevent moisture from the environment from being mixed into the system before and during the reaction.

[0073] When each polycondensation component is dissolved in the solvent, heating may be performed as necessary. From the viewpoint of obtaining a polyimide precursor having a high degree of polymerization, the preferred reaction temperature during synthesis of the polyimide precursor is 0°C to 120°C, or 40°C to 100°C, or 60°C to 100°C, and the preferred polymerization time is 1 to 100 hours, or 2 to 10 hours. By setting the polymerization time to 1 hour or more, a polyimide precursor having a uniform degree of polymerization can be obtained, and by setting the polymerization time to 100 hours or less, a polyimide precursor having a high degree of polymerization can be obtained.

[0074] The resin composition of the present embodiment may be a combination of a polyimide precursor having a structure represented by formula (1) and another additional polyimide precursor. From the viewpoint of reducing the oxygen dependency of the yellowness index (YI) and total light transmittance of a cured product (e.g., a polyimide film), the mass ratio of the additional polyimide precursor is preferably 30 mass % or less, and more preferably 10 mass % or less, based on the total amount of polyimide precursors in the resin composition.

[0075] In a preferred embodiment of the present invention, the polyimide precursor may be partially imidized. The partially imidized polyimide precursor can improve the viscosity stability of the resin composition during storage at room temperature. In this case, the imidization rate is preferably 5% or more, more preferably 8% or more, and preferably 80% or less, more preferably 70% or less, and even more preferably 50% or less, from the viewpoint of balancing the solubility of the polyimide precursor in the resin composition and the storage stability of the solution. This partial imidization is obtained by heating the polyimide precursor to dehydrate and ring-close it. This heating can be performed at a temperature of preferably 120 to 200°C, more preferably 150 to 180°C, for preferably 15 minutes to 20 hours, more preferably 30 minutes to 10 hours. In addition, N,N-dimethylformamide dimethyl acetal or N,N-dimethylformamide diethyl acetal is added to the polyamic acid obtained by the above reaction, and the mixture is heated to esterify a part or all of the carboxylic acid, and then used as the polyimide precursor in the present embodiment, thereby obtaining a resin composition with improved viscosity stability during storage at room temperature. Alternatively, these ester-modified polyamic acids can be obtained by sequentially reacting the above-mentioned acid dianhydride component with one equivalent of a monohydric alcohol relative to the acid anhydride group and a dehydration condensing agent such as thionyl chloride or dicyclohexylcarbodiimide, and then condensing the resulting mixture with a diamine component.

[0076] In one embodiment, the resin composition contains a solvent. The solvent is preferably one that has good solubility for the polyimide precursor and can appropriately control the solution viscosity of the resin composition, and the reaction solvent of the polyimide precursor can be used as the solvent for the composition. Among them, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone (GBL), the compound represented by the general formula (4), and the like are preferable. Specific examples of the solvent composition include N-methyl-2-pyrrolidone (NMP) alone, or a mixed solvent of N-methyl-2-pyrrolidone (NMP) and γ-butyrolactone (GBL) (for example, NMP:GBL (mass ratio) = 10:90 to 90:10), and the like.

[0077] [Additional Ingredients] The resin composition of the present embodiment may contain additional components in addition to (a) the polyimide precursor and (b) the solvent, such as (c) a surfactant and (d) an alkoxysilane compound.

[0078] (c) Surfactants By adding a surfactant to the resin composition of the present embodiment, the coatability of the resin composition can be improved. Specifically, the occurrence of streaks in the coating film can be prevented. Examples of such surfactants include silicone surfactants, fluorine surfactants, and other nonionic surfactants. Examples of these surfactants include silicone surfactants such as organosiloxane polymers KF-640, 642, 643, KP341, X-70-092, and X-70-093 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.), SH-28PA, SH-190, SH-193, SZ-6032, SF-8428, DC-57, and DC-190 (all trade names, manufactured by Toray Dow Corning Silicones Co., Ltd.), SILWET L-77, L-7001, FZ-2105, FZ-2120, FZ-2154, FZ-2164, FZ-2166, L-7604 (all trade names, manufactured by Nippon Unicar Co., Ltd.), DBE-814, DBE-224, DBE-621, CMS-626, CMS-222, KF-352A, KF-354L, KF-355A, KF-6020, DBE-821, DBE-712 (Gelest), BYK-307, BYK-310, BYK-378, BYK-333 (all trade names, manufactured by BYK Japan), Grano Examples of fluorine-based surfactants include Megafac F171, F173, R-08 (trade names, manufactured by Dainippon Ink and Chemicals, Inc.), Fluorad FC4430, FC4432 (trade names, manufactured by Sumitomo 3M Limited), and the like; and examples of nonionic surfactants other than these include polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenol ether, and the like.

[0079] Among these surfactants, silicone surfactants and fluorine surfactants are preferred from the viewpoint of the coatability (streak suppression) of the resin composition, and silicone surfactants are preferred from the viewpoint of the influence of the oxygen concentration during the curing step on the yellowness index (YI) value and total light transmittance. When the (c) surfactant is used, the blending amount thereof is preferably 0.001 to 5 parts by mass, more preferably 0.01 to 3 parts by mass, per 100 parts by mass of the (a) polyimide precursor in the resin composition.

[0080] (d) Alkoxysilane Compounds When the polyimide film obtained from the resin composition according to the present embodiment is used for a flexible substrate or the like, from the viewpoint of obtaining good adhesion between the support and the polyimide film in the manufacturing process, the resin composition may contain 0.01 to 20 parts by mass of an alkoxysilane compound relative to 100 parts by mass of (a) polyimide precursor. By the content of the alkoxysilane compound relative to 100 parts by mass of the polyimide precursor being 0.01 parts by mass or more, good adhesion between the support and the polyimide film can be obtained. In addition, from the viewpoint of storage stability of the resin composition, it is preferable that the content of the alkoxysilane compound is 20 parts by mass or less. The content of the alkoxysilane compound is more preferably 0.02 to 15 parts by mass, more preferably 0.05 to 10 parts by mass, and particularly preferably 0.1 to 8 parts by mass relative to 100 parts by mass of the polyimide precursor. Furthermore, by using an alkoxysilane compound as an additive to the resin composition according to the present embodiment, in addition to the improvement in adhesion described above, it is also possible to improve the coatability of the resin composition (suppression of streaks) and reduce the dependency of the yellowness index (YI) value of the obtained cured film on the oxygen concentration during curing.

