Adhesive tape
Adhesive tapes with a polyolefin foam base material and controlled compressive strength address flexibility and impact resistance issues, ensuring stability and conformability to curved surfaces in electronic devices.
Patent Information
- Application Number
- JP2022199112
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2037-08-30
AI Technical Summary
Existing adhesive tapes for electronic devices lack flexibility under high compression, leading to issues such as deformation, peeling, and damage due to insufficient base material strength, which is either too hard or too soft, failing to conform to curved surfaces and withstand internal and external stress.
Adhesive tapes with a polyolefin foam base material having a specific compressive strength range of 65% at 4.5 MPa or less and 80% at 20 MPa or less, utilizing a polyolefin resin composition with ethylene-vinyl acetate copolymer to maintain rubber elasticity and adjust compressive strength, ensuring the tape can follow curved surfaces without sudden hardness.
The adhesive tapes exhibit excellent conformability to curved adherends, providing impact resistance and stability, preventing peeling and damage, while maintaining dimensional stability.
Smart Images

Figure 0007565330000008 
Figure 0007565330000009 
Figure 0007565330000010
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive tape that is excellent in flexibility when highly compressed and has excellent performance such as impact resistance and stability when greatly deformed. [Background technology]
[0002] Portable electronic devices such as smartphones and tablet terminals generally have a structure in which a touch panel and a housing that houses a liquid crystal module are combined. For example, adhesive tape is used to fix the touch panel to the housing. Also, in electronic devices such as in-car displays and TVs, adhesive tape is used to fix a liquid crystal display (LCD) panel or an organic EL panel to the housing.
[0003] In recent years, electronic devices have become thinner, smaller, and more complex in design. As a result, for example, FPCs (Flexible Printed Circuits) are bent at sharper angles inside the device, resulting in an internal structure that is constantly subject to strong repulsive forces. In addition, in order to enlarge the display area of the LCD, the width of the frame (picture frame) surrounding the liquid crystal panel is narrowed, which is called narrowing of the picture frame. In addition, as electronic devices become more complex in design, the number of LCD panels with curved designs is increasing. Therefore, the adhesive tape that secures the housing and top panel must also be made thinner and have better conformability to curved objects. However, in order to withstand the repulsive forces of FPCs from the inside and impacts from the outside, not only the adhesive strength of the adhesive layer but also the strength of the base material is required.
[0004] If the strength of the base material of a narrow adhesive tape is insufficient, the adhesive tape will deform significantly in the thickness direction, and internal or external stresses will cause interlayer fracture, which may damage the device. Furthermore, the dimensional stability will be poor when the tape is applied to a housing, which may cause twisting. On the other hand, if the base material is too hard, the tape will not be able to conform to the curved adherend, causing the adhesive tape to peel off and damaging the device.
[0005] Incidentally, for the substrate of this type of adhesive tape, a polyolefin foam mainly composed of polyethylene or an acrylic foam in which various fillers are added to acrylic resin is generally used. For example, Patent Document 1 describes a waterproof double-sided tape having an adhesive layer on at least one side of a foam substrate. It also describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and that the interlaminar strength is preferably 6 to 50 N / cm and the 25% compressive strength is preferably 30 to 500 kPa.
[0006] Patent Document 2 describes an adhesive sheet having an adhesive layer on one or both sides of a foam substrate and used for fixing a housing and a component during the manufacture of an electronic device, etc. The foam substrate is described as being preferably a polyolefin foam, particularly a polyethylene foam, with an interlaminar strength of 20 N / cm or more and a 25% compressive strength of 80 kPa or more.
[0007] Patent Document 3 describes an impact-resistant double-sided adhesive tape having adhesive layers on both sides of a foam substrate. The foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and has a 25% compressive strength in the thickness direction of 380 kPa or less and an interlaminar strength of 400 mJ / cm. 2 It is described that a strength of 39 N / cm or more is preferable.
[0008] Patent Document 4 describes an adhesive tape having an adhesive layer on at least one surface of a foam substrate and used for fixing components of portable electronic devices, etc. The tape describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and that the interlaminar strength is preferably 20 N / cm or more and the 25% compressive strength is preferably 80 kPa or more.
[0009] Patent Document 5 describes an adhesive tape having an adhesive layer on at least one surface of a foam substrate and used for fixing components of portable electronic devices, etc. It also describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and that the 25% compressive strength is preferably 160 kPa or more and the interlaminar strength is preferably 13 N / cm or more.
