Ziel and method for producing the same

A high-purity, porous twill with controlled impurities and surface roughness addresses the issue of silica-based crystal contamination in float glass manufacturing, improving yield and durability.

JP7565260B2Active Publication Date: 2024-10-10COORSTEK GK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021213750
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-10-10
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

Silica-based foreign crystals, such as tridymite and cristobalite, are mixed into molten glass during the float glass manufacturing process, reducing the yield of plate glass products.

Method used

A twill made of fused silica with a high purity and controlled impurity levels, combined with a porous structure and specific surface roughness, is used to adjust molten glass flow, minimizing crystal precipitation and improving durability.

Benefits of technology

The twill suppresses the mixing of silica-based foreign crystals, enhancing the yield and longevity of plate glass production by reducing wear and tear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565260000003
    Figure 0007565260000003
  • Figure 0007565260000004
    Figure 0007565260000004
  • Figure 0007565260000005
    Figure 0007565260000005
Patent Text Reader

Abstract

To prevent a silica based foreign crystal from mixing into molten glass to improve the yield of a sheet glass product manufactured by a float glass manufacturing apparatus.SOLUTION: A tool is used for controlling the flow of molten glass when manufacturing sheet glass by a float molding method. A base consists of a molten silica refractory having a molten silica content of 99 wt.% or more and a bulk density of 1.90 g / cm3 or more and 1.99 g / cm3 or less; an area having at least a thickness of 3 mm from the surface has air permeability having 0.005 MPa or more of an internal pressure after 60 minutes in an air permeability evaluation method; and the area having the thickness has a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less and a K concentration of 50 ppm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zirl for adjusting the flow rate of molten glass when producing sheet glass by a float forming method, and to a method for producing the zirl. [Background technology]

[0002] The float forming method is a method in which glass raw materials are heated in a melting tank, the molten glass is fed to a molten glass supplying section of a float glass manufacturing apparatus, the amount of molten glass is adjusted, and the molten glass is fed onto molten tin in a float bath, and formed into ribbon-shaped glass, as shown in Patent Document 1 (JP Patent Publication 2011-157249 A), for example. The molten glass supplying section is provided with a twill to adjust the flow rate of the molten glass.

[0003] Fig. 3 shows the molten glass supply section shown in Patent Document 1. Explaining based on this figure, molten glass 20 is fed by a supply pipe 21 to a molten glass supply section 22 of a float glass manufacturing apparatus. The molten glass 20 fed to the molten glass supply unit 22 has the amount of molten glass adjusted by a twill 23 installed in the molten glass supply unit 22, and the molten glass becomes a molten glass flow of a constant width, which is then fed from a lip tile 24 onto molten tin 26 in a float bath 25 and formed into a ribbon-shaped glass 27.

[0004] In this case, the molten glass flow of a constant width formed in the molten glass supply section 22 is supplied as is to the float bath 25 and formed into ribbon-shaped glass 27, so that the widthwise ends of the molten glass flow become the widthwise ends of the ribbon-shaped glass 27 (parts other than the product), and the widthwise center of the molten glass flow becomes the widthwise center of the ribbon-shaped glass 27 (part that becomes the product).

[0005] The zirconia 23 is a rectangular plate-like body made of a heat-resistant material such as silica glass ceramic as shown in FIG. 4, and is suspended by a suspension rod 23b via a metal fitting 23a attached to the upper part. As shown in FIG. 3, the twill 23 is installed in the molten glass supply section 22 of the float bath 25 with its side surface facing the opening of the supply pipe 21 so as to be movable up and down.

[0006] This twill 23 has a width approximately equal to the width of the opening of supply pipe 21 and the width of molten glass supply section 22, and the amount of molten glass supplied to float bath 25 is adjusted by moving it up and down to change its height. The twill 23 can also be placed in its lowest position to stop the supply of molten glass 20 to the float bath 25 .

[0007] As described above, the twill 23 is a thick, roughly rectangular plate-like body (base) that serves to block a portion of the molten glass while allowing the remaining molten glass to pass through. Since the twill 23 comes into contact with the high-temperature molten glass and is simultaneously exposed to a high-temperature atmosphere, it must be made of a heat-resistant material.