[0081] Examples of the alkoxysilane compound include 3-ureidopropyltriethoxysilane, bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltripropoxysilane, γ-aminopropyltributoxysilane, γ-aminoethyltriethoxysilane, γ-aminoethyltripropoxysilane, γ-aminoethyltributoxysilane, γ-aminobutyltriethoxysilane, γ-aminobutyltrimethoxysilane, γ-aminobutyltripropoxysilane, γ-aminobutyltributoxysilane, phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, and alkoxysilane compounds represented by the following structures, and the like. It is preferable to use one or more selected from these.

[0082] [ka]

[0083] The method for producing the resin composition in the present embodiment is not particularly limited, and can be, for example, the following method.

[0084] When the solvent used in synthesizing the (a) polyimide precursor is the same as the solvent contained in the (b) resin composition, the synthesized polyimide precursor solution can be used as it is as a resin composition. If necessary, the (b) solvent and one or more additional components may be added to the (a) polyimide precursor at a temperature range of room temperature (25°C) to 80°C, and the mixture may be stirred and mixed before being used as a resin composition. For this stirring and mixing, a suitable device such as a Three-One Motor (manufactured by Shinto Chemical Co., Ltd.) equipped with stirring blades or a planetary centrifugal mixer may be used. If necessary, heat of 40 to 100°C may be applied.

[0085] On the other hand, when the solvent used in synthesizing (a) the polyimide precursor and the solvent contained in (b) the resin composition are different, the solvent in the synthesized polyimide precursor solution may be removed by an appropriate method such as reprecipitation or solvent distillation to isolate (a) the polyimide precursor, and then (b) the solvent and, if necessary, additional components may be added and stirred and mixed at a temperature range of room temperature to 80°C to prepare the resin composition.

[0086] After preparing the resin composition as described above, the composition may be heated, for example, at 130 to 200°C for 5 minutes to 2 hours to dehydrate and imidize a part of the polyimide precursor to an extent that the polymer does not precipitate. Here, the imidization rate can be controlled by controlling the heating temperature and heating time. As described above, the partially imidized polyimide precursor can improve the viscosity stability of the resin composition during storage at room temperature.

[0087] From the viewpoint of slit coating performance, the solution viscosity of the resin composition is preferably 500 to 100,000 mPa·s, more preferably 1,000 to 50,000 mPa·s, and particularly preferably 3,000 to 20,000 mPa·s. Specifically, in terms of preventing leakage from the slit nozzle, the solution viscosity is preferably 500 mPa·s or more, more preferably 1,000 mPa·s or more, and even more preferably 3,000 mPa·s or more. In addition, in terms of preventing clogging of the slit nozzle, the solution viscosity is preferably 100,000 mPa·s or less, more preferably 50,000 mPa·s or less, and even more preferably 20,000 mPa·s or less. In addition, in terms of viscosity during synthesis, if the solution viscosity of the resin composition is higher than 200,000 mPa·s, a problem of difficulty in stirring during synthesis may occur. However, even if the solution becomes highly viscous during synthesis, it is possible to obtain a resin composition with a viscosity that is easy to handle by adding a solvent and stirring after the reaction is completed. The solution viscosity of the resin composition in this disclosure is a value measured at 23°C using an E-type viscometer (e.g., VISCONICEHD, manufactured by Toki Sangyo Co., Ltd.).

[0088] The water content of the resin composition according to the present embodiment is preferably 3,000 ppm by mass or less. From the viewpoint of viscosity stability during storage of the resin composition, the water content of the resin composition is preferably 2,500 ppm by mass or less, preferably 2,000 ppm by mass or less, preferably 1,500 ppm by mass or less, more preferably 1,000 ppm by mass or less, even more preferably 500 ppm by mass or less, preferably 300 ppm by mass or less, and preferably 100 ppm by mass or less.

[0089] <Method of manufacturing polyimide film> In this embodiment, A coating step of coating the resin composition of the present embodiment on a surface of a support; a film-forming step of heating the resin composition to form a polyimide film; and a peeling step of peeling the polyimide film from the support.

[0090] [Coating process] In the coating step, the resin composition is coated on the surface of the support. The support is not particularly limited as long as it has heat resistance at the heating temperature in the subsequent film formation step (heating step) and has good releasability in the peeling step. For example, glass (e.g., alkali-free glass) substrate; silicon wafer; resin substrate such as PET (polyethylene terephthalate), OPP (oriented polypropylene), polyethylene glycol terephthalate, polyethylene glycol naphthalate, polycarbonate, polyimide, polyamideimide, polyetherimide, polyetheretherketone, polyethersulfone, polyphenylenesulfone, polyphenylenesulfide; metal substrate such as stainless steel, alumina, copper, nickel, etc. can be used.

[0091] When a thin polyimide molded product is to be formed, for example, a glass substrate or a silicon wafer is preferred, and when a thick polyimide molded product (e.g., a thick film or a sheet) is to be formed, for example, a support made of PET (polyethylene terephthalate), OPP (oriented polypropylene), etc. is preferred.

[0092] Examples of coating methods include coating methods using a doctor blade knife coater, air knife coater, roll coater, rotary coater, flow coater, die coater, bar coater, spin coat, spray coat, dip coat, and printing techniques such as screen printing and gravure printing. The resin composition of the present embodiment is particularly useful for slit coating (i.e., coating with a slit coater). The coating thickness should be appropriately adjusted depending on the desired thickness of the polyimide film and the content of the polyimide precursor in the resin composition, and is preferably about 1 to 1,000 μm. The coating step can be performed at room temperature, but the resin composition may be heated, for example, in the range of 40 to 80° C., in order to reduce the viscosity and improve workability.

[0093] [Optional drying process] Following the coating step, a drying step may be performed, or the drying step may be omitted and the process may proceed directly to the next film formation step (heating step). The drying step is performed for the purpose of removing the organic solvent in the resin composition. When performing the drying step, a suitable device such as a hot plate, a box-type dryer, or a conveyor-type dryer may be used. The drying step is preferably performed at 80 to 200°C, and more preferably at 100 to 150°C. The drying step is preferably performed for 1 minute to 10 hours, and more preferably for 3 minutes to 1 hour. As described above, a coating film containing a polyimide precursor is formed on a support.

[0094] [Film formation process] Subsequently, a film forming step (heating step) is performed. The heating step is a step for removing the organic solvent remaining in the coating film in the drying step and for advancing the imidization reaction of the polyimide precursor in the coating film to obtain a polyimide film. This heating step can be performed using an apparatus such as an inert gas oven, a hot plate, a box-type dryer, or a conveyor-type dryer. This step can be performed simultaneously with the drying step, or both steps can be performed sequentially.