[0010] Patent Document 6 describes an adhesive tape having an adhesive layer on at least one surface of a foam substrate and used for fixing components of portable electronic devices, etc. It also describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and that the 25% compressive strength is preferably 250 kPa or more and the interlaminar strength is preferably 25 N / cm or more.
[0011] Patent Document 7 describes an adhesive tape having adhesive layers on both sides of a foam substrate and used for fixing an organic EL display, etc. The tape describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and that the interlaminar strength is preferably 10 to 18 N / cm and the 25% compressive strength is preferably 30 kPa or more.
[0012] Patent Document 8 describes an adhesive tape having an adhesive layer on at least one surface of a foam substrate and used for fixing a protective panel for a screen display unit or an image display module, etc. The tape describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and that the interlaminar strength is preferably 6 to 50 N / cm and the 25% compressive strength is preferably 30 kPa or more.
[0013] Patent Document 9 describes an adhesive tape having adhesive layers on both sides of a foam substrate and used for fixing components of electronic devices, etc. The paper describes that the foam substrate is preferably a polyolefin foam, particularly a polyethylene foam, and preferably has an interlaminar strength of 10 to 50 N / cm and a 25% compressive strength of 10 to 500 kPa.
[0014] However, the foam substrates in Patent Documents 1 to 9 are made of relatively hard foams, and therefore have too high compressive strength when highly compressed, i.e., have poor flexibility when highly compressed, and are considered to have poor performance, such as poor impact resistance and stability when greatly deformed.
[0015] Patent Document 10 describes a polyolefin resin foam sheet used as a heat insulating material for electronic devices, etc., and an adhesive tape having an adhesive layer on at least one surface of the sheet. It also describes that the polyolefin foam sheet is preferably made of a polyethylene resin, has a 50% compressive strength of 120 kPa or less, and contains 70 to 100% closed cells.
[0016] However, the foamed sheet of Patent Document 10 has a low 50% compression strength, but the compression strength at a compression rate exceeding that is unknown. Therefore, the flexibility at high compression is unknown, and it is considered that the performance such as impact resistance and stability when greatly deformed may be inferior. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] JP 2015-98554 A [Patent Document 2] JP 2015-187263 A [Patent Document 3] JP 2016-183274 A [Patent Document 4] International Publication No. 2013 / 099755 [Patent Document 5] International Publication No. 2013 / 141167 [Patent Document 6] International Publication No. 2013 / 154137 [Patent Document 7] International Publication No. 2013 / 191106 [Patent Document 8] International Publication No. 2013 / 176031 [Patent Document 9] International Publication No. 2014 / 156816 [Patent Document 10] JP 2017-66404 A Summary of the Invention [Problem to be solved by the invention]
[0018] The present invention has been made to solve the problems of the prior art as described above. That is, an object of the present invention is to provide an adhesive tape that is excellent in flexibility when highly compressed and has excellent performance such as impact resistance and stability when greatly deformed. [Means for solving the problem]
[0019] Means for Solving the Problems The inventors of the present invention have conducted intensive research in order to achieve the above-mentioned object and have discovered that it is extremely effective to set the compressive strength of an adhesive tape having a foam substrate within a specific range when highly compressed, thereby completing the present invention.
[0020] That is, the present invention is an adhesive tape having an adhesive layer on one or both sides of a polyolefin foam substrate containing closed cells, and the adhesive tape has a 65% compressive strength of 4.5 MPa or less and an 80% compressive strength of 20 MPa or less, as measured in a compressive strength measurement method in accordance with JIS K 7181. Effect of the Invention
[0021] According to the findings of the present inventors, the specification of the compressive strength of an adhesive tape having a foam substrate at high compression is very suitable as an index for evaluating the conformability to a curved adherend. This is because an adhesive tape having a foam substrate has a property that, when compressed during application, the compressive strength increases suddenly from a certain point where the bubbles in the foam are completely crushed, and the tape becomes hard. When the adherend is curved, the hardened adhesive tape cannot sufficiently conform to the adherend. The present inventors have focused on this point and have made it possible to provide an adhesive tape that is excellent in, for example, impact resistance and stability when greatly deformed (such as conformability to a curved adherend) by suppressing a sudden increase in the compressive strength by setting the compressive strength at high compression within the above-mentioned specific range. [Brief description of the drawings]
[0022] [Figure 1] FIG. 2 is a schematic diagram for explaining a method for measuring bending moments in Examples and Comparative Examples. [Diagram 2] 1 is a graph showing master curves in the measurement of compressive strength in Examples 1 to 3 and Comparative Example 1. [Diagram 3] FIG. 2 is a schematic diagram for explaining an evaluation method of a 10-face drop impact test in Examples and Comparative Examples. [Figure 4] FIG. 2 is a schematic diagram for explaining an evaluation method of the electrostatic resistance test in the examples. [Diagram 5] 1 is a graph showing master curves in the measurement of compressive strength in Example 4 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] <Foam base material> The foam substrate used in the present invention is a substrate made of a foam of a polyolefin resin composition. The polyolefin resin composition preferably contains an ethylene-vinyl acetate copolymer and another polyolefin resin. The ethylene-vinyl acetate copolymer exhibits higher rubber elasticity than linear low-density polyethylene. Therefore, if an appropriate amount of ethylene-vinyl acetate copolymer is blended into the polyolefin resin composition, even if the bubble diameter of the closed bubbles in the foam substrate is reduced, the rubber elasticity suitable for the application of the adhesive tape substrate tends to be maintained. As a result, it becomes possible to reduce the bubble diameter, and it becomes easy to adjust the compression strength and interlayer strength at high compression. On the other hand, examples of other polyolefin resins include polyethylene resins, polypropylene resins, and mixtures thereof. In particular, linear low-density polyethylene (LLDPE) and ethylene propylene rubber (EPDM) are more preferable.
