Optically finished thin high aspect ratio diamond substrates or windows and methods for their manufacture - Patents.com
By growing thin diamond films on sacrificial substrates and optically finishing them before separation, the challenges of polishing fragile, high-aspect-ratio diamond parts are overcome, facilitating efficient and cost-effective production for various applications.
Patent Information
- Application Number
- JP2021036391
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-04-07
- Filing Date
- 2021-03-08
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2036-04-18
AI Technical Summary
Polishing thin diamond films with high aspect ratios and large dimensions is challenging due to their fragility and the difficulty in holding them in place during the polishing process, which is exacerbated by their high hardness and brittleness, leading to costly and inefficient manufacturing processes.
The method involves growing thin diamond films on sacrificial substrates like silicon, which are then optically finished and polished before being separated, using CVD techniques to achieve surfaces with roughness below 10 nm and aspect ratios exceeding 100, allowing for both planar and non-planar shapes.
This approach enables the production of thin diamond substrates or windows with optically finished surfaces, reducing the risk of fracture and enabling efficient, cost-effective manufacturing of large-area, high-aspect-ratio diamond parts suitable for applications in optics, electronics, and photonics.
Smart Images

Figure 0007565235000002 
Figure 0007565235000003 
Figure 0007565235000004
Abstract
Description
[Technical field]
[0001] Interaction of Related Applications This application is a continuation of U.S. Provisional Application No. 62 / 148,339, filed April 16, 2015. and claims the benefit of U.S. Patent Application No. 15 / 093,160, filed April 7, 2016. and is incorporated herein by reference.
[0002] FIELD OF THEINVENTION The present application relates to a thin diamond film having at least one optically finished surface. The diamond film, substrate or window is The present invention also provides a diamond ?lm that has a large aspect ratio, which is de?ned as a square. The present invention relates to a method for manufacturing a film, substrate or window.
[0003] 2. Description of Related Art Diamond is the hardest material known, with a Mohs hardness of 10. This makes diamonds useful in applications such as cutting, machining, drilling, milling, etc. Diamond also has a maximum thermal conductivity of 2000-2200 W / (m K). It is the most thermally conductive material known, and this thermal conductivity allows for temperature control under extreme conditions. In addition, diamond has a low coefficient of friction, making it desirable for This coefficient of friction makes diamond a versatile material for applications such as brakes. Diamond on diamond provides a low coefficient of friction and is therefore suitable for use in harsh conditions. Diamonds are also advantageous in lubrication applications under microwave, infrared, and visible light. Diamond is an excellent optical material for transmitting light and other ultraviolet electromagnetic waves. is very stable when used as a detector of high fluence nuclear radiation. The compound may contain strong acids, strong bases, strong oxidizing agents, or strong reducing agents even under high or cryogenic conditions. Diamond is also highly inert in the chemical environments in which it is used. It is widely used in the jewelry industry.
[0004] Diamonds are a versatile and valuable material, yet their availability is limited by their natural abundance. Diamonds mined from the earth are generally single crystals, and the number of Geometric dimensions are limited in size and often require large dimensions in industrial applications. Too small. In most cases, naturally formed diamonds contain impurities and crystal defects. The crystal size is relatively large, the chemical composition is relatively pure, and the crystal defects are relatively absent. Diamond crystals are very expensive and often valuable.
[0005] Synthetic diamonds are grown in chemical reactors at extremely high pressures and temperatures. It is known that it can be commercially produced under such harsh synthesis conditions (HTHP process). Therefore, the size of the reactor is limited, as is the size of the diamond. The company has developed a number of processes, equipment and safety features related to the harsh and demanding diamond growth conditions. In most cases, the HTHP process results in high costs for Incorporation of catalytic impurities into the diamond produces diamonds with a yellowish color. However, the HTHP process cannot produce large diameter diamond wafers.
[0006] Industrially, diamonds are grown in a reactor using a process called chemical vapor deposition (CVD). In this case, suitable growth conditions are determined by microwave enhanced plasma, tungsten Hot filament, DC jet plasma, laser induced plasma, acetylene torch The CVD growth process can produce low stress films or large crack-free films. Although it is difficult to obtain diamonds of a suitable size, different substrates and / or The successful growth of thin polycrystalline diamond films on thick free-standing diamond films. are also well known in the art.
[0007] In many diamond applications, the surface of the diamond film, substrate or window is exposed to light or For the purpose of propagating electromagnetic waves, acting as a medium for sound waves, or for the purpose of transmitting light / electromagnetic waves Reflective or from electronics, photonics or optoelectronics As a substrate that removes thermal energy via bonding mechanisms such as brazing or adhesive bonding For working purposes it needs to be optically smooth.
[0008] Diamonds are one of the hardest materials in the world, so polishing them takes time. This is expensive and can generate a lot of heat. The reason for holding the diamond in place is that the heat generated by friction melts the adhesive or Diamonds are not a good choice because they can break easily. Moreover, CVD growth of diamond films, substrates or windows requires expensive capital equipment. This is a time-consuming process that grows diamond in a very small area. Therefore, CVD diamond requires high and one or more requirements for an optically finished diamond surface are met. If so, for many applications only a thin diamond substrate or window is required. Summary of the Invention [Problem to be solved by the invention]
[0009] The diamond film, substrate or window is very thin (e.g., less than 400 microns thick). ) especially where the diamond film, window or substrate is less than 400 microns thick. In general, it is difficult to hold the diamond film, substrate, or window in place during polishing. This is because the diamond film, substrate or window has at least one dimension, e.g., a diameter. This is especially true for thin diamond films, windows, etc. Or, the high aspect ratio (thickness) is exceeded beyond the limit of polishing the substrate to an optically finished surface. The ratio of maximum dimension (e.g., but not limited to, diameter) to thickness, particularly in diamond. If the aspect ratio of the diamond part is 100 or more, the diamond part can be polished and manufactured well. There are also challenges with this.
[0010] A large area diamond that is thin and optically finished on one or both sides of the diamond surface. In particular, it is necessary to manufacture glass films, windows or substrates with a maximum dimension of 30 mm or more ( For example, but not limited to, a diamond part having a diameter of 100 or more Thin (thickness less than 400 microns) or thick (400 microns) with an aspect ratio of It is necessary to fabricate a diamond film, window or substrate (thicker than 100 nm). or for electromagnetic wave management, non-planar such as domes, cones, pyramids or any non-planar shape. A diamond piece with a surface is needed to take advantage of the unique properties of diamond. do. [Means for solving the problem]
[0011] The thin diamond substrate or window described herein comprises at least one optically finished Surface roughness and aspect ratio of 100 or more, or thickness of 400 microns or less and width of 25 Includes combinations of maximum shape dimensions of mm or more.
[0012] The thickness of the thin diamond substrate or window is 400 microns or less, 350 microns or less, 3 The thickness may be 0.00 microns or less, 250 microns or less, or 200 microns or less. The maximum dimensions of the diamond substrate or window are 25mm or more, 40mm or more, 50mm or more, 60mm or more The thickness of the thin diamond substrate or window may be 1.5 mm or more, 80 mm or more, or 100 mm or more. The aspect ratio is 100 or more, 125 or more, 150 or more, 175 or more, or 200 or more. This is also fine.
[0013] The CVD diamond described herein is grown on a sacrificial substrate, e.g., made of silicon. The surface of the as-grown diamond may be optically finished as required. The grain surface is polished by conventional polishing processes to 50nm or less, 30nm or less, 20nm or less. Optical finish level with surface roughness (Ra) of 10 nm or less, 15 nm or less Then, a sacrificial substrate on which diamond will grow may be prepared (chemically and / or mechanically). and removing the diamond (mechanically) from the diamond to obtain a free-standing diamond having at least one optically finished surface. A piece of window film, substrate or window may be manufactured.
[0014] CVD diamond is optically finished (e.g., 20 nm or less, 15 nm or less, Grown on the surface of a sacrificial substrate with a surface roughness Ra of 10 nm or less, 5 nm or less, or 2 nm or less In this case, the nucleation side of the CVD-grown diamond has a surface roughness that closely matches that of the sacrificial substrate. In one example, the nucleation side of a CVD grown diamond has a thickness of 20 nm or less and a thickness of 15 nm or less. For Ra of the substrate of ≦nm, ≦10nm, ≦5nm, or ≦2nm, respectively: Ra of 50nm or less, 30nm or less, 20nm or less, 15nm or less, or 10nm or less After the diamond is grown by CVD on the surface of the sacrificial substrate, the C The VD grown diamond side may be polished, if desired, by conventional polishing processes. The CVD diamond described herein can be applied to the surface of a non-optically finished sacrificial substrate. Grown on a surface (e.g., a chemically etched and / or mechanically finished surface) In this case, the growth side surface of the CVD grown diamond is polished by a conventional polishing process. In this case, the CVD grown diamond is Optically finished surface roughness (Ra) of 20 nm or less, 15 nm or less, or 10 nm or less It has only one raised surface.
[0015] Similar processes have been used to fabricate non-planar optically finished surfaces (<50 nm, <30 nm). , 20 nm or less, 15 nm or less, or 10 nm or less of surface roughness (Ra) In one example, the non-planar surface may be a dome, a cone, or a , pyramids, aspheric surfaces, parabolic and hyperbolic surfaces, or other non-planar shapes. Also disclosed is a method for manufacturing the thin diamond window or substrate described in at least one embodiment. To grow a thin diamond substrate or window having an optically finished surface. Controlled growth conditions are also disclosed.
[0016] Various preferred and non-limiting examples or aspects of the present invention are described in the following numbered sections: stated in.
[0017] Item 1: A diamond film including at least one optically finished surface; Aspect ratio is the maximum dimension of the substrate or window divided by the thickness of the diamond film, substrate, or window. is 100 or more, the diamond film, substrate or window.
[0018] Item 2: A thickness of 400 microns or less (0.4 mm or less) and a maximum thickness of 25 mm or more 2. A diamond film, substrate or window as described in claim 1 having a large dimension.
[0019] Item 3: At least one optically finished surface is 50 nm or less, 30 nm or less , 20 nm or less, 15 nm or less, or 10 nm or less of surface roughness (Ra), 3. The diamond film, substrate or window according to claim 2.
[0020] Clause 4: The maximum dimension is 25 mm or more, 40 mm or more, 50 mm or more, 60 mm or more, Any of items 1 to 3, which is 70mm or more, 80mm or more, or 100mm or more The diamond film, substrate or window according to any one of the preceding claims.
[0021] Item 5: The thickness is 400 microns or less, 350 microns or less, or 300 microns or less. , 250 microns or less, or 200 microns or less, any one of items 1 to 4 The diamond film, substrate or window according to any one of the preceding claims.
[0022] Item 6: The aspect ratio is 125 or more, 150 or more, 175 or more, or 200 or more. 6. A diamond film, substrate or window according to any one of items 1 to 5.
[0023] Clause 7: The maximum dimension is the diameter of the diamond film, substrate or window. Item 7. A diamond film, substrate or window according to any one of items 1 to 6.
[0024] Item 8: The 1.06 micron light scattering coefficient at a distance of 34 cm from the shielding lens is 20 / cm or less, 15 / cm or less, 10 / cm or less, 7 / cm or less, or 5 / cm or less, A diamond film, substrate or window according to any one of items 1 to 7.
[0025] Item 9: Diamond nucleation density is 1.0×10 5 / cm 2 That's it, 1.0 x 10 6 / cm 2 That's it, 1.0 x 10 7 / cm 2 That's it, 1.0 x 10 8 / cm 2 or more or 1.0×1 0 9 / cm 2 The diamond ?lter according to any one of items 1 to 8 above. Room, substrate or window.
