Nano-barium titanate microcrystals and method for producing same, barium titanate powder and method for producing same
The rapid mixing and atmospheric pressure hydrothermal synthesis of nano barium titanate microcrystals address the challenges of particle size and uniformity, resulting in high-purity barium titanate powder suitable for industrial production.
Patent Information
- Application Number
- JP2021564091
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-25
- Filing Date
- 2019-08-14
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2039-08-14
AI Technical Summary
Existing methods for producing nano-barium titanate powder face challenges such as particle agglomeration, large particle size, poor uniformity, high impurity content, and high production costs, particularly in atmospheric pressure hydrothermal methods, which are difficult to scale up for industrial use.
A method involving rapid mixing of a highly concentrated nano-titanium dioxide aqueous dispersion with barium hydroxide at a lower temperature, followed by atmospheric pressure hydrothermal synthesis, to produce nano barium titanate microcrystals with small particle size, uniform distribution, and high purity, suitable for large-scale continuous production.
The method achieves nano barium titanate microcrystals with average particle sizes of 10-30 nm, uniform distribution, and high purity, enabling the production of high-quality barium titanate powder with improved dispersibility and reduced energy consumption, suitable for industrial applications.
Smart Images

Figure 0007564823000005 
Figure 0007564823000006 
Figure 0007564823000007
Abstract
Description
[Technical field]
[0001] The present invention relates to nanomaterial technology, and in particular to nano-barium titanate microcrystals and a manufacturing method thereof, and barium titanate powder and a manufacturing method thereof. [Background technology]
[0002] Barium titanate (BaTiO3) has good dielectric, ferroelectric and piezoelectric properties, and is widely used in the electronic ceramic industry as a basic material for manufacturing electronic components such as multilayer ceramic capacitors (MLCC), positive temperature coefficient thermistors (PTC), and dynamic random access memories (DRAM).
[0003] At present, the mainstream process for producing nano barium titanate powder can be broadly divided into solid-phase sintering and liquid-phase synthesis, where the liquid-phase synthesis can be further divided into sol-gel, co-precipitation, hydrothermal, etc. In the solid-phase sintering method, the oxides or acid salts of the metal elements (Ti and Ba) that compose barium titanate are mixed, finely ground, and then calcined at a high temperature of about 1100°C to form the required powder through a solid-phase reaction. Although the process of the solid-phase sintering method is relatively simple, the obtained powder is prone to particle aggregation, has a large particle size, a high content of impurities, and poor material uniformity, making it difficult to meet the demand for high performance and miniaturization of electronic components. The powder obtained by the sol-gel and co-precipitation methods has high purity and small particle size, but the complicated process, high raw material costs, and difficult industrial production.
[0004] The hydrothermal method can be further divided into high pressure hydrothermal method and normal pressure hydrothermal method. The high pressure hydrothermal method is to obtain barium titanate powder by hydrothermally treating Ba(OH)2 aqueous solution containing dispersed TiO2 fine particles in a closed system such as a high pressure reaction vessel at a certain temperature and water autogenous pressure. Under high temperature and high pressure hydrothermal conditions, a special physicochemical environment that cannot be obtained under normal pressure conditions can be provided, so that the precursor is fully dissolved in the reaction system and reaches a certain degree of supersaturation, which leads to nucleation and crystallization to produce powder or nanocrystals. Therefore, the barium titanate powder obtained by the high pressure hydrothermal method has the advantages of high purity, high crystallinity, small particle size, uniform particle distribution, and ensures that the raw materials are environmentally friendly. However, the hydrothermal reaction is carried out under high temperature, high pressure, and closed conditions, which not only increases the energy consumption of the reaction process and has a low safety factor, but can only be produced in batches and cannot be continuously produced on a large scale. In addition, the reaction is carried out under alkaline conditions and high temperature and high pressure environments, which makes the requirements for the reaction vessel even stricter, and the costs of equipment input and operation requirements are high.
[0005] The atmospheric pressure hydrothermal method generally uses titanium metal organic compounds such as tetrabutyl titanate as the titanium source, barium hydroxide as the barium source, and alcoholic substances such as n-butanol as the solvent, and simultaneously converts the titanium source and produces barium titanate in the reaction system. The atmospheric pressure hydrothermal method is carried out at atmospheric pressure and a low temperature of 50-110°C, so the requirements for equipment are simple and safe, and industrialization is relatively easy and has already matured. However, in previous research, the barium titanate produced by the atmospheric pressure hydrothermal method has a large particle size, generally above 100 nm, and the particle size distribution is not concentrated and the dispersibility is poor, making it difficult to meet the high-quality demand for barium titanate in the electronic ceramic industry.
