Method for producing resin composition, resin composition

The use of a maleimide derivative as a scavenger in the polymerization of (meth)acrylic monomers reduces residual monomer content to 1.0% or less, addressing odor and flammability issues while maintaining adhesive properties and solvent compatibility.

JP7565124B1Active Publication Date: 2024-10-10HARVES CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024039169
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-10-10
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Existing resin compositions made from (meth)acrylic monomers suffer from residual monomers that cause odor, toxicity, skin irritation, and flammability issues, and solvent-based adhesives pose fire hazards and have limited solvent compatibility due to increased molecular weight, leading to restricted use and performance degradation.

Method used

A polymerization process involving a maleimide derivative compound as a scavenger is used to reduce residual (meth)acrylic monomer content to 1.0% or less, combined with a fluorinated solvent to create a non-flammable adhesive solution.

Benefits of technology

The process effectively minimizes residual monomer odor and flammability, maintains adhesive strength, and ensures solubility in fluorinated solvents, producing a practical and safe adhesive solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565124000001_ABST
    Figure 0007565124000001_ABST
Patent Text Reader

Abstract

The amount of residual monomer during polymerization using (meth)acrylic monomer as a raw material is further reduced. [Solution] A method for producing a resin composition includes a polymerization step in which a (meth)acrylic monomer is included in a raw material and a polymerized composition is produced by polymerizing the (meth)acrylic monomer, and a maleimide derivative addition step in which a maleimide derivative compound is added when the conversion rate of the (meth)acrylic monomer in the polymerization step is 70% or more and / or when the polymerization reaction of the (meth)acrylic monomer has stopped.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a method for producing a resin composition. [Background technology]

[0002] (Odor issues) In the case of polymers and copolymers of (meth)acrylic monomers, some unreacted monomers with low alkyl chain numbers may remain in the final resin composition obtained by polymerization, and the odor derived from these residual monomers may have a negative impact on the working environment. Furthermore, when this resin composition is used as a product, the residual monomers may be toxic or corrosive, and may cause skin irritation if they come into contact with the human body.

[0003] (Flammable Issues) In addition, solvent-based adhesives, which are made by dissolving the adhesive resin composition in a liquid to make it easier to apply, are widely used. However, adhesive resin compositions generally only dissolve in organic solvents, and solvent-based adhesives that use organic solvents have a flash point and are often considered hazardous materials under the Fire Service Act. Such solvent-based adhesives are subject to various restrictions, such as restrictions on storage space and quantity, and use in explosion-proof facilities.

[0004] The odor can be reduced by increasing the molecular weight of the (meth)acrylic monomer, thereby decreasing the vapor pressure of the remaining (meth)acrylic monomer. However, increasing the molecular weight of the (meth)acrylic monomer reduces the polarity (SP value) and deteriorates the solubility. As a result, when used as a solution-type adhesive, the types of organic solvents that can be selected are limited to those with low polarity. In addition, there is also the issue that increasing the molecular weight of the (meth)acrylic monomer increases the glass transition point of the polymer, thereby decreasing the adhesiveness as an adhesive.

[0005] Therefore, there is a need for a method for reducing the amount of remaining (meth)acrylic monomer in the polymerization reaction of the (meth)acrylic monomer in the production process of the resin composition, without increasing the molecular weight of the (meth)acrylic monomer.

[0006] As a method for reducing the amount of (meth)acrylic monomer remaining in the resin composition, which is the final product, a method of adding a scavenger to the resin composition is known (see Patent Documents 1 and 2). In Patent Document 1, by adding a scavenger, the low copolymerizability between the remaining (meth)acrylic monomer and the scavenger is utilized, and the amount of remaining (meth)acrylic monomer is reduced by relatively promoting the polymerization reaction between the remaining (meth)acrylic monomers themselves rather than the polymerization reaction between the remaining (meth)acrylic monomer and the scavenger. In the examples of Patent Document 2, a polyfunctional (meth)acrylic monomer having multiple (meth)acryloyl groups per molecule is used as a scavenger. This scavenger is highly reactive, and reduces the amount of remaining (meth)acrylic monomer by the reaction between the remaining (meth)acrylic monomer and the scavenger.

[0007] In Patent Document 1, a monofunctional vinyl ether compound is used as a scavenger, and the amount of (meth)acrylic monomer remaining in the end is about 0.3 to 0.7 parts by mass per 100 parts by mass of the resin composition. However, this amount of remaining is not enough to be said to be reduced. However, if a larger amount of scavenger is added, the amount of remaining (meth)acrylic monomer may be reduced further, but the amount of unreacted scavenger added remains even more, so the odor from the scavenger becomes a problem. In other words, since the scavenger itself is treated in the same way as the remaining monomer, it is difficult to substantially reduce the total amount of remaining monomer. Furthermore, if the unreacted scavenger remains when used as an adhesive, it will cause a decrease in adhesive strength due to migration to the interface with the adherend.

[0008] In addition, in Patent Document 2, since the scavenger has multiple (meth)acryloyl groups, the scavenger promotes crosslinking between resins, which may cause the resin to polymerize beyond the target molecular weight, resulting in thickening or gelation of the resin composition. For this reason, it is not possible to add a sufficient amount of scavenger, making it difficult to sufficiently reduce the amount of remaining (meth)acrylic monomers and obtain the target molecular weight at the same time.

[0009] As described above, the technology of adding a scavenger is a promising method for reducing the amount of residual (meth)acrylic monomer, but there is still room for improvement in its effectiveness, and the development of such technology is desired.

[0010] Meanwhile, in order to improve the flammability of the organic solvent in the solvent-based pressure-sensitive adhesive, the selection of a non-flammable solvent has been investigated.