[0026] Item 10: (a) providing a silicon substrate; and (b) depositing a conductive layer on a surface of the silicon substrate. CVD growth of diamond films, substrates or windows with aspect ratios of 100 or more wherein the aspect ratio is less than the maximum dimension of the diamond film, the substrate or the window. divided by the thickness of the diamond film, substrate or window. A method for forming a diamond film, substrate or window.
[0027] Item 11: The silicon substrate is 2 mm or more, 4 mm or more, 6 mm or more, or 8 mm or more. 11. The method of claim 10, wherein the thickness of the substrate is 0.1 mm.
[0028] Item 12: Further, before step (b), 20 nm or less, 15 nm or less, 10 nm or less, Silicon substrate surface with optical finish with surface roughness (Ra) of 5nm or less or 2nm or less 12. The method of claim 10 or 11, comprising polishing the surface.
[0029] Item 13: The nucleation side of the as-grown diamond film, substrate or window is the Ra of the polished surface of the silicon substrate is larger than the Ra of the polished surface of the silicon substrate; The Ra of the surface is 20 nm or less, 15 nm or less, 10 nm or less, 5 nm or less, or 2 nm or less. R of the nucleation side of the as-grown diamond film, substrate or window is below a is 50 nm or less, 30 nm or less, 20 nm or less, 15 nm or less, or 10 nm or less, respectively 13. The method according to any one of items 10 to 12, which is as follows:
[0030] Item 14: The silicon substrate surface, the as-grown diamond film, and the substrate The nucleation side of the plate or window has a surface roughness (Ra) of 750 nm or more, respectively. Clause 10. 14. A method according to any one of claims 1 to 13.
[0031] Item 15: Further, the diamond film, the substrate or the window is still on the silicon substrate. While in the step of FIG. 1, the growth surface of the diamond film, substrate or window is thinned to 50 nm or less, 30 nm or less. Polishing is performed to a surface roughness (Ra) of 0.01 mm or less, 20 nm or less, 15 nm or less, or 10 nm or less. 15. The method according to any one of items 10 to 14, comprising the steps of:
[0032] Item 16: A surface of the silicon substrate, and the as-grown diamond film. The nucleation side of the substrate or window is non-planar, the shape of the nucleation side of the window is an inverted shape that matches the surface shape of the silicon substrate; 16. The method according to any one of items 0 to 15.
[0033] Item 17: The nucleation side of the as-grown diamond film, substrate or window is domed. , a cone, a pyramid, an aspheric surface, a parabola, or a hyperbola; 17. The method according to any one of items 10 to 16.
[0034] Item 18: Further, the grown diamond film, substrate or window may be removed from the silicon. Any one of claims 10 to 17, including a step of chemically or mechanically removing the substrate. The method according to
[0035] Item 19: The growth side of the as-grown diamond film, substrate or window is Grown diamond film, having a greater thermal conductivity than the nucleation side of the substrate or window; 19. The method according to any one of items 10 to 18.
[0036] Item 20: Further, a light pipe may be attached to the growth surface of the grown diamond film, substrate or window. applying a thermal coating to the grown diamond film, substrate and / or or removing the silicon substrate from the window, the grown diamond film, the substrate, or applying said light management coating to the nucleation side of the window. 20. The method according to any one of items 10 to 19.
[0037] Item 21: Further, the diamond film grown on the surface of a silicon substrate, the substrate or The method includes a step of cutting the silicon substrate having a window into one or more pieces. 10. The method according to any one of claims 1 to 9.
[0038] Item 22: Step (b) is a process for producing a gas containing at least one of oxygen, carbon monoxide, carbon dioxide, nitrogen and boron. and growing the diamond film, substrate, or window by CVD in an atmosphere containing at least one of 22. The method according to any one of items 10 to 21, comprising the step of:
[0039] Item 23: Before step (b), the surface of the silicon substrate is seeded with diamond particles. 23. The method according to any one of items 10 to 22.
[0040] Item 24: (1) In a bath of aqueous diamond slurry or organic diamond slurry (2) ultrasonic treatment of the silicon substrate using diamond powder; (3) diamond cutting of the silicon substrate. Any of items 10 to 23, wherein the silicon substrate is seeded with diamond particles. One method for doing this is as follows.
[0041] Item 25:(1) Submicron or micron sized diamond powder in liquid suspension (2) sonicating the silicon substrate in an ultrasonic bath comprising: Ultrasonics consisting of nanocrystalline diamond powder with an average particle size of less than 100 nm in suspension and ultrasonic treatment of the silicon substrate in a bath. 25. The method according to any one of claims 10 to 24, wherein the silicon substrate is seeded with diamond particles. The liquid suspension may be one or more of water, alcohol, hydrocarbon or other organic solvent. may include.
[0042] Item 26: The maximum dimension of the silicon substrate is 25 mm or more, 50.8 mm or more, 66 mm or more m or more, 76 mm or more, 101 mm or more, or 127 mm or more, items 10 to 25 The method according to any one of the above.
[0043] 27. The maximum dimension of the silicon substrate is the diameter of the silicon substrate. 27. A method according to any one of claims 1 to 26.
[0044] Item 28: Diamond film grown by CVD on silicon substrate, including substrate or window , 200 microns or more, 300 microns or more, 500 microns or more, 1 mm or more, 2 mm or 5mm or more in total thickness, and 20mm or more, 30mm or more, 40mm or more in diameter , 50mm or more, 75mm or more, 100mm or more, 125mm or more, or 150mm or more A diamond-silicon composite substrate. [Brief description of the drawings]
[0045] [Figure 1A] FIG. 1A is a flow diagram of an example method for CVD growth of a diamond film, window or substrate on a sacrificial substrate, in one pass of the method, only the nucleation side or surface of the grown diamond film, window or substrate has an optically finished surface, and in another pass of the method, both nucleation sides or surfaces of the grown diamond film, window or substrate have an optically finished surface. [Figure 1B]FIG. 1B is a flow diagram of an example method for CVD growth of a diamond film, window or substrate on a sacrificial substrate, where the nucleation side or surface of the grown diamond film, window or substrate does not have an optically finished surface, and the growth side or surface of the grown diamond film, window or substrate has an optically finished surface. [Diagram 2] FIG. 2 is an example of a microwave plasma CVD reactor that can be used to grow diamond films, windows or substrates on a sacrificial substrate (eg, silicon). [Figure 3A] FIG. 3A is a photograph of a diamond film, window or substrate conformally grown onto a sacrificial substrate that includes a "II-VI" pattern formed on the growth surface of the sacrificial substrate. [Figure 3B] FIG. 3B is an enlarged view of the nucleation side of the diamond film, window or substrate shown in FIG. 3A. [Figure 3C] FIG. 3C is an enlarged view of the growth side of the diamond film, window or substrate shown in FIG. 3A. [Figure 4] FIG. 4 is a graph of Raman intensity versus wavelength showing Raman graphs of the growth side center, growth side edge, nucleation side center and nucleation side edge of the diamond film, window or substrate shown in FIG. 3A. [Figure 5A] FIG. 5A is a diamond film, window or substrate of one shape conformally grown on an "inverse shape" sacrificial substrate in the microwave plasma CVD reactor of FIG. 2 following the guidelines set forth herein. [Figure 5B] FIG. 5B is a shaped diamond film, window or substrate conformally grown on an "inverse shape" sacrificial substrate in the microwave plasma CVD reactor of FIG. 2 following the guidelines set forth herein. [Figure 5C] FIG. 5C is a shaped diamond film, window or substrate conformally grown on an "inverse shape" sacrificial substrate in the microwave plasma CVD reactor of FIG. 2 following the guidelines set forth herein. [Figure 5D]FIG. 5D is a shaped diamond film, window or substrate conformally grown on an "inverse shape" sacrificial substrate in the microwave plasma CVD reactor of FIG. 2 following the guidelines set forth herein. [Figure 5E] FIG. 5E is a diamond film, window or substrate of one shape conformally grown on an "inverse shape" sacrificial substrate in the microwave plasma CVD reactor of FIG. 2 following the guidelines set forth herein. [Figure 5F] FIG. 5F is a diamond film, window or substrate of one shape conformally grown on an "inverse shape" sacrificial substrate in the microwave plasma CVD reactor of FIG. 2 following the guidelines set forth herein. [Figure 6A] FIG. 6A is an enlarged cross-sectional view (field of view=4.33 mm) of a lapped diamond-silicon composite substrate grown according to Example 3 described herein. [Figure 6B] FIG. 6B is an enlarged cross-sectional view (field of view=649.6 μm) of a lapped diamond-silicon composite substrate grown according to Example 3 described herein. [Figure 7] FIG. 7 is a photograph of a free-standing diamond film 4 grown according to Example 6 described herein, placed in a tray. [Figure 8] FIG. 8 is an SEM photograph of the nucleation side / surface of the free-standing diamond film 4 shown in FIG. [Figure 9] FIG. 9 is three graphs of the light scattering coefficient of free-standing diamond films 4 grown according to Examples 8-10, respectively, described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0046] The following examples are described with reference to the accompanying drawings, in which like reference numbers indicate similar or functionally equivalent elements. Corresponds to the element.
[0047] In one example, the diamond film, window or substrate is provided with at least one optically finished In another example, the diamond may include a curved surface and have an aspect ratio of 100 or more. The window or substrate shall have a thickness of 400 microns or less and a geometric dimension of 25 mm or more. The optically finished surface may include a combination of 50 Surface roughness Ra of nm or less, 30 nm or less, 20 nm or less, 15 nm or less, or 10 nm or less
[0043]
[0048] Diamond film, window or substrate: 25mm or more, 40mm or more, 50mm or more, Have a maximum geometric dimension of 60 mm or more, 70 mm or more, 80 mm or more, or 100 mm or more It is okay to do so.
[0049] Diamond film, window or substrate is 400 microns or less, 350 microns or less, 3 It may be 00 microns or less, 250 microns or less, or 200 microns or less.
[0050] The aspect ratio of the diamond film, substrate or window (herein referred to as diamond film) The thickness of the diamond film, substrate or window is defined as the maximum dimension of the diamond film, substrate or window relative to the thickness of the diamond film, substrate or window. (defined as 100 or more, 125 or more, 150 or more, 175 or more, or 200 or more) This is also fine.
[0051] Diamond film, window or substrate on one or both sides for transmitting visible light or electromagnetic waves The side surfaces may be optically finished. High quality diamond with low absorption of light energy. In fact, a small amount of light absorption may be desirable. According to Le's law,
[0052]
number
[0053] where A is the absorbance, I is the transmitted light intensity, I0 is the incident light intensity, and ε λ is the absorption coefficient, and l is the light path and c is the concentration of light-absorbing molecules.
[0054] One method to reduce the light absorption through a diamond film, window or substrate is to If the quality of the glass does not change, the length of the optical path, e.g., the transparent diamond film, window, or reducing the thickness l of the substrate. Also, the diamond film, window or substrate can be transparent. The light scattering during the measurement is proportional to the length of the optical path (the distance between the light and the diamond film, substrate, or window). This can be directly correlated to the thickness of the diamond film, substrate or window, if any. In this paper, a thin diamond film, a substrate, and a quartz crystal are used to absorb and / or scatter a minimal amount of light. Or the window may have both sides optically finished.