[0095] The heating step may be carried out in an air atmosphere, but it is recommended to carry out the heating step in an inert gas atmosphere from the viewpoints of safety and obtaining good transparency, low retardation in the thickness direction (Rth) and low yellowness index (YI) of the obtained polyimide film. Examples of the inert gas include nitrogen and argon. The heating temperature may be appropriately set according to the type of polyimide precursor and the type of solvent in the resin composition, but is preferably 250°C to 550°C, more preferably 300°C to 450°C. If it is 250°C or higher, imidization proceeds well, and if it is 550°C or lower, inconveniences such as a decrease in transparency and deterioration in heat resistance of the obtained polyimide film can be avoided. The heating time is preferably about 0.1 to 10 hours.

[0096] In the present embodiment, the oxygen concentration of the surrounding atmosphere in the heating step is preferably 2,000 mass ppm or less, more preferably 100 mass ppm or less, and even more preferably 10 mass ppm or less, from the viewpoints of the transparency and yellowness index (YI) value of the resulting polyimide film. By performing heating in an atmosphere with an oxygen concentration of 2,000 mass ppm or less, the yellowness index (YI) value of the resulting polyimide film can be set to 30 or less.

[0097] [Peeling process] Next, in the peeling step, the polyimide film on the support is peeled off after being cooled, for example, to room temperature to about 50° C. This peeling step can be carried out in the following modes (1) to (4), for example.

[0098] (1) A method in which a structure including a polyimide film / support is prepared by the above method, and then a laser is irradiated from the support side of the structure to ablate the interface between the support and the polyimide film, thereby peeling off the polyimide resin. Examples of the type of laser include a solid (YAG) laser and a gas (UV excimer) laser. It is preferable to use a spectrum with a wavelength of 308 nm or the like (see JP-T-2007-512568, JP-T-2012-511173, etc.). (2) A method in which a release layer is formed on a support before a resin composition is applied to the support, and then a structure including a polyimide film / release layer / support is obtained, and the polyimide film is peeled off. Examples of the release layer include a method using Parylene (registered trademark, manufactured by Nippon Parylene LLC) or tungsten oxide, and a method using a vegetable oil-based, silicone-based, fluorine-based, alkyd-based, or other release agent (see JP2010-67957A, JP2013-179306A, etc.). This method (2) may be used in combination with the above-mentioned laser irradiation (1).

[0099] (3) A method of obtaining a polyimide film by using an etchable metal substrate as a support, obtaining a structure including a polyimide film / support, and then etching the metal with an etchant. Examples of metals that can be used include copper (specific example is electrolytic copper foil "DFF" manufactured by Mitsui Mining & Smelting Co., Ltd.) and aluminum. Examples of etchants that can be used include ferric chloride for copper and dilute hydrochloric acid for aluminum. (4) A method in which after obtaining a construct containing a polyimide film / support by the above-mentioned method, an adhesive film is attached to a surface of the polyimide film, the adhesive film / polyimide film is separated from the support, and then the polyimide film is separated from the adhesive film.

[0100] Among these peeling methods, from the viewpoints of the refractive index difference between the front and back sides of the resulting polyimide film, the yellowness index (YI) value, and the elongation, method (1) or (2) is appropriate. From the viewpoint of the refractive index difference between the front and back sides of the resulting polyimide film, method (1), i.e., carrying out an irradiation step of irradiating with a laser from the support side prior to the peeling step, is more appropriate. In the method (3), when copper is used as the support, the yellowness index (YI) value of the obtained polyimide film tends to be large and the elongation tends to be small. This is considered to be due to the influence of copper ions.

[0101] The thickness of the polyimide film obtained by the above method is not particularly limited, but is preferably in the range of 1 to 200 μm, and more preferably 5 to 100 μm.

[0102] <Applications of polyimide film> The polyimide film obtained from the polyimide precursor according to the present embodiment can be used, for example, as a semiconductor insulating film, a TFT-LCD insulating film, an electrode protective film, etc., and can also be suitably used, in particular, as a TFT substrate, a color filter substrate, and a touch panel substrate in the manufacture of flexible devices. Examples of flexible devices to which the polyimide film according to the present embodiment can be used include TFT devices for flexible displays, flexible solar cells, flexible touch panels, flexible lighting, flexible batteries, flexible printed circuit boards, flexible color filters, and surface cover lenses for smartphones.

[0103] The process of forming a TFT on a flexible substrate using a polyimide film is typically carried out at a wide temperature range of 150 to 650° C. Specifically, when manufacturing a TFT device using amorphous silicon, a process temperature of 250 to 350° C. is generally required, and the polyimide film of the present embodiment must be able to withstand that temperature, so specifically, it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition onset temperature equal to or higher than the process temperature.

[0104] When fabricating a TFT device using a metal oxide semiconductor (IGZO, etc.), a process temperature of 320°C to 400°C is generally required. The polyimide film of this embodiment must be able to withstand this temperature, so it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition onset temperature that are equal to or higher than the maximum temperature of the TFT fabrication process.

[0105] When manufacturing a TFT device using low-temperature polysilicon (LTPS), a process temperature of 380°C to 520°C is generally required, and the polyimide film of this embodiment must be able to withstand that temperature, so it is necessary to appropriately select a glass transition temperature and a thermal decomposition onset temperature that are equal to or higher than the maximum temperature of the TFT manufacturing process. On the other hand, due to the thermal history, the optical properties (particularly light transmittance, retardation property, and yellowness index) of the polyimide film tend to decrease as it is exposed to a high-temperature process. However, the polyimide obtained from the polyimide precursor of the present embodiment has good optical properties even after being subjected to the thermal history.

[0106] As examples of applications of the resin composition and polyimide film of the present embodiment, a display and a laminate, as well as methods for producing these, will be described below.

[0107] [Display and its manufacturing method] This embodiment also provides a flexible device including a polyimide film that is a cured product of the resin composition of this embodiment. A suitable example of the flexible device is a flexible display. In one embodiment, the polyimide film has excellent optical properties (e.g., Rth and / or yellowness). Therefore, in a preferred embodiment, the polyimide film is disposed in a location that is visible when the display is observed from the outside (specifically, the screen portion of the flexible display).

[0108] In this embodiment, A coating step of coating (preferably slit coating) the resin composition of the present embodiment on a surface of a support such as a glass substrate; a film-forming step of heating the resin composition to form a polyimide film; an element forming step of forming an element on the polyimide film; and a peeling step of peeling the polyimide film on which the elements are formed from the support.