[0011] One such adhesive is a water-emulsion adhesive that uses water as a solvent. However, compared to organic solvent adhesives, this water-emulsion adhesive is inferior in terms of weather resistance and water resistance. Furthermore, water-emulsion adhesives have problems such as deterioration (rotting) of the aqueous solution depending on the storage environment and separation due to freezing. If a preservative is added to deal with this, the adhesive function will decrease. Also, water has a large latent heat of evaporation, which slows down the drying speed, making the adhesive less convenient to use.

[0012] In recent years, therefore, a technique has been proposed in which a fluorine-containing solvent such as hydrofluoroether (HFE) is mixed into the solvent for the resin composition (see Patent Documents 3 and 4).

[0013] In Patent Document 3, the fluorine solvent used to eliminate the flash point is mainly composed of hydrofluoroether (HFE) HFE-347, but compared to organic solvents, it has poor compatibility with resin compositions mainly composed of polymers of (meth)acrylic monomers. To solve this problem, Patent Document 3 mixes hexamethyldisiloxane, but if the ratio of HFE solution in the solution is increased to reduce flammability, there is a problem that the adhesive component, which is the resin composition, separates. For this reason, HFE cannot be used as the main component of the solvent.

[0014] In addition to HFE, there are many fluorine solvents that are not flammable or have a high flash point and good solubility. However, generally, those that are highly soluble in resin compositions mainly composed of polymerized (meth)acrylic monomers are also highly soluble in amorphous resins, so that if the substrate to which the solvent is applied is made of a similar resin material, the solvent may corrode or dissolve the substrate. As a result, if a fluorine solvent other than HFE is selected, the applications are limited.

[0015] In order to improve the compatibility of a resin composition with HFE, a proposal has been proposed to introduce fluorine atoms into the resin composition to be dissolved. Patent Document 4 introduces a technology for providing a non-flammable surface treatment agent by combining a solution of HFE and a lower alcohol component with a fluorine-containing polymer (fluorine-containing resin composition).

[0016] However, in recent years, some fluorine-containing polymers (fluorine-containing resin compositions) have been subject to concerns about their accumulation in the human body and their long-term persistence in the natural environment due to their high stability. Furthermore, they are more difficult to produce than general compounds, resulting in higher production costs and naturally limiting their applications. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] Special Publication No. 2009-520056 [Patent Document 2] Japanese Patent Application Publication No. 6-287529 [Patent Document 3] JP 2006-274173 A [Patent Document 4] JP 2014-9335 A Summary of the Invention [Problem to be solved by the invention]

[0018] The present invention has been made in consideration of at least some of the problems pointed out above, and aims to provide a production technique for further reducing the amount of residual monomer during polymerization using a (meth)acrylic monomer as a raw material, and a resin composition obtained thereby. [Means for solving the problem]

[0019] The present invention, which achieves the above-mentioned object, provides a method for producing a resin composition, comprising: a polymerization step of producing a polymerized composition by polymerizing a (meth)acrylic monomer contained in a raw material; and a maleimide derivative addition step of adding a maleimide derivative compound in a state where a conversion rate of the (meth)acrylic monomer is 70% or more in the polymerization step and / or in a state where the polymerization reaction of the (meth)acrylic monomer has been terminated.

[0020] The method for producing the resin composition may be characterized in that in the polymerization step, a (meth)acrylate monomer is used as the (meth)acrylic monomer.

[0021] The method for producing the resin composition may be characterized in that, as the (meth)acrylic monomer, one or more (meth)acrylate monomers having an ester moiety with 1 to 8 carbon atoms are used.

[0022] The method for producing the resin composition may be characterized in that in the maleimide derivative adding step, the amount of the (meth)acrylic monomer remaining is reduced to 1.0% by weight or less.

[0023] The method for producing the resin composition may further include a dissolving step of dissolving the polymerized composition obtained through the maleimide derivative adding step in a fluorine-based solvent of at least any one of hydrofluoroether, hydrofluoroolefin, and hydrofluorocarbon.

[0024] In relation to the method for producing the resin composition, the polymer composition may be characterized in that it has a crosslinkable site.

[0025] The present invention, which achieves the above-mentioned object, is a resin composition comprising: a polymerized composition obtained by polymerizing a (meth)acrylic monomer; and a maleimide derivative compound that is added as a scavenger and exists in an unreacted state with the (meth)acrylic monomer.

[0026] The above resin composition may be characterized in that the (meth)acrylic monomer is a (meth)acrylate monomer.

[0027] In relation to the above resin composition, the polymer composition may be obtained by polymerizing a (meth)acrylate monomer having an ester moiety with 1 to 8 carbon atoms, and may be used as a pressure-sensitive adhesive. Effect of the Invention

[0028] According to the present invention, a resin composition can be obtained in which the amount of remaining monomers at the time of polymerization is reduced. [Brief description of the drawings]

[0029] [Figure 1] 1 is a table showing raw materials and verification results of examples and comparative examples of the resin composition of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings.

[0031] In this embodiment, a maleimide derivative compound that is solid and does not have an odor is used as a scavenger added in the latter half of the polymerization process or after the polymerization process. This reduces the amount of remaining (meth)acrylic monomer to 1.0% by weight or less, more preferably 0.5% by weight or less, based on 100 parts by weight of the initial input. As a result, a resin composition that has almost no odor derived from the (meth)acrylic monomer can be obtained. The maleimide derivative compound has low copolymerizability with the (meth)acrylic monomer. Therefore, by adding the maleimide derivative compound as a scavenger, the polymerization reaction between the remaining (meth)acrylic monomers is relatively promoted due to the low polymerization reactivity of the (meth)acrylic monomer and the maleimide derivative compound.