[0055] Electronics, photonics, and other devices that reflect visible light or electromagnetic waves, or for temperature control. Optical or optoelectronic devices (such as, but not limited to, laser diodes) laser diode array (bar), surface-emitting semiconductor laser, surface-emitting semiconductor laser Diamond filters are used for bonding to devices such as laser arrays and light emitting devices. At least one surface of the film, window or substrate may be optically finished. The thickness of the diamond film, window or substrate for this purpose is several (1-9) microns to several tens (1 In one example, the thickness may be in the range of 0 to 99 microns, or in the range of several hundred microns (100 to 999). The thinner the diamond film, window or substrate, the lower the cost. For processing, a diamond film, window or substrate with a thickness of 150 to 200 microns is often used. In many applications, this can be sufficient to remove thermal energy from the heat source. For example, thicker diamond films, windows or other materials than are required for applications such as electromagnetic wave reflection or temperature control. The substrate simply represents an increase in cost and is not necessarily required.
[0056] Herein, when referring to the diamond films, windows or substrates described herein, The terms diamond film, window, and substrate, individually or in combination, may be used interchangeably. This may also be done.
[0057] Diamond is a hard material, but at the same time, it is very brittle. For example, 400 x 10 -6 m or less) and when the maximum geometric dimension is large, The Monde film strips are very fragile. For example, CVD reduces their thickness and their maximum Growing large diamond film pieces alone is difficult.
[0058] One example prior art polycrystalline diamond film growth process is The process of growing a diamond film on a metal substrate at high temperatures until a specific thickness is reached Then, the coefficient of thermal expansion (CTE) of the diamond film (1×10 -6 m / mK) and the CTE of the metal substrate (4.6 × 10 for tungsten). -6 m / mK, Mori For budene, it is 5.0 x 10 -6 m / mK, etc.) due to the difference in The diamond film on the metal substrate is delaminated undesirably. If the thickness is 1 mm or more, the diamond film will avoid delamination, but this is often not desirable. Undesirable cracks occur, and the diamond parts are cut out from the diamond film (harvested). If the diamond film thickness is less than 500 microns, In this case, the problem of diamond film fracture or cracking becomes evident. When the thickness is less than 300-400 microns, (such as tungsten or molybdenum) Diamond particles that are not significantly cracked or fractured in size are removed from the metal substrate. Therefore, in the prior art, one or more optical a thin (e.g., 400×10 -6 The process for manufacturing the diamond film, window or substrate is the same as that of the conventional Assuming a thinning / polishing process is used, thick as-grown diamond films This would be an expensive growth and manufacturing process.
[0059] As mentioned above, diamond is hard and brittle. Diamond films are thin and large. If the diamond has a large dimension, e.g., diameter, it becomes fragile. Diamond is also inert. The process of polishing diamonds mainly involves mechanical forces that require diamond particles. Therefore, especially when the diamond thickness is less than 400 microns and the maximum dimension is For example, if the diameter is 40 mm or more, a thin piece of diamond is placed in place during grinding. It becomes difficult to hold the diamond film. The thickness of the diamond film becomes thinner (e.g. 300 μm). In the case of diamonds with a maximum dimension of 25 mm or more, it is almost impossible to grind diamond pieces with a maximum dimension of 25 mm or more. Therefore, in the conventional method, the maximum dimension is significant and at least one To produce a thin diamond film, window or substrate piece having an optically finished surface To achieve this, it is expensive to use a thick piece of as-grown diamond wafer. But it is also difficult.
[0060] Fabricating thin diamond films, substrates or windows following the guidelines set forth herein An example method is shown in the flow diagram of Figures 1A and 1B. For example, a large diameter sacrificial substrate (eg, silicon) is used.
[0061] Referring to FIG. 1A, a diamond foil having one or both optically finished surfaces is shown. An example of producing a film will be described with reference to the flow diagram of FIG. 1A.
[0062] In step 100, a substrate is provided having at least one optically finished surface. In step 102, the optically finished surface is optionally polished with diamond particles. In step 104, the surface is optically finished. The substrate having the seeded surface (seeded or unseeded) is then placed in a CVD growth apparatus ( For example, it is placed inside a CVD reactor 16) as shown in FIG. A bond film is grown on the substrate by CVD.
[0063] In one example, a diamond film has one optically finished surface (the nucleation surface). If it is desired to have a chemically and / or mechanically modified substrate material, following step 106, Step 116 is performed in which the nucleation surface of the diamond film is optically fine. Since CVD growth occurred on the elevated substrate surface, removal of the substrate in step 116 At step 118, a free-standing diamond is formed having an optically finished surface on one side (the nucleation side). Produce a film.
[0064] In one example, it is desirable to have an optically finished growth surface of the diamond film. If so, proceed to step 106 and remove the diamond while the diamond film is still on the substrate. A step 108 is performed of polishing the growth surface of the diamond film. When it is desired to produce a composite substrate comprising a diamond growth surface and a layer of substrate material, Following step 108, the substrate layer is thinned and bonded to a substrate and polished to an optically finished datum. A step 114 is performed to produce a composite substrate including a growth surface of the diamond film.
[0065] Alternatively, it may be desirable to have a diamond film with an optically finished surface on both sides. If so, step 108 is followed by a step in which the substrate material is chemically and / or mechanically removed. 110 is performed. The nucleation surface of the diamond film is then exposed to the optically finished substrate surface. The diamond film is grown on the surface by CVD and the growth surface of the diamond film is polished in step 108. Thus, removal of the substrate in step 110 results in removal of both optically finished surfaces in step 112. The method produces a free-standing diamond film having two crystallographically distinct sides (a growth side and a nucleation side).
[0066] Now, referring to FIG. 1B, a diamond having an optically finished surface on its growth surface is shown. An example of manufacturing a glass film is described below. In step 200, an optically finished surface is A bare substrate is provided. In step 202, a diamond film is grown by CVD. The substrate surface is optionally polished with diamond particles and / or diamond cutters. Next, in step 204, the substrate (seeded or unseeded) is The substrate (1) is placed inside a CVD growth device (for example, the CVD reactor 16 shown in FIG. 2). In step 206, a diamond film is grown by CVD on the substrate.
[0067] In step 208, the growth surface of the diamond film is etched to a surface where the diamond film is still growing. The diamond film is bonded to a substrate and polished to an optical finish. If it is desired to fabricate a composite substrate including a film growth surface, proceed to step 210 and form a substrate. The plate is thinned to produce the composite substrate.
[0068] To produce a free-standing diamond film having a single optically finished surface If desired, proceed from step 208 to step 212 and chemically and / or mechanically treat the substrate. Then, in step 214, a diamond foil having an optically finished surface is removed. The growth surface of the film and the nuclei growing on the side of the substrate that does not have an optically finished surface. The nucleation of diamond films with optically unfinished surfaces is achieved by the growth side. A free-standing diamond film with a grown side is fabricated.
[0069] The coefficient of thermal expansion (CTE) of silicon is approximately 3.0×10 -6 m / mK, while The CTE of diamond is approximately 1.0×10 -6 m / mK. Diamond Film Diamond films are generally grown at high temperatures on a substrate (sacrificial or permanent). When the growth of diamond is completed, the temperature is substantially reduced from the diamond growth temperature to room temperature, and ,The CTE mismatch between the grown diamond film and the substrate (e.g., silicon) This usually results in cracking of the diamond film and / or the substrate. This is particularly serious when one or more dimensions of the substrate are large. Unlike silicon (tungsten and molybdenum), silicon is brittle and difficult to grow during the CVD diamond growth process. During the process, the CVD plasma cannot remain on the substrate.
[0070] In the following Comparative Example 1, a silicon wafer (6 inches in diameter, 625 microns thick) was The diamond films were grown on the sacrificial substrates. Unfortunately, the plasma preparation process During the process, each of these silicon wafers fractured.
[0071] Surprisingly, only a thick (>2 mm) piece of sacrificial substrate, e.g. a silicon disk, In one example, a silicon disk was found to be able to withstand the plasma conditioning process. The thickness of the screen is 2mm or more, 4mm or more, 6mm or more, or 8mm or more. It may be a thickness.
[0072] In another example, a substrate having an optically finished surface for CVD diamond growth, e.g. A sacrificial substrate, such as silicon, is used. After CVD diamond is grown on the sacrificial substrate, The sacrificial substrate is chemically (by etching agents or hydrogen fluoride) and / or mechanically (by polishing and / or is removed (by lapping), resulting in an optically A finished diamond surface (on the nucleation side) is obtained. This results in Efficient and economical production of thin pieces of free-standing diamond film with optically finished surfaces can be manufactured in
[0073] In another example, while the diamond film is still on the sacrificial substrate (e.g., silicon), The as-grown diamond (growth) surface (opposite the nucleation side) is polished. The total thickness of the diamond film and sacrificial substrate combined is approximately 100 mm, which is the same as the conventional polishing process. The combination is achieved without significant risk of the diamond film fracturing during the process. The thickness can be sufficient to allow the alignment to be held and polished. After achieving an optical finish on the growth side of the bond film, the diamond film and the sacrificial The assembly with the sacrificial substrate is then subjected to a process of chemically and / or mechanically removing the sacrificial substrate. At the end of this process, a thin piece of diamond film is optically It has raised surfaces on both sides (growth and nucleation).
[0074] The growth side of the polycrystalline diamond film is better than the nucleation side of the diamond film. In this case, only the growth surface of the diamond is exposed to light. Therefore, in another example, the lens is not optically finished (e.g. , chemically etched and / or mechanically lapped surfaces) sacrificial materials such as silicon A sacrificial substrate may be used as the sacrificial substrate.
[0075] In one example, the nucleation side of a piece of diamond film grown on a sacrificial substrate is coated with another It can have good thermal conductivity compared to conventional temperature management materials. Therefore, it can be optically finished. It is sufficient to have a nucleation side of the diamond surface that is raised. A sacrificial substrate such as silicon having an optically finished surface on the nucleation side of the diamond film. After the diamond film has grown, the growth surface (opposite the nucleation side) is Depending on the application, flat lapping may be performed followed by chemical etching and / or mechanical lapping / The sacrificial substrate can be removed by polishing. This process results in a much faster process than conventional polishing. Without relying on processes, the risk of the diamond film fracturing or breaking during polishing is avoided. A thin (e.g., 400×10 -6 m or less) This may result in a diamond film.
[0076] In another example, a diamond is deposited on a sacrificial substrate having at least one optically finished surface. After CVD growth of the diamond film, photoelectron microscopy of the diamond film (after removal of the sacrificial substrate) Chemically finished (nucleation) surfaces can be used, for example, for anti-reflection coatings, beam splitters, etc. The lens may be covered with a light management coating such as a total reflector coating or a total reflective coating. Such diamond films can be laser-cut to different geometric dimensions suited to specific applications. Laser cutting may be performed while the diamond layer is still attached to the sacrificial substrate (e.g., silicon). This can be done while the diamond is still on the surface, before laser cutting. The surfaces may be lapped and / or polished, if desired.
[0077] In one example, the diamond film is of optical quality (having an absorbance of 0.5 / cm or less, In one example, the absorption of electromagnetic waves such as infrared light, near infrared light, visible light, or ultraviolet light is low. The diamond film may also have a low loss tangent for microwave applications. (1×10 -2 In one example, the diamond film also has a loss tangent of Mechanical and / or thermal grade diamond (may be dark, e.g. 800W / In one example, the diamond ?ber may have a thermal conductivity of 100 kPa or more. The rum also uses detector grade diamond (with charge collection distances of 100 microns or more). The diamond may be of a grade of diamond (e.g., SiO2 ...
[0078] In one example, diamond films are formed using a microwave-assisted plasma CVD process, a thermal field lamination CVD process, thermal spray CVD process, arc discharge plasma CVD process , DC thermal plasma CVD process, high frequency plasma CVD process, water plasma CVD process, acetylene torch CVD process, ultra-high frequency plasma CVD process, etc. It is also possible to grow it by doing the above.