[0024] The polyolefin resin composition can be produced by a known method. For example, it can be obtained by irradiating a resin composition containing an ethylene-vinyl acetate copolymer and any other polyolefin resin with an electron beam to crosslink the resin. Foaming may be carried out simultaneously with or at a different time from the crosslinking.
[0025] The polyolefin resin composition may contain other additives within the range that does not impair the effects of the present invention. Specific examples of such additives include extenders, crosslinking agents, antioxidants, stabilizers, and coupling agents. The polyolefin resin composition may further contain light-shielding fillers and pigments. Specific examples of light-shielding fillers include carbon black, carbon nanotubes, and black inorganic fillers. Specific examples of pigments include carbon black, aniline black, acetylene black, and ketjen black.
[0026] The polyolefin foam substrate contains closed cells. Therefore, the pressure-sensitive adhesive tape of the present invention is also excellent in terms of waterproofness and dustproofness. The average cell diameter of the closed cells is preferably 0.04 to 0.45 mm, more preferably 0.10 to 0.35 mm. The density of the foam substrate is preferably 50 to 300 kg / m 3 , more preferably 80 to 200 kg / m 3 A foam substrate having such an average cell size and density is a substrate containing a relatively large number of relatively small closed cells.
[0027] The expansion ratio of the foam constituting the polyolefin foam substrate is preferably 2.0 to 15 times, more preferably 4.0 to 12 times.
[0028] The thickness of the polyolefin foam substrate is preferably 0.06 to 2.0 mm, and more preferably 0.1 to 1.8 mm.
[0029] The interlaminar strength of the polyolefin foam substrate is preferably 7 N / cm or more, more preferably 8 to 17 N / cm. The interlaminar strength is an index representing the strength of the foam substrate. A specific method for measuring the interlaminar strength is described in the Examples section.
[0030] The tensile modulus of the foam substrate is preferably 70 to 500 N / mm 2 , more preferably 100 to 450 N / mm 2 A specific method for measuring the tensile modulus is described in the section of Examples.
[0031] The bending moment (bending stiffness) in the MD and TD directions of the substrate is preferably 1 to 35 gf / cm, more preferably 2 to 30 gf / cm. A specific method for measuring the bending moment will be described in the Examples section.
[0032] It is better for the foam substrate not to have a support film. If a support film is present, the hard film will contact the adherend in all directions, including the thickness direction, flow direction, and width direction, from the foam, and may not be able to follow. The support film here is a film that compensates for the drawback of soft foams being easily stretched when handled. For example, a film-supported foam in which a foam and a support film are integrally molded is known as a commercially available product.
[0033] <Adhesive layer> The adhesive layer used in the present invention is not particularly limited. As the adhesive composition constituting the adhesive layer, various known adhesive compositions such as acrylic, rubber, silicone, and urethane compositions can be used. Among them, from the viewpoints of impact resistance, adhesive strength, waterproofness, and the like, an acrylic adhesive composition containing a (meth)acrylic acid ester copolymer is preferred. On the other hand, it is preferred that the adhesive layer does not contain a tackifier resin. This is because if a tackifier resin is contained, the adhesive may soften and the impact resistance and adhesiveness may decrease.