[0006] Therefore, it is currently a problem to be solved to develop a production process for nano-barium titanate microcrystals based on atmospheric pressure hydrothermal method, obtain high quality barium titanate powder, and have higher production efficiency. Summary of the Invention [Problem to be solved by the invention]
[0007] In response to the above-mentioned deficiencies in existing technology, the present invention provides a method for producing nano-barium titanate microcrystals. Based on an atmospheric pressure hydrothermal synthesis process, the produced nano-barium titanate microcrystals have the characteristics of small particle size, uniform particle size distribution, and high purity, and have a very high yield, and can be used as a raw material for high-quality barium titanate powder.
[0008] The present invention further provides nano-barium titanate microcrystals produced using the above-mentioned production method, which have the characteristics of small particle size, uniform particle size distribution, and high purity, and can be used as a raw material for producing high-quality barium titanate powder.
[0009] The present invention provides a method for producing barium titanate powder using the above-mentioned nano-barium titanate microcrystals as raw material, and can produce nano-barium titanate powder with high purity, good crystallinity and dispersibility, and small particle size, with a very high yield.
[0010] The present invention further provides a barium titanate powder produced by the above-mentioned production method, which has the characteristics of small and controllable particle size, high purity, good crystallinity and dispersibility, and has a very high yield. [Means for solving the problem]
[0011] In order to achieve the above object, the present invention provides a method for producing nano barium titanate microcrystals, the method comprising the steps of: A nano-titanium dioxide aqueous dispersion at a lower temperature is rapidly mixed with a barium hydroxide aqueous solution at a higher temperature, and the temperature of the resulting mixture is lowered by at least 2°C compared to the temperature of the barium hydroxide aqueous solution by high-speed mixing of the two, wherein the mass concentration of the nano-titanium dioxide aqueous dispersion is 20% or more; In an inert atmosphere, the mixture is subjected to a hydrothermal synthesis reaction at normal pressure at 90 to 110°C, and the reaction product is collected, washed and dried to obtain nano-barium titanate microcrystals.
[0012] At present, when using atmospheric pressure hydrothermal synthesis to produce nano-barium titanate powder, if the concentration of TiO2 as the titanium source is high, the nano-barium titanate powder will have a large particle size, the particle size distribution will not be concentrated, and the aggregation phenomenon between particles will be very serious; however, if the concentration of TiO2 is too low, not only will the production efficiency decrease, but the particle size of the barium titanate particles will also be large. In response to this situation, the present invention provides a solution by using a high-concentration (mass concentration ≧20%) nano-titanium dioxide aqueous dispersion as raw material, first rapidly mixing the nano-titanium dioxide aqueous dispersion with a barium hydroxide aqueous solution, and then carrying out atmospheric pressure hydrothermal synthesis, thereby reducing the amount of solvent in the atmospheric pressure hydrothermal synthesis reaction process, improving production efficiency, and not only realizing large-scale continuous production, but also having the advantages of small particle size, uniformity and high purity in the obtained nano-barium titanate microcrystal particles. By using the nano-barium titanate microcrystals as raw material, barium titanate powder with better crystal growth can be obtained through calcination or other means, and the barium titanate powder also has the characteristics of small particle size, uniform particle size distribution, high purity and good dispersibility.
[0013] The rapid mixing between the nano-titanium dioxide aqueous dispersion and the barium hydroxide aqueous solution, or the rapid mixing between the titanium source and the barium source, is realized by the degree of temperature drop of the mixed system, that is, by the obvious temperature drop caused directly by the rapid mixing of the two, and does not include the obvious temperature drop caused by means such as external cooling during the mixing process. In general industrial production, the rapid mixing of the two is performed by heating the heating equipment, but the amount of titanium dioxide aqueous dispersion at low temperature is large and the addition speed is fast, so the heating equipment is not sufficient to maintain the rapid temperature rise of the system, and the temperature of the mixed system is at least 2°C lower than the temperature of the barium hydroxide aqueous solution before mixing. In the specific implementation process of the present invention, monitoring the temperature of the mixed system to drop by 2°C or more during the mixing process represents the realization of the so-called "rapid mixing". For example, the temperature of the barium hydroxide aqueous solution mixed system is significantly lowered by rapidly adding the nano-titanium dioxide aqueous dispersion to the barium hydroxide aqueous solution, and it is considered that the "rapid mixing" of the two is achieved when the temperature drops by 2°C or more.