[0079] In one example, the growth temperature of the diamond film is in the range of 600°C to 1300°C or higher. In one example, the growth rate of the diamond film may be in the submicron to 20 microns per hour range. In one example, the CVD growth of diamond films The methane concentration for this purpose may range from less than 1% to 5% in hydrogen. So, other additives such as oxygen, carbon monoxide, carbon dioxide, nitrogen, boron, etc. are also in the CVD growth apparatus for the purposes of diamond growth rate control and / or diamond quality control. May be added.
[0080] In one example, a silicon substrate, either optically finished or not, is used. The surface of a sacrificial substrate such as a silicon wafer is treated with ultrasonic waves using diamond particles to form a hydrated diamond layer. Diamond powder or slurry using organic diamond slurry The seeding may be performed by grinding with a sharp edge or by diamond cutting.
[0081] In one example, a sacrificial substrate such as silicon for diamond growth is 25 mm or more in diameter and Diameter 2 inches (50.8 mm) or more, diameter 66 mm or more, diameter 3 inches (76.2 mm) or less Above 4 inches (101.6 mm) in diameter or more, or 5 inches (127 mm) in diameter or more This is also fine.
[0082] In one example, the thickness of the sacrificial substrate, such as silicon, is 2 mm or more, 4 mm or more, 6 mm or more, or It may be 8 mm or more.
[0083] In one example, the surface of a sacrificial substrate (e.g., silicon) is optically finished and chemically etched. and / or mechanically finished, for example by lapping and / or polishing. In one example, the surface roughness of the optically finished surface of a sacrificial substrate (e.g., silicon) may be The thickness Ra is set to 20 nm or less, 15 nm or less, 10 nm or less, 5 nm or less, or 2 nm or less. This is also fine.
[0084] In one example, a dome requiring an optically finished surface, e.g., of diamond structure. (Figure 5A), cone (Figure 5B), pyramid (Figure 5C), aspheric (Figure 5D), parabolic (Figure 5E), hyperbola (FIG. 5F), or other non-planar shapes of diamond structures. In this case, it is difficult to polish the diamond surface. Even if it were possible, the thickness Grinding a piece of diamond block of large dimensions into such a non-planar shape is This requires excessive time and cost, and results in excessive wasted diamonds. For example, in one example, CVD diamond is used to create an optically finished surface profile for the final die. On a sacrificial substrate (e.g., silicon) that has the inverse of the desired contour and shape of the diamond substrate. After diamond growth, the sacrificial substrate (e.g., silicon) may be etched (e.g., For example, with KOH or HF) and / or by polishing and lapping. In one example, a diamond film is grown by CVD. The contours of the non-planar surfaces of the sacrificial substrate that can be fabricated are then cut using a diamond cutting process or a common optical fabrication process. The non-planar surface of the sacrificial substrate may be fabricated by one or more of the common fabrication processes. The material may be fabricated into any suitable and / or desired shape that may be formed using a manufacturing process. Such shapes include, for example, a dome (Figure 5A), a cone (Figure 5B), a pyramid (Figure 5C), Including aspheric (FIG. 5D), parabolic (FIG. 5E), hyperbolic (FIG. 5F), or other non-planar shapes .
[0085] Examples of diamond films described herein include optical windows for light / electromagnetic wave management; Substrates for thermal management of electronics, photonics and optoelectronics; Substrates for uses including activation, acoustic wave management, electromagnetic wave management, friction control and detectors; and Mechanical applications such as, but not limited to, milling, cutting, drilling, lathing, etc. It may also be used as a material for
[0086] In another example, the diamond film, substrate or window is 34 cm away from the shielding lens. The 1.06 micron light scattering coefficient is 20 / cm or less, 15 / cm or less, 10 / cm or less, Such a light scattering coefficient may be 7 / cm or less, or 5 / cm or less. It may be suitable for temperature control applications, acoustic control applications, etc.
[0087] In another example, the diamond film, substrate or window may have a diameter of 1.0×10 5 / cm 2 That's it, 1 .0×10 6 / cm 2 That's it, 1.0 x 10 7 / cm 2 That's it, 1.0 x 10 8 / cm 2 End or 1.0×10 9 / cm 2 The diamond nucleation density may be equal to or greater than 100 nm. Such diamond nucleation density is important for acoustic wave propagation for sound control, phono for temperature control, and Such diamond nuclei may be suitable for photon propagation for light management. The resulting density is also important for mechanical applications, chemical inertness where low porosity is desirable, surface friction control, etc. It may be suitable.
[0088] The following examples and comparative examples are offered by way of illustration and not by way of limitation.
[0089] Scanning electron microscope (SEM) images were taken using an Energy Dispersive X-ray (EDAX) detector. The results were obtained using a scanning electron microscope equipped with
[0090] The Raman spectra were obtained by Raman microscopy (confocal). It is widely used as a standard for evaluating diamonds, single crystals or polycrystals. Each of the forms (allotropes) that can be used (e.g., diamond, graphite, buckyball, etc.) It has easily distinguishable characteristics. By combining photoluminescence (PL) technology, Raman spectroscopy can be used to determine phase purity, crystal size and orientation, defect levels and structure, and impurity types. Nondestructive methods for evaluating various properties of diamond, including the concentration and stress, as well as strain In particular, the 1332 cm -1 Width of the primary diamond Raman peak (half The full width at half maximum (FWHM) is the Raman intensity ratio between the diamond peak and the graphite peak ( 1350cm -1 D band and 1600 cm -1 As with the G-band, diamond It is a direct indicator of the quality of the diamond particles and the film. The peak shift of diamond Raman can be estimated from the Raman peak shift of diamond. The change in the Dramman peak shift is about 3.2 cm -1 / GPa, and low under tensile stress. It has been reported that the peak shifts to a higher wave number under compressive stress. The Raman spectra shown were obtained using a Raman spectrometer equipped with a 514 nm excitation laser. .
[0091] The surface roughness (Ra) of the polished diamond film piece or silicon piece ) and Peak-to-Valley (PV) measurements were taken using an interference filter with a 20x objective lens. The area measured was 200 microns by 350 microns.
[0092] The enhancement of chemical vapor deposition of diamond by microwave plasma has been demonstrated in the art. FIG. 2 shows a method for growing polycrystalline diamond using the method described herein. An example of a microwave plasma CVD system 2 that can be used to grow 4 FIG. 2 is a schematic diagram showing a CVD system 2 according to the present invention. A mixture of reactive gases 6 containing fluorine is flowed into a microwave plasma CVD reactor 16. The flow rate of the mixture of exhaust gas 1 and reactive gas 6 is regulated by a mass flow controller 8. 0 flows from the CVD reactor 16 primarily to the vacuum pump 12. is typically generated by a magnetron 14 and passes through a quartz window 18 into a CVD reactor 16 Within the reactor 16, the microwave energy is converted into a plasma 20, The hydrogen molecules of the reactive gas 6 are radicalized into hydrogen free radicals, and similarly, the reactive gas 6 methane molecule into methyl free radical, methylene free radical, methine free radical and radicalize it into secondary or tertiary free radicals containing two or more carbon atoms. The bottom of reactor 16 supports a substrate 24 on which polycrystalline diamond film 4 is grown. A substrate holder 22 or base is placed on the substrate. A substrate 24 of tungsten, tantalum, or a suitable carbide former as required is placed in a substrate holder. The sensor 22 may be disposed on the sensor 22.
[0093] During generation of the plasma 20, the free radicals containing carbon species are radicalized to form the carbon atoms of the substrate 24. They impact the surface and the carbon species settles there through a mechanism known as "hit and stick." The hydrogen free radicals generated by the plasma 20 are fixed molecules that still contain hydrogen atoms. Collisions with surface carbon species remove hydrogen atoms from these fixed carbon species, resulting in a larger number of hydrogen atoms. The surface carbon atoms are then abstracted until all hydrogen atoms are abstracted to form fewer C-C bonds. Forming free radicals. Some pure carbon-carbon bonds are sp in nature. 3 and Some pure carbon-carbon bonds are obtained, which is desirable for the diamond lattice. Qualitatively sp 2which is undesirable since it is inherently found in graphite. However, hydrogen free radicals are sp 3 To remove carbon from the diamond lattice Faster than sp 2 Carbon can be removed from the graphite seeds.
[0094] The size of the plasma 20 is adjusted to be large enough to cover the surface of the substrate 24. In the case of a diamond growth method, the concentrations of hydrogen and methane in the reactive gas 6 mixture influence the diamond growth temperature as well as the growth temperature. It is well known in the art that β-acetylglucosamine is a critical parameter for monad growth. The microwave energy and pressure in the reactor 16 are highly dependent on the substrate size. Those skilled in the art can easily produce high quality diamond films by following the procedures and instructions set forth herein. The plasma 20 is then introduced into substrates 24 of different sizes for the purposes of window or substrate seeding, deposition and growth. You should be able to adjust it to the appropriate size, large enough to cover the
[0095] In the following examples and comparative examples, the symbols shown in FIG. 2 represent the same or functionally equivalent Used for elements.
[0096] Example 1: Method for producing diamond films with one optically finished surface
[0097] 3A-3C, and still referring to FIG. 2, in one example, a 66 mm diameter, The 11.5 mm thick monocrystalline silicon pieces were produced using a standard silicon manufacturing method. The silicon substrate 24 was used as the silicon substrate 24. The surface 1 of the substrate 24 was diamond cut to obtain a Ra The diamond-like surface is 6-7 nm thick and has an optically finished surface. The logo "II-VI" is also made of diamond. The grooves are cut into the surface 1 of the silicon substrate 24 in a "II-VI" pattern. The silicon substrate 24 was then diamond turned and optically finished. The substrate was placed in a CVD reactor 16 with the surface (surface 1) facing the quartz window 18. and methane, e.g., 1,850 mL / min hydrogen and 13.6 mL / min methane. A mixture of reactive gases 6 containing the reactive gases 6 is subjected to microwave plasma under the control of a mass flow controller 8. The plasma 20 was then allowed to flow into the CVD reactor 16. After the plasma 20 was generated, the size of the plasma 20 was gradually increased. The output of the magnetron 14 and the pressure of the reactor 16 are adjusted so as to cover the surface 1 of the silicon substrate 24. The diamond growth temperature at the center of the silicon substrate 24 was adjusted by, for example, The temperature was controlled at 800° C. using a thermometer 26. After 168 hours of diamond growth, the growth reaction The polycrystalline diamond film 4 having a thickness of 285 microns is then deposited on the silicon substrate 24. The diamond film 4 is then deposited on the silicon substrate 1. The plate was peeled off using a KOH aqueous solution at high temperature, followed by peeling off using HF-HNO3. A free-standing diamond film 4 having a thickness of 285 microns and an aspect ratio of 231 was obtained. The nucleation surface of the free-standing diamond film 4 grown on the surface 1 of the silicon substrate 24 is 9 It is measured to have a surface roughness (Ra) of .1 nm and is considered optically finished. Ta.
[0098] FIG. 3A shows the nucleation surface or side of a free-standing diamond film 4 that is optically transparent. As can be seen in FIG. 3A, in the diamond cut grooves on the surface 1 of the substrate 24, The "II-VI" logo, which has grown to fit the The non-planar surface of the room 4 may be readily fabricated using one or more conventional manufacturing methods. By growing diamond on a "reverse" surface (e.g. silicon) Importantly, the diamond film shown in FIG. The non-planar (nucleation) surface of film 4 is optically finished. Micrographs of the nucleation side (Ra=9.1 nm) and growth side of diamond film 4 shown in It is.