[0034] The components of the acrylic pressure-sensitive adhesive composition are not particularly limited, but preferably contain an acrylic copolymer (A) containing 10-20% by mass of (meth)acrylic acid alkyl ester (A1) having an alkyl group with 1-3 carbon atoms, 50-80% by mass of (meth)acrylic acid alkyl ester (A2) having an alkyl group with 4-12 carbon atoms, 10-15% by mass of carboxyl group-containing monomer (A3), 0.01-0.5% by mass of hydroxyl group-containing monomer (A4), and 1-5% by mass of vinyl acetate (A5) as polymer chain components. In this case, a crosslinking agent capable of reacting with the carboxyl group and / or hydroxyl group of the acrylic copolymer (A) may be blended to form a crosslinked structure with the acrylic copolymer (A). In addition, a silane coupling agent or an antioxidant may be blended to improve resilience.
[0035] The thickness of the pressure-sensitive adhesive layer is preferably 5 to 125 μm, and more preferably 10 to 80 μm.
[0036] The adhesive layer can be formed, for example, by crosslinking the adhesive composition. The adhesive composition can be applied to a substrate and crosslinked by heating to form an adhesive layer on the foam substrate. The adhesive composition can also be applied to a release paper or other film and crosslinked by heating to form an adhesive layer, which can then be attached to one or both sides of the foam substrate. For applying the adhesive composition, a coating device such as a roll coater, a die coater, or a lip coater can be used. When heating is performed after application, the solvent in the adhesive composition can be removed along with the crosslinking reaction caused by heating.
[0037] <Adhesive tape> The pressure-sensitive adhesive tape of the present invention has a pressure-sensitive adhesive layer on one or both sides of a polyolefin foam substrate. The pressure-sensitive adhesive layer may be formed on only one side of the substrate, but is preferably formed on both sides to form a double-sided pressure-sensitive adhesive tape.
[0038] The thickness of the pressure-sensitive adhesive tape of the present invention is preferably 0.2 to 2.0 mm, more preferably 0.3 to 2.0 mm, and the width of the pressure-sensitive adhesive tape is preferably 0.8 to 10 mm, more preferably 1 to 5 mm.
[0039] The pressure-sensitive adhesive tape of the present invention has a 65% compressive strength of 6.0 MPa or less (preferably 0.09 to 5.5 MPa, more preferably 0.15 to 5.0 MPa) and an 80% compressive strength of 20 MPa or less (preferably 0.5 to 17 MPa, more preferably 0.7 to 14 MPa) measured by a compressive strength measurement method according to JIS K 7181. Similarly, the 70% compressive strength is preferably 7.0 MPa or less (more preferably 0.3 to 6.5 MPa), and the 75% compressive strength is preferably 9.5 MPa or less (more preferably 0.4 to 9.0 MPa). The pressure-sensitive adhesive tape of the present invention having such compressive strength is excellent in performance such as impact resistance and stability when greatly deformed, since a sudden increase in compressive strength is suppressed.
[0040] When the foam substrate of the pressure-sensitive adhesive tape of the present invention has a thickness of 0.06 mm or more and less than 0.9 mm, the 65% compressive strength of the pressure-sensitive adhesive tape is 6.0 MPa or less (preferably 0.15 to 5.5 MPa, more preferably 0.3 to 5.0 MPa), the 80% compressive strength is 20 MPa or less (preferably 2.0 to 17 MPa, more preferably 3.0 to 14 MPa), the 70% compressive strength is preferably 7.0 MPa or less (more preferably 0.8 to 6.5 MPa), and the 75% compressive strength is preferably 9.5 MPa or less (more preferably 1.0 to 9.0 MPa).
[0041] When the foam substrate of the pressure-sensitive adhesive tape of the present invention has a thickness of 0.9 mm or more and 2.0 mm or less, the 65% compression strength of the pressure-sensitive adhesive tape is preferably 0.5 MPa or less (more preferably 0.09 to 0.4 MPa or less, particularly preferably 0.15 to 0.35 MPa), the 80% compression strength is preferably 2.5 MPa or less (more preferably 0.5 to 2.0 MPa, particularly preferably 0.7 to 1.5 MPa), the 70% compression strength is preferably 0.8 MPa or less (more preferably 0.3 to 0.7 MPa), and the 75% compression strength is preferably 1.3 MPa or less (more preferably 0.4 to 1.0 MPa).