[0008] The substrate of the twill is generally made of a so-called siliceous refractory material mainly composed of fused silica. A method for producing the siliceous refractory material is described in, for example, Patent Document 2 (JP Patent Publication No. 11-60330). Specifically, a compound containing at least one element selected from the group consisting of boron and phosphorus is added to 100% by weight of particle size-adjusted fused silica powder in an amount of 0.5 to 10% by weight, calculated as B2O3 or P2O5, and an appropriate molding aid is further mixed in to produce a molding mixture (slip). This molding mixture is poured into a plaster mold and molded into the desired shape (so-called slip casting) to obtain a molded body, and this molded body is fired in an atmosphere containing 50% or more by volume of water vapor, thereby producing a fused siliceous refractory material.

[0009] Incidentally, examples of glass manufactured by float glass manufacturing apparatuses include glass used as cover glass for display devices of mobile devices such as mobile phones, smartphones, personal digital assistants (PDAs), and tablet terminals. The glass used for the cover glass of these display devices is required to have high strength so as to be resistant to breakage when dropped, and therefore chemically strengthened glass is used.

[0010] As a glass suitable for such chemical strengthening, lithium aluminosilicate glass has been proposed as disclosed in Patent Document 3. Furthermore, as shown in Patent Document 4, a glass made of SiO2, Al2O3, MgO+CaO+SrO+BaO, and Na2O+K2O has been proposed.

[0011] Furthermore, as shown in Patent Document 5, Fe2O3 is contained in these glasses because it has the effect of improving the solubility by absorbing heat rays. In addition, Na2O and K2O are components that improve the meltability of the glass and reduce the crystal growth rate, and are sometimes added for the purpose of improving the ion exchange performance. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] JP 2011-157249 A [Patent Document 2] Japanese Patent Application Publication No. 11-60330 [Patent Document 3] International Publication No. 2018 / 074335 [Patent Document 4] JP 2001-26437 A [Patent Document 5] Patent Publication No. 2021-31317 Summary of the Invention [Problem to be solved by the invention]

[0013] When glass used for the cover glass of the above-mentioned display device and the like is manufactured by the above-mentioned float glass manufacturing apparatus, there is a problem that silica-based foreign crystals are mixed into the molten glass, resulting in a decrease in the yield of plate glass products.

[0014] The present inventors have conducted extensive research into the cause of inclusion of silica-based foreign crystals in molten glass. As a result, it was found that when molten siliceous refractory ziel comes into contact with molten glass containing a high Fe content at high temperatures, the precipitation of tridymite crystals increases on the surface of the molten siliceous refractory ziel, and foreign matter (tridymite crystals) is mixed into the plate glass. In addition, it was found that in the case of a fused siliceous refractory zirconia made by conventional slip casting, a dense layer having a higher density than the inside of the zirconia is formed on the surface of the zirconia, and the presence of this dense layer causes the precipitation of the tridymite crystals.

[0015] Furthermore, it was found that when the surface layer of fused silica zircon contains large amounts of Ca, Na, and K, contact with high-temperature molten glass increases the precipitation of cristobalite crystals, causing foreign matter (cristobalite crystals) to be mixed into the plate glass.

[0016] The present invention has been made to solve the above-mentioned technical problems, and has an object to provide a twill and a method for manufacturing the twill that suppresses the inclusion of silica-based foreign crystals in molten glass and improves the yield of flat glass products manufactured in a float glass manufacturing apparatus. [Means for solving the problem]

[0017] The zir according to the present invention, which has been made to solve the above technical problems, is a zir used for adjusting the flow rate of molten glass when producing plate glass by a float forming method, and the base has a fused silica content of 99% by weight or more and a bulk density of 1.90 g / cm 3 More than 1.99g / cm 3The present invention is characterized in that it is made of the following fused silica refractory, and that at least a 3 mm thick region from the surface has air permeability such that the internal pressure after 60 minutes is 0.005 MPa or more as measured by an air permeability evaluation method, and that in the thickness region, the Ca concentration is 100 ppm or less, the Na concentration is 50 ppm or less, and the K concentration is 50 ppm or less.

[0018] Here, it is desirable for the center line average roughness Ra of the surface of the substrate to be 1 μm or more and 10 μm or less.

[0019] The method for producing a zircon according to the present invention, which has been made to solve the above technical problems, is a method for producing a zircon used to adjust the flow rate of molten glass when producing plate glass by a float forming method, and includes adding a solvent to fused silica powder to produce a raw material slurry, forming the raw material slurry, and firing the raw material slurry. The fired body Then, the surface layer of the sintered body is removed by grinding.

