Method for processing coated cutting tools
Optimizing laser shock peening energy density and surface treatments on coated cutting tools with cermet or cemented carbide matrices addresses performance issues, enhancing toughness and wear resistance, and extending tool life.
Patent Information
- Application Number
- JP2022513121
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-08-27
AI Technical Summary
Existing methods for treating coated cutting tools with cermet or cemented carbide matrices, such as laser shock peening, do not optimize energy density settings, leading to suboptimal performance in terms of edge line toughness, wear resistance, and chipping resistance.
Applying laser shock peening (LSP) with specific energy density ranges (0.4 to 1.6 J/mm², preferably 0.9 to 1.4 J/mm²) to coated cutting tools, using CVD or PVD layers like TiN, TiCN, or TiAlN as absorbent layers, and optionally followed by shot blasting, to enhance residual stress and surface finish.
Improves cutting tool performance by enhancing edge line toughness, wear resistance, and chipping resistance while maintaining coating thickness and appearance, extending tool life through optimized LSP energy density and surface treatment.
Smart Images

Figure 0007564867000004 
Figure 0007564867000005 
Figure 0007564867000006
Abstract
Description
[Technical field]
[0001] The present invention relates to laser shock peening of coated cutting tools having a cermet or cemented carbide substrate and a coating comprising a layer produced by CVD and / or PVD. [Background technology]
[0002] Cermets and cemented carbides are materials composed of hard elements in a metallic binder. These materials are common substrates in cutting tools, due to their properties of high hardness, high wear resistance, high toughness, etc. These substrates are usually coated with wear-resistant coatings, such as CVD coatings, e.g. with layers of TiCN and alumina, or PVD coatings, e.g. with layers of TiN and TiAlN.
[0003] Coated cutting tools are usually surface treated to further improve their life in cutting. Common surface treatments are brushing to smooth the outer surface or shaping of the cutting edge, shot blasting to smooth the surface and affect the residual stress level of the surface area of the cemented carbide or coating.
[0004] Laser shock peening is a method of influencing the properties of a surface zone using a laser. A short, high-intensity laser pulse is scanned over the surface. Each laser pulse creates a local plasma that forms on the surface, which generates a shock wave that propagates within the object being treated. This shock wave affects the surface zone of the material, resulting in increased hardness, toughness and changes in the residual stress levels.
[0005] WO 2018 / 215996 discloses a method for treating cemented carbide cutting tools by laser shock peening. Summary of the Invention
[0006] It is an object of the present invention to provide an improved method for treating coated cutting tools containing a cermet or cemented carbide substrate.
[0007] At least one of these objects is achieved by the method according to claim 1. Preferred embodiments are recited in the dependent claims.
[0008] The present invention relates to a method for treating a coated cutting tool using laser shock peening (LSP), the coated cutting tool comprising a substrate and a coating, the substrate being a cemented carbide or cermet, preferably a cemented carbide, the coating comprising a CVD layer and / or a PVD layer, the method comprising the steps of subjecting at least a part of the cutting tool to LSP, the LSP energy density being between 0.4 and 1.6 J / mm 2 Within 0.9 to 1.4 J / mm 2 Within 1.1 to 1.3 J / mm 2 Within.
[0009] Surprisingly, the LSP energy density was 0.4 to 1.6 J / mm 2 Within 0.9 to 1.4 J / mm 2 It was found that performing laser shock peening at settings within 100 nm was optimal for cutting tool performance. If the LSP energy density is too low, the impact from the LSP will be too low to result in improved edge line toughness or wear resistance. If the LSP energy density is too high, there is a high risk of reduced stress in the surface area, thereby reducing edge line chipping resistance.
[0010] In one embodiment of the present invention, the LSP includes applying a laser pulse to at least a portion of a cutting tool, the laser pulse energy density being between 0.04 and 1.0 J / mm. 2 , preferably 0.04 to 0.5 J / mm 2 , more preferably 0.04 to 0.1 J / mm 2 , and even more preferably 0.05 to 0.07 J / mm 2 It is.
[0011] In one embodiment of the present invention, black paint or black tape is applied to the coated cutting tool prior to application of the LSP. The advantage of using black paint or black tape is that it preserves the underlying coating without loss of thickness or change in appearance.
[0012] In one embodiment of the present invention, the coating includes one or more outer layers of TiN, TiCN, TiC, TiB2, ZrCN, TiAlN, or TiSiN. These layers can be used as absorbing layers instead of paint or tape. The advantage of these layers is that they can be deposited as part of the CVD or PVD coating, thus eliminating the extra step of applying black tape or black paint. An additional advantage is that the use of these layers induces higher levels of residual stress in the surface region of the substrate, making the effect of LSP more visible.