[0109] [Manufacturing method for flexible OLED displays] FIG. 1 is a diagram showing the structure of a top-emission type flexible organic EL display as an example of a display provided in one embodiment of the present invention, above a polyimide substrate. The organic EL structure 25 in FIG. 1 is described as follows: for example, an organic EL element 250a emitting red light, an organic EL element 250b emitting green light, and an organic EL element 250c emitting blue light are arranged in a matrix as one unit, and a partition (bank) 251 defines the light-emitting region of each organic EL element. Each organic EL element is composed of a lower electrode (anode) 252, a hole transport layer 253, a light-emitting layer 254, and an upper electrode (cathode) 255. In addition, a TFT 256 (selected from low-temperature polysilicon (LTPS) and metal oxide semiconductor (IGZO, etc.)) for driving the organic EL element, an interlayer insulating film 258 having a contact hole 257, and a lower electrode 259 are provided on the lower layer 2a showing a CVD multi-layer film (multi-barrier layer) made of silicon nitride (SiN) or silicon oxide (SiO). The organic EL elements are sealed with a sealing substrate 2b, and a hollow portion 261 is formed between each organic EL element and the sealing substrate 2b.

[0110] The manufacturing process for a flexible organic EL display includes a step of preparing a polyimide film on a glass substrate support and preparing the organic EL substrate shown in FIG. 1 on top of it, a step of preparing a sealing substrate, an assembly step of bonding the two substrates together, and a peeling step of peeling the organic EL display prepared on the polyimide film from the glass substrate support. The organic EL substrate manufacturing process, the sealing substrate manufacturing process, and the assembly process may be performed using known manufacturing processes. Examples are given below, but are not limited to these. The peeling process may be the same as the peeling process of the polyimide film described above.

[0111] Referring to FIG. 1, for example, first, the polyimide film of the present disclosure is prepared on a glass substrate support by the above-mentioned method, and a multi-barrier layer (lower substrate 2a in FIG. 1) consisting of a multi-layer structure of silicon nitride (SiN) and silicon oxide (SiO) is prepared on the upper part by a CVD method or a sputtering method, and a metal wiring layer for driving a TFT is prepared on the upper part by using a photoresist or the like. An active buffer layer such as SiO is prepared on the upper part by a CVD method, and a TFT device (TFT 256 in FIG. 1) such as a metal oxide semiconductor (IGZO) or low temperature polysilicon (LTPS) is prepared on the upper part. After preparing a TFT substrate for a flexible display, an interlayer insulating film 258 having a contact hole 257 is formed by a photosensitive acrylic resin or the like. An ITO film is formed by a sputtering method or the like, and a lower electrode 259 is formed so as to be paired with the TFT.

[0112] Next, after forming a partition (bank) 251 with photosensitive polyimide or the like, a hole transport layer 253 and a light-emitting layer 254 are formed in each space partitioned by the partition. In addition, an upper electrode (cathode) 255 is formed so as to cover the light-emitting layer 254 and the partition (bank) 251. Thereafter, using a fine metal mask or the like as a mask, an organic EL material emitting red light (corresponding to the organic EL element 250a emitting red light in FIG. 1), an organic EL material emitting green light (corresponding to the organic EL element 250b emitting green light in FIG. 1), and an organic EL material emitting blue light (corresponding to the organic EL element 250c emitting blue light in FIG. 1) are deposited by a known method to prepare an organic EL substrate, which is sealed with a sealing film or the like (sealing substrate 2b in FIG. 1), and then the device above the polyimide substrate is peeled off from the glass substrate support by a known peeling method such as laser peeling, thereby preparing a top-emission type flexible organic EL display. When the polyimide of the present embodiment is used, a see-through type flexible organic EL display is prepared. Also, a bottom emission type flexible organic EL display may be produced by a known method.

[0113] [Manufacturing method for flexible LCD displays] A flexible liquid crystal display can be manufactured using the polyimide film of this embodiment. As a specific manufacturing method, the polyimide film of the present invention is manufactured on a glass substrate support by the above-mentioned method, and a TFT substrate made of, for example, amorphous silicon, metal oxide semiconductor (IGZO, etc.), or low-temperature polysilicon is manufactured by using the above-mentioned method. Separately, a polyimide film is manufactured on a glass substrate support according to the coating process and film formation process of this embodiment, and a color filter glass substrate (CF substrate) equipped with the polyimide film is manufactured using a color resist or the like according to a known method. A seal material made of a thermosetting epoxy resin or the like is applied by screen printing to one of the TFT substrate and the CF substrate in a frame-shaped pattern lacking a liquid crystal injection port, and spherical spacers made of plastic or silica having a diameter equivalent to the thickness of the liquid crystal layer are scattered on the other substrate.

[0114] Next, the TFT substrate and the CF substrate are attached to each other, and the sealing material is cured. Finally, the liquid crystal material is injected into the space surrounded by the TFT substrate, CF substrate, and sealing material by decompression, and then a thermosetting resin is applied to the liquid crystal injection port and the liquid crystal material is sealed by heating to form a liquid crystal layer. Finally, the glass substrate on the CF side and the glass substrate on the TFT side are peeled off at the interface between the polyimide film and the glass substrate by a laser peeling method or the like to produce a flexible liquid crystal display.

[0115] [Method of manufacturing laminate] In this embodiment, A coating step of coating the resin composition of the present embodiment on a surface of a support; a film-forming step of heating the resin composition to form a polyimide film; and an element forming step of forming an element on the polyimide film.

[0116] The element in the laminate may be one exemplified as the flexible device (e.g., flexible display). For example, a glass substrate is used as the support. The preferred specific procedures for the coating step and the film forming step are the same as those described above with respect to the above-mentioned method for producing a polyimide film. In the element forming step, the above-mentioned element is formed on a polyimide film as a flexible substrate formed on a support. Thereafter, the polyimide film and the element may be peeled off from the support in a peeling step, if desired. EXAMPLES

[0117] The present invention will be described in more detail below with reference to examples, but these are described for the purpose of illustration only and the scope of the present invention is not limited to the following examples. Various evaluations in the examples and comparative examples were carried out as follows.

[0118] <Weight average molecular weight> The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by gel permeation chromatography (GPC) under the following conditions.