[0014] Of course, in order to ensure the consistency of the growth size of the subsequent barium titanate particles, the raw material addition or mixing speed should ensure that the temperature of the entire mixed solution is quickly balanced and stable. In actual industrial production, high-efficiency mixing equipment and high-speed liquid addition equipment are generally used, or online continuous mixing equipment is used to rapidly and uniformly mix the nano titanium dioxide aqueous dispersion with the barium hydroxide aqueous solution. In the rapid mixing process, generally, several representative monitoring points are selected to test the temperature change during the mixing process, and it is appropriate that the temperature at each monitoring point decreases by more than 2°C, and the decrease range is basically the same.
[0015] In addition, in order to ensure the consistency of the growth size of the subsequent barium titanate particles, the temperature difference between the mixed system and the barium hydroxide aqueous solution should not be too large, and is generally controlled to 2-20°C, usually 2-10°C. In this way, the precipitation of the barium source due to a sudden drop in temperature can also be effectively avoided.
[0016] The preparation of the above mixture can be carried out under air environment. Of course, in order to further prevent the occurrence of side reactions, the preparation of the mixture can also be carried out under an inert atmosphere, for example, under protection of an inert gas such as nitrogen or argon.
[0017] Specifically, the above-mentioned mixed system can be prepared by adding a nano-titanium dioxide aqueous dispersion to a barium hydroxide aqueous solution, by adding a barium hydroxide aqueous solution to a nano-titanium dioxide aqueous dispersion, or by mixing the nano-titanium dioxide aqueous dispersion with a barium hydroxide aqueous solution in a parallel flow manner.
[0018] In a preferred embodiment of the present invention, a nano-titanium dioxide aqueous dispersion at a lower temperature is added to a barium hydroxide aqueous solution at a higher temperature and mixed rapidly, and the temperature of the resulting mixture is lower than the temperature of the barium hydroxide aqueous solution by at least 2° C., for example, 2 to 20° C., and further for example, 2 to 10° C. By preparing the mixture in this manner, the requirements for the process and equipment are low and it is easier to realize, regardless of the introduction and transportation of the high-temperature barium hydroxide aqueous solution.
[0019] It is understandable that the nano-titanium dioxide as raw material should have a smaller particle size, which is helpful to obtain nano-barium titanate microcrystals and barium titanate powder with smaller particle size. Generally, in the nano-titanium dioxide aqueous dispersion used, the nano-titanium dioxide has a volumetric median particle size D50≦30nm. The correspondingly prepared nano-barium titanate microcrystals generally have an average particle size of 10-30nm, and the particle size distribution is relatively uniform. And the nano-barium titanate microcrystals are mainly composed of cubic phase, and the cubic phase content can reach 100%. In addition, the nano-barium titanate microcrystals are also characterized by high purity and good dispersibility.
[0020] The nano-titanium dioxide aqueous dispersion used in the present invention is formed by dispersing nano-titanium dioxide powder in water. The present invention is not particularly limited to the source of nano-titanium dioxide powder or nano-titanium dioxide aqueous dispersion, which can be commercially available or self-produced. For example, according to the process described in patent application 201610879270.3 or 201610879701.6, nano-titanium dioxide powder can be produced and then dispersed in deionized water in proportion to obtain nano-titanium dioxide aqueous dispersion.
[0021] Rationally controlling the concentration of nano-titanium dioxide aqueous dispersion helps to avoid problems such as aggregation of nano-barium titanate microcrystals during the synthesis process, so the mass concentration of nano-titanium dioxide aqueous dispersion is generally controlled to 20-50%. In this way, the nano-barium titanate microcrystals not only have excellent dispersibility, but also have the advantages of small particle size, relatively uniform particle size, and high purity. In addition, it can be ensured that the nano-barium titanate microcrystals have a very high yield and are particularly suitable for industrial continuous production.
[0022] The present invention is not particularly limited by the temperature of the nano-titanium dioxide aqueous dispersion, which can be prepared at room temperature (25°C), and can be appropriately heated to improve the mass concentration of nano-titanium dioxide, but the temperature must be lower than the temperature of the barium hydroxide aqueous solution. In the specific implementation process of the present invention, the temperature of the nano-titanium dioxide aqueous dispersion does not exceed 50°C, and is generally 20-50°C.