[0032] Furthermore, in this embodiment, the (meth)acrylic monomer is a (meth)acrylate monomer in which the number of carbon atoms in the ester portion is limited to about 1 to 8, thereby increasing the solubility in a solvent mainly composed of HFE. This (meth)acrylate monomer is generally considered to be difficult to reduce the amount remaining during the polymerization process, and at the same time, has a strong odor due to its low molecular weight, making it difficult to put into practical use. However, the present inventors have found that by using a maleimide derivative compound as a scavenger as in this embodiment, the amount of the remaining (meth)acrylate monomer can be reduced extremely efficiently. As a result, a resin composition or a pressure-sensitive adhesive solution that is both odor-reducing and non-flammable can be produced.

[0033] The (meth)acrylic monomer used as a raw material for the polymerization reaction is preferably the main component (50% by weight or more) of the raw materials for the polymerization reaction. Furthermore, the (meth)acrylate monomer with the carbon number limited to about 1 to 8 is preferably the main component (50% by weight or more) of the raw materials for the polymerization reaction, and more preferably the main component (50% by weight or more) of the (meth)acrylic monomer in the raw materials.

[0034] The maleimide derivative compound used in the present embodiment contains one or more maleimide groups. There may be a plurality of maleimide groups in the maleimide derivative compound. Since the maleimide derivative compound reacts relatively slowly, even if it has a multifunctional group, it is difficult for a crosslinking reaction to occur, and therefore it has the advantage that thickening / decreasing and gelling are unlikely to occur.

[0035] By appropriately adjusting reaction conditions such as the type of maleimide derivative compound as a scavenger, the addition of multiple types, the addition amount, reaction temperature, addition timing, etc., it is possible to reduce the amount of remaining (meth)acrylic monomer. According to experiments and verifications by the present inventors, it is possible to finally reduce the amount of remaining (meth)acrylic monomer to 1.0 wt % or less, and more preferably 0.5 wt % or less.

[0036] In the present embodiment, the polymerization reaction technique of the (meth)acrylic monomer may be selected from general techniques. For example, it is preferable to carry out a radical polymerization reaction, and the initiator in this case is preferably an organic peroxide or an azo compound.

[0037] When the resin composition obtained in this embodiment is used as an adhesive, it similarly becomes an adhesive with low odor, excellent adhesion, and high practicality that is soluble in a fluorine-containing solvent.

[0038] The resin composition obtained in this embodiment is soluble in a fluorine-based solvent, particularly HFE. By diluting and dissolving in a fluorine-based solvent, a non-flammable solution-type resin composition can be provided. As the fluorine-based solvent, it is preferable to select one or more from hydrofluoroethers, hydrofluoroolefins, and hydrofluorocarbons, each of which has a boiling point of less than 80°C.

[0039] The resin composition of the present embodiment can be used as an adhesive for use in adhesive sheets, double-sided tapes, adhesive processed products, etc. The polymer of the (meth)acrylic monomer becomes an acrylic polymer, which is a so-called non-fluorine-based resin. By dissolving the acrylic polymer as the main component in a non-flammable fluorine-based solvent (for example, the main component is hydrofluoroether), it is possible to produce a non-flammable solvent-based adhesive that can be used inside electronic devices, etc.

[0040] The method for producing the resin composition according to this embodiment will be described below. In this embodiment, a (meth)acrylic monomer is used as the main component of the raw material used to generate the polymerized composition. The main component means that the (meth)acrylic monomer is 50% by weight or more in the entire raw material before being dissolved in the polymerization solvent. This (meth)acrylic monomer is divided into (meth)acrylate monomer having one or more ester groups and (meth)acrylic acid having no ester group. One or more types of substances can be used as the raw material.

[0041] In this embodiment, a (meth)acrylic carboxyl group-containing monomer may be used as the substance contained in the raw material. The concept of the (meth)acrylic carboxyl group-containing monomer includes the above-mentioned (meth)acrylic acid.

[0042] As the (meth)acrylate monomer, for example, one having an alkyl carbon number of 1 to 8 in the ester moiety can be selected. In general, when the alkyl group has a small number of carbon atoms, it tends to be soft, and when the number of carbon atoms is large, it tends to be hard. Therefore, one or more monomers having different carbon numbers can be freely selected as necessary.

[0043] Specific (meth)acrylate monomers that can be used include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, N-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl acrylate, N-octyl acrylate, isooctyl acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, deoxy (meth)acrylate, ethyl ... Examples of the acrylates include silyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, isobornyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3,5,5-trimethylcyclohexane acrylate, p-cumylphenol EO-modified (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, 2-methyladamantyl (meth)acrylate, and 2-ethyladamantyl (meth)acrylate.

[0044] Examples of (meth)acrylate monomers include hydroxyl group-containing (meth)acrylates having organic functional groups such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and glycerol (meth)acrylate; epoxy group-containing monomers such as glycidyl (meth)acrylate, α-ethyl glycidyl acrylate, and 3,4-epoxybutyl (meth)acrylate; amino group-containing (meth)acrylate monomers such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate; (meth)acrylamide, Nt-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; Examples of monomers having a perfluoroalkyl group include perfluorohexylethyl (meth)acrylate, perfluorohexyl (meth)acrylate, perfluoropentylpropyl (meth)acrylate, perfluoropentylethyl (meth)acrylate, perfluorobutylethyl (meth)acrylate, perfluorobutylmethyl (meth)acrylate, perfluoropropylethyl (meth)acrylate, perfluoropropylmethyl (meth)acrylate, perfluoroethylethyl (meth)acrylate, perfluoroethylmethyl (meth)acrylate, and trifluoroethyl (meth)acrylate.

