Core-shell type lithium-containing polyacrylic water-based adhesive, and preparation method therefor and use thereof

By designing a core-shell lithium-containing polyacrylic acid water-based adhesive, the problems of low adhesion and poor flexibility in lithium-ion batteries are solved, and efficient lithium-ion battery charge and discharge performance is achieved.

WO2024207816A1PCT designated stage expired Publication Date: 2024-10-10SHENZHEN HAOFEI NEW MATERIAL CO LTD

Patent Information

Application Number
PCT/CN2023/141443
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2023-12-25
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

The adhesive used for negative electrodes in existing lithium-ion batteries has low adhesion and poor flexibility, and cannot meet the needs of efficient charging and discharging.

Method used

A core-shell lithium-containing polyacrylic acid water-based adhesive is used, and specific polymerized monomers and lithium ions are selected and introduced during emulsion polymerization to form an adhesive with high adhesion, flexibility and low swelling.

Benefits of technology

It improves the first charge and discharge efficiency of lithium-ion batteries, reduces the loss of lithium ions, and solves the problems of adhesion and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023141443-FTAPPB-I100001
    Figure PCTCN2023141443-FTAPPB-I100001
Patent Text Reader

Abstract

Provided in the present invention are a core-shell type lithium-containing polyacrylic water-based adhesive, and a preparation method therefor and the use thereof. The core-shell type lithium-containing polyacrylic water-based adhesive comprises a polymer having a core-shell structure and lithium ions, wherein a polymerization monomer of the polymer having a core-shell structure comprises a basic monomer, an optional first functional monomer, a second functional monomer and a crosslinking monomer. The core-shell type lithium-containing polyacrylic water-based adhesive provided in the present invention has the characteristics of a relatively high adhesive force, relatively good flexibility and a low expansion rate, and making a lithium-ion battery using the adhesive have a high first-time charging and discharging efficiency, and solves the problems of low adhesion, poor flexibility, low first effect, etc., currently present in an adhesive for a negative electrode of a lithium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

A core-shell lithium-containing polyacrylic acid aqueous adhesive and its preparation method and application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 6, 2023, with application number 202310357773.4 and application name “A core-shell type lithium-containing polyacrylic acid aqueous adhesive and its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The invention belongs to the technical field of water-based adhesives, and particularly relates to a core-shell type lithium-containing polyacrylic acid water-based adhesive, a preparation method and an application thereof. Background Art

[0003] Lithium-ion batteries, as secondary batteries, are widely used in various fields due to their advantages, including high energy conversion rate, high energy density, high charge and discharge rate, no memory effect, and environmental friendliness. Polymer adhesives, with their excellent bonding properties, can bind various particles together and tightly bond them to the current collector, making them an indispensable component of lithium-ion batteries. In addition to high adhesion, high-performance adhesives also require the following properties: good flexibility, electrolyte resistance, compactness, chemical and electrochemical stability, low cost, and environmental friendliness.

[0004] Currently, the adhesives used in lithium-ion battery industry fall into three main categories: polyvinylidene fluoride (PVDF), styrene-butadiene rubber latex and carboxymethyl cellulose (SBR / CMC), and polyacrylic acid (PAA). PVDF offers advantages such as good adhesion to aluminum foil and strong resistance to electrochemical corrosion, but poor adhesion to copper foil. NMP solvent is moisture-sensitive, toxic, and its volatilization can pollute the environment. SBR / CMC adhesives have poor process performance and demanding conditions, significantly affected by factors such as stirring, pH, and electrode material ratio. Both PVDF and SBR / CMC adhesives are relatively expensive. PAA adhesives, with their strong adhesion, excellent stability, low price, and environmental friendliness, are currently a hot topic in negative electrode binder research. However, conventional PAA adhesives cannot meet the comprehensive requirements for negative electrode sheets.

[0005] Therefore, in this field, the PAA adhesive needs to be modified to simultaneously meet the requirements for adhesion, flexibility and electrochemical performance.