[0020] Here, it is preferable that the fused silica powder is a fused silica powder with a purity of 99% or more, with a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less, and a K concentration of 50 ppm or less, the solvent is ion-exchanged water, and the firing temperature is 1050°C to 1100°C. It is also preferable that the molding is a casting method and the thickness to be ground away is 1 mm or more. After the grinding, it is preferable to polish the surface of the substrate until the center line average roughness Ra is 1 μm or more and 10 μm or less. Effect of the Invention

[0021] According to the present invention, it is possible to obtain a zirconia and a method for producing the zirconia, which can suppress the inclusion of silica-based foreign crystals in molten glass and improve the yield of plate glass products. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of an apparatus used in a breathability evaluation method. [Diagram 2]FIG. 1 is a schematic diagram showing a test device for performing an erosion test. [Diagram 3] FIG. 1 is a schematic diagram showing a manufacturing apparatus (molten glass supply section) for manufacturing sheet glass by a float forming method. [Figure 4] FIG. 1 is a diagram showing the external shapes of a Ziel of the present invention and a conventional Ziel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the zirconia according to the present invention and a method for producing the zirconia according to the present invention will be described. However, the present invention is not limited to the embodiment. The zircon according to the present invention is a zircon used for adjusting the flow rate of molten glass when producing sheet glass by a float forming method.

[0024] The Ziel substrate has a fused silica content of 99% by weight or more and a bulk density of 1.90 g / cm 3 More than 1.99g / cm 3 It is made of the following fused silica refractories: Furthermore, at least a 3 mm thick region from the surface of the Ziel base has air permeability such that the internal pressure after 60 minutes in the air permeability evaluation method is 0.005 MPa or more. Furthermore, in the thickness region, the Ca concentration is 100 ppm or less, the Na concentration is 50 ppm or less, and the K concentration is 50 ppm or less.

[0025] Thus, the Ziel substrate according to the present invention has a fused silica content of 99% by weight or more and a bulk density of 1.90 g / cm 3 For the above reasons, severe wear of the zirconia due to contact with the molten glass can be suppressed. The bulk density of the Ziel substrate is 1.99 g / cm 3or less, and at least a 3 mm thick region from the surface has a porous structure with air permeability such that the internal pressure after 60 minutes in the air permeability evaluation method is 0.005 MPa or more, thereby making it possible to suppress the precipitation of tridymite crystals due to the Fe component in the molten glass. As a result, it is possible to achieve a long service life and suppress the amount of foreign matter mixed into the molten glass.

[0026] Although it has not been fully elucidated what phenomenon suppresses the precipitation of tridymite crystals, it is presumed that, because tridymite crystals have a greater thermal expansion than fused siliceous refractories, the above-mentioned moderate porosity of the fused siliceous refractories makes it possible to suppress the precipitation (protrusion) of tridymite crystals from the base.

[0027] The substrate is made of a fused siliceous refractory containing at least 99% by weight of fused silica, and has a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less, and a K concentration of 50 ppm or less in at least a 3 mm thick region from the surface. The Ca, Na, and K concentrations can be verified by grinding the sample from the back side to a specified thickness, crushing it in an agate mortar, and performing specified component analysis on each crushed sample using ICP analysis.

[0028] In this way, since the Ca concentration is 100 ppm or less, the Na concentration is 50 ppm or less, and the K concentration is 50 ppm or less in at least a 3 mm thick region from the surface, the generation and precipitation of cristobalite crystals due to contact with high-temperature molten glass can be suppressed.

[0029] The air permeability evaluation method was carried out by cutting out a sample S of 8 mm thickness and 35 mm diameter from the surface of the twill substrate, fixing the sample S with an O-ring 2 under a compressive load of 1 kN in a SUS 1-inch union joint (inner diameter 38 mm) 1 shown in FIG. 1, and placing the sample S in a container 3 connected to the union joint 1 with an internal space of 754 cm 3This method evaluates breathability by drawing a vacuum using a vacuum pump 4 through a tube (diameter 80 mm x 150 mm) and measuring the internal pressure of the internal space after 60 minutes using a vacuum gauge 5.

[0030] The surface of the substrate preferably has a center line average roughness Ra of 1 μm or more and 10 μm or less. This can further reduce wear caused by contact with molten glass, and improve durability.

[0031] Next, a method for producing a zirconia according to the present invention will be described. The method for producing a tweel according to the present invention comprises adding a solvent to fused silica powder to produce a raw material slurry, molding the slurry, firing the slurry, and then grinding off the surface of the fired body. By grinding off the surface layer of the fired body in this manner, the dense surface layer formed by the molding and firing is removed, and air permeability is obtained such that the internal pressure after 60 minutes in the air permeability evaluation method is 0.005 MPa or more, and the precipitation of tridymite crystals can be suppressed.