[0042] Generally, if the proportion of closed bubbles in a foam is reduced, the interlaminar strength is increased, but the compressive strength of the foam is also increased. Conversely, if the proportion of closed bubbles is increased, the compressive strength is decreased, but the interlaminar strength is also decreased. If the interlaminar strength of the foam substrate is low, for example, when the adhesive tape is used in an electronic device, the foam substrate may undergo interlaminar destruction when an impact force is applied to the electronic device, which may cause the electronic device to malfunction. On the other hand, according to the findings of the present inventors, a foam substrate having a relatively small average bubble diameter and containing a relatively large number of small closed bubbles has a low compressive strength at high compression, and the interlaminar strength is not so low. Therefore, in the present invention, it is preferable to use such a type of foam substrate. EXAMPLES
[0043] The present invention will be described in more detail below with reference to examples and comparative examples. In the following description, "parts" means parts by mass and "%" means % by mass.
[0044] <Pressure-sensitive adhesive layer manufacturing examples 1 to 3> In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, the components (A1) to (A5) in the amounts (% by mass) shown in the table, ethyl acetate, n-decanethiol as a chain transfer agent, and 0.1 parts of lauryl peroxide as a peroxide radical polymerization initiator were charged. Nitrogen gas was sealed in the reaction apparatus, and the polymerization reaction was carried out under a nitrogen gas stream with stirring at 68°C for 3 hours, and then at 78°C for 3 hours. The mixture was then cooled to room temperature, and ethyl acetate was added. As a result, an acrylic copolymer (A) with a solid content concentration of 30% was obtained.
[0045] The weight average molecular weight (Mw) and theoretical Tg of each acrylic copolymer are shown in the table. The weight average molecular weight (Mw) is a value obtained by measuring the molecular weight of the acrylic copolymer in terms of standard polystyrene by the GPC method using the following measuring device and conditions. Equipment: LC-2000 series (manufactured by JASCO Corporation) Columns: Shodex KF-806M x 2, Shodex KF-802 x 1 Eluent: Tetrahydrofuran (THF) ·Flow rate: 1.0mL / min Column temperature: 40℃ ·Injection volume: 100μL Detector: Refractometer (RI) Measurement sample: An acrylic polymer was dissolved in THF to prepare a solution with an acrylic polymer concentration of 0.5% by mass, and then filtered to remove any impurities.
[0046] The theoretical Tg is a value calculated according to the FOX formula.
[0047] [Table 1]
[0048] The abbreviations in Table 1 are as follows. "MA": Methyl acrylate "2-EHA": 2-Ethylhexyl acrylate "BA": n-butyl acrylate "AA": acrylic acid "4-HBA": 4-hydroxybutyl acrylate "Vac": Vinyl Acetate
[0049] Then, 0.04 parts of an isocyanate-based crosslinking agent (Coronate (registered trademark) L-45E, 45% solution) manufactured by Nippon Polyurethane Industry Co., Ltd. as a crosslinking agent (B), 0.001 parts of an epoxy-based crosslinking agent (TEDRAD (registered trademark)-C) manufactured by Mitsubishi Gas Chemical Co., Ltd. as a silane coupling agent (C) 0.1 parts of a silane coupling agent (trade name KBM-403) manufactured by Shin-Etsu Chemical Co., Ltd. as an antioxidant (D) 0.2 parts of an antioxidant (Irganox (registered trademark) 1010) manufactured by BASF was added and mixed with respect to 100 parts of the solid content of each acrylic copolymer (A) to prepare a pressure-sensitive adhesive composition. Furthermore, this pressure-sensitive adhesive composition was applied to a silicone-treated release paper so that the thickness after drying was 0.075 mm. Next, the solvent was removed and dried at 110 ° C., and a crosslinking reaction was carried out to form pressure-sensitive adhesive layers 1 to 3.
[0050] <Example 1> A substrate made of a polyethylene (PE)-based foam containing an appropriate amount of ethylene-vinyl acetate copolymer (EVA) with a thickness of 1.0 mm (tensile modulus = 141 N / mm 2 , bending moment = 25gf / cm, expansion ratio = 11 times, average cell diameter = 0.123mm, density = 90kg / m 3 Both sides of this substrate were subjected to a corona discharge treatment, the adhesive layer on the release paper obtained in Production Example 1 was attached to both sides of the substrate, and the substrate was cured at 40° C. for 3 days to obtain a double-sided adhesive tape.
[0051] <Examples 2 and 3> Double-sided pressure-sensitive adhesive tapes were obtained in the same manner as in Example 1, except that the pressure-sensitive adhesive layers obtained in Production Examples 2 and 3 were used as the pressure-sensitive adhesive layers.
[0052] <Comparative Example 1> The substrate was a 1.0 mm thick film-supported polyurethane foam (manufactured by S&K POLYTEC, product name NANOCELL TM PSR, tensile modulus = 5302N / mm2 , bending moment = 21 gf / cm, expansion ratio = 2.4 times, average cell diameter = 0.063 mm, density = 410 kg / m 3 A double-sided adhesive tape was obtained in the same manner as in Example 1, except that ) was used.