[0023] It should be explained that the nano-titanium dioxide in the nano-titanium dioxide aqueous dispersion has a very high concentration (≧20%), so in order to achieve a high yield of nano-barium titanate powder, the barium hydroxide aqueous solution also needs to contain a high concentration of barium ions, so as to ensure the molar ratio of barium ions to titanium atoms and the rapid mixing between the barium source and the titanium source. Generally, in the barium hydroxide aqueous solution, the concentration of the barium source should be close to the saturation solubility, for example, the mass concentration of the barium source is 20% or more, and can even reach 50% to 70% or more. Therefore, in order to ensure that there is almost no precipitation of the barium source in the barium hydroxide aqueous solution, the temperature of the barium hydroxide aqueous solution is generally controlled to be 70°C or more, generally 70-110°C, and even 90-110°C, so as to ensure the ratio of the barium source and the titanium source.
[0024] The preparation of the aqueous barium hydroxide solution must be carried out in an inert atmosphere, for example under the protection of an inert gas such as nitrogen.
[0025] In an ideal state, when the molar ratio of Ba and Ti is 1, the two can be fully reacted to produce barium titanate and the remaining raw materials can be avoided. As can be understood, an excess of titanium source or barium source is favorable to proceeding with the reaction in the direction toward the synthesis of barium titanate, for example, excess Ba helps to reduce the content of titanium dioxide impurities in the reaction product, but a large amount of residual barium not only results in the waste of barium source raw materials, but also may introduce barium carbonate impurities when the reaction product is collected and contacted with air. Considering the hydrothermal reaction efficiency and economic factors comprehensively, the molar ratio of Ba and Ti is generally controlled to 1-4:1, and further 1.5-2:1, to ensure the sufficient reaction of titanium dioxide, and the finally obtained nano-barium titanate microcrystals have higher purity.
[0026] After the preparation of the mixed system is completed, the mixed system can carry out atmospheric pressure hydrothermal synthesis reaction. Usually, the mixed system is first stirred, and its temperature reaches 90-110°C to maintain effective mixing of the barium source and the titanium source, and then kept at this temperature for a while. Specifically, the time of atmospheric pressure hydrothermal synthesis reaction is preferably 30 minutes or more.
[0027] According to the inventor's research, if the incubation time exceeds 24 hours, the reaction time of atmospheric pressure hydrothermal synthesis will continue to be extended, which will not have much impact on the size of nano-barium titanate crystallites. Therefore, taking into consideration the actual production efficiency and product quality, the atmospheric pressure hydrothermal synthesis reaction time is usually controlled to not exceed 24 hours, and further, for example, not exceed 3 to 24 hours.
[0028] After the atmospheric pressure hydrothermal synthesis reaction is completed, the temperature is lowered, the reaction product is collected, and high-quality nano-barium titanate microcrystals are obtained through treatments such as washing and drying. In the specific implementation process of the present invention, the reaction product is first subjected to solid-liquid separation using means such as suction filtration, and then the reaction product is washed with deionized water or deionized water and ethanol, and finally dried at 60 to 90°C to obtain nano-barium titanate microcrystals.
[0029] The present invention provides nano-barium titanate microcrystals produced by the above-mentioned production method. The nano-barium titanate microcrystals provided by the present invention have a very small particle size, with an average particle size of 100 nm or less, which can reach 5-30 nm, and is generally 10-30 nm. The particle size of the nano-barium titanate microcrystals is basically normal distribution, the particle size distribution is relatively narrow, and the lattice constant ratios (c / a) of the nano-barium titanate microcrystals are all about 1.0000, and in the XRD diagram, the diffraction peaks between 2θ angles of 44° and 46° appear as single peaks without obvious splitting, indicating that the nano-barium titanate microcrystals are in a standard cubic phase, are relatively complete in growth, and have a relatively good crystal type. The ratios of barium and titanium (Ba / Ti ratio) are all about 1, which means that the nano-barium titanate microcrystals have a very high purity.
[0030] The present invention also provides a method for producing a barium titanate powder, comprising the steps of: First, nano-barium titanate microcrystals are produced according to the above-mentioned production method, The nano barium titanate crystallites are calcined at 200-1300°C, and the calcination time is 1-10 hours to obtain barium titanate powder.
[0031] In the present invention, nano-barium titanate microcrystals are used as the raw material and calcined at high temperatures to obtain barium titanate powder with small and uniform particle size, high purity, good dispersibility, and excellent crystal growth.