[0032] The method for producing the twill according to the present invention preferably comprises adding ion-exchanged water to fused silica powder having a purity of 99% or more, with a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less, and a K concentration of 50 ppm or less, to produce a raw material slurry, which is then molded and fired at 1050°C to 1100°C, and then the surface layer of the fired body is ground off. This manufacturing method will be described in detail below.

[0033] First, 10% by weight of ion-exchanged water is added to 90% by weight of fused silica powder having a purity of 99% or more and a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less, and a K concentration of 50 ppm or less to produce a raw material slurry. The raw material slurry is then placed in a mold, molded, and fired at 1050° C. to 1100° C. Thereafter, the surface layer of the fired body is ground off to produce the Ziel base body.

[0034] In this way, it is preferable to use the casting method as the molding method, and to grind and remove the surface layer of the fired body to a thickness of 1 mm or more. The casting method can create a mold more inexpensively than press molding, and is suitable for molding large, complex-shaped products such as zircon. Therefore, the casting method, in which a slurry is poured into a plaster mold, is preferably used as a molding method for fused silica substrates.

[0035] In addition, a dense layer is generated on the surface of the base material of the cast zirconia when it starts to adhere to the plaster mold. This dense layer remains as a dense layer even after firing. And because the presence of this dense layer causes the precipitation of the tridymite crystals, the surface layer (dense layer) of the fired body is ground off. By grinding and removing the surface layer (dense layer) of this fired body, it is possible to obtain air permeability such that the internal pressure after 60 minutes in the air permeability evaluation method is 0.005 MPa or more, and the precipitation of tridymite crystals can be suppressed.

[0036] By grinding and removing the thickness of 1 mm or more, the dense layer on the surface of the twill substrate can be removed. For more reliable removal, removal of 3 mm or more is preferable. The removal (grinding) of the dense layer on the surface can be performed, for example, with a grinder.

[0037] After the grinding, the surface of the substrate is preferably polished until the center line average roughness Ra is 1 μm or more and 10 μm or less. This makes it possible to further reduce wear caused by contact with the molten glass. The polishing can be performed using a belt sander. EXAMPLES

[0038] A fused siliceous refractory material manufactured by casting was prepared, and the contact surface of the plaster mold was flat-ground to manufacture a sample. The detailed manufacturing method is shown below. A raw material slurry was generated by adding 10% by weight of ion-exchanged water to 90% by weight of fused silica powder with a purity of 99% or more and a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less, and a K concentration of 50 ppm or less. The raw material slurry was then poured into a Ziel-shaped gypsum mold shown in Figure 4 and molded.

[0039] The obtained molded body was dried at 110°C to 130°C and appropriately fired at 1050°C to 1100°C to obtain a Ziel 23-shaped body (external dimensions: total length 1100 mm x total height 800 mm x width 120 mm) made of fused siliceous refractory material as shown in Figure 4. Thereafter, the entire surface of the zirconia-shaped body was ground with a grinder and further polished with a belt sander.

[0040] Then, by carrying out the grinding and polishing, the surface grinding amount shown in Table 1 was ground and polished to obtain a ziel base body (Examples 1 to 3, Comparative Example 1, Comparative Example 2) made of a fused siliceous refractory. Note that the case where the ziel-shaped body of Example 2 was used and the grinding and polishing were not carried out was taken as a conventional example. Then, for each sample, the bulk density, air permeability evaluation, surface roughness Ra, and purity measurements were performed, and a tridymite formation test was also performed.

[0041] The specific evaluation method is as follows. The density (bulk density) was measured by cutting a block of 3 mm thick x 100 mm x 100 mm from the surface of the twill substrate, and measuring a portion of this block in accordance with JIS R2205. The sample was immersed in boiling water and measured by the Archimedes method. The purity of the fired surface (twill substrate surface) was measured by cutting a 3 mm thick x 10 mm x 10 mm thick sample from the block and grinding it in an agate mortar. Each ground sample was analyzed for the specified components by ICP analysis.

[0042] For the evaluation of breathability, a sample of 3 mm thickness x 35 mm diameter was cut out from the block and fixed with an O-ring 2 under a compressive load of 1 kN in a SUS 1-inch union joint 1 (inner diameter 38 mm) shown in FIG. The internal space connected to the union joint 1 is 754 cm 3 A vacuum was drawn by a vacuum pump 4 through a tube (D80×150 mm), and the internal pressure of the internal space 3 was measured after 60 minutes had passed.

[0043] The surface roughness Ra was measured using a commercially available surface roughness meter (small surface roughness measuring instrument SURFTEST SJ-210 manufactured by Mitutoyo Corporation) in accordance with JIS B0601:2013.