[0045] Examples of (meth)acrylic carboxyl group-containing monomers include carboxyl group-containing monomers such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, and 2-(meth)acryloyloxypropyl succinic acid; and monomers other than (meth)acrylic monomers. Examples of monomers that can be appropriately used include carboxyl group-containing monomers such as crotonic acid, fumaric acid, maleic acid, itaconic acid, monomethyl maleate, and monomethyl itaconate; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; heterocyclic basic monomers such as vinylpyrrolidone, vinylpyridine, and vinylcarbazole; and vinyl monomers such as styrene, vinyl acetate, vinyl pivalate, vinyl monochloroacetate, vinyl crotonate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl caprylate, vinyl laurate, vinyl palmitate, vinyl octylate, and vinyl cinnamate.

[0046] In this embodiment, it is preferable to use (meth)acrylate monomers among (meth)acrylic monomers, specifically, it is preferable to use methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl acrylate, and 2-ethylhexyl acrylate, and it is particularly preferable to use methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate. In general, the shorter the carbon chain, the stronger the odor tends to be.

[0047] In the present embodiment, the maleimide derivative compound used as a scavenger may have a maleimide structure (group) in the compound. The maleimide structure (group) may be one or more in the compound. In the manufacturing process, the timing, method, and reaction temperature of adding the maleimide derivative compound can be appropriately selected and adjusted, but it is preferably added in the latter half of the polymerization reaction of the (meth)acrylic monomer (conversion rate of 70% or more) or at a stage when the polymerization reaction is sufficiently completed, and the reaction temperature is preferably in the range of room temperature to about 100°C. In addition, when multiple types of (meth)acrylic monomers are contained, it is preferable to add the maleimide derivative compound when the conversion rate of any one of the (meth)acrylic monomers is 70% or more. The amount of the maleimide derivative compound to be added can be appropriately selected, but it is preferably 0.05% by weight or more and 5% by weight or less, and more preferably 0.1% by weight or more and 3% by weight or less, based on 100 parts by weight of the (meth)acrylic monomer before the polymerization reaction. If the amount is too large, the maleimide derivative compound may precipitate in the resin composition.

[0048] If the amount of maleimide derivative compound added is too small, the amount of remaining (meth)acrylic monomer increases. If the amount of maleimide derivative compound added is excessive, the maleimide derivative compound remains in the final resin composition, causing a decrease in adhesive strength and precipitation. Maleimide derivative compounds that can serve as useful scavengers in this embodiment are those that have a relatively large number of maleimide groups compared to the molecular weight of the maleimide derivative compound, that is, the smaller the molecular weight per maleimide group, the higher the effect per weight. The theoretical amount of maleimide derivative compound added is preferably the above amount, but it is also possible to add a larger amount to hasten the reaction.

[0049] Taking these points into consideration, by using an appropriate amount of a maleimide derivative compound as a scavenger, it is possible to reduce the remaining amount of (meth)acrylic monomer to 1.0% by weight or less, more desirably 0.5% by weight or less, and thereby suppress odor.

[0050] As described above, the portion of the maleimide derivative compound added in this embodiment that functions as a scavenger remains in an unreacted state in the final resin composition, rather than being intramolecularly copolymerized. Note that, although it also depends on the timing of addition, if the timing of addition is too early, a part of the maleimide derivative compound will chemically react with the raw material. As a result, it is preferable that the resin composition produced in this embodiment contains at least 0.05% by weight or more of the maleimide derivative compound remaining in an unreacted state, preferably 0.1% by weight or more. It is also preferable that the resin composition produced in this embodiment contains 5% by weight or less, preferably 3% by weight or less of the maleimide derivative compound remaining in an unreacted state.

[0051] Examples of the maleimide derivative compound include aromatic maleimides having a monomaleimide structure, such as N-phenylmaleimide, 4-carboxyphenylmaleimide, 4-hydroxyphenylmaleimide, 3-hydroxyphenylmaleimide, and N-(4-anilinophenyl)maleimide; aliphatic maleimides having a monomaleimide structure, such as N-ethylmaleimide, N-butylmaleimide, N-laurylmaleimide, N-cyclohexylmaleimide, and N-(4-carboxycyclohexylmethyl)maleimide; aromatic maleimides having a bismaleimide structure, such as 4,4-bismaleimide diphenylamine; and aliphatic maleimides having a bismaleimide structure, such as N,N-dodecamethylene bismaleimide and hexamethylene glycol bis(6'-maleimide hexanoate). In particular, from the viewpoint of solubility in fluorine-based solvents, aliphatic maleimides having a monomaleimide structure are advantageous, and N-ethylmaleimide, N-butylmaleimide, N-laurylmaleimide, and N-cyclohexylmaleimide are particularly preferred. Furthermore, one of these may be used alone, or two or more may be used in combination.

[0052] The resin composition obtained by the polymerization reaction of the (meth)acrylic monomer may contain (may be added with) a crosslinking agent as necessary. A general crosslinking agent can be used, but it can be selected according to the raw materials that make up the polymer composition. Note that in order to crosslink, a pair structure is required, for example, a hydroxyl group (-OH) for acrylic acid (-COOH), and an acrylic acid or isocyanate (-NCO) for a hydroxyl group (-OH).

[0053] For example, when a carboxyl group-containing monomer such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, monomethyl maleate, or monomethyl itaconate is used as the (meth)acrylic monomer constituting the polymerization composition, an epoxy resin, a melamine resin, or a polyisocyanate can be used as the crosslinking agent.

[0054] When a hydroxyl group-containing (meth)acrylate such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, or glycerol (meth)acrylate is used as the (meth)acrylic monomer constituting the polymerizable composition, an epoxy resin, a melamine resin, a polyisocyanate, or the like can be used as a crosslinking agent.