[0032] Specifically, the particle size of barium titanate powder is closely related to the calcination temperature. According to the inventor's research, the grain growth by low-temperature calcination below 500℃ is not clear, but the grains of barium titanate grow gradually by high-temperature calcination at 500~1300℃, and the grain size increase becomes more significant with the increase of calcination temperature. Therefore, the appropriate calcination temperature can be selected according to the actual grain size requirements of the product.
[0033] In addition, when the calcination temperature is below 1100°C, the degree of crystallization of the barium titanate powder is improved with the increase of the calcination temperature. However, if the calcination temperature is too high, for example, above 1100°C, high temperature calcination will have a negative effect on the growth of the crystal type. Therefore, the calcination temperature is generally controlled to be 200-1100°C, and more preferably 300-1300°C.
[0034] The present invention further provides a barium titanate powder produced by the above-mentioned production method, specifically, the powder is obtained by calcining the nano-barium titanate microcrystals at high temperature.
[0035] The barium titanate powder has a smaller particle size, a uniform particle size distribution, and good dispersibility. Moreover, the barium titanate powder has the characteristics of good grain growth and high purity, so as to meet the needs of the electronic ceramic industry for high-quality barium titanate products.
[0036] In the method for producing nano-barium titanate microcrystals provided by the present invention, a high-concentration nano-titanium dioxide aqueous dispersion is used as a titanium source, and a normal pressure hydrothermal synthesis process is used to produce nano-barium titanate microcrystals with small particle size, uniformity, high purity and good dispersibility. In particular, by rationally selecting the reaction raw materials and controlling the normal pressure hydrothermal synthesis reaction conditions, nano-barium titanate microcrystals with an average particle size not exceeding 50 nm, even 10-20 nm, can be obtained, and the nano-barium titanate microcrystals are in a cubic phase or mostly in a cubic phase. The nano-barium titanate microcrystals obtained by the method are further calcined or otherwise processed as raw materials to obtain barium titanate powder with a predicted particle size, which has very high purity, crystallinity and good dispersibility, and can meet the demand for barium titanate in the electronic ceramic industry.
[0037] At the same time, the synthesis of nano barium titanate microcrystals is carried out at normal pressure and does not require high temperatures, which not only ensures the safety of production and reduces production energy consumption and equipment costs, but also realizes the continuous production of nano barium titanate microcrystals and even barium titanate powder, which helps to improve production efficiency. In addition, the mass concentration of the aqueous dispersion of nano titanium dioxide used is more than 20%, which further improves production efficiency.
[0038] The nano-barium titanate microcrystals provided by the present invention are characterized by small particle size, narrow distribution range, high purity, and good dispersibility. Using the nano-barium titanate microcrystals as raw material, barium titanate powder with a predicted particle size can be obtained. The barium titanate powder has very high purity, crystallinity, and excellent dispersibility, and can meet the demand for barium titanate in the electronic ceramic industry.
[0039] The method for producing barium titanate powder provided in the present invention uses the above-mentioned nano-barium titanate microcrystals as raw material, and through simple high-temperature calcination, can obtain barium titanate powder with high purity and good dispersibility. During the high-temperature calcination process, the barium titanate powder can achieve good grain growth and effective control of grain size, so as to meet the demand for barium titanate in the electronic ceramic industry.