[0119] The solvent used was NMP (Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography, dissolved by adding 24.8 mmol / L lithium bromide monohydrate (Wako Pure Chemical Industries, Ltd., purity 99.5%) and 63.2 mmol / L phosphoric acid (Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography) just before measurement). A calibration curve for calculating the weight average molecular weight was prepared using standard polystyrene (Tosoh Corporation). Column: Shodex KD-806M (Showa Denko) Flow rate: 1.0mL / min Column temperature: 40℃ Pump: PU-2080Plus (JASCO) Detector: RI-2031Plus (RI: differential refractometer, manufactured by JASCO) and UV-2075Plus (UV-VIS: ultraviolet-visible spectrometer, manufactured by JASCO)

[0120] <Shear rate dependency (TI) evaluation> The viscosity of the resin compositions prepared in the examples and comparative examples was measured at 23°C using a temperature-controlled viscometer (TVE-35H manufactured by Toki Sangyo Kikai Co., Ltd.) at a rotation speed and cone rotor at which the viscosity of the resin composition to be measured could be measured, and a shear rate dependency evaluation was performed. Specifically, the viscosity ηa (mPa s) at the measurement rotation speed a (rpm) and the viscosity ηb (mPa s) at the measurement rotation speed b (rpm) were measured (where a*10=b), and the TI expressed by the following formula was calculated. TI=ηa / ηb Specific examples of measurable rotational speeds are, for example, 0.5, 1, 2.5, 5, 10, 20, 50, and 100 rpm. Specific examples of measurable cone rotors are, for example, 1°34' (cone rotor angle) x R24 (cone rotor diameter), 1°34' x R12, 0.8° x R24, 0.8° x R12, 3° x R24, 3° x R12, 3° x R17.65, 3° x R14, 3° x R12, and 3° x R9.7.

[0121] <Coating evaluation> The resin compositions prepared in the examples and comparative examples were applied to a 300 mm x 300 mm glass substrate with a coating area of ​​295 mm x 295 mm using a slit coater (manufactured by SCREEN Finetech Solutions Co., Ltd.), and coating evaluation was performed.

[0122] (Slit nozzle evaluation) The resin compositions (varnishes) prepared in the Examples and Comparative Examples were filled into the nozzle of a slit coater, and evaluated according to the following criteria, with the results shown in the table. After starting to dispense varnish from the nozzle and stopping the dispense, varnish drips from the slit nozzle: Liquid leakage No varnish coming out of the nozzle: Clogged Coating can be done without leakage or clogging: No problems

[0123] (Court Gap) The resin compositions (varnishes) prepared in the examples and comparative examples were coated (coating speed 100 mm / sec) on a glass substrate so that the film thickness after imidization (heating at 100°C for 1 hour and then at 400°C for 30 minutes at an oxygen concentration of 10 mass ppm or less) was 10 μm. The coat gap setting value of the slit coater at that time is shown in the table.

[0124] (Edge Evaluation) The resin compositions prepared in the Examples and Comparative Examples were coated onto a glass substrate, transferred to a drying furnace and heated at 100°C for 1 hour, and then the edges of the coating were observed at 10x magnification using an optical microscope and evaluated according to the following criteria. In addition, the edge bead (protrusion at the edge) of the coating film was measured using a stylus step gauge (P-15: manufactured by KLA Tencor) and evaluated according to the following criteria. When observing the edge with a microscope, dripping of 0.5 mm or more is observed: Dripping When measuring the thickness of the edge of the bead, the thickness is 30% or more of the coating thickness: Bead No sagging or edge abnormalities: No problem

[0125] (Slit coating possible) The (slit nozzle evaluation), (coat gap) and (edge ​​evaluation) were evaluated according to the following criteria and the results are shown in the table. In the compositions using the polyimide precursors having the predetermined weight average molecular weights in the Examples and Comparative Examples, at least one of the solid contents in the range of 7 to 28 mass % met all of the following evaluation results: In the compositions using polyimide precursors having a predetermined weight average molecular weight in each of the Examples and Comparative Examples, when the solid content is in the range of 7 to 28% by mass, none of the following evaluation results are satisfied: Slit nozzle evaluation: No problem Coat gap: 50μm or more Edge rating: No problem

[0126] <Cured film thickness uniformity (standard deviation)> In the above <Coating Evaluation> (Coat Gap), the polyimide films according to the Examples and Comparative Examples prepared on the glass substrate (i.e., polyimide films formed on a 300mm*300mm glass substrate with a size of 295mm*295mm) were used. Using the glass substrate on which the polyimide film was formed, the film thickness was measured at positions spaced 20mm apart from the center of the coating surface toward the end faces of MD (i.e., the slit coating direction) and TD (the direction perpendicular to MD) (therefore, the very end was located 7.5mm from the end face) (15 points in MD and 15 points in TD, a total of 30 points). A contact step gauge was used to measure the film thickness. From the results, the film thickness uniformity of the polyimide film (standard deviation of the film thickness at 30 points) was calculated and evaluated according to the following criteria. Good: In-plane thickness uniformity (3 sigma) is 1.0 μm or less Acceptable: In-plane thickness uniformity (3 sigma) is greater than 1.0 μm and less than 2.0 μm Poor: In-plane thickness uniformity (3 sigma) exceeds 2.0 μm

[0127] <Cured film elongation> The resin compositions prepared in the examples and comparative examples were spin-coated on a 6-inch silicon wafer substrate having an aluminum deposition layer on its surface so that the film thickness after curing was 10 μm, and the substrate was pre-baked at 100° C. for 6 minutes. Thereafter, a vertical curing furnace (manufactured by Koyo Lindberg Co., Ltd., model name VF-2000B) was used to adjust the oxygen concentration in the chamber to 10 mass ppm or less, and a heat curing treatment was performed at 400° C. for 30 minutes to produce a wafer on which a polyimide film was formed. Next, a dicing saw (manufactured by Disco Corporation, DAD 3350) was used to make a 3 mm-wide cut in the polyimide film of the wafer, and the film piece was immersed in a dilute hydrochloric acid aqueous solution overnight to peel off and dry. This was cut to a length of 50 mm to prepare a sample.

[0128] The elongation of the above samples was measured using a TENSILON (UTM-II-20 manufactured by Orientec Co., Ltd.) at a test speed of 40 mm / min and an initial load of 0.5 fs. The results were evaluated according to the following criteria and shown in the table. Excellent: 40% or more Good: 20% or more, less than 40% Acceptable: Less than 20%

[0129] <Haze of hardened film> In the above <Coating Evaluation> (Coat Gap), the polyimide films according to the Examples and Comparative Examples prepared on a glass substrate were used.

[0130] The haze (converted to a film thickness of 10 μm) of the obtained sample was measured in accordance with the JIS K7105 transparency test method using a SC-3H haze meter manufactured by Suga Test Instruments Co., Ltd. The measurement results were evaluated according to the following criteria and are shown in the table. Excellent: Haze is 0.5 or less Good: Haze is greater than 0.5 and less than 1.5 Acceptable: Haze is greater than 1.5

[0131] <Cured film yellowness (YI)> The polyimide films according to the examples and comparative examples prepared on glass substrates in the above <Coating Evaluation> (Coat Gap) were used. The yellowness index (YI) value (10 μm film thickness equivalent) of the obtained samples was measured using a D65 light source with a Spectrophotometer: SE600 manufactured by Nippon Denshoku Industries Co., Ltd. The results are shown in the table.