[0006] Summary of the Invention

[0007] To address the shortcomings of the prior art, the present invention provides a core-shell lithium-containing polyacrylic acid aqueous adhesive, its preparation method, and its application. The core-shell lithium-containing polyacrylic acid aqueous adhesive exhibits high adhesion, good flexibility, and low swelling, while also reducing lithium ion loss during charge and discharge, enabling the adhesive to play a greater role in lithium-ion batteries.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In one aspect, the present invention provides a core-shell lithium-containing polyacrylic acid aqueous adhesive, wherein the core-shell lithium-containing polyacrylic acid aqueous adhesive comprises a core-shell polymer and lithium ions, wherein the polymerization monomers of the core-shell polymer comprise a basic monomer, an optional first functional monomer, a second functional monomer, and a cross-linking monomer;

[0010] The basic monomer is selected from any one or a combination of at least two of acrylate monomers, vinyl acetate or styrene; the first functional monomer is selected from any one or a combination of at least two of lithium acrylate, lithium methacrylate, lithium crotonate, lithium allyl acetate, lithium isovalerate, lithium 5-hexanoate, lithium hexadienedioate, lithium 6-heptanoate, lithium isoheptanoate, lithium (E)-2-octenoate or lithium acetylacetonate; the second functional monomer is selected from any one or a combination of at least two of acrylic acid, methacrylic acid, acrylonitrile, acrylamide, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate, and 4-hydroxybutyl acrylate; the crosslinking monomer is selected from any one or a combination of at least two of diacetone acrylamide, N-hydroxymethyl acrylamide, divinylbenzene, aziridine, glycidyl methacrylate, ethoxylated trimethylolpropane triacrylate or a silane coupling agent.

[0011] In the present invention, a core-shell structured polymer is obtained by polymerizing a basic monomer, an optional first functional monomer, a second functional monomer, and a cross-linking monomer, and lithium ions are introduced into the adhesive, so that the aqueous adhesive is a lithium-containing core-shell polyacrylic acid aqueous adhesive. This adhesive has high bonding strength, good flexibility, and low swelling, reduces the loss of lithium ions during the charge and discharge process, and enables the adhesive to play a greater role in lithium-ion batteries.

[0012] In the present invention, the core-shell type lithium-containing polyacrylic acid aqueous adhesive is obtained by emulsion polymerization.

[0013] In the present invention, the lithium ions in the core-shell lithium-containing polyacrylic acid aqueous adhesive can be introduced through the first functional monomer, can be introduced through the lithium-containing pH adjuster in emulsion polymerization, or can be introduced simultaneously through the first functional monomer and the lithium-containing pH adjuster in emulsion polymerization.

[0014] Preferably, the pH regulator containing lithium is selected from any one of lithium hydroxide, lithium carbonate or lithium bicarbonate, or a combination of at least two thereof.

[0015] Preferably, the polymerized monomers of the core include the following components in parts by weight: 12-80 parts (e.g., 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts or 80 parts) of the base monomer, 0.25-55 parts (e.g., 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts) of the base monomer, , 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or 55 parts) of an optional first functional monomer, 0.25-30 parts (e.g., 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts or 30 parts) of a second functional monomer and 0.25-15 parts (e.g., 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts or 15 parts) of a crosslinking monomer.

[0016] Preferably, the polymerized monomers of the shell include the following components in mass percentages: 10-75 parts (e.g., 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts or 75 parts) of the basic monomer, 0.25-55 parts (e.g., 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 2 The invention further comprises the following: 1) an optional first functional monomer, 2) an optional second functional monomer, 3) an optional second functional monomer, 4) an optional first functional monomer, 5 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or 55 parts) of an optional first functional monomer, 0.25-30 parts (e.g., 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts or 30 parts) of a second functional monomer, and 0.1-15 parts (e.g., 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts or 15 parts) of a crosslinking monomer.

[0017] On the other hand, the present invention provides a method for preparing the core-shell type lithium-containing polyacrylic acid aqueous adhesive as described above, the preparation method comprising the following steps:

[0018] (1) preparing a core pre-emulsified liquid, a core pre-emulsified seed emulsion, a shell pre-emulsified liquid, a bottom reaction liquid, and an initiator solution;

[0019] (2) adding the pre-emulsified seed emulsion to the reaction liquid at the bottom of the kettle, heating it, adding the initiator solution, and reacting;

[0020] (3) adding the core pre-emulsion and the initiator solution to the reaction solution obtained in step (2) to react;

[0021] (4) adding the shell pre-emulsion and the initiator solution to the reaction solution obtained in step (3), reacting to obtain the core-shell type lithium-containing polyacrylic acid aqueous adhesive.