[0053] The tensile modulus of the substrates and the bending moment of the substrates and pressure-sensitive adhesive tapes in the examples and comparative examples were measured by the following methods. The measured values are shown in Table 2.
[0054] (tensile modulus) The substrate was cut into a strip (long side in MD) of 10 mm width (W) and 70 mm length to prepare a test piece. The thickness was measured with a 1 / 100 dial gauge (N=5), and the average value of the five points was taken as the thickness (t). The cross-sectional area (S) of the test piece was calculated using the following formula. Cross-sectional area S(mm 2 )=t×W t: thickness (mm) W: Width (mm)
[0055] In accordance with JIS K7161 2014, the chuck spacing (L) of a commercially available tensile testing device (manufactured by Toyo Seiki Seisakusho, device name Strograph V-10C, full scale 50N) was set to 20mm, and the upper and lower ends of the test piece were chucked. The test piece was then pulled at a pulling speed of 10mm / min to obtain a tensile load-displacement curve. A linear equation was obtained from the tensile loads at which the displacements of the tensile load-displacement curve were 0.05mm and 0.25mm. The displacement x (mm) at a tensile load F = 10N was obtained from the linear equation obtained, and the tensile modulus of elasticity, which is an index of the stiffness of the base material, was calculated from the following equation. Tensile modulus (N / mm 2 )=(F / S) / (x / L) F: Tensile load = 10 (N) S: Cross-sectional area (mm 2 ) x: Displacement (mm) when tensile load is 10N L: Chuck distance = 20 (mm)
[0056] The linear equations and tensile moduli are as follows: Examples 1 to 3: Linear equation y = 0.705x + 0.01475, tensile modulus 141 N / mm 2 Comparative Example 1: Linear equation y=1.9x+0.01, tensile modulus 380N / mm 2 Comparative Example 2: Linear equation y=1.195x+0.0761, tensile modulus 240N / mm 2 Comparative Example 3: Linear equation y=29.65x-1.1825, tensile modulus 5302N / mm 2
[0057] (bending moment) The substrate (or double-sided adhesive tape 1) was cut into a strip of 38 mm width and 50 mm length, which was used as a test piece. The obtained test piece was sandwiched between four terminals 2 as shown in FIG. 1. Then, in accordance with JIS P8125, it was installed in a portion of a commercially available Taber stiffness tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.) that operates during testing, and 10 g weights were attached to the pendulum, and the scale was read at a bending speed of 3° / sec and a bending angle of 15°, which was used as the measured value. Then, this measured value was substituted into the following formula to calculate the bending moment (M) in the MD direction and the TD direction. Bending moment (gf / cm) = 38.0 nk / w n: Scale reading (1 for a 10g weight) k: Moment per division (gf / cm) w: width of test piece
[0058] [Table 2]
[0059] <Compressive strength> The double-sided adhesive tapes obtained in the Examples and Comparative Examples were overlapped until the thickness reached 12 mm, and the compressive strength was measured at compression ratios of 0 to 80% in accordance with JIS K 7181 using measurement (analysis) software Trapezium X and measurement mode single (AG-20kNX, manufactured by Shimadzu Corporation), and a master curve was created to obtain compressive strengths of 60%, 65%, 70%, 75%, and 80%. The results are shown in Table 3. Furthermore, the master curves of the Examples and Comparative Examples are shown in FIG. 2.
[0060] <Interlaminar strength> Aluminum foil with one side anodized was attached to both sides of the double-sided adhesive tape obtained in the examples and comparative examples, and pressed with a 2 kg roller by rolling it back and forth once. After pressing, it was aged for 30 minutes at 23°C and 50% Rh, and the aluminum foil was chucked at the top and bottom with a commercially available tensile tester (manufactured by Toyo Seiki Seisakusho, device name Strograph V1-C, full scale 100N). It was then pulled at a pulling speed of 300 mm / min, and the force (N / cm) required to tear the foam was measured. The results are shown in Table 3.
[0061] [Table 3]
[0062] <Evaluation test> The double-sided pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Table 4.
[0063] (tensile strength / elongation) The double-sided adhesive tape was cut into a strip (long side in the MD direction) with a width (W) of 10 mm and a length of 70 mm, which was used as a test piece. In accordance with JIS K7161 2014, the chuck interval (L) of the tensile tester (manufactured by Toyo Seiki Seisakusho, device name Strograph V1-C, full scale 200N) was set to 50 mm, and the upper and lower ends of the test piece were chucked. The tape was then pulled at a pulling speed of 300 mm / min, and the force (N / cm) applied when the adhesive tape broke and the length (%) stretched until the tape broke were measured.