[0099] In another example, a second piece of single crystal silicon, typically 66 mm in diameter and 11.5 mm thick, is The silicon substrate 24 was manufactured by a conventional silicon manufacturing method. Surface 1 was diamond turned to an optically finished surface with Ra of 6-7 nm. The entire silicon substrate 24 including the surface 1 is then immersed in a diamond ethanol suspension slurry. The silicon substrate 24 was then subjected to ultrasonic treatment using a diamond cutting machine. The substrate was then placed in the CVD reactor 16 with the polished surface (surface 1) facing the quartz window 18. Hydrogen and methane, e.g., 1,850 mL / min hydrogen and 13.6 mL / min A mixture of reactive gases 6 containing methane is fed into the microchannel under the control of a mass flow controller 8. The plasma 20 was then introduced into the microwave plasma CVD reactor 16. After the plasma 20 was generated, the plasma 20 The output of the magnetron 14 and the size of the reactor are set so that the surface 1 of the silicon substrate 24 is covered by the size of the reactor. The pressure of 16 was adjusted. The diamond growth temperature at the center of the silicon substrate 24 was adjusted by, for example, For example, the temperature was controlled at 800°C by a photothermometer 26. After 148 hours of diamond growth, (The diamond growth reaction was stopped.) A polycrystalline diamond film with a thickness of 233 microns was obtained. Film 4 was conformally deposited on the surface of silicon substrate 24 facing quartz window 18. The silicon substrate 24 is peeled off from the diamond film 4 using a KOH aqueous solution at high temperature. Then, it was peeled off using HF-HNO3, and the diameter was 66 mm, the thickness was 233 microns, and the aspect ratio was A free-standing diamond film with a thickness ratio of 283 was obtained. The nucleation surface of this free-standing diamond film 4 had a surface roughness (R a) and was considered optically finished.
[0100] The quality of the diamond film 4 in this latter example was confirmed by Raman spectroscopy, as shown in Figure 4. As shown in Figure 4, the growth side of the diamond crystal was approximately 2.8 cm -1 of Narrow FWHM (FWHM of single crystal diamond piece is 3.5cm -1 (compared to As can be seen, the quality is excellent, with the Raman peaks centered at 1331.9–1332.1. cm -1 This suggests that there is no stress in the diamond film 4 on the growth side. The diamond crystals on the growing side are also about 3.8 to 4.1 cm -1 This is evidenced by the FWHM of The Raman peak is centered at 1331.6 cm -1 And the nuclear It is shown that the stress is low in the diamond film 4 on the generating side.
[0101] Example 2: Fabrication of diamond films with optically finished one or two surfaces Construction
[0102] In another example, a piece of monocrystalline silicon 2 with a diameter of 2 inches (50.8 mm) and a thickness of 10 mm is The silicon substrate 24 was fabricated using a general silicon fabrication method. Both surfaces of the silicon substrate 24 are optically finished by a conventional chemical mechanical polishing process. The silicon substrate 24 was then entirely covered with diamond (0 The silicon substrate 2 was then sonicated in a 2.25 micron (1.0001 μm) ethanol suspension slurry. 4 in a CVD reactor 16 with one of the optically finished surfaces facing the quartz window 18. A mixture of reactive gases 6, e.g., hydrogen at 1,850 mL / min and 13.6 Methane was flowed into the microwave plasma CVD reactor 16 at a rate of mL / min. After the plasma 20 starts to be generated, the size of the plasma 20 increases to the surface of the silicon substrate 24 facing the quartz window 18. The output of the magnetron 14 and the pressure 16 of the reactor were adjusted so as to cover the surface of the silicon substrate. The diamond growth temperature at the center of the plate 24 is measured, for example, using a photometric pyrometer 26 at 8°C. After 140 hours of diamond growth, the growth reaction was stopped and the quartz window 18 was A thickness of 200 to 220 microns is deposited conformally on the surface of the opposing silicon substrate 24. A polycrystalline diamond film 4 was obtained. The growth surface of the diamond film 24 was , lapping and polishing while the diamond film 24 is still on the silicon substrate 24. After lapping and polishing, the surface roughness of the silicon substrate 24 was The thickness of the diamond film 4 was about 125 microns. was peeled off from the diamond film 4 using aqueous KOH at high temperature, followed by HF-HN Peeled off using O3, 2 inch (50.8 mm) diameter, 125 micron thickness, aspect ratio The free-standing diamond film 4 was obtained with a ratio of 406. The side surfaces are of optical finish quality and can be used as optical windows or substrates for other applications. can.
[0103] In another example, a second tube of monocrystalline silicon with a diameter of 2 inches (50.8 mm) and a thickness of 10 mm was used. A piece was fabricated using standard silicon manufacturing methods and used as the silicon substrate 24 . Both surfaces of the silicon substrate 24 are optically polished by a conventional chemical mechanical polishing process. The silicon substrate 24 was then entirely finished to a surface roughness of less than 1 nm. The silicon substrate 24 was then ultrasonically treated in a slurry of 1000g of methanol. Place the wafer in a CVD reactor 16 (FIG. 2) with one of the finished surfaces facing the quartz window 18. A mixture of reactive gases 6, e.g., hydrogen at 2,700 mL / min and methane was supplied to the microwave plasma CVD reaction vessel under the control of the mass flow controller 8. After the plasma 20 was generated, the size of the plasma 20 was increased by 1 / 2 mm from the quartz window 18. The output of the magnetron 14 and the reactor 1 are arranged so as to cover the surface of the silicon substrate 24 facing the magnetron 14. The pressure in the gas chamber 6 was adjusted. The diamond growth temperature in the center of the silicon substrate 24 was adjusted to, for example, For example, the temperature was controlled at 832 to 866°C using a photothermometer 26. After a long time, the growth reaction is stopped and a deposition is performed conformally on the surface of the silicon substrate 24 facing the quartz window 18. A polycrystalline diamond film 4 having a thickness of 110 to 130 microns was obtained. The growth surface of the diamond film 4 is then etched by the silicon substrate 24. While still on the substrate, it was lapped and polished to a surface roughness (Ra) of 5.8 nm. After dicing and polishing, the thickness of the diamond film 4 on the silicon substrate 24 is 60-70 mm. The silicon substrate 24 was then heated to a high temperature using a KOH solution to form a diamond layer. The film was then stripped from the 4th band, then stripped with HF-HNO3, and the 2-inch (50.8 m) diameter 4 m), a free-standing diamond film with a thickness of 60-70 microns and an aspect ratio of 781 The surfaces of both sides of the free-standing diamond film 4 are of optical finish quality. It can be used as a window or as a substrate for other applications.
[0104] In yet another example, a 2-inch (50.8 mm) diameter, 10 mm thick monocrystalline silicon The third piece is fabricated using conventional silicon manufacturing techniques and used as silicon substrate 24. Both surfaces of the silicon substrate 24 were polished by a conventional chemical mechanical polishing process. The silicon substrate 24 was then optically finished to an Ra of less than 1 nm. The sample was polished with 25 micron diamond slurry, followed by a standard cleaning process. The silicon substrate 24 is polished with a diamond slurry to an optically finished surface. The reactant gas 6 was mixed with the quartz window 18 and placed in the CVD reactor 16 (FIG. 2). For example, 2,700 mL / min of hydrogen and 16.2 mL / min of methane are Under the control of the flow controller 8, the mixture was allowed to flow into the microwave plasma CVD reactor 16. After the plasma 20 starts to be generated, the size of the plasma 20 becomes equal to the size of the silicon substrate facing the quartz window 18. The output of the magnetron 14 and the pressure of the reactor 16 were adjusted so as to cover the surface of the sintered body 24. The diamond growth temperature at the center of the silicon substrate 24 is measured, for example, using a photometric pyrometer 26. The temperature was controlled at 794 to 835°C. After 95 hours of diamond growth, the growth reaction was stopped. A 2 inch diameter hole was deposited on the surface of the silicon substrate 24 facing the quartz window 18. A polycrystalline diamond film 4 having a diameter of 50.8 mm and a thickness of 156 microns was obtained. The Mondo film had an aspect ratio of 326. Diamond film 4 to silicon After peeling off the silicon substrate 24, the surface roughness of the nucleation side of the diamond film 4 was 7.7 nm. The growth side surface of the diamond film 4 is measured to be as-grown diamond. The surface was determined to have typical roughness.
[0105] Example 3: Single crystal Si substrate (166 mm diameter) with both sides chemically etched. Diamond film grown on a 10 mm thick substrate (1 mm thick) with one optically polished surface Production of diamond films having
[0106] In another example, a piece of single crystal silicon with a diameter of 166 mm and a thickness of 10 mm was The silicon substrate 24 was fabricated by the silicon manufacturing method. The side surface is finished by a common chemical etching process to a surface roughness of 918 nm. The silicon substrate 24 was then polished with diamond powder to obtain a C A mixture of reactive gases 6, e.g., 2,800 mL / min of hydrogen and 84 mL / min of methane under the control of mass flow controller 8. The mixture was then flowed into the microwave plasma CVD reactor 16. After the plasma 20 was generated, The size of the magnet 20 is set so as to cover the surface of the silicon substrate 24 facing the quartz window 18. The output of the ion implanter 14 and the pressure of the reactor 16 were adjusted. The diamond growth temperature was controlled at 1120° C., for example, using a photometric pyrometer 26. After the diamond growth for 2 h, the growth reaction is stopped and the silicon substrate 24 facing the quartz window 18 is removed. A polycrystalline diamond film 4 having a thickness of 350 microns was obtained by depositing the film conformally on the surface of the substrate. This resulted in the formation of a diamond-silicon (diamond-on-silicon) composite substrate. Then, while the diamond film 4 was still on the silicon substrate 24, The diamond film 4 growth surface was then lapped flat. After lapping, the thickness of the diamond film 4 was The thickness was 300 microns. The diamond-silicon composite substrate was then wrapped again. The total thickness on the silicon substrate was about 1.7 to 1.8 mm. 1 and 2 show enlarged cross-sectional views of the lapped diamond-silicon composite substrate in this example (respectively, Field of view = 4.33 mm and 649.6 μm.
[0107] The surface of the lapped diamond film 4 is then polished to an optical finish. A thin diamond film 4 (i.e., The diamond film 4 is an optical mirror and or as a substrate for electronics, photonics or optoelectronics It may also be used as.
[0108] Next, one piece of 50 mm diameter was used to polish the exposed diamond growth surface, and Then, multiple pieces with a diameter of 1 inch (25.4 mm) were removed from the diamond-silicon composite substrate. The exposed die of a 50 mm diameter diamond-silicon composite substrate piece was cut by a laser. The diamond growth surface was polished to an Ra of 1 nm. The finished diamond thickness was The diameter was 170-180 microns. The silicon substrate was then cut from a piece of 50 mm diameter at high temperature. The stripping was performed using a KOH aqueous solution at 40°C, followed by stripping using HF-HNO3. 133 microns thick in the center, 144-176 microns thick around the edges, A free-standing diamond film piece with a curvature ratio of 376 was obtained. The optically finished growth surface of the doped film can be used as an optical mirror or for other purposes such as temperature control. The nucleation side of a diamond film with a diameter of 50 mm can be used as a substrate for The surface roughness (Ra) of the chemically etched silicon The surface roughness of the diamond-silicon substrate is approximately 918 nm. Instead of removing a 50 mm piece of composite substrate, a diamond that is at least optically finished is The silicon was then etched to obtain a 50 mm piece of diamond-silicon composite substrate with a bonded surface. The contact substrate may be thinned and polished.