[0055] When an epoxy group-containing monomer such as glycidyl (meth)acrylate, α-ethyl glycidyl acrylate, or 3,4-epoxybutyl (meth)acrylate is used as the (meth)acrylic monomer constituting the polymer composition, an acid, an amine, an acid anhydride, or the like can be used as a crosslinking agent.

[0056] As the (meth)acrylic monomer constituting the polymerization composition, an amino group-containing (meth)acrylate monomer such as dimethylaminoethyl (meth)acrylate or diethylaminoethyl (meth)acrylate, or a monomer containing an amide group such as (meth)acrylamide, Nt-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, diacetone acrylamide maleic acid amide, or maleimide, or a monomer having an active hydrogen group in the molecule is used, and an epoxy resin, melamine resin, polyisocyanate, or the like can be used as a crosslinking agent.

[0057] When using an isocyanate group-containing (meth)acrylate such as 2-(meth)methacryloyloxyethyl isocyanate, 2-[0-(1'-methylpropylideneamino)carboxyamino]ethyl methacrylate, 2-[(3,5-dimethylpyrazolyl)carbonylamino]ethyl methacrylate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, 2-(2-methacryloyloxyethyloxy)ethyl isocyanate, or 2-isocyanatoethyl acrylate as the (meth)acrylic monomer constituting the polymerizable composition, amine compounds, polyols, etc. can be used as crosslinking agents. One of these may be used alone, or two or more may be used in combination.

[0058] The resin composition may contain other additives as necessary, such as pigments such as titanium dioxide, inorganic or organic fillers, film-forming assistants, plasticizers, antifreeze agents, preservatives, antifungal agents, antibacterial agents, defoamers, dispersants, thickeners, leveling agents, pH adjusters, fibers, matting agents, UV absorbers, antioxidants, light stabilizers, and tackifiers.

[0059] As a method for polymerizing the (meth)acrylic monomer of this embodiment, a general polymerization method can be used, but radical polymerization is particularly preferable. The radical polymerization method can be freely selected from solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and the like, depending on the type of solvent and the form of the final liquid.

[0060] When an initiator is required for the above polymerization method, a wide range of general initiators can be used. For radical polymerization, examples include benzoyl peroxide (BPO), lauroyl peroxide (LPO), AIBN, etc. Specific product names include Niper BW, Perloyl L, Perbutyl O, Perloyl IB, and Perloyl TCP (all manufactured by NOF Corporation), and they can be selected and used appropriately.

[0061] In the present embodiment, a wide variety of general chain transfer agents can be used in the polymerization step as necessary. Specific examples include 1-butanethiol, 1-decanethiol, 1-dodecanethiol, 1-hexadecanethiol, 1-octanethiol, and thiophenol, and can be appropriately selected and used.

[0062] The polymerization reaction can be carried out without a solvent, but an organic solvent or water generally used in radical polymerization can be used. As the organic solvent, a general organic solvent such as toluene, ethyl acetate, or butyl acetate can be used. However, since general organic solvents have a flash point and an odor, hexafluorometa-xylene (HFMX) is preferable.

[0063] A wide range of general organic solvents can be selected as the solution for dissolving (diluting) the resin composition obtained in this embodiment. Among these, fluorine solvents are preferable because they have advantages such as no flash point and a fast drying speed. For example, one or more of hydrofluoroethers (HFEs), hydrofluoroolefins (HFOs), and hydrofluorocarbons (HFCs) can be selected. Among these, HFCs are preferable from the viewpoint of solubility, but many of them have high ozone depletion potential (ODP) and global warming potential (GWP), so they are used in consideration of the burden on the environment. On the other hand, HFEs and HFOs do not have ODPs and many of them have relatively small GWPs, but they are slightly less soluble than HFCs, so these points should be considered when adopting them.

[0064] Specific examples of HFEs include AE-3000 (AGC), Novec7100 (3M), and Novec7200 (3M); examples of HFCs include Solkan 365mfc (Solvay); and examples of HFOs include AS-300 (AGC) and Celefin1233Z (Central Glass).

[0065] The resin composition according to the present embodiment is characterized by a small amount of remaining (meth)acrylic monomer. In addition, since a maleimide derivative compound is used as a scavenger, the resin composition obtained in the present embodiment contains maleimide groups in the resin in the molar ratio of the addition amount. Even if the maleimide derivative compound or its reaction product remains, it does not become compatible with or react with the polymerized compound of the (meth)acrylic monomer. Therefore, when the resin composition is used as an adhesive, the maleimide derivative compound has little effect on its adhesive properties.

[0066] <Resin composition manufacturing method> The method for producing a resin composition according to the present embodiment includes a polymerization step and a maleimide derivative adding step.

[0067] [Polymerization step (I)] (Polymerization of Monomers) In a reactor having a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube, for example, under a nitrogen atmosphere, a (meth)acrylic monomer is dissolved in a polymerization solvent. Furthermore, an initiator is added, and the temperature is raised to a desired polymerization temperature (for example, within a range of 10 to 220 degrees, specifically within a range of 50 to 120 degrees). The polymerization temperature may be set based on the 10-hour half-life temperature of the initiator: T10 (the temperature at which half of the initiator is decomposed in 10 hours). In practice, the temperature is set within a range of about T10±20°C with respect to T10.

[0068] After the temperature is increased, polymerization is carried out for a desired time (for example, within a range of 3 to 50 hours) while controlling the temperature so that the temperature of the reaction solution is always within the polymerization temperature range while checking the heat generated by polymerization. This results in a polymerization reaction solution. In this polymerization reaction solution, the (meth)acrylic monomer remains.