[0064] (10-sided drop impact test) As shown in FIG. 3, the double-sided adhesive tape 4 was cut into a frame of 60 mm×120 mm with a predetermined width (about 1 mm), one of the release papers was peeled off, and the tape was attached to a glass plate 5 having a thickness of 0.5 mm. The other release paper was then peeled off, and the tape was attached to a polycarbonate plate 3 having a thickness of 1.5 mm. The attached member was subjected to a pressure treatment (0.5 MPa) at 23° C. for 5 seconds using an autoclave, and then aged in an atmosphere of 23° C. for 24 hours. The attached member was then dropped 20 times from a height of 1 m. The drop was performed so that the place where the attached member collided with the landing surface changed each time. Specifically, the places where the attached member collided with the landing surface were the 10 places indicated by the arrows in FIG. 3. The evaluation was performed according to the following criteria. "◯": The tape did not peel off even after being dropped 20 times. "X": The tape peeled off before being dropped 20 times.
[0065] (Static electricity resistance test) The double-sided adhesive tape 1 was cut into a strip of 0.8 mm wide and 80 mm long, and the release paper on one side was peeled off and the strip was stuck between the copper electrode 7 and the copper electrode 8 (electrode distance 1.0 mm) formed on the acrylic plate 6 of 2.0 mm thick x 80 mm x 120 mm. The release paper on the other side was peeled off and the acrylic plate 6 of 2.0 mm thick x 80 mm x 80 mm was stuck. This sample was subjected to a pressure treatment (0.5 MPa) at 23°C for 5 seconds using an autoclave. Then, as shown in FIG. 4, the electrostatic resistance of this sample was evaluated based on IEC61000-4-2 (electrostatic resistance standard). Specifically, an electrostatic gun was used to apply each voltage 50 times to the copper electrode 7, and the applied voltage (ESD resistance voltage) when the current was conducted to the copper electrode 8 side was measured. The sample was placed on a stainless steel table 10 via an insulating sheet 9, and the copper electrode was grounded to the stainless steel table 10.
[0066] [Table 4]
[0067] <Evaluation of Examples 1 to 3 and Comparative Example 1> As is clear from the evaluation results in Table 4, the pressure-sensitive adhesive tapes of Examples 1 to 3 were excellent in all properties.
[0068] On the other hand, the adhesive tape of Comparative Example 1 had too high compressive strength when highly compressed, i.e., the flexibility of the tape was poor, and therefore the drop impact resistance was poor. Specifically, in the 10-sided drop impact test, the foam substrate (foam) was destroyed, causing the adhesive tape to peel off. The static electricity resistance was also poor.
[0069] <Example 4> The substrate was a 0.3 mm thick polyethylene (PE) foam containing an appropriate amount of ethylene-vinyl acetate copolymer (EVA) (tensile modulus = 276 N / mm 2 , bending moment = 3gf / cm, expansion ratio = 5.3 times, average cell diameter = 0.207mm, density = 186kg / m 3 ) was used, an adhesive tape was produced in the same manner as in Example 1 and evaluated in the same manner. The results are shown in Tables 5 to 7 and FIG.
[0070] <Comparative Example 2> The substrate was a 0.3 mm thick polyethylene (PE) foam containing an appropriate amount of ethylene-vinyl acetate copolymer (EVA) (tensile modulus = 215 N / mm 2 , bending moment = 15 gf / cm, expansion ratio = 2.7 times, average cell diameter = 0.188 mm, density = 363 kg / m 3 ) was used, an adhesive tape was produced in the same manner as in Example 1 and evaluated in the same manner. The results are shown in Tables 5 to 7 and FIG.
[0071] [Table 5]
[0072] [Table 6]
[0073] [Table 7]
[0074] <Evaluation of Example 4 and Comparative Example 2> As is clear from the evaluation results in Table 7, the thin pressure-sensitive adhesive tape of Example 4 was excellent in all properties.