[0013] In one embodiment of the present invention, the thickness of the outer layer is preferably 2-5 μm. As the thickness of the outer layer becomes thinner, the thickness of the wear-resistant layer underneath it decreases during LSP. When the thickness exceeds 5 μm, the induced residual stress in the base material is smaller, and therefore the improvement of tool life by LSP is not very significant.
[0014] In one embodiment of the present invention, the coated cutting tool further comprises a layer of Al2O3 located between the substrate and the outer layer, the layer of Al2O3 being preferably an α-Al2O3 layer, which is advantageous in that it is a very wear resistant layer.
[0015] In one embodiment of the present invention, the coated cutting tool further includes a layer of TiCN located between the base material and the outer layer.
[0016] In one embodiment of the present invention, the coated cutting tool further includes a layer of TiAlN located between the base material and the outer layer.
[0017] In one embodiment of the present invention, the total coating thickness is 2 to 20 μm. In one embodiment of the present invention, the total coating thickness is 2 to 10 μm.
[0018] In one embodiment of the present invention, the cutting tool includes a rake face, a flank face and a cutting edge therebetween, with a portion of the cutting edge and at least a portion of the rake face being subjected to the LSP.
[0019] In one embodiment of the present invention, the LSP step is followed by a blasting, polishing and / or brushing step, preferably a blasting step such as shot blasting. The advantage of blasting, polishing and brushing is that the surface of the cutting tool can be finished by any of these techniques, thereby improving the cutting performance of the cutting tool. Shot blasting is advantageous in that it can affect both the surface roughness and the residual stress level of the coating, thereby achieving a lower surface roughness and a lower tensile stress level or a higher compressive stress level of the coating, thereby extending the life of the cutting tool.
[0020] In one embodiment of the present invention, the cutting tool comprises a rake face, a flank face and an edge therebetween, and only a part of the cutting edge of the cutting tool and a part of the rake face and / or the flank face is LSPed, the width (b) of said area being at most 5 mm from the cutting edge, preferably the width (b) of said area being 1-5 mm from the cutting edge. It is advantageous to apply LSP at least to the area involved in cutting. The extension from the edge to the rake face, when applied, has at least a cutting depth a p It must be.
[0021] In one embodiment of the present invention, the LSP is applied along the entire cutting edge of the cutting tool.
[0022] In one embodiment of the present invention, the LSP is applied to the entire rake face of the cutting tool.
[0023] In one embodiment of the present invention, the LSP is applied to the entire rake face, the entire cutting edge, and also the entire flank face of the cutting tool.
[0024] In one embodiment of the present invention, the wavelength of the laser during the LSP process is within 1,000 to 1,100 nm, preferably within 1,050 nm to 1,070 nm, and more preferably about 1,064 nm.
[0025] In one embodiment of the present invention, the frequency of the laser during the LSP process is within 150,000-250,000 Hz, preferably about 200,000 Hz.
[0026] In one embodiment of the present invention, the pulse duration of the laser during the LSP process is within 0.005-0.02 ns, preferably about 0.01-0.02 ns.
[0027] In one embodiment of the present invention, the average power of the laser during the LSP process is within 13-16W, preferably about 15W.
[0028] In one embodiment of the present invention, the spot size of the laser during the LSP process is within 0.03-0.05 mm, preferably about 0.04 mm.
[0029] In one embodiment of the present invention, the peak power density of the laser during the LSP process is 3 to 7 GW / mm 2 Within 6GW / mm 2 This level of peak power density can be varied by changing either the frequency, pulse length, laser efficiency, or spot size. Peak power densities between 3 and 7 GW / mm 2 If the pressure is within this range, the peak pressure obtained will be higher, which has the advantage of improving the life of the cutting tool.
[0030] In one embodiment of the present invention, the LSP is applied to the coated cutting tool when the coated cutting tool is immersed in water.
[0031] Further objects and features of the present invention will become apparent from the following examples considered in conjunction with the accompanying drawings. [Brief description of the drawings]
[0032] [Figure 1] 1 is a diagram of a cutting tool (1) that can be treated according to the invention, showing the rake face (2), the flank face (4) and the cutting edge (3). The geometry of the cutting tool corresponds to the geometry used in the following examples. [Diagram 2] FIG. 1 is a schematic diagram of the location and extent of LSP regions according to one embodiment of the present invention, showing the rake face (2) and cutting edge (3) of a cutting tool (1). [Diagram 3] Schematic of laser pulses (circles) scanned with a pulse step length x over a certain area. The pulses overlap each other so that the whole or part of the area is processed by LSP. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] definition By "cutting tool" is meant herein a cutting tool for metal cutting applications such as an insert, an end mill or a drill. The field of application can be, for example, turning, milling or drilling.