[0109] Example 4: Polycrystalline Si substrate (166 mm diameter) with both sides chemically etched Diamond film grown on a 10 mm x 10 mm thick substrate - one surface optically polished Production of diamond films having
[0110] In another example, a piece of polycrystalline silicon 166 mm in diameter and 10 mm thick was The silicon substrate 24 was fabricated by the silicon manufacturing method. The side surface is finished by a common chemical etching process to a surface roughness of 816 nm. The silicon substrate 24 was then polished with diamond powder to obtain a C A mixture of reactive gases 6, e.g., 2,800 mL / min of hydrogen and 84 mL / min of methane under the control of mass flow controller 8. The mixture was then flowed into the microwave plasma CVD reactor 16. After the plasma 20 was generated, The size of the magnet 20 is set so as to cover the surface of the silicon substrate 24 facing the quartz window 18. The output of the ion implanter 14 and the pressure of the reactor 16 were adjusted. The diamond growth temperature was controlled at, for example, 1120° C. using a photometric pyrometer 26. After the diamond growth for 2 h, the growth reaction is stopped and the silicon substrate 24 facing the quartz window 18 is removed. A polycrystalline diamond film 4 with a thickness of 175 microns was obtained by depositing the film conformally on the surface of the The diamond 4 growth surface was then examined by measuring the diamond film 4 on the silicon substrate 2. 4 While still on the plate, it was lapped flat and then polished to an optical finish. The silicon substrate 24 is peeled off from the diamond film 4 using a KOH aqueous solution at high temperature, and then The specimen was peeled off using HF-HNO3, and the diameter was 166 mm, the thickness was less than 175 microns, and the asperity A piece of free-standing diamond film 4 was obtained with a curvature ratio of 948. The yamond-grown surface may also be used as a substrate for other applications such as optical mirrors or temperature control. Instead of removing the silicon substrate 24, a diamond that has been finished to at least optical finish can be used. The silicon is then grown on the diamond-silicon composite substrate so as to obtain a diamond-silicon composite substrate having a diamond growth surface. The silicon substrate 24 may be thinned and polished.
[0111] Example 5: A surface optically finished by a chemical mechanical polishing process (e.g., Ra: The diamond was grown on a polycrystalline silicon substrate (diameter 166 mm, thickness 10 mm) with a thickness of 1.3 nm. Diamond Film - Diamond film with optically finished surface on one or both sides. Film manufacturing
[0112] In another example, a piece of polycrystalline silicon 166 mm in diameter and 10 mm thick was The silicon substrate 24 was fabricated by the silicon manufacturing method. The side surface is finished by a common chemical etching process to a surface roughness of 816 nm. The surface 1 of the silicon substrate 24 was polished by a chemical mechanical polishing process. The entire silicon substrate 24 was then polished to an optical finish (Ra: about 1.3 nm). The optically finished surface (surface 1) facing the window 18 is used for growing diamond. To do this, a wet diamond slurry is ultrasonically treated and placed in a CVD reactor 16 (Figure 2). A mixture of reactive gas 6, e.g., hydrogen at 2,800 mL / min and 16.8 m Methane was introduced at 8 L / min into the microwave plasma CV under the control of a mass flow controller. After the plasma 20 was generated, the size of the plasma 20 was changed to that of the silicon dioxide gas. The output of the magnetron 14 and the pressure of the reactor 16 are adjusted so as to cover the surface 1 of the silicon substrate 24. The diamond growth temperature at the center of the silicon substrate 24 was measured using, for example, a photothermometer. After 164 hours of diamond growth, the growth reaction The reaction was stopped, and a 166 mm diameter, 29 mm thick silicon oxide film was deposited on the surface 1 of the silicon substrate 24. A 5 micron polycrystalline diamond film 4 was obtained, which resulted in a diamond-silicon A composite substrate was formed, with the diamond film 4 still on the silicon substrate 24. Between these, the diamond growth surface was lapped flat. The long surface is further polished to an optical finish, resulting in a diamond film with an aspect ratio of 563. In this example, the diamond-silicon composite substrate had a total thickness of 1.7–2.0 mm. The silicon substrate 24 side of this diamond-silicon composite substrate was polished until it had a surface roughness of 100 nm. The diamond-silicon composite substrate was laser cut into one piece with a diameter of 75 mm and one piece with a diameter of 3 Two pieces were made of 8.5 mm and two pieces of 1 inch (25.4 mm) diameter. , optically finished surface with diamond thickness of 150-200 microns or less To obtain each piece, the exposed diamond growth surface of each piece was optically polished. The surface roughness (Ra) of the polished diamond growth surface of the 75 mm piece was 2.75 nm ( The average particle diameters of the specimens were measured to be 3.59, 2.35, 2.43, 2.57 and 2.89 nm. The silicon substrate was stripped using KOH aqueous solution at high temperature, followed by HF-HNO3 , 1 inch (25.4 mm), 38.5 mm and 75 mm diameter free standing diamond fills Each free-standing diamond film 4 had a thickness of 150 microns and The aspect ratios are 169, 256 and 500. Each piece has an optically finished diamond. The diamond growth surface can be used, for example, as an optical window, an optical mirror, or for other purposes such as temperature control. It can be used as a substrate for applications.
[0113] Laser is used to peel off the silicon substrate and form a piece of free-standing diamond film 4. The lapped diamond-silicon composite substrate pieces remaining after cutting were then immersed in KOH water at high temperature. The nucleation surface of this piece of free-standing diamond film 4 had a surface roughness of It has a mirror surface finish with an average grain size of approximately 20 microns and a roughness of 15.3 nm. While fine-tuning the nucleation density, the surface roughness of the nucleation surface was reduced to less than 10 nm. Instead of removing the silicon substrate 24, it is possible to provide a substrate that is at least optically finished. To fabricate a piece of diamond-silicon composite substrate using the diamond surface, The silicon substrate 24 (while the diamond layer 4 is still there) can be thinned and polished. Pieces of diamond-silicon composite substrates can be used for applications such as optical mirrors or electronics. It may also be used as a substrate for photonics, optoelectronics, etc.
[0114] Example 6: One surface optically finished by chemical mechanical polishing process (Ra: 1 nm Diamond growth on polycrystalline Si substrate (diameter 166 mm, thickness 10 mm) with less than - Production of thin films of diamond with optically finished one or both surfaces
[0115] In another example, a piece of polycrystalline silicon 166 mm in diameter and 10 mm thick was The silicon substrate 24 was fabricated by the silicon manufacturing method. The silicon substrate 2 was then finished by a standard chemical etching process. Surface 1 of 4 was chemically mechanically polished to a mirror finish with a roughness Ra of less than 1 nm. High diamond nucleation density on the surface 1 of the silicon substrate 24, good diamond-silica To achieve diamond-to-silicon bonding and to grow on the surface 1 To avoid the diamond film from peeling off from surface 1, a two-step seeding process was used. A sachusetts ... law was used.
[0116] First, the entire silicon substrate 24 is covered with diamond powder / metal with an average size of 0.25 μm. The mixture was sonicated in an ultrasonic bath consisting of a ethanol suspension. The same growth conditions as those described in the second diamond nucleation and growth step described later were applied. For the first diamond nucleation and growth step on surface 1 for 1 hour, surface 1 was treated with quartz. The first diamond nucleation was performed in a CVD reactor 16 (FIG. 2) facing the window 18. The process results in low density diamond nucleation (10 5 / c m 2 The first step of diamond nucleation was performed on the silicon substrate 24 The resultant is taken out of the CVD reactor 16 and immersed in a nanocrystalline diamond powder (commonly The particles were sonicated in a methanol aqueous suspension (particle size less than 20 nm).
[0117] After ultrasonic treatment in the nanocrystalline diamond powder / methanol suspension, the second diamond For the first nucleation growth process and for the continuous diamond growth on the first diamond nucleation Next, the silicon substrate 24 containing the first step diamond nucleation is placed with the surface 1 facing the quartz window 18. The mixture was then fed again into the CVD reactor 16. In this second step, the flow rate was 2,800 mL / min. A mixture of hydrogen and methane at 16.8 mL / min was fed into the mass flow controller 8. Then, the gas was flowed into the CVD reactor 16. After the plasma 20 was generated, the size of the plasma 20 was The first step diamond on the surface 1 of the silicon substrate 24 is The power of the magnetron 14 and the pressure of the reactor 16 were adjusted to cover the nucleation. The diamond growth temperature at the center of the sample is measured using a photothermometer 26 at, for example, 800° C. was controlled.
[0118] After 140 hours of diamond growth (second step diamond nucleation), diamond growth The reaction was stopped and conformally deposited on the surface 1 of a silicon substrate 24 with an aspect ratio of 593. A polycrystalline diamond film 4 having a thickness of 280 μm was obtained. While on the silicon substrate 24, the diamond growth surface of the diamond film 4 is polished. and measured at different locations on the polished diamond growth surface of diamond film 4. The surface roughness (Ra) was 3.28, 6.75, 15.4, 11.4, 12.2 and 6.97. nm, aspect ratio was 790, and thickness was 210 μm.
[0119] Silicon-diamond composite substrates were laser cut into 5-inch (12.7 mm) diameter pieces. After that, the silicon substrate 24 was peeled off from this piece using a KOH aqueous solution at high temperature, and a 5 inch ( 127 mm), 210 μm thick, and with an aspect ratio of 605. A photograph of the free-standing diamond film 4 placed on a tray is shown in FIG.
[0120] The surface roughness of the nucleation side of the free-standing diamond film 4 is The average surface roughness (Ra) measured at different locations on the surface of the four plates was 2.08, 2.46, 2.38, and The diamonds after the second nucleation step were measured to be 2.07, 1.98 and 1.90 nm. The diamond nucleation density on the nucleation side / surface of the diamond film 4 was observed by SEM (Figure 8). Therefore, 10 9 / cm 2 It was estimated to exceed .
[0121] A free-standing diamond film 4 with optically finished growth and nucleation surfaces was prepared. , Optical windows, mirrors, or optical applications, temperature control, acoustic control, detectors, microwave / electromagnetic May be used as a substrate for applications such as wave management, mechanical applications, chemical inertness, friction control, etc. .
[0122] Alternatively, a diamond substrate having at least an optically finished diamond growth surface is used. To obtain a piece of a diamond-silicon composite substrate, a silicon substrate 24 (diamond film 4) was The diamond-silicon composite substrate may be thinned and polished while still attached. are used as optical mirrors or in electronics, photonics, and optoelectronics. The semiconductor device may be used as a substrate for a semiconductor device or the like.
[0123] Example 7: Optically finished silicon substrates (diameter 100 nm) using nanodiamond seeding The lack of good adhesion of diamond films grown on a substrate (166 mm x 10 mm thick) Accomplished.
[0124] In another example, a piece of polycrystalline silicon 166 mm in diameter and 10 mm thick was The silicon substrate 24 was fabricated by the silicon fabrication method and used as the silicon substrate 24. The surface 1 of the silicon substrate 24 is then finished by a conventional chemical etching process. The surface was then chemically and mechanically polished to a mirror finish with a roughness Ra of less than 1 nm. The entire plate 24 is immersed in a bath of nanocrystalline diamond powder (typical particle size 20 nm) in an ultrasonic bath. The mixture was sonicated in a 100% (less than 100%) / methanol suspension.
[0125] After ultrasonic treatment in a nanocrystalline diamond powder / methanol suspension, the silicon-based The plate 24 was placed in the CVD reactor 16 with the surface 1 facing the quartz window 18. A mixture of 2,800 mL / min of hydrogen and 16.8 mL / min of methane was Under the control of the controller 8, the gas is allowed to flow into the CVD reactor 16. The plasma 20 begins to be generated. Then, the magnetron 14 is turned on so that the size of the plasma 20 covers the surface 1 of the silicon substrate 24. The output of the reactor 16 and the pressure of the reactor 16 were adjusted. The diamond growth temperature at the center of the substrate was The temperature was controlled to 821 to 840° C. using, for example, a photothermometer 26.