[0040] In addition, the method for producing the barium titanate powder is characterized by its simple and reliable process, and is suitable for industrial mass production. Effect of the Invention
[0041] The barium titanate powder provided by the present invention has the characteristics of high purity, high dispersibility, excellent grain growth, and the particle size can be controlled, so that it can meet the demand for barium titanate in the electronic ceramic industry. [Brief description of the drawings]
[0042] [Figure 1] 1 is a particle size distribution curve measured by dispersing the nano titanium dioxide used in Examples 1 to 5 of the present invention in deionized water at a mass concentration of 1%. [Diagram 2] 1 is a particle size distribution curve measured by dispersing the nano titanium dioxide used in Examples 1 to 5 of the present invention in deionized water at a mass concentration of 10%. [Diagram 3] 1 is a particle size distribution curve measured by dispersing the nano titanium dioxide used in Examples 1 to 5 of the present invention in deionized water at a mass concentration of 50%. [Figure 4] 1 is an XRD pattern of nano-barium titanate microcrystals produced in Example 1 of the present invention. [Diagram 5] 1 is an XRD pattern of nano-barium titanate microcrystals produced in Example 3 of the present invention. [Figure 6] 1 is an XRD pattern of nano-barium titanate microcrystals produced in Example 4 of the present invention. [Figure 7] 1 is an XRD pattern of nano-barium titanate microcrystals produced in Example 5 of the present invention. [Figure 8] 1 is an XRD pattern of nano-barium titanate microcrystals produced in Example 6 of the present invention. [Figure 9] 1 is an XRD pattern of nano-barium titanate microcrystals produced in Example 7 of the present invention. [Figure 10] 3 is a TEM photograph of nano-barium titanate microcrystals produced in Example 2 of the present invention. [Figure 11] 1 is a TEM photograph of the barium titanate powder produced in Example 8 of the present invention. [Figure 12] 1 is a TEM photograph of the barium titanate powder produced in Example 9 of the present invention. [Figure 13] 1 is a SEM photograph of the barium titanate powder produced in Example 10 of the present invention. [Figure 14] 1 is a SEM photograph of the barium titanate powder produced in Example 11 of the present invention. [Figure 15] 1 is a SEM photograph of the barium titanate powder produced in Example 12 of the present invention. [Figure 16] 1 shows XRD patterns of nano-barium titanate microcrystals produced in Example 2 of the present invention and barium titanate powders produced in Examples 8 to 13. [Figure 17] FIG. 17 is a partially enlarged view of FIG. [Figure 18] 1 is an XRD pattern of barium titanate microcrystals produced in Comparative Example 1 of the present invention. [Figure 19] 1 is an XRD pattern of barium titanate microcrystals produced in Comparative Example 2 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] In order to make the objectives, technical solutions and advantages of the embodiments of the present invention clearer, the following will clearly and completely describe the technical solutions in the embodiments of the present invention in combination with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative labor belong to the scope of protection of the present invention.
[0044] In the present invention, the following detection techniques or means are used to characterize the nano barium titanate crystallites and barium titanate powders: (1) The surface morphology of the sample is observed using a scanning electron microscope and a transmission electron microscope, and the particle sizes of approximately 200 particles are statistically calculated to obtain the average particle size of the primary particles of barium titanate. (2) Using an X-ray diffractometer (D8 Advance), collect X-ray diffraction patterns in the range of 20-80° with parameters of a step length of 0.02° and an integration time of 2 s. Refining the structure using the Rietveid method in Topas software and calculating the lattice constant ratio (c / a). (3) Analyze the specific surface area of the material using the BET method. (4) Detect the ratio of barium to titanium in the barium titanate powder using ICP-MS.
[0045] [Example 1] At room temperature, uniformly disperse the nano titanium dioxide powder in deionized water and slowly stir until uniformly mixed to obtain 100 g of a nano titanium dioxide water dispersion with a mass concentration of 48%, which is set aside. Under the protection of a nitrogen atmosphere at atmospheric pressure, add 355 g of barium hydroxide octahydrate and 150 mL of deionized water to a three-neck round-bottom flask and heat with stirring at 100 °C until the barium hydroxide is completely dissolved. The nano titanium dioxide aqueous dispersion is rapidly added to the three-necked round-bottom flask, and the original heating power to the three-necked round-bottom flask is maintained during the addition process. After the temperature of the resulting mixed system is measured to be 97±2°C, stirring is continued, and the temperature is raised to 100°C to carry out reflux reaction for 5 hours. After the reaction is completed, the reaction product is taken out, filtered, washed and dried to obtain nano barium titanate microcrystals.
[0046] The nano-titanium dioxide powder used in this embodiment has a volumetric D50≦10 nm, and the particle size distribution curves measured by dispersing the nano-titanium dioxide powder in deionized water at concentrations of 1%, 10% and 50% are shown in Figures 1, 2 and 3, respectively.
[0047] [Examples 2 to 3] Except for changing the reflux reaction time to 10 h and 20 h, the other operation steps in Examples 2 and 3 are the same as those in Example 1, and nano-sized barium titanate microcrystals are obtained.
[0048] [Example 4] Without changing the volume of deionized water, reduce the mass of titanium dioxide and barium hydroxide to half of the original amount, add another 51 g of sodium hydroxide, and other operation steps are the same as in Example 2 to obtain nano-barium titanate microcrystals.
[0049] [Example 5] The mass concentration of the nano-titanium dioxide aqueous dispersion is maintained at 48%, the mass of the nano-titanium dioxide aqueous dispersion is reduced to half of the original amount, i.e., 50 g, the molar ratio of titanium dioxide to barium hydroxide is changed, and the other operating steps are the same as those in Example 2, and nano-barium titanate microcrystals are obtained.