[0069] [Maleimide derivative addition step (II)] (Preparation by adding additional initiator) The polymerization reaction solution obtained in the polymerization step (I) is heated to a temperature higher than the polymerization temperature (for example, 90° C.), and an initiator is added under normal pressure and nitrogen atmosphere, followed by stirring for a predetermined time (for example, 60 minutes).

[0070] (Addition of maleimide derivative compound) Thereafter, a maleimide derivative compound is added as a scavenger and stirred for a predetermined time (for example, 10 minutes to 5 hours). During this time, the remaining (meth)acrylic monomers undergo a polymerization reaction with each other. As a result, almost no (meth)acrylic monomer remains in the polymerization reaction solution. Specifically, the amount of remaining (meth)acrylic monomer is 1.0% by weight or less, and more preferably 0.5% by weight or less.

[0071] In this embodiment, the "end" of the polymerization step (I) means that no further polymerization reaction occurs. In this embodiment, since sufficient time is ensured in the polymerization step (I), the polymerization step (I) is once ended. Therefore, the polymerization reaction (second polymerization reaction) of the (meth)acrylic monomer remaining in the polymerization reaction solution is promoted by performing the maleimide derivative addition step (II) after the polymerization step (I) is ended. In this embodiment, the maleimide derivative compound is added after the polymerization reaction of the (meth)acrylic monomer is ended in the polymerization step (I), but the present invention is not limited thereto. For example, in the polymerization step (I), the maleimide derivative compound may be added in an overlapping manner even during the polymerization reaction, as long as the conversion rate of the (meth)acrylic monomer is 70% or more. More preferably, the maleimide derivative compound is added when the conversion rate of the (meth)acrylic monomer is 90% or more. More preferably, the maleimide derivative compound is added when the conversion rate of the (meth)acrylic monomer is 95% or more. When a plurality of types of (meth)acrylic monomers are contained, it is preferable to add the maleimide derivative compound when the conversion rate of any one of the (meth)acrylic monomers is 70% or more.

[0072] Examples and Comparative Examples Next, the resin compositions of Examples 1 to 12 were produced by the resin composition production method of this embodiment, and the results of examining their properties are shown below. The compositions of the raw materials used in Examples 1 to 12 and the examination results are shown in Figure 1. The abbreviations of the (meth)acrylic monomers in Figure 1 and the carbon numbers of their ester or carboxylic acid moieties are as follows: Ethyl acrylate (EA / Ethyl acrylate): carbon number 2 Butyl acrylate (BA / N-butyl acrylate): carbon number 4 2-Ethylhexyl acrylate (2EHA / 2-Ethylhexyl acrylate): carbon number 8 Isooctyl acrylate (IOA / Isooctyl acrylate): Carbon number 8 Methyl methacrylate (MMA / Methyl acrylate): Carbon number 1 Decyl acrylate (DA / Decyl acrylate): Carbon number 10 Lauryl acrylate (LA / Lauryl acrylate): Carbon number 12 Vinyl acetate (VAc): carbon number 2 Acrylic acid (AA / acrylic acid): carbon number 1 Hydroxyethyl acrylate (HEA / Hydroxyethyl acrylate): Carbon number 2 Perfluorohexylethyl acrylate (C6FA / Perfluorohexylethyl acrylate): Carbon number 6

[0073] Example 1 [Polymerization step (I)] <Polymerization of Monomer> In a reactor having a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube, 85 parts by weight of butyl acrylate (BA), 15 parts by weight of methyl methacrylate (MMA), and 173 parts by weight of hexafluorometaxylene (HFMX) as a fluorine-based solvent for polymerization were charged under a nitrogen atmosphere, and 0.2 parts by weight of initiator lauroyl peroxide (LPO) was added and heated to 70°C. After confirming the heat generation due to polymerization heat, polymerization was performed for 20 hours while controlling the temperature so that the temperature of the reaction solution was always 70±5°C, and a polymerization reaction solution was obtained. In the polymerization reaction solution after 20 hours, the monomer conversion rate was 100% for MMA and 97.6% for BA. In other words, it was confirmed that 2.4% of BA remained. In the polymerization step (I), it is preferable to react until the conversion rate reaches 95% or more. The method for measuring the conversion rate will be described later.

[0074] [Maleimide derivative addition step (II)] <Addition of additional initiator> The polymerization reaction solution obtained in the step (I) was heated to 90° C., and 0.1 parts by weight of an initiator LPO was added under normal pressure and a nitrogen atmosphere, followed by stirring for 60 minutes. <Addition of scavenger> Thereafter, 2 parts by weight of N-ethylmaleimide was added as a scavenger, and the mixture was stirred for 60 minutes.

[0075] [Verification step (III)] <(Meth)acrylic monomer conversion measurement>

[0076] After the stirring was completed, about 1 g of the reaction liquid was sampled, and the conversion rate of the BA monomer was confirmed by the following method. (Step 1) The reaction solution before polymerization in the polymerization step (I) was diluted with tetrahydrofuran (THF) and subjected to gas chromatography (GC) measurement using a Shimadzu Gas Chromatograph GC02014 under the measurement conditions of a heating rate of 20°C / min, from 50°C to 250°C. (Step 2) The area ratio (monomer / HFMX) of the (meth)acrylic monomer component to the polymerization solvent obtained in the measurement of step 1 was calculated and recorded. This is defined as the "pre-reaction area ratio S0." (Step 3) At each verification timing, such as after the end of the polymerization step (I) and after the end of the maleimide derivative addition step (II), the polymerization reaction solution was sampled and the same operations as those in steps 1 and 2 were carried out to calculate and record the area ratio of the (meth)acrylic monomer component to the polymerization solvent (monomer / HFMX). These values ​​were defined as the "post-reaction area ratio Si." (Step 4) The value obtained by the following calculation was regarded as the conversion rate (%) at each verification timing. Calculation formula: {1-(S0-Si) / S0}×100(%) In the table of FIG. 1, when a plurality of (meth)acrylic monomers are used and the conversion rates of the (meth)acrylic monomers are different, the average value of the conversion rates of the (meth)acrylic monomers is shown.