[0126] After 189 hours of diamond growth, the diamond growth reaction was stopped and the silicon substrate was A polycrystalline diamond film 4 having a thickness of 320 μm is conformally deposited on the surface 1 of the However, the diamond film 4 undergoes partial (but substantial) delamination from the silicon substrate 24, resulting in the diamond film Subsequent polishing of the growth surface of 4 was not possible. As a result, the exfoliated diamond The nucleation surface of the bond film 4 was measured to have an average surface roughness (Ra) of 2–4 nm. Nevertheless, an optically finished growth surface could not be achieved.
[0127] Example 8: Optically polished polycrystalline silicon seeded with 0.25 mm diamond particles Diamond growth on a silicon substrate (diameter 166 mm, thickness 10 mm)
[0128] In another example, a piece of polycrystalline silicon 166 mm in diameter and 10 mm thick was The silicon substrate 24 was fabricated by the silicon fabrication method and used as the silicon substrate 24. The surface 1 of the silicon substrate 24 is then finished by a conventional chemical etching process. The surface was then chemically and mechanically polished to a mirror finish with a roughness Ra of less than 1.5 nm. The entire silicon substrate 24 is immersed in a diamond powder / methanol suspension with an average size of 0.25 μm. 1. The substrate is then sonicated in an ultrasonic bath at 1000 rpm, and then placed in the CVD reactor 1 with the surface 1 facing the quartz window 18. 6 (Figure 2).
[0129] A mixture of 2,800mL / min of hydrogen and 16.8mL / min of methane was fed into the mass flowmeter. Under the control of the row controller 8, the gas was allowed to flow into the CVD reactor 16. After the start of the plasma generation, the magnetron 1 is turned on so that the size of the plasma 20 covers the surface 1 of the silicon substrate 24. The output of the reactor 4 and the pressure of the reactor 16 were adjusted. was controlled to 845 to 868° C. using, for example, a photothermometer 26.
[0130] After 163 hours of diamond growth, the diamond growth reaction was stopped and the aspect ratio was 56 A 295 μm thick polycrystalline diamond film is conformally deposited on the surface 1 of a silicon substrate 24 of FIG. A silicon-diamond composite substrate having a bond film 4 was obtained.
[0131] While the diamond film is attached to the silicon substrate, the diamond film 4 The growth surface is polished to an optical finish (Ra 3-5 nm) and has a diameter of 99 microns (diamond The thickness of the diamond film was 4) and the aspect ratio was 168. While bonded to the silicon substrate 24, the silicon-diamond composite substrates were The silicon substrate 24 of each piece is then removed (K OH aqueous solution), thereby forming a piece of free-standing diamond film 4. The nucleation surfaces of these pieces of free-standing diamond film 4 had an average surface roughness (Ra) of 5 ~9 nm, and the nucleation density is 10 5 / cm 2 That's it. Freestanding diamond film One of these pieces of 4 has a thickness of 99 microns, as shown in graph (a) of FIG. At a distance of 34.0 mm from the shielding lens, the light scattering at 1.06 μm wavelength is 8.22 / It was characterized as having a light scattering coefficient of 1.0 cm.
[0132] Example 9: First seeding step (seeded with 0.25 mm diamond particles) followed by a second seeding step (Nanodiamond particle seeding) on an optically finished silicon substrate (2 inch diameter) Diamond growth on the ridge (50.8 mm, thickness 10 mm)
[0133] In another example, a piece of polycrystalline silicon with a diameter of 50.8 mm and a thickness of 10 mm was placed on a The silicon substrate 24 was fabricated by the same method as in Example 1, and used as the silicon substrate 24. The surface was then chemically and mechanically polished to a mirror finish with a roughness Ra of less than 1.5 nm. The entire substrate 24 is immersed in a diamond powder / methanol suspension with an average size of 0.25 μm. The mixture was sonicated (seeded) in a CVD reactor 16 (FIG. 2).
[0134] A mixture of 2,800 mL / min of hydrogen and 16.8 mL / min of methane was then The plasma was then allowed to flow into the CVD reactor 16 under the control of the mass flow controller 8. After the plasma generation starts, the size of the plasma 20 is increased so as to cover the surface 1 of the silicon substrate 24. The output of the tron 14 and the pressure of the reactor 16 were adjusted. The diamond growth temperature was controlled at 780° C., for example, using a photothermometer 26. After the diamond growth for 10 min, the diamond growth reaction is stopped and the surface 1 of the silicon substrate 24 is A diamond-seeded silicon substrate 24 was observed having diamond particles deposited therearound. It was.
[0135] The diamond-seeded silicon substrate 24 is then removed from the CVD reactor 16 and ultrasonically Nanocrystalline diamond powder (typical particle size <20 nm) / methanol in wave bath The diamond-seeded Si nanodiamonds were then treated with ultrasonic waves in an aqueous suspension. The substrate was then reloaded into the CVD reactor 16 with the surface 1 again facing the quartz window 18. A mixture of 2,800 mL / min of hydrogen and 16.8 mL / min of methane was The gas was allowed to flow into the CVD reactor 16 under the control of the flow controller 8. After the start of generation, the magnetron is rotated so that the size of the plasma 20 covers the surface 1 of the silicon substrate 24. The output of the nozzle 14 and the pressure of the reactor 16 were adjusted. The diamond growth temperature was controlled at 790-821° C., for example, using a photometric pyrometer 26.
[0136] After an additional 143 hours of diamond growth, the diamond growth reaction was stopped and the thickness was reduced to 2 Silicon die with diamond film 4 of 45 microns and aspect ratio 207 The diamond growth surface was a diamond film 4, which was still a silicon substrate. While still on the contact substrate 24, it is polished to an optical finish (Ra 3-5 nm) and The thickness of the diamond film was 1.0 mm and the aspect ratio was 258.
[0137] Then, the silicon substrate 24 is removed from the silicon-diamond composite substrate to form a free-standing diamond. The diamond film 4 was removed (dissolved in KOH solution) leaving the diamond film 4. The nucleation surface of doped film 4 has an average surface roughness (Ra) of 2.73 nm and a 10 9 / cm 2 Below The latter two of these have a high nucleation density and a smooth surface finish, e.g. This is highly desirable for applications such as temperature control, optical control, semiconductor device, and friction control. As shown in graph (b) of Figure 9, the band film 4 is placed 34 mm away from the scattered light collecting lens. At this distance, light scattering at 1.06 μm wavelength is characterized as having a light scattering coefficient of 2.69 / cm. Light scattering at 1.06 μm wavelength is considered low micron light scattering in the art. , highly suitable for optical, thermal, acoustic applications, etc.
[0138] Example 10: Optically finished nanodiamond nanoparticles by one-step seeding Diamond grown on a silicon substrate (2 inch (50.8 mm) diameter, 10 mm thick)
[0139] In another example, a piece of polycrystalline silicon with a diameter of 50.8 mm and a thickness of 10 mm was placed on a The silicon substrate 24 was fabricated by the silicon manufacturing method. The surface is polished to a mirror finish with a roughness of less than 1.5 nm by chemical mechanical polishing, and the other surface is polished to a standard The silicon substrate 24 was then etched by a conventional chemical etching process. , nanocrystalline diamond powder (typical particle size less than 20 nm) / Meta in ultrasonic bath The mixture was sonicated in a methanol suspension.
[0140] The silicon substrate is placed in the CVD reactor 16 with the surface 1 facing the quartz window 18. A mixture of 2,800 mL / min of hydrogen and 16.8 mL / min of methane was then was flowed into the CVD reactor 16 under the control of the mass flow controller 8. After the plasma 20 starts to be generated, the size of the plasma 20 is increased so as to cover the surface 1 of the silicon substrate 24. The output of the netron 14 and the pressure of the reactor 16 were adjusted. The diamond growth temperature was controlled at, for example, 800° C. using a photometric pyrometer 26 .
[0141] After 118 hours of diamond growth, the diamond growth reaction was stopped and the silicon substrate was A silicon substrate having a 190 μm thick diamond film 4 conformally deposited on its surface 1. The diamond growth surface was treated with diamond film 4 While still on the silicon substrate 24, it is polished to an optical finish and then etched to a thickness of 140 microns (datum). The thickness of the diamond film was 4).
[0142] Then, the silicon substrate 24 is removed from the silicon-diamond composite substrate to form a free-standing diamond. The diamond film 4 was removed (dissolved in KOH solution) leaving the diamond film 4. The nucleation surface of the doped film 4 has an average surface roughness (Ra) of 2–3 nm and a 9 / cm 2 End and a smooth surface finish, the latter two of which can be controlled by, for example, temperature. These are highly desirable for applications such as optical management, semiconductor device management, and friction control.
[0143] This free-standing diamond film 4 also has a shielding lens as shown in graph (c) of FIG. At a distance of 34 mm from the lens, the light scattering coefficient for the 1.06 μm wavelength is 2.09 / cm. It was characterized as having a number
[0144] Under the same diamond growth conditions, on different silicon substrates 24, this Example 10 Some additional experiments following the guidelines of the authors have run into problems. The diamond film 4 is peeled off from the silicon substrate 24, and the growth surface of the peeled diamond film is No further polishing could be performed on the nanodiamond-seeded surface. In one embodiment, a thin diamond substrate having at least one optically finished surface is fabricated. This suggests that the process may not be reliable for creating
[0145] Comparative Example 1: Silicon wafer (diameter 6 inches (15.24 mm), thickness 625 microns) ) Failure of diamond film growth on
[0146] In one example, three silicon wafers, 24 (n type, 6 inch (152.4 mm) diameter) The surface 1 of each silicon wafer 24 was chemically and mechanically polished. The other surface of each silicon wafer 24 is then chemically etched. Then, the surface 1 (optically finished) of each silicon wafer 24 was polished with a diamond. The surface was polished with Bland powder.
[0147] Next, one of the silicon wafers 24 is optically finished for diamond growth. The substrate was placed in a microwave plasma CVD reactor 16 with the coated surface 1 facing the quartz window 18. A mixture of reactive gas 6, e.g., hydrogen at 2,500 mL / min and 75 mL / min methane was flowed into the microwave plasma CVD reactor 16. After the start of the plasma generation, the magnetron 14 is turned on so that the plasma 20 covers the surface 1 of the silicon wafer 24. The power and pressure of the reactor 16 were adjusted. During this plasma adjustment process, the silicon wafer The Har-24 broke into many small pieces.
[0148] This experiment was repeated with two other silicon wafers, varying the powder velocity and pressure. The other two silicon wafers 24 were also broken into numerous small pieces with similar results. It was crushed.
[0149] Comparative Example 2: Optically finished diamond imperfections less than 400 microns thick achievement
[0150] In one example, CVD grown diamonds with diameters of 50 mm, 75 mm, 85 mm, and 100 mm were The chips were cut from as-grown diamond wafers with a thickness of more than 550 microns. The as-grown surface of each diamond piece was then lapped flat. Next, the diamond pieces were subjected to a dipping process on each of the surfaces, either the growth surface or the nucleation surface. One side is polished to an optical finish using conventional polishing processes. These diamond pieces can reach a thickness of 400 microns when grinding. The diamonds are crushed before being polished, and the traditional diamond polishing process is unable to achieve an aspect ratio of 125. It was suggested that this would be difficult.
[0151] From the above, as disclosed herein, the diamond film, substrate or window can be ) at least one optically finished surface and an aspect ratio of 100 or greater; or 2) A combination of a thickness of 400 or less and a maximum or longest geometric dimension of 25 mm or more It consists of one of the following.