[0034] By "hardmetal" is meant herein a material comprising at least 50% by weight of WC, possibly other hard constituents common in the art of making hardmetals, and a metallic binder phase, preferably selected from one or more of Fe, Co and Ni.
[0035] By "cermet" is meant herein a material comprising a hard component, which is one or more of titanium carbonitride, titanium carbide and titanium nitride, and a metallic binder phase. The metallic binder phase in the cermet is preferably selected from one or more of Fe, Co and Ni, preferably Co. Other hard components common in the cermet art are selected from carbides, nitrides or carbonitrides of Ti, Ta, Nb, Zr, V and Cr. The cermet material does not contain free hexagonal WC. Cermet materials based on titanium carbonitride are the most common cermet materials today.
[0036] "LSP energy density," as used herein, refers to the average energy density applied to an LSP treated portion or area of a cutting tool. Increasing the pulse overlap or increasing the laser pulse energy density results in an increase in the LSP energy density.
[0037] "Laser pulse energy density" herein refers to the average energy density of one single laser pulse. Increasing the pulse duration or increasing the effect results in an increase in laser pulse energy density.
[0038] "Shot blasting," as used herein, refers to a process that uses abrasive particles to remove material from a treatment surface, typically by abrasive wear. Shot blasting is well known in the art of cutting tools and is known to induce residual stresses in coatings on cutting tools, for example. EXAMPLES
[0039] Exemplary embodiments of the present invention will now be disclosed in more detail and compared with comparative embodiments.Coated cutting tools (inserts) were prepared, analyzed and evaluated in cutting tests.
[0040] Base material The cemented carbide preform of ISO type R390-11T308M-PM was manufactured for grinding (see Fig. 1).
[0041] Two different cemented carbide compositions were produced. Matrix A was produced from a powder mixture having a composition of about 13.50 wt% Co, 0.57 wt% Cr, and balance WC. Matrix B was produced from a powder mixture having a composition of about 9.14 wt% Co, 1.15 wt% Ta, 0.27 wt% Nb, 0.05 wt% Ti, and balance WC. The powder mixture was ground, dried, pressed into green bodies, and sintered at 1,450°C to form sintered cemented carbide matrix.
[0042] coating CVD coatings were deposited on the two cemented carbide compositions. The CVD coatings consisted of an inner TiN layer with a thickness of 0.5 μm, followed by a wear-resistant TiCN layer with a thickness of 3.5 μm, and a wear-resistant α-Al2O3 layer on top with a thickness of 3 μm. An outer TiN layer was then deposited with a thickness of 2 μm. The total coating thickness was approximately 9 μm.
[0043] LSP Processing The LSP was applied to an area of the rake face that also extended to the edge of the coated cutting tool. The width of this area, b, measured perpendicularly from the cutting edge of the cutting tool was about 3 mm. The extension along the main cutting edge, a, was about 6 mm, and the extension along the secondary cutting edge, c, was about 3 mm. See schematic of the LSP area in Figure 2.
[0044] The LSP process was performed with 6 mm of water on the surface. The cutting tool was immersed in the water during the LSP process.
[0045] The laser settings during LSP were as follows: Wavelength: 1,064nm Frequency: 200kHz Pulse duration: 0.01ns Pulse diameter, d: 0.04mm Laser power: 14.8W Peak power density: 5.89GW / mm 2
[0046] The laser pulse energy density is 0.059 J / mm 2 and was calculated as follows: Laser pulse energy density [J / mm 2 ]=laser pulse energy / pulse area Laser pulse energy [J] = laser power / frequency Pulse area [mm 2 ]=πd 2 / 4
[0047] The LSP energy density is adjusted by changing the pulse distance, i.e., the pulse step length x, and by varying the pulse overlap, i.e., by decreasing the pulse distance and increasing the pulse overlap, resulting in a higher LSP energy density. The laser pulse overlap is related to the pulse step length x and the pulse diameter d. Laser pulse overlap = dx / d
[0048] The LSP energy densities of the samples are shown in Table 1. LSP energy density [J / mm 2 ]=laser pulse energy × 1mm 2 Number of pulses per 1mm 2 Number of pulses per second = 1 / x 2
[0049] TIFF0007564867000001.tif102170
[0050] Shot Blasting Process Following LSP, the cutting tools were shot blasted to remove the outer TiN layer. The shot blast time was adjusted slightly to remove all TiN from the area of the rake face that had been treated with LSP. Shot blasting was performed with alumina abrasive and 2.1 bar air pressure. Samples A0 and B0 were also subjected to shot blasting.
[0051] Cutting performance 1 Next, inserts with base material A were tested in a milling operation with the following parameters: Work material: Dievar uncured, PL129 200x200x100, MC P3.0.Z.AN, CMC03.11, Charge: M10205 v c =200m / min f z =0.15mm a e =12mm a p =3.0 z=1 Cut length = 12mm No cutting fluid was used. Insert type R390-11T308M-PM
[0052] The tool life criterion was chipping of at least 0.5 mm of the edge line. Tool life is presented as the average number of cut entrances to achieve this criterion. The average tool life is shown in Table 2, where the tool life is the average number of cuts and is the average of 8 parallel cutting tests.