[0075] On the other hand, the thin adhesive tape of Comparative Example 2 had too high compressive strength when highly compressed, i.e., the flexibility of the tape was poor, and therefore the drop impact resistance was poor. Specifically, the adhesive tape peeled off in the 10-sided drop impact test. [Industrial Applicability]
[0076] The adhesive tape of the present invention has excellent flexibility when highly compressed, and is excellent in performance such as impact resistance and stability when greatly deformed. Therefore, it is useful for various applications in fields where such properties are required. In particular, it can be suitably used in applications for electronic devices such as smartphones, tablet terminals, in-vehicle displays, and TVs, and is particularly suitable for use in small electronic devices that are often subjected to impact forces due to accidents such as dropping. [Explanation of symbols]
[0077] 1 Double-sided adhesive tape 2 Terminal 3 Polycarbonate plate 4 Double-sided adhesive tape 5. Glass Plate 6 Acrylic board 7 copper electrode 8 copper electrode 9. Insulation sheet 10 Stainless steel table
Claims
1. A pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on one or both sides of a polyolefin foam substrate containing closed cells, The polyolefin foam substrate comprises an ethylene-vinyl acetate copolymer and another polyolefin resin, The density of the polyolefin foam substrate is 50 to 300 kg / m 3 and The thickness of the polyolefin foam substrate is 0.06 mm or more and less than 0.9 mm, or 0.9 mm or more and 2.0 mm or less; when the thickness of the polyolefin foam substrate is 0.06 mm or more and less than 0.9 mm, the 65% compressive strength of the pressure-sensitive adhesive tape measured in accordance with JIS K 7181 is 0.3 MPa or more and 5.0 MPa or less, and the 80% compressive strength of the pressure-sensitive adhesive tape measured in accordance with JIS K 7181 is 3.0 MPa or more and 14 MPa or less, When the thickness of the polyolefin foam substrate is 0.9 mm or more and 2.0 mm or less, the 65% compressive strength of the pressure-sensitive adhesive tape, as measured in a compressive strength measurement conforming to JIS K 7181, is 0.15 MPa or more and 0.35 MPa or less, and the 80% compressive strength of the pressure-sensitive adhesive tape, as measured in a compressive strength measurement conforming to JIS K 7181, is 0.7 MPa or more and 1.5 MPa or less.
2. The tensile modulus of the polyolefin foam substrate is 70 to 500 N / mm 2 2. The adhesive tape according to claim 1,
3. 3. The pressure-sensitive adhesive tape according to claim 1, wherein the other polyolefin resin is a polyethylene resin, a polypropylene resin, or a mixture thereof.
4. The pressure-sensitive adhesive tape according to claim 1 , wherein the polyolefin foam substrate does not have a support film.
5. The pressure-sensitive adhesive tape according to claim 1 , wherein the pressure-sensitive adhesive layer comprises a (meth)acrylic acid ester copolymer.
6. The pressure-sensitive adhesive tape according to claim 1 , wherein the pressure-sensitive adhesive layer does not contain a tackifier resin.
7. The adhesive tape according to any one of claims 1 to 6, wherein the adhesive tape has a thickness of 0.2 to 2.0 mm.
8. The pressure-sensitive adhesive tape according to claim 1 , wherein the polyolefin foam substrate has an interlaminar strength of 7 N / cm or more.
9. The pressure-sensitive adhesive tape according to claim 1 , wherein the polyolefin foam substrate has a thickness of 0.06 mm or more and less than 0.9 mm.
10. The pressure-sensitive adhesive tape according to claim 9, wherein the pressure-sensitive adhesive tape has a 70% compressive strength of 0.8 MPa or more and 6.5 MPa or less, as measured in a compressive strength measurement according to JIS K 7181.
11. The pressure-sensitive adhesive tape according to claim 9 or 10, wherein the pressure-sensitive adhesive tape has a 75% compressive strength of 1.0 MPa or more and 9.0 MPa or less, as measured in a compressive strength measurement according to JIS K 7181.
12. The pressure-sensitive adhesive tape according to claim 1 , wherein the polyolefin foam substrate has a thickness of 0.9 mm or more and 2.0 mm or less.
13. The pressure-sensitive adhesive tape according to claim 12, wherein the pressure-sensitive adhesive tape has a 70% compressive strength of 0.3 MPa or more and 0.7 MPa or less, as measured in a compressive strength measurement according to JIS K 7181.
14. The pressure-sensitive adhesive tape according to claim 12 or 13, wherein the pressure-sensitive adhesive tape has a 75% compressive strength of 0.4 MPa or more and 1.0 MPa or less, as measured in a compressive strength measurement according to JIS K 7181.
15. The pressure-sensitive adhesive tape according to claim 1 , which is an adhesive tape for electronic devices.
Citation Information
Patent Citations
Crosslinked synthetic resin foam
JP1984041338A
Foamed self-adhesive tape or sheet
JP1984091178A
Self-adhesive tape or sheet
JP1984091179A
Self-adhesive tape or sheet
JP1991041179A
Laminate and adhesive tape
JP1997239882A