[0077] <Evaluation of the effect of adding maleimide derivative compounds in reducing the amount of remaining monomer> After the addition of the maleimide derivative compound, i.e., after the completion of the maleimide derivative addition step (II), the conversion rate of the (meth)acrylic monomer was 99.5% or more, 99.0% or more but less than 99.5%, and x, respectively. When multiple types of (meth)acrylic monomers were used and the conversion rates of the (meth)acrylic monomers differed, the conversion rate of the one with the fewer carbon chains (the one with the stronger odor) was used for evaluation.

[0078] <Odor Intensity Evaluation> The odor caused by the residual monomer in the resin composition was scored by sensory evaluation. The judging method in the sensory evaluation was as follows: 1 was a good case where almost no odor was detected, 3 (standard) was a case where a slight odor from the monomer remained, 5 was the strongest odor (similar to that of Comparative Example 5), 2 was intermediate between 1 and 3, and 4 was intermediate between 3 and 5. Each sample was quantified by five people using this judging method, and the average was calculated. An average value of 2 or less was ◯, a value greater than 2 but less than 3.5 was △, and a value of 3.5 or more was ×.

[0079] <Evaluation of solubility in fluorinated solvents> The solvent of the resin composition solution (polymerization solution) finally obtained through the [polymerization step (I)] and [maleimide derivative addition step (II)] was distilled off to solidify it. HFE-347pc-f: 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (trade name Asahiklin AE-3000, manufactured by AGC Co., Ltd.) was prepared as a fluorine-based solvent, and 1 part by weight of each solidified resin composition was added to 99 parts by weight of the solvent, stirred at room temperature for about 30 minutes or more, and left for 24 hours to prepare a verification solution. If this verification solution is colorless and transparent and does not contain floating matter or precipitate, it is marked as ◯, if it is slightly cloudy but no floating matter or precipitate is observed, it is marked as △, and if floating matter or precipitate is observed, it is marked as ×.

[0080] <Adhesiveness evaluation> About 3 ml of the verification solution prepared for the above solubility evaluation was placed in a metal dish with a diameter of about 7 cm and dried at 130 °C for 10 hours using a thermostatic chamber. After that, a cylindrical probe was lowered using a tensile tester to press the circular end face against the adhesive coating deposited on the bottom of the metal dish to adhere it, and then the maximum pull-up stress (adhesive strength) was measured when the probe was pulled up. The material of the probe was SUS304, the radius of the circular contact surface between the probe and the adhesive coating was 5 mm, the probe's lowering speed when adhering the probe and the adhesive coating was 10 mm / sec, the adhesion load between the probe and the adhesive coating was 2 N, the pressure time between the probe and the adhesive coating was 1 second, and the probe's pull-up speed was 10 mm / sec. For the adhesiveness evaluation, the pull-up stress (adhesive strength) was measured at three arbitrary points on the adhesive coating in the metal dish, and the average value was used. An average value of 0.1kgf or more was marked as ◯, an average value of less than 0.1kgf but 0.03kgf or more was marked as △, and an average value of less than 0.03kgf was marked as ×.

[0081] <Evaluation of thickening by adding scavenger> The change in viscosity of the polymerization solution was evaluated by visual observation. If an increase in viscosity was confirmed by adding the scavenger, it was rated as "yes" and if not, it was rated as "no".

[0082] (Examples 2 to 4) The production and verification were carried out in the same manner as in Example 1, except that the type of the maleimide derivative compound used in step (II) was changed.

[0083] (Examples 5 to 8) The production and verification were carried out in the same manner as in Example 4, except that the type of the (meth)acrylic monomer used in the step (I) was changed.

[0084] Example 9 Except for changing the type of (meth)acrylic monomer used in step (I), production and verification were carried out in the same manner as in Example 4. In addition, 10 parts by weight of decyl acrylate (DA) having 10 carbon atoms was used as the (meth)acrylic monomer.

[0085] (Examples 10 to 12) The production and verification were carried out in the same manner as in Example 4, except that the amount of the maleimide derivative compound added in step (II) was changed.

[0086] Next, the resin compositions of Comparative Examples 1 to 7 were produced and their properties were examined, and the results are shown below.

[0087] (Comparative Examples 1 to 2) Decyl acrylate (DA) or lauryl acrylate (LA) was used as the (meth)acrylic monomer in step (I). In step (II), no maleimide derivative compound was added. Other than these, the same production and verification were performed as in Example 1.

[0088] Comparative Example 3 In step (I), isooctyl acrylate (IOA) and acrylic acid (AA) were used as (meth)acrylic monomers by referring to Patent Document 1. In step (II), vinyl acetate was used as a scavenger. Other than these, the production and verification were performed in the same manner as in Example 1.

[0089] Comparative Example 4 In step (I), butyl acrylate (BA) and acrylic acid (AA) were used as the (meth)acrylic monomers by referring to Patent Document 2. In step (II), triethylene glycol diacrylate was used as the scavenger. Other than these, the same production and verification were performed as in Example 1.

[0090] Comparative Example 5 The production and verification were carried out in the same manner as in Example 1, except that no scavenger was added in step (II).

[0091] Comparative Example 6 The production and verification were carried out in the same manner as in Example 5, except that no scavenger was added in step (II).

[0092] Comparative Example 7 In step (I), 2-ethylhexyl acrylate (2EHA) and perfluorohexylethyl acrylate (C6FA) were used as (meth)acrylic monomers. In step (II), no scavenger was added. Other than these, the same production and verification were performed as in Example 1.