[0022] Preferably, the core pre-emulsion comprises basic monomers, optional first functional monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water. In the present invention, optional means that it may or may not contain.

[0023] Preferably, the core pre-emulsion comprises 12.25-65 parts (e.g., 13, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, or 65 parts) of base monomer, 0.245-50 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts) of optional first functional monomer, 0.245-25 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, or 25 parts) of second functional monomer, and 0.25-15 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, or 15 parts) of crosslinking monomer.

[0024] Preferably, the amount of emulsifier in the core pre-emulsion is 0.25%-4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example, 0.25%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.

[0025] Preferably, the amount of deionized water in the core pre-emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0026] Preferably, the core pre-emulsified seed emulsion comprises an essential monomer, an optional first functional monomer and a second functional monomer;

[0027] Preferably, the core pre-emulsified seed emulsion includes 0.05-30 parts (e.g., 0.05, 0.1, 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of basic monomer, 0.05-25 parts (e.g., 0.05, 0.1, 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20 or 25 parts) of optional first functional monomer and 0.05-8 parts (e.g., 0.05, 0.1, 0.3, 0.5, 1, 3, 5 or 8 parts) of second functional monomer.

[0028] Preferably, the amount of emulsifier in the core pre-emulsified seed emulsion is 0.005%-4% of the total weight of the basic monomer, the first functional monomer, and the second functional monomer in the seed emulsion, for example, 0.005%, 0.008%, 0.01%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3% or 4%.

[0029] Preferably, the amount of deionized water in the core pre-emulsified seed emulsion is 10%-80% of the total weight of the basic monomers, the first functional monomers, the second functional monomers and the cross-linking monomers in the seed emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0030] Preferably, the shell pre-emulsion comprises a basic monomer, a second functional monomer, a cross-linking monomer, an emulsifier and deionized water.

[0031] Preferably, the shell pre-emulsion comprises 10-75 parts (e.g., 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts or 75 parts) base monomer, 0.2-55 parts (e.g., 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, or 55 parts) of an optional first functional monomer, 0.2-30 parts (e.g., 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts, or 30 parts) of a second functional monomer, and 0.1-15 parts (e.g., 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, or 15 parts) of a crosslinking monomer.

[0032] Preferably, the amount of emulsifier in the shell pre-emulsion is 0.2%-4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example, 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.

[0033] Preferably, the amount of deionized water in the shell pre-emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the shell pre-emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 48%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0034] Preferably, the reaction liquid at the bottom of the kettle comprises an emulsifier, deionized water and a buffer.

[0035] Preferably, the content of each component in the bottom reaction liquid is 0.1 to 3 parts (for example, 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts or 3 parts) of emulsifier, 50 to 120 parts (for example, 50 parts, 60 parts, 70 parts, 75 parts, 80 parts, 90 parts, 100 parts, 110 parts or 120 parts) of deionized water, and 0.25 to 1 part (for example, 0.25 parts, 0.3 parts, 0.5 parts, 0.7 parts or 1 parts) of buffer.

[0036] Preferably, the emulsifiers in the core pre-emulsified liquid, the core pre-emulsified seed emulsion, the shell pre-emulsified liquid and the bottom reaction liquid are independently selected from any one of sodium lauryl sulfate, sodium dodecylbenzenesulfonate, polyoxyethylene octylphenol ether-10, allyloxy fatty alcohol oxyethylene ether ammonium sulfate or disodium nonylphenol polyoxyethylene ether succinate monoester sulfonate or a combination of at least two thereof.

[0037] Preferably, the buffer is sodium bicarbonate, ammonia water, ammonium bicarbonate, or sodium hydroxide.

[0038] Preferably, the initiator solution comprises an initiator and deionized water.

[0039] Preferably, the amount of deionized water in the initiator solution is 1-20 parts relative to 1 part by weight of the initiator, for example, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 13 parts, 15 parts, 18 parts or 20 parts.

[0040] Preferably, the initiator is selected from inorganic peroxide initiators.

[0041] Preferably, the initiator is selected from any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof.