[0050] [Examples 6 to 7] The manufacturing process of Examples 6 to 7 was almost the same as that of Example 2, with the only difference being that the median particle size D50 of the nano-titanium dioxide in Example 6 was approximately 17 nm measured by a volumetric meter, and the median particle size D50 of the nano-titanium dioxide in Example 7 was approximately 29 nm measured by a volumetric meter.
[0051] The reaction conditions in the above Examples 1 to 7 are specifically shown in Table 1, and the product shapes of the synthesized nano-barium titanate microcrystals are specifically shown in Table 2.
[0052] [Table 1]
[0053] [Table 2]
[0054] Figure 4 is an X-ray diffraction (XRD) pattern of the nano barium titanate microcrystals obtained in Example 1, and Figures 5, 6, 7, 8 and 9 are XRD patterns of the nano barium titanate microcrystals obtained in Examples 3 to 7, respectively, and the XRD pattern of Example 2 is similar to Figure 4. As can be seen from the above XRD patterns, the diffraction peaks of the nano barium titanate microcrystals obtained in Examples 1 to 7 with 2θ angles of 44° to 46° appear as single peaks without obvious splitting, which means that the lattice growth is good.
[0055] As can be seen in combination with the lattice constant ratios (c / a) in Table 2, the lattice constant ratios (c / a) of the nano-barium titanate crystallites produced in Examples 1 to 7 were all about 1.0000, which is a typical cubic phase.
[0056] As can be seen from the Ba / Ti ratio data in Table 2, the nano-barium titanate microcrystals obtained in Examples 1 to 7 all have a Ba / Ti ratio of approximately 1, with most of them concentrated between 0.990 and 1.001. Therefore, the nano-barium titanate microcrystals have extremely high purity.
[0057] Fig. 10 is a transmission electron microscope (TEM) photograph of the nano-barium titanate microcrystals obtained in Example 2, and the morphology of the nano-barium titanate microcrystals in Example 1 is similar to this. As can be seen by combining Fig. 1 with Table 2, the nano-barium titanate microcrystals produced in Examples 1 and 2 all have an average particle size of about 15 nm, good dispersibility, no obvious aggregation, and relatively uniform particle size, and the nano-barium titanate microcrystals in Examples 3 to 7 all have an average primary particle size of about 50 nm or less.
[0058] [Examples 8 to 13] The nano-barium titanate microcrystal obtained in Example 2 is calcined in a muffle furnace for about 3h to obtain barium titanate powder, where the calcination temperatures in Examples 8 to 13 are 300°C, 500°C, 700°C, 900°C, 1100°C, and 1300°C, respectively. The specific calcination process and product shape may be specifically referred to Table 3.
[0059] [Table 3]
[0060] Figures 11 and 12 are TEM photographs of the barium titanate powders obtained in Examples 8 to 9. As can be seen from the results of Figures 11 to 12 and Table 3, the barium titanate powders obtained in Examples 8 to 9 have good particle dispersion, no clear aggregation is observed, and the average particle size of the primary particles is about 20 nm in all cases, which suggests that crystal grain growth due to low-temperature calcination performed at 300°C to 500°C is not evident.
[0061] Figures 13, 14 and 15 are scanning electron microscope (SEM) photographs of the barium titanate powders in Examples 10 to 12, respectively. As can be seen from Figures 13 to 15 combined with Table 3, when the calcination temperature is increased from 500°C to 1300°C, the barium titanate crystal grains gradually grow and the grain size increases from about 20 nm to about 200 nm, which means that high-temperature calcination at 500°C to 1300°C results in a significant increase in the crystal grains.
[0062] Figure 16 is the XRD pattern of the nano barium titanate microcrystals produced in Example 2 of the present invention and the barium titanate powder produced in Examples 8 to 13, and Figure 17 is an enlarged view of the diffraction peak at 2θ angle of 45° in Figure 16. As can be seen from Figures 16 and 17, the nano barium titanate microcrystals have better crystal growth after calcination, and with the increase in calcination temperature, the crystallization degree of the barium titanate powder is better and better. In particular, when the calcination temperature is 300°C to 1100°C (Examples 8 to 12), the diffraction peak at 2θ angle around 45° appears as a single peak without obvious split, and when the calcination temperature is 1300°C (Example 13), the diffraction peak at 45° is split.
[0063] As can be seen from the test results in Table 4, the grain growth is not obvious due to low-temperature calcination performed at 300°C~500°C, but when the calcination temperature is increased from 500°C to 1300°C, the barium titanate grains grow gradually and the grain size increases from 20nm to about 300nm, which means that high-temperature calcination at 500°C~1300°C brings about a significant increase in grain size.