[0053] TIFF0007564867000002.tif97170
[0054] Cutting performance 2 The inserts with base material B were then tested in a milling operation with the following parameters: Work material: Dievar uncured, PL129 200x200x100, MC P3.0.Z.AN, CMC03.11, Charge: M10205 v c =160m / min f z =0.2mm a e =12mm a p =3.0 z=1 Cut length = 12mm No cutting fluid was used. Insert type R390-11T308M-PM
[0055] The tool life criterion was chipping of at least 0.5 mm of the edge line. Tool life is presented as the average number of cut entrances to achieve this criterion. The average tool life is shown in Table 3, where the tool life is the average number of cuts and is the average of 8 parallel cutting tests.
[0056] TIFF0007564867000003.tif97170
[0057] While the present invention has been described in connection with various exemplary embodiments, it is to be understood that the present invention is not limited to the disclosed exemplary embodiments, but on the contrary, is intended to cover various modifications and equivalent arrangements within the scope of the appended claims. Moreover, it should be recognized that any disclosed form or embodiment of the present invention may be incorporated in any other disclosed or described or suggested form or embodiment, as a general matter of design choice. It is therefore intended to be limited only as indicated by the scope of the appended claims.
Claims
1. A method for treating a coated cutting tool (1) using laser shock peening (LSP), the coated cutting tool consisting of a base material and a coating, the base material being a cemented carbide or a cermet, the coating comprising a CVD layer and / or a PVD layer, the method comprising the steps of subjecting at least a part of the coated cutting tool (1) to LSP, the LSP energy density being between 0.4 and 1.6 J / mm 2 Within The method, wherein the coated cutting tool (1) comprises a rake face (2), a flank face and a cutting edge (3) therebetween, and the LSP is applied to a portion of the cutting edge (3) and at least a portion of the rake face (2).
2. The method of claim 1, wherein the LSP comprises applying a laser pulse to at least a portion of the coated cutting tool, and wherein a laser pulse energy density is between 0.04 and 1.0 J / mm2.
3. A method according to claim 1 or 2, wherein the wavelength of the laser during the process of applying the LSP is 1,000 to 1,100 nm.
4. 4. The method according to any one of claims 1 to 3, wherein black paint or black tape is applied to the coated cutting tool (1) before applying LSP.
5. The coating is TiN, TiCN, TiC, TiB 2 5. The method of claim 1 , further comprising one or more outer layers of ZrCN, TiAlN or TiSiN.
6. The coated cutting tool (1) comprises an Al layer located between the base material and the outer layer. 2 O 3 The method of claim 5 further comprising a layer of.
7. A method as described in claim 5 or 6, wherein the coated cutting tool (1) further comprises a layer of TiCN located between the base material and the outer layer.
8. A method according to any one of claims 5 to 7, wherein the coated cutting tool (1) further comprises a layer of TiAlN located between the base material and the outer layer.
9. The method of claim 1, wherein the total thickness of the coating is from 2 to 20 μm.
10. The method of claim 1, wherein the step of applying the LSP is followed by a blasting, polishing, and / or brushing step.
11. A method according to any one of claims 1 to 10, wherein the coated cutting tool (1) comprises a cutting face (2), a flank face (4) and a cutting edge (3) therebetween, the LSP being applied only to a portion of the cutting edge (3) of the coated cutting tool (1) and to a portion of the cutting face (2) and / or the flank face (4), and the width (b) of the area is up to 5 mm from the edge.
12. A method according to any one of claims 1 to 11, wherein the frequency of the laser during the process of applying the LSP is within 150,000 to 250,000 Hz.
13. The peak power density of the laser during the process of applying the LSP is 3 to 7 GW / mm 2 The method of any one of claims 1 to 12, wherein the 14. The method according to any one of claims 1 to 13, wherein the LSP energy density is within 0.4 to 1.4 J / mm 2 .
15. The method according to any one of claims 1 to 14, wherein the LSP energy density is within 0.9 to 1.4 J / mm 2 .
16. The method according to any one of claims 1 to 15, wherein the LSP energy density is within 1.1 to 1.3 J / mm 2 .
Citation Information
Patent Citations
Pulse laser surface treatment method
JP2005272989A
Method for manufacturing coated member and coated member
JP2009293110A
Coated cutting tool
JP2012223872A
Tool and method of manufacturing the same
JP2013107143A
Method and system for improving the surface fracture toughness of brittle materials, and a cutting tool produced by such method
WO2018215996A1