[0132] <Cured film Rth (retardation, thickness direction retardation)> The polyimide films according to the examples and comparative examples prepared on the glass substrate in the above <Coating Evaluation> (Coat Gap) were used. The Rth (converted to a film thickness of 10 μm) of the obtained samples was measured using a retardation birefringence measuring device (KOBRA-WR, manufactured by Oji Scientific Instruments). The wavelength of the measuring light was 589 nm. The results are shown in the table.

[0133] <Comparative Example 1-1> In a 3L separable flask with a stirring rod, NMP (812g) was added while introducing nitrogen gas, and 4,4'-DAS (4,4'-diaminodiphenylsulfone) (14.2g), TFMB (12.2g), and methylphenyl silicone oil (10.56g) modified with amines at both ends were added as diamines while stirring, followed by PMDA (15.3g) and BPDA (8.8g) as acid dianhydrides (molar ratio of acid dianhydride and diamine (100:98)). Next, the mixture was heated to 80°C using an oil bath and stirred for 4 hours, after which the oil bath was removed and the mixture was returned to room temperature to obtain a transparent NMP solution of polyamic acid (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set at -20°C, the same below), and was thawed and used for evaluation.

[0134] <Comparative Examples 1-2 to 1-6> The same procedure as in Comparative Example 1-1 was repeated, except that the amount of NMP was changed to obtain the solid content shown in Table 1.

[0135] <Example 1-1> Into a 3 L separable flask equipped with a stirring bar, 4,4'-DAS (15.3 g) and TFMB (12.4 g) as diamines, and a polymerization solvent (NMP) in an amount twice the total mass of these diamines were added while introducing nitrogen gas. Next, a dropping funnel was set on the separable flask, and while introducing nitrogen gas into the dropping funnel, PMDA (15.3 g) and BPDA (8.8 g) as acid dianhydrides and a polymerization solvent (NMP) of twice the mass of these acid dianhydrides were added. Then, the mixture was stirred with a small stirring blade at room temperature. Next, set another dropping funnel on the separable flask, and while introducing nitrogen gas into the dropping funnel, add the methylphenyl silicone oil X-22-1660B-3 (10.56 g) modified with amines at both ends as diamine and the polymerization solvent (NMP) of twice the mass of the silicone oil.Then, stir with a small stirring blade at room temperature. Then, while stirring the diamine solution in the separable flask, the acid dianhydride solution and silicone oil were simultaneously added dropwise at room temperature while stirring with the small stirring blade of the dropping funnel. The dropping was performed at a low speed for more than 30 minutes. After the dropping, the solution was washed with a washing solvent (NMP), and the remaining matter was dropped (molar ratio of acid dianhydride to diamine (100:99)). After that, an additional solvent (NMP) was added to obtain the final solid content shown in Table 1. The mixture was then stirred at room temperature for 30 minutes, and then heated to 70°C using an oil bath and stirred for 4 hours. The oil bath was then removed and the mixture was returned to room temperature to obtain a transparent NMP solution of polyamic acid (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set at -20°C, the same applies below), and was thawed before use when evaluating.

[0136] <Examples 1-2 to 1-17, 2-1 to 2-14, 3-1 to 3-16, 4-1 to 4-12> The formulation of the acid dianhydride and diamine was as shown in Tables 1 to 4, and the amount of the polymerization solvent used was changed accordingly (i.e., adjusted to twice the mass of the acid dianhydride or diamine). Furthermore, for Examples 1-5 to 1-8, 2-5 to 2-14, 3-3 to 3-16, and 4-5 to 4-12, "heated to 70 ° C. and stirred for 4 hours" was changed to "heated to 40 ° C. and stirred for 12 hours", and for Examples 1-9, 2-9, 3-9, and 4-9, "additional solvent (NMP)" was changed to "additional solvent (NMP and GBL) (adjusted so that NMP / GBL after addition is 100 / 100 (w / w))". Other than that, it was the same as Example 1-1. The solid content shown in Tables 1 to 4 was adjusted to the value shown in the table by changing the amount of the additional solvent. In Examples 1-16, 2-12, 2-13, 3-14, 3-15, 4-10, and 4-11, the reaction time was further extended after "stirring for 12 hours", but when the weight average molecular weight was measured, it did not increase compared to after stirring for 12 hours.

[0137] <Comparative Examples 2-1 to 2-6, 3-1 to 3-6, 4-1 to 4-7> Comparative Examples 2-1, 3-1, and 4-1 were carried out in the same manner as Comparative Example 1-1, except that the amount of NMP in Comparative Example 1-1 was changed to 745 g (Comparative Example 2-1), 799 g (Comparative Example 3-1), and 850 g (Comparative Example 4-1), and the mixture of acid dianhydride and diamine was as shown in Table 2. In addition, Comparative Examples 2-2 to 2-6 were carried out in the same manner as Comparative Example 2-1, Comparative Examples 3-2 to 3-6 were carried out in the same manner as Comparative Example 3-1, and Comparative Examples 4-2 to 4-7 were carried out in the same manner as Comparative Example 4-1, except that the amount of NMP was changed to the solid content in Tables 2 to 4.

[0138] <Comparative Example 5-1> In a 3L separable flask equipped with a stirring bar, add NMP (620 g) while introducing nitrogen gas. Then, 4,4'-DAS (24.8 g) was added as a diamine while stirring, followed by PMDA (21.8 g) as an acid dianhydride (molar ratio of acid dianhydride to diamine (100:100)). Next, the temperature was raised to 80°C using an oil bath and stirred for 4 hours, after which the oil bath was removed and the temperature was returned to room temperature to obtain a transparent NMP solution of polyamic acid (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer and was thawed before use for evaluation.

[0139] <Comparative Examples 5-2 to 5-6> The same procedure as in Comparative Example 5-1 was repeated, except that the amount of NMP was changed to obtain the solids content shown in Table 5.