[0044] Blocks measuring 10 mm thick x 50 mm x 50 mm were cut out from the surfaces of the twill substrates of Examples 1 to 3, Comparative Examples 1 and 2, and the conventional example, and corrosion tests were carried out using automotive sheet glass powder having the composition of Table 2 as the corrosion material. The corrosion test conditions were as shown in Fig. 2, in which molten glass made from the glass powder in Table 2 was placed in an alumina crucible 10, and the opening of the alumina crucible 10 was blocked with a sample so that the observation surface faced the molten glass. Then, the sample was heated at 1200°C for 240 hours. The amount of tridymite generated on the inner surface of the sample exposed at 1200°C for 240 hours was obtained from the powder X-ray diffraction measurement results. Quantification was performed by comparing the peak intensity with a commercially available X-ray standard sample. The results are shown in Table 1.

[0045] [Table 1]

[0046] [Table 2]

[0047] As shown in Table 1, it was confirmed that the tweel substrates of Examples 1 to 3 were able to significantly reduce the tridymite generation rate compared to the tweel substrates of the conventional example and the comparative example.

[0048] Next, the twill substrates of Example 2, the conventional example, and Comparative Example 1 were used in a float furnace for one month, and the yield of plate glass products and the amount of wear of each twill substrate due to defects caused by the inclusion of silica-based foreign crystals such as tridymite and cristobalite were confirmed. As a result, it was confirmed that the tweed substrate of Example 2 had a yield ten times higher than that of the conventional tweed substrate.

[0049] It was also confirmed that the wear amount of the twill substrate of Comparative Example 1 was 1.5 times that of the twill substrates of Example 2 and the conventional example. This is because the center line average roughness Ra of the surface of Comparative Example 1 was 15 μm, which was larger than those of Example 2 and the conventional example, and the bulk density of Comparative Example 1 was 1.85 g / cm 3 It was confirmed that this was due to the small size of the

[0050] In this way, the twill of the present invention can reduce the amount of wear and tear, and also suppress the inclusion of silica-based foreign crystals in the molten glass, thereby improving the yield of flat glass products manufactured in a float glass manufacturing apparatus. [Explanation of symbols]

[0051] 1 Union fitting 2 O-rings 3. Container (internal space) 4. Vacuum pump 5 Vacuum gauge

Claims

1. A twill used to adjust the flow rate of molten glass when producing sheet glass by a float forming method, The substrate has a fused silica content of 99% by weight or more and a bulk density of 1.90 g / cm 3 Above, 1.99g / cm 3 It is made of the following fused silica refractories: At least a 3 mm thick region from the surface has air permeability such that the internal pressure after 60 minutes in an air permeability evaluation method is 0.005 MPa or more; Furthermore, in the thickness region, the Ca concentration is 100 ppm or less, the Na concentration is 50 ppm or less, and the K concentration is 50 ppm or less.

2. 2. The method according to claim 1, wherein the center line average roughness Ra of the surface of the substrate is 1 μm or more and 10 μm or less.

3. A method for producing a twill used to adjust the flow rate of molten glass when producing sheet glass by a float forming method, comprising: A method for producing a tweel, comprising adding a solvent to fused silica powder to produce a raw material slurry, molding the slurry, sintering the slurry to produce a sintered body, and then grinding off the surface of the sintered body.

4. The method for producing a twill according to claim 3, characterized in that the fused silica powder is a fused silica powder having a purity of 99% or more, with a Ca concentration of 100 ppm or less, a Na concentration of 50 ppm or less, and a K concentration of 50 ppm or less, the solvent is ion-exchanged water, and the firing temperature is 1050 ° C. to 1100 ° C.

5. 5. The method for producing a zirconia sieve according to claim 3, wherein the forming is performed by a casting method, and the thickness to be removed by grinding is 1 mm or more.

6. 6. The method for producing a zirconia zirconia according to claim 5, further comprising polishing the surface of the substrate until the centerline average roughness Ra of the surface is 1 [mu]m or more and 10 [mu]m or less after the grinding.

Citation Information

Patent Citations

  • Production of fused silica-based refractory

    JP1999060330A

  • Float glass for display substrate and its production

    JP2001026437A

  • Apparatus for metering the glass melt in the feed channel of a float installation for producing suspended glass ribbons

    JP2005527450A

  • Tweel for controlling amount of molten glass and method for feeding molten glass

    JP2011157249A

  • Method for manufacturing lithium alumino silicate glass, and float glass plate

    JP2021031317A