[0042] Preferably, the reaction in step (2) to step (4) is carried out under stirring, and the stirring speed is 100-500r / min (e.g., 100r / min, 150r / min, 200r / min, 250r / min, 300r / min, 350r / min, 400r / min, 450r / min, 500r / min)

[0043] Preferably, before adding the core pre-emulsified seed emulsion in step (2), the bottom reaction liquid is first added to a reactor at 40-75°C (e.g., 40°C, 45°C, 48°C, 50°C, 55°C, 60°C, 65°C, 70°C or 75°C).

[0044] Preferably, the heating in step (2) is to 75-85°C, such as 75°C, 78°C, 80°C, 83°C or 85°C.

[0045] Preferably, the mass of the reaction liquid at the bottom of the kettle in step (2) is 3-85 times that of the seed emulsion pre-emulsified with the core, for example, 3 times, 5 times, 8 times, 10 times, 20 times, 30 times, 40 times, 45 times, 50 times, 60 times, 70 times, 80 times or 85 times.

[0046] Preferably, the amount of the initiator solution added in step (2) is 0.06%-25% by weight of the core pre-emulsified seed emulsion, for example 0.06%, 0.8%, 1%, 3%, 6%, 9%, 12%, 15%, 18%, 21% and 25%.

[0047] Preferably, the reaction time in step (2) is 10-30 min, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 23 min, 25 min, 28 min or 30 min.

[0048] Preferably, the weight ratio of the core pre-emulsion in step (3) to the bottom reaction liquid in step (2) is 1:0.15-1, for example, 1:0.15, 1:0.3, 1:0.5, 1:0.7, 1:0.8 or 1:1.

[0049] Preferably, the amount of the initiator solution added in step (3) is 0.0045%-25% by weight of the core pre-emulsion, for example 0.0045%, 0.2%, 0.5%, 1%, 3%, 6%, 9%, 12%, 15%, 18%, 21% and 25%.

[0050] Preferably, the reaction temperature in step (3) is 75-85°C, such as 75°C, 78°C, 80°C, 83°C or 85°C.

[0051] Preferably, the reaction time in step (3) is 10-30 min, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 23 min, 25 min, 28 min or 30 min.

[0052] Preferably, the weight ratio of the core pre-emulsion in step (3) to the shell pre-emulsion in step (4) is 1:0.25-3, for example, 1:0.25, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:1.5, 1:1.8, 1:2, 1:2.5, 1:2.8 or 1:3.

[0053] Preferably, the amount of the initiator solution added in step (4) is 0.06%-15% by weight of the shell pre-emulsion, for example 0.006%, 0.1%, 0.5%, 1%, 3%, 5%, 8%, 10%, 13% or 15%.

[0054] Preferably, the reaction temperature in step (4) is 80-90°C, such as 80°C, 83°C, 85°C, 88°C or 90°C.

[0055] Preferably, the reaction time of step (4) is 0.5-2.5 h, for example, 0.5 h, 0.8 h, 1 h, 1.5 h, 1.8 h, 2 h, 2.3 h or 2.5 h.

[0056] In the present invention, after the reaction in step (4) is completed, the temperature is lowered to 60-70°C (e.g., 60°C, 63°C, 65°C, 68°C or 70°C), a residual monomer scavenger is added, and then the temperature is lowered to below 50°C (e.g., 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 10°C, etc.), the pH is adjusted to 7-8 (e.g., 7, 7.3, 7.5, 7.8 or 8), and the material is filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0057] Preferably, the residual monomer eliminator is bleaching powder and tert-butyl peroxide.

[0058] Preferably, the reagent used to adjust the pH is any one of ammonia water, lithium hydroxide, lithium carbonate, lithium bicarbonate, sodium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof.

[0059] In the present invention, when the core pre-emulsion and the shell pre-emulsion include the first functional monomer, the reagent used to adjust the pH is any one of ammonia water, lithium hydroxide, lithium carbonate, lithium bicarbonate, sodium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two of them; when the core pre-emulsion and the shell pre-emulsion do not include the first functional monomer, the reagent used to adjust the pH is a lithium-containing pH adjuster selected from any one of lithium hydroxide, lithium carbonate or lithium bicarbonate, or a combination of at least two of them.