[0093] As can be seen from Examples 1 to 12, when a maleimide derivative compound is added as a scavenger, the amount of (meth)acrylic monomer remaining in the produced resin composition is reduced, and the monomer odor can be effectively removed without deteriorating the adhesive properties of the resin product. Specifically, the conversion amount of (meth)acrylic monomer in the resin composition is 99.0% or more, preferably 99.5% or more.

[0094] As can be seen from Example 9, when a (meth)acrylic monomer having an ester moiety with more than 8 carbon atoms (specifically, decyl acrylate (DA)) is used, the adhesion and solubility (particularly solubility in fluorine solvents) are somewhat reduced.

[0095] As can be seen from Examples 1 to 12, even if a (meth)acrylic monomer having 1 to 8 carbon atoms in the acrylic group of the ester moiety is used, which is considered to have a high vapor pressure and a strong odor, the amount of the remaining monomer can be reduced by adding a maleimide derivative compound as a scavenger. As a result, when a resin composition produced using a raw material in which such a low molecular weight (meth)acrylic monomer is the main component (50% or more of the total amount of (meth)acrylic monomer) is used as an adhesive, the odor, which was previously considered impossible, can be improved. Furthermore, by using such a low molecular weight (meth)acrylic monomer as the main component, solubility in fluorine solvents can be ensured, and it becomes possible to provide a non-flammable adhesive solution.

[0096] It can be seen that the resin compositions produced in Examples 1 to 12 are widely soluble in organic solvents and alcohol-based solvents, and therefore have an advantage in terms of environmental protection.

[0097] As can be seen from Example 12, when the (meth)acrylic monomer is 100 parts by weight, the amount of the maleimide derivative compound added is preferably 0.05 parts by weight or more, and the conversion amount of the (meth)acrylic monomer can be 99.0% or more. As can be seen from Example 11, the amount of the maleimide derivative compound added is preferably 0.1 parts by weight or more.

[0098] On the other hand, as can be seen from Comparative Examples 1, 2, 5, 6, and 7, when the maleimide derivative compound is not added as a scavenger, the conversion rate of the (meth)acrylic monomer is always 98% or less. As in Comparative Examples 1, 2, and 7, the adhesive strength is reduced or the resin composition is not easily dissolved in a fluorine solvent. As in Comparative Examples 5 and 6, odor is generated. As can be seen from Comparative Example 3, when vinyl acetate is used as a scavenger, the conversion rate of the (meth)acrylic monomer can be increased to 99.4%, but the adhesive strength of the resin composition is reduced due to the residual vinyl acetate. As can be seen from Comparative Example 4, when triethylene glycol diacrylate is used as a scavenger, the conversion rate of the (meth)acrylic monomer can be increased to 99.9%. However, this triethylene glycol diacrylate promotes crosslinking between resins during the polymerization reaction, causing the resin to polymerize and become viscous. As a result, the solubility in the solvent is significantly reduced.

[0099] The resin composition of the present invention or the manufacturing method thereof is not limited to the above-mentioned embodiment, and it is needless to say that various modifications can be made within the scope of the present invention.

Claims

1. A polymerization step of producing a polymer composition by polymerizing a (meth)acrylic monomer contained in a raw material, the (meth)acrylic monomer; a maleimide derivative adding step of adding a maleimide derivative compound in a state where a conversion rate of the (meth)acrylic monomer is 97.5% or more in the polymerization step and / or in a state where the polymerization reaction of the (meth)acrylic monomer is stopped; A method for producing a resin composition comprising the steps of:

2. In the polymerization step, a (meth)acrylate monomer is used as the (meth)acrylic monomer. A method for producing the resin composition according to claim 1.

3. The (meth)acrylic monomer is one or more (meth)acrylate monomers having an ester moiety with 1 to 8 carbon atoms. A method for producing the resin composition according to claim 1.

4. In the maleimide derivative adding step, the residual amount of the (meth)acrylic monomer is reduced to 1.0% by weight or less. A method for producing the resin composition according to claim 1.

5. The method further comprises a dissolving step of dissolving the polymerized composition obtained through the maleimide derivative adding step in at least one fluorine-based solvent selected from hydrofluoroether, hydrofluoroolefin, and hydrofluorocarbon. A method for producing the resin composition according to claim 1.

6. The polymerizable composition is characterized in that it has a crosslinkable site. A method for producing the resin composition according to claim 1.

7. A method for producing a resin composition for use as an adhesive, comprising the steps of: A polymerization step of producing a polymer composition by polymerizing a (meth)acrylic monomer contained in a raw material, the (meth)acrylic monomer; a maleimide derivative addition step in which a maleimide derivative compound is added as a scavenger in the polymerization step to promote polymerization between the (meth)acrylic monomers while allowing the maleimide derivative compound to remain unreacted with the (meth)acrylic monomer by functioning as the scavenger; A method for producing a resin composition comprising the steps of:

8. a polymer composition obtained by polymerizing a (meth)acrylic monomer; A maleimide derivative compound added as a scavenger, a conversion rate of the (meth)acrylic monomer in the polymer composition is 99.0% or more due to the maleimide derivative compound, and the maleimide derivative compound remains in an unreacted state with the (meth)acrylic monomer, A resin composition used as an adhesive.

9. The (meth)acrylic monomer is a (meth)acrylate monomer, The resin composition according to claim 8.

Citation Information

Patent Citations

  • Preparation of acrylic pressure-sensitive adhesive

    JP1994287529A

  • Heat-resistant methacrylic resin and its preparation

    JP1997324016A

  • Azeotrope solvent composition and mixed solvent composition

    JP2006274173A

  • Method for free radical polymerization of vinyl monomers

    JP2009520056A