[0140] <Example 5-1> Into a 3 L separable flask equipped with a stirring bar, 4,4'-DAS (24.3 g) as a diamine and NMP in an amount of twice the total mass of the diamine were added while introducing nitrogen gas. Next, a dropping funnel was set on the separable flask, and while introducing nitrogen gas into the dropping funnel, PMDA (10.9 g), BPDA (14.7 g), and NMP in an amount twice the mass of the acid dianhydrides were added. Then, the mixture was stirred with a small stirring blade at room temperature. Then, while stirring the diamine solution in the separable flask, the acid dianhydride solution was added dropwise at room temperature while stirring with the small stirring blade of the dropping funnel. The dropping was performed at a slow speed and took 30 minutes or more. After the dropping, the solution was washed with a washing solvent (NMP), and the remaining matter was dropped (molar ratio of acid dianhydride to diamine (100:98)). After that, additional solvent (NMP) was added to obtain the final solid content shown in Table 5. The mixture was then stirred at room temperature for 30 minutes, and then heated to 70°C using an oil bath and stirred for 4 hours. The oil bath was then removed and the mixture was returned to room temperature to obtain a transparent NMP solution of polyamic acid (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set at -20°C, the same applies below), and was thawed before use when evaluating.

[0141] <Examples 5-2 to 5-9, 6-1 to 6-9, 7-1 to 7-4, 8-1, and 8-2> The formulation of the acid dianhydride and diamine was as shown in Tables 5 to 9, and the amount of the polymerization solvent used was changed accordingly (i.e., adjusted to twice the mass of the acid dianhydride or diamine), and further, for Examples 5-3 to 5-9, 6-5 to 6-9, 7-4, 8-1, and 8-2, the above "heated to 70 ° C. and stirred for 4 hours" was changed to "heated to 40 ° C. and stirred for 12 hours", and for Examples 5-7, 6-4, and 7-4, "additional solvent (NMP)" was changed to "additional solvent (NMP and GBL) (adjusted so that NMP / GBL after addition is 100 / 100 (w / w))". Other than that, it was the same as Example 5-1. The solid content shown in Tables 5 to 9 was adjusted to the value shown in the table by changing the amount of the above-mentioned additional solvent. In Examples 5-8, 5-9, and 6-6 to 6-9, the reaction time was further extended after "stirring for 12 hours", but when the weight average molecular weight was measured, it did not increase compared to after stirring for 12 hours.

[0142] <Comparative Examples 6-1 to 6-6, 7-1 to 7-8, 8-1 to 8-2> Comparative Examples 6-1, 7-1, 8-1 to 8-2 were carried out in the same manner as Comparative Example 5-1, except that the amount of NMP in Comparative Example 5-1 was changed to 664g (Comparative Example 6-1), 718g (Comparative Example 7-1), 401g (Comparative Example 8-1), and 344g (Comparative Example 8-2), respectively, and the mixture of the acid dianhydride and the diamine was as shown in Tables 6 to 8. Comparative Examples 6-2 to 6-6 were carried out in the same manner as Comparative Example 6-1, except that the amount of NMP was changed to the solid content in Table 6, and Comparative Examples 7-2 to 7-6 were carried out in the same manner as Comparative Example 7-1, except that the amount of NMP was changed to the solid content in Table 7. Comparative Examples 7-7 and 7-8 were carried out in the same manner as Comparative Example 7-1, except that the amount of NMP was changed from 718g to 215g (Comparative Example 7-7) and 163g (Comparative Example 7-8), respectively, the mixture of the acid dianhydride and the diamine was as shown in Table 7, and "4 hours stirring" was changed to "3 hours stirring".

[0143] <Comparative Example 9-1> In a 3L separable flask with a stirring rod, NMP (495 g) was added while introducing nitrogen gas, and TFMB (30.9 g) was added as a diamine while stirring, followed by BPAF (9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride) (45.8 g) as an acid dianhydride, and X-22-1660B-3 (10.56 g) as methylphenyl silicone oil modified with amines at both ends (molar ratio of acid dianhydride and diamine (100:99)). Next, the temperature was raised to 80 ° C. using an oil bath and stirred for 4 hours, after which the oil bath was removed and the temperature was returned to room temperature to obtain a transparent NMP solution of polyamic acid (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer, and was thawed and used when evaluating.

[0144] <Comparative Examples 9-2 to 9-3> The same procedure as in Comparative Example 9-1 was repeated, except that the amount of NMP was changed from 495 g to 438 g (Comparative Example 9-2) and 374 g (Comparative Example 9-3), and the composition of the acid dianhydride and diamine was as shown in Table 9.

[0145] <Example 9-1> Into a 3 L separable flask equipped with a stirring bar, TFMB (31.3 g) as a diamine and NMP (63 g) in an amount twice the total mass of the diamine were added while introducing nitrogen gas. Next, a dropping funnel was set on the separable flask, and BPAF (45.8 g) and NMP (92 g) were added as an acid dianhydride while introducing nitrogen gas into the dropping funnel. Then, the mixture was stirred with a small stirring blade at room temperature. Next, another dropping funnel was set on the separable flask, and while introducing nitrogen gas into the dropping funnel, both ends amine-modified methylphenyl silicone oil X-22-1660B-3 (10.56 g) and NMP (21 g) of twice the mass of the silicone oil were added. Then, the mixture was stirred with a small stirring blade at room temperature. Then, while stirring the diamine solution in the separable flask, the acid dianhydride solution was added dropwise at room temperature while stirring with the small stirring blade of the dropping funnel. The dropping was performed at a slow speed and took 30 minutes or more. After the dropping, the solution was washed with a washing solvent (NMP), and the remaining matter was dropped (molar ratio of acid dianhydride to diamine (100:100)). Additional solvent (NMP) was then added to achieve the final solids content in Table 9. The mixture was then stirred at room temperature for 30 minutes, and then heated to 40°C using an oil bath and stirred for 12 hours. The oil bath was then removed and the temperature was returned to room temperature to obtain a transparent NMP solution of polyamic acid (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set at -20°C, the same applies below), and was thawed before use when evaluating.

[0146] <Examples 9-2 and 9-3> The same procedure as in Example 9-1 was carried out except that the amount of the polymerization solvent used was changed accordingly (i.e., adjusted to twice the mass of the acid dianhydride or diamine) and the mixture of the acid dianhydride and diamine was as shown in Table 9. The solid content shown in Table 9 was adjusted to the value shown in the table by changing the amount of the additional solvent.

[0147] <Example 10-1> In a 3L separable flask with a stirring rod, NMP (246g) was added while introducing nitrogen gas, and 4,4'-DAS (14.4g), TFMB (12.4g), and methylphenyl silicone oil (10.56g) modified with amines at both ends were added as diamines while stirring, followed by PMDA (15.3g) and BPDA (8.8g) as acid dianhydrides (molar ratio of acid dianhydride and diamine (100:99)). Next, the mixture was heated to 70°C using an oil bath and stirred for 8 hours, after which the oil bath was removed and the mixture was returned to room temperature to obtain a transparent NMP solution of polyamic acid. The obtained varnish was stored in a freezer (set at -20°C, the same below) and was thawed and used for evaluation.