[0064] [Comparative Example 1] The manufacturing process of Comparative Example 1 is almost the same as that of Example 2, with the only difference being that when preparing the mixed system, the titanium dioxide aqueous dispersion is slowly added to the three-neck flask containing the barium hydroxide aqueous solution, and the mixture is mixed by rapid stirring while being added, and the temperature of the entire mixed system is kept constant at 100°C.
[0065] The specific physical test results of the nano barium titanate crystallites are shown in Table 4, and the XRD pattern is shown in FIG.
[0066] [Comparative Example 2] The manufacturing process of Comparative Example 2 is almost the same as that of Example 2, the only difference being that when preparing the mixed system, the mass of nano-titanium dioxide powder remains the same, but the mass concentration of nano-titanium dioxide is 8%.
[0067] The specific physical test results of the nano barium titanate crystallites are shown in Table 4, and the XRD pattern is shown in FIG.
[0068] As can be seen from Figures 18 and 19, in Comparative Examples 1 and 2, nano-barium titanate microcrystals with good crystal grain growth can be obtained by slowly adding the nano-titanium dioxide aqueous dispersion or by reducing the concentration of the nano-titanium dioxide aqueous dispersion.
[0069] However, a comparison of the test results of Comparative Examples 1-2 and Example 2 shows that when the titanium dioxide aqueous dispersion is added slowly to keep the mixture almost constant, or when a low-concentration nano-titanium dioxide aqueous dispersion is used, the average particle size of the obtained nano-barium titanate microcrystals increases. In addition, when the concentration of the nano-titanium dioxide aqueous dispersion is reduced, the production efficiency of the nano-barium titanate microcrystals is significantly reduced.
[0070] [Table 4]
[0071] Finally, it should be explained that the above embodiments are only used to describe the technical means of the present invention, and are not limited thereto. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical means described in the above embodiments, or equally replace some or all of the technical features thereof, and these modifications or replacements do not cause the essence of the corresponding technical means to depart from the scope of the technical means of the embodiments of the present invention.
Claims
1. A method for producing nano barium titanate microcrystals, comprising the steps of: A nano-titanium dioxide aqueous dispersion liquid having a lower temperature is rapidly mixed with a barium hydroxide aqueous solution having a higher temperature, and the temperature of the resulting mixture is lowered by 2°C to 20°C compared to the temperature of the barium hydroxide aqueous solution by the rapid mixing of the two, wherein the nano-titanium dioxide aqueous dispersion liquid has a mass concentration of 20% or more and a temperature of 20°C to 50°C, and the barium hydroxide aqueous solution has a mass concentration of 20% or more and a temperature of 70°C or more; In an inert atmosphere, the mixture is subjected to a normal pressure hydrothermal synthesis reaction at 90 to 110 ° C., and the reaction product is collected, washed and dried to obtain nano-barium titanate microcrystals. A method for producing nano-barium titanate microcrystals, comprising:
2. adding the nano titanium dioxide aqueous dispersion at the lower temperature to the barium hydroxide aqueous solution at the higher temperature and rapidly mixing to obtain the mixed system; The method according to claim 1 .
3. The temperature of the nano titanium dioxide aqueous dispersion is controlled to be 50° C. or less, and the temperature of the barium hydroxide aqueous solution is controlled to be 70° C. or more during the rapid mixing. The method according to claim 1 or 2.
4. In the nano-titanium dioxide aqueous dispersion, the median particle size of the nano-titanium dioxide is 30 nm or less as measured by a volume meter. The method according to claim 1 or 2.
5. In the above mixture, the molar ratio of Ba ions to Ti atoms is 1 to 4:1; The method according to claim 1 or 2.
6. The mass concentration of the barium hydroxide aqueous solution is 20% or more. The method according to claim 1 .
7. The atmospheric pressure hydrothermal synthesis reaction time is 30 minutes or more; The method according to claim 1 or 2.
8. A method for producing a barium titanate powder, comprising the steps of: Producing nano-barium titanate microcrystals according to the method of any one of claims 1 to 7; and calcining the nano-barium titanate microcrystals at 200 to 1300° C. to obtain barium titanate powder. A method for producing a barium titanate powder comprising the steps of:
Citation Information
Patent Citations
Manufacture of diatomic cation titanate
JP1988074915A
Method for manufacturing barium titanate and barium titanate powder manufactured by the same method
JP2014024750A