[0152] Optically finished surfaces are <50nm, <30nm, <20nm, <15nm or less, or a surface roughness (Ra) of 10 nm or less.
[0153] The maximum or longest geometric dimension is 40mm or more, 50mm or more, 60mm or more, 70mm or more , it may be 80 mm or more or 100 mm or more.
[0154] The thickness of the diamond film, substrate or window is 400 microns or less, 350 microns or less. It may be 300 microns or less, 250 microns or less, or 200 microns or less.
[0155] The maximum or longest geometric dimension of the diamond film, substrate or window is determined by the diamond filler. The aspect ratio, defined as the ratio of the thickness of the film, substrate or window divided by the thickness of the film, substrate or window, is 100 or more, 125 or less. or more, 150 or more, 175 or more, or 200 or more.
[0156] Diamond film, substrate or window: 20 / cm or less, 15 / cm or less, 10 / cm or less 1.0 at a distance of 34 cm from the occlusion lens, 7 / cm or less, or 5 / cm or less It may have a light scattering coefficient of 6 microns.
[0157] A piece of sacrificial substrate (e.g. silicon) is grown on which a diamond film, substrate or window will be grown. The sacrificial substrate may be 2 mm or more, 4 mm or more, 6 mm or more, or 8 mm or more. The thickness may be 0.01 to 0.01 mm.
[0158] The sacrificial substrate may have an optically finished surface, i.e., the surface is 20 Surface roughness (Ra) of 15 nm or less, 10 nm or less, 5 nm or less, or 2 nm or less do.
[0159] After CVD diamond growth on the sacrificial substrate, the diamond is removed by chemical (caustic, hydrogen fluoride or ionizing) The sacrificial substrate may be removed by chemical etching (electrochemical etching) and / or mechanically (polishing or lapping). At least one optically finished surface of the diamond film, substrate or window is , it may be a growth surface, a nucleation surface, or both.
[0160] The growth surface of the diamond film, substrate or window is While still attached to the silicon substrate, it is optically polished by conventional polishing processes. The total thickness of the diamond film, substrate or window and sacrificial substrate may be equal to or greater than that of a conventional polishing process. The process holds the diamond film, substrate or window in place without fracturing during polishing. The diamond film, substrate or window growth surface is thick enough to be polished to an optical level. After this finishing is achieved, the sacrificial substrate may be removed, for example chemically and / or mechanically. The process results in at least one optically finished surface (e.g., a growth surface). For example, a thin diamond film, substrate or window having a thickness of 400 microns or less. obtained.
[0161] The growth side of the polycrystalline diamond film, substrate or window piece is It may have a greater thermal conductivity than the nucleation side of the plate or window. Only the growth side of the film, substrate, or window may be optically finished. It is not necessary to optically finish the nucleation side of the film, substrate, or window. The diamond growth surface does not need to be optically finished. The growth surface may be chemically etched and / or mechanically lapped. The diamond film grown on this surface of the sacrificial substrate then nucleates on the substrate or window. has no optical finish.
[0162] In one example, the nucleation side of the diamond film, substrate or window having an optical finish is The thermal conductivity of the thermal insulating material may be greater than that of conventional thermal management materials such as copper.
[0163] In one example, a substrate having at least one optically finished surface for diamond growth is provided. The sacrificial substrate (e.g., silicon) is coated with an optically finished diamond film on the nucleation side. After diamond growth, the diamond film may be The growth surface of the substrate or window is then lapped and / or polished flat, if necessary. After that, the sacrificial substrate is removed, for example by chemical etching and / or mechanical lapping / polishing. This process eliminates the need for traditional diamond polishing processes. to avoid the risk of fracturing or destroying the diamond film, substrate or window during polishing. , a diamond film, substrate or window having an optically finished surface (on the nucleation side) Pieces of can be manufactured.
[0164] Light management coatings, e.g. anti-reflection coatings, beam splitter coatings coating, total reflection coating, etc., for the growth and / or nucleation of diamond films, windows or substrates. The diamond film, substrate or window described herein may be applied to a growing surface. It may be laser cut into a variety of geometric dimensions for a variety of different applications. The diamond film, substrate or window is still on the silicon substrate (the diamond film, substrate or window is still on the silicon substrate) Laser cut while still on the surface (as is), lapped and / or polished may be carried out.
[0165] The diamond film, substrate or window is of optical quality (infrared, near infrared, visible or ultraviolet). low absorption of electromagnetic waves such as ambient light, and also, or alternatively, microwave The diamond film, substrate or window may further comprise: Or, alternatively, mechanical and / or thermal grade diamonds (the latter generally darker in color). (There is one.)
[0166] The diamond film, substrate or window may be formed by a microwave assisted plasma CVD process, a thermal filament CVD process, thermal spray CVD process, arc discharge plasma CVD process process, direct current thermal plasma CVD process, high frequency plasma CVD process, water plasma CV D process, acetylene torch CVD process, ultra-high frequency plasma CVD process, etc. Therefore, it may be allowed to grow.
[0167] The growth temperature of the diamond film, substrate or window is in the range of 600°C to 1300°C or higher. The use of higher growth temperatures is envisioned.
[0168] Growth rates of diamond films, substrates or windows range from submicron to 20 microns per hour / hour. Higher growth rates are envisioned.
[0169] The methane concentration for growing diamond films, substrates or windows is 1% in hydrogen. The range may range from less than 5%.
[0170] Other additives, including, for example, oxygen, carbon monoxide, carbon dioxide, nitrogen and / or boron, may also be used. In addition, the growth apparatus may be configured to control the diamond growth rate and / or the quality of the grown diamond. may be added to.
[0171] One or both surfaces of a sacrificial substrate (e.g., silicon) are etched with, for example, a hydrous diamond slab. Diamond powder was prepared by ultrasonic treatment with a diamond slurries or organic diamond slurries. Optically finished, if necessary, by polishing with abrasives or by diamond turning, and and / or may be diamond seeded if desired.
[0172] The sacrificial substrate (e.g., silicon) for diamond growth should be at least 30 mm in diameter and 2 mm in diameter. inch or more, diameter 66 mm or more, diameter 3 inches or more, diameter 4 inches or more, or diameter 5 inches or more It may be 1 inch or more.
[0173] The diamond growth surface of the sacrificial substrate (e.g., silicon) is optically polished or chemically polished. The optically finished surface of the sacrificial substrate (e.g., silicon) may be The surface roughness (Ra) of the surface is 20 nm or less, 15 nm or less, 10 nm or less, 5 nm or less, or may be 2 nm or less.
[0174] The grown diamond film, substrate or window may have one or more non-planar surfaces. In one non-limiting example, the nucleation side of the non-planar surface may be a dome, cone, pyramid, or , aspheric, parabolic, hyperbolic, or other non-planar shapes. These features are formed by optically finishing the sacrificial substrate (e.g., silicon) with an optical finish. The substrate may have an optically finished surface that can be grown conformally over the contour of the surface. Such an optically finished surface profile of the sacrificial substrate is essential for the final diamond part. After diamond growth, a sacrificial substrate (e.g., a silicon The surface of the material may be chemically, for example by etching (e.g., with KOH or HF) and / or polished. It may be removed mechanically by polishing and lapping. The desired contour of the planar surface is cut using a diamond cutting process or a typical optical manufacturing process. Therefore, it may be manufactured.
[0175] The diamond film, substrate or window may be used in optical windows; electronics, photonics or Substrates for thermal management of optoelectronics; chemical inertness, acoustic management, electromagnetic management, wear Substrates for use including friction controls and detectors; and, for example, milling, cutting, drilling It may also be used as a material for mechanical applications such as lacework.
[0176] In one example, a diamond-silicon composite substrate is formed by CVD deposition of diamond on a silicon layer. At least the growth surface of the diamond layer is optically finished to a thickness of 50 nm or less. , 30nm or less, 20nm or less, 15nm or less, or 10nm or less of surface roughness (Ra) The total thickness of the composite substrate may be 300 microns or more, 500 microns or more, or 1 mm or more. The diameter of the diamond-silicon composite substrate may be 2 mm or more, or 5 mm or more. 20mm or more, 30mm or more, 40mm or more, 50mm or more, 75mm or more, 100mm It may be 125 mm or more, or 150 mm or more.
[0177] The diamond film, substrate or window described in all the above embodiments may be, for example, Optical windows for transmission, optical windows for light reflection, light splitters, microwave windows, detectors, Electronics, photonics and / or optoelectronics (e.g., limited Laser diodes, diode laser bars, and other laser diodes are not intended to be used as laser diodes. Array of surface-emitting semiconductor lasers (VCSELs) The present invention can be used for applications such as temperature control substrates for semiconductor devices (electronics, semiconductor devices, etc.).
[0178] These examples are described with reference to the accompanying drawings. Upon reading and understanding the above examples, It is contemplated that other design and modification may be made thereto. Thus, the embodiments described above may be modified in various ways. , should not be construed as a limiting disclosure.
Claims
1. (a) a substrate having a polished surface, the polished surface having an optically finished surface having a surface roughness (Ra) of 20 nm or less; (b) a diamond film, substrate or window connected to the polished surface of the substrate, the diamond film, substrate or window having an aspect ratio of a maximum dimension of the diamond film, substrate or window divided by a thickness of the diamond film, substrate or window of 100 or greater; Equipped with A diamond film, substrate or window intermediate, wherein the Ra of the nucleation side surface of the diamond film, substrate or window is greater than the Ra of the polished surface of the substrate, and for the polished surface of the substrate having an Ra of 20 nm or less, the Ra of the nucleation side surface of the diamond film, substrate or window is 50 nm or less.
2. The intermediate body according to claim 1 , wherein the thickness of the substrate is 2 mm or more.
3. 3. An intermediate body as described in claim 1 or 2, wherein the surface of the diamond film, substrate or window opposite the side connected to the polished surface of the substrate has a surface roughness (Ra) of 50 nm or less.
4. the polished surface of the substrate and the nucleation side surface of the diamond film, substrate or window are non-planar; 4. An intermediate body according to any one of claims 1 to 3, wherein the shape of the nucleation side surface of the diamond film, substrate or window is an inverse shape that matches the surface shape of the substrate.
5. 5. The intermediate body of any one of claims 1 to 4, wherein the nucleation side surface of the diamond film, substrate or window has any one of the following shapes: a dome, a cone, a pyramid, an aspheric surface, a parabola and a hyperbola.
6. An intermediate body according to any one of claims 1 to 5, wherein a growth side surface of the diamond film, substrate or window has a greater thermal conductivity than a nucleation side surface of the diamond film, substrate or window.
7. 7. The intermediate of any one of claims 1 to 6, further comprising a light management coating on a growth side surface of the grown diamond film, substrate or window.
8. The intermediate of any one of claims 1 to 7, further comprising one or more pieces of said substrate.
9. the diamond film, substrate or window is a CVD grown diamond film, substrate or window; 9. An intermediate according to any one of claims 1 to 8, wherein the CVD grown diamond film, substrate or window is CVD grown in an atmosphere comprising at least one of oxygen, carbon monoxide, carbon dioxide, nitrogen and boron.
10. An intermediate according to any one of claims 1 to 9, wherein the diamond film, substrate or window comprises diamond grain seeds.
11. The intermediate body according to any one of claims 1 to 10, wherein the maximum dimension of the substrate is 30 mm or more.
12. The intermediate body according to any one of claims 1 to 11, wherein the largest dimension of the substrate is the diameter of the substrate.
13. A diamond film, substrate or window obtained by removing the substrate from the intermediate body according to any one of claims 1 to 12.
Citation Information
Patent Citations
Self-supporting diamond water and its production
JP1996133893A