[0148] <Examples 10-2 to 10-5> The same procedure as in Example 10-1 was repeated, except that the amount of NMP was changed from 246 g to 225 g (Example 10-2), 242 g (Example 10-3), 185 g (Example 10-4), and 201 g (Example 10-5), and the composition of the acid dianhydride and diamine was as shown in Table 10. The evaluation results are shown in Table 10.

[0149] [Table 1]

[0150] [Table 2]

[0151] [Table 3]

[0152] [Table 4]

[0153] [Table 5]

[0154] [Table 6]

[0155] [Table 7]

[0156] [Table 8]

[0157] [Table 9]

[0158] [Table 10] [Industrial Applicability]

[0159] The resin composition of the present disclosure can be suitably applied to applications such as flexible devices (e.g., flexible substrates), particularly flexible displays. For example, the resin composition of the present disclosure can be suitably used to form transparent substrates for display devices such as liquid crystal displays, organic electroluminescence displays, field emission displays, and electronic paper. More specifically, the resin composition of the present disclosure can be used to form substrates for thin film transistors (TFTs), substrates for color filters, substrates for transparent conductive films (ITO, Indium Thin Oxide), and the like. [Explanation of symbols]

[0160] 2a Bottom Board 2b Sealing substrate 25 Organic EL structure 250a Red light emitting organic EL element 250b Green light-emitting organic electroluminescence element 250c Blue light emitting organic electroluminescence element 251 Partition (bank) 252 Lower electrode (anode) 253 Hole transport layer 254 Light-emitting layer 255 Upper electrode (cathode) 256 TFT 257 Contact Hole 258 Interlayer insulating film 259 Lower Electrode 261 Hollow part

Claims

1. The following formula (1): 【Chemistry 1】 {In the formula, R 1 When there are a plurality of R, each independently represents a divalent organic group; 2 each independently represents a tetravalent organic group, and n is a positive integer.} and a solvent (excluding solvents containing 70 mass% or more of a non-amide solvent relative to 100 mass% of the total solvent). A resin composition comprising: The polyimide precursor is represented by the following formula (3): 【Chemistry 2】 {In the formula, R 3 and R 4 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m is an integer of 1 to 200. The weight average molecular weight of the polyimide precursor is 150,000 to 250,000; The solid content of the resin composition is 10 to 25% by mass, The viscosity of the resin composition was measured at 23° C. using a temperature-adjusted viscometer, and the viscosity was calculated based on the following formula: TI=ηa / ηb {In the formula, ηa (mPa·s) is the viscosity of the resin composition at a measured rotation speed a (rpm), and ηb (mPa·s) is the viscosity of the resin composition at a measured rotation speed b (rpm), where a*10=b.} The resin composition has a shear rate dependency (TI) of 0.9 to 1.

1.

2. The resin composition according to claim 1 , wherein the polyimide precursor is a copolymer of a tetracarboxylic dianhydride including pyromellitic dianhydride and a diamine.

3. 3. The resin composition according to claim 1, wherein the polyimide precursor is a copolymer of a tetracarboxylic dianhydride, including 3,3',4,4'-biphenyltetracarboxylic dianhydride, and a diamine.

4. The resin composition according to any one of claims 1 to 3, wherein the resin composition is a resin composition for slit coating.

5. R in the formula (1) 1 At least one of the following formula (2): 【Chemistry 3】 The resin composition according to any one of claims 1 to 4, wherein the group is represented by:

6. The polyimide precursor is a copolymer of a tetracarboxylic dianhydride and one or more diamines selected from the group consisting of 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 2,2'-bis(trifluoromethyl)benzidine and 9,9-bis(4-aminophenyl)fluorene. The resin composition according to any one of claims 1 to 5.

7. The resin composition according to any one of claims 1 to 6, wherein the polyimide precursor has a weight average molecular weight of 160,000 to 220,000.

8. The resin composition according to any one of claims 1 to 7, wherein the resin composition is a resin composition for flexible devices.

9. The resin composition according to any one of claims 1 to 8, wherein the resin composition is a resin composition for a flexible display.

10. A polyimide film which is a cured product of the resin composition according to any one of claims 1 to 9.

11. 11. The polyimide film according to claim 10, which has a thickness direction retardation (Rth) of 300 or less in terms of a 10 μm film thickness and / or a yellowness index (YI) of 20 or less in terms of a 10 μm film thickness.

12. A flexible device comprising the polyimide film according to claim 10 or 11.

13. A flexible display comprising the polyimide film according to claim 10 or 11.

14. The flexible display according to claim 13 , wherein the polyimide film is disposed at a location that is visible when the flexible display is observed from the outside.

15. A coating step of coating the resin composition according to any one of claims 1 to 9 on a surface of a support; a film-forming step of heating the resin composition to form a polyimide film; and a peeling step of peeling the polyimide film from the support.

16. The method for producing a polyimide film according to claim 15 , wherein the coating step includes slit coating the resin composition.

17. R in the formula (1) 1 At least one of the following formula (2): 【Chemistry 4】 The method for producing a polyimide film according to claim 15 or 16, wherein the group is represented by the formula:

18. The method for producing a polyimide film according to any one of claims 15 to 17, further comprising, prior to the peeling step, an irradiation step of irradiating the polyimide film with a laser from the support side.

19. A coating step of coating the resin composition according to any one of claims 1 to 9 on a surface of a support; a film-forming step of heating the resin composition to form a polyimide film; an element forming step of forming an element on the polyimide film; and peeling the polyimide film on which the elements are formed from the support.

20. The method for manufacturing a display according to claim 19 , wherein the applying step includes slit coating the resin composition.

21. The method for manufacturing a display according to claim 19 or 20, wherein the polyimide film is disposed at a position that is visible when the display is observed from the outside.

Citation Information

Patent Citations

  • Radiation-sensitive polymer composition, insulation film, and organic el element

    JP2014074772A

  • Radiation-sensitive resin composition, insulating film, method of forming the same, and organic el element

    JP2015052770A

  • Flexible color filter, manufacturing method for the same, and flexible light-emitting device having the same

    JP2015072365A

  • Polyimide precursor film layer / inorganic substrate laminate, method for manufacturing the same, method for manufacturing polyimide film layer / inorganic substrate laminate, and method for manufacturing flexible electronic device

    JP2015202675A

  • Glass film laminate

    JP2016037048A