[0060] In the present invention, by designing the monomer types and mass ratios in the core and shell pre-emulsions, a core-shell lithium-containing polyacrylic acid aqueous adhesive that is hard inside and soft outside is prepared. By introducing lithium ions, carboxylates, and ester groups into the adhesive, it is given good flexibility, low swelling properties, and good adhesion, reducing the loss of lithium ions during the charge and discharge process, allowing the adhesive to play a greater role in lithium-ion batteries.

[0061] On the other hand, the present invention provides a negative electrode plate for a lithium-ion battery, comprising the core-shell lithium-containing polyacrylic acid aqueous adhesive as described above.

[0062] In another aspect, the present invention provides a lithium-ion battery, comprising the lithium-ion battery negative electrode sheet as described above.

[0063] Compared with the prior art, the present invention has the following beneficial effects:

[0064] The core-shell lithium-containing polyacrylic acid aqueous adhesive provided by the present invention has high bonding strength, good flexibility, and low expansion rate, and can enable the lithium-ion battery using the core-shell lithium-containing polyacrylic acid aqueous adhesive to have high initial charge and discharge efficiency, thereby solving the problems of low bonding, poor flexibility, and low initial efficiency of current adhesives for lithium-ion battery negative electrodes. DETAILED DESCRIPTION

[0065] The technical solution of the present invention is further described below by way of specific embodiments. It should be understood by those skilled in the art that the embodiments are merely to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0066] Example 1

[0067] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0068] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0069] Core pre-emulsion: Dissolve 0.90 parts of disodium nonylphenol sulfonate and 0.76 parts of polyoxyethylene octylphenol ether-10 in 25.5 parts of deionized water. Add 0.64 parts of lithium acrylate and 0.21 parts of lithium methacrylate and disperse until dissolved. Then, add 28.26 parts of ethyl methacrylate, 22.95 parts of butyl acrylate, 3.61 parts of lauric acrylate, 0.85 parts of acrylonitrile, 0.85 parts of acrylamide, 0.64 parts of acrylic acid, 0.22 parts of methacrylic acid, and 0.85 parts of hydroxyethyl methacrylate in this order to emulsify. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0070] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 4.5 parts of deionized water, add 0.11 parts of lithium acrylate and 0.04 parts of lithium methacrylate, and disperse and dissolve. Then, add 4.99 parts of ethyl methacrylate, 4.05 parts of butyl acrylate, 0.64 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.11 parts of acrylic acid, 0.03 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0071] Shell pre-emulsion: Dissolve 1.06 parts of disodium nonylphenol polyoxyethylene ether sulfonate monosodium succinate and 0.89 parts of polyoxyethylene octylphenol ether-10 in 50 parts of deionized water, add 0.75 parts of lithium acrylate and 0.25 parts of lithium methacrylate, and disperse and dissolve. Then, add 40.5 parts of ethyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 0.75 parts of acrylic acid, 0.25 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order, and emulsify to obtain a shell pre-emulsion.

[0072] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0073] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0074] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 15.22 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 88.24 parts of the core pre-emulsion and 1.9 parts of the initiator solution were simultaneously added dropwise. After the addition was complete, the reaction was continued for 15 minutes, and then 134.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the system was kept at 87°C for 1 hour. After the end of the holding period, the system was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then cooled to 45°C. The pH was adjusted to 7.33 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0075] Example 2

[0076] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0077] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0078] Core pre-emulsion: Dissolve 0.90 parts of disodium nonylphenol sulfonate and 0.76 parts of polyoxyethylene octylphenol ether-10 in 25.50 parts of deionized water. Add 0.96 parts of lithium acrylate and 0.32 parts of lithium methacrylate and disperse until dissolved. Then, add 28.26 parts of ethyl methacrylate, 22.95 parts of butyl acrylate, 3.61 parts of lauric acrylate, 0.85 parts of acrylonitrile, 0.85 parts of acrylamide, 0.96 parts of acrylic acid, 0.32 parts of methacrylic acid, and 0.85 parts of hydroxyethyl methacrylate in this order to emulsify. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0079] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 4.5 parts of deionized water, add 0.17 parts of lithium acrylate and 0.06 parts of lithium methacrylate, and disperse and dissolve. Then, add 4.99 parts of ethyl methacrylate, 4.05 parts of butyl acrylate, 0.64 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.17 parts of acrylic acid, 0.06 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0080] Shell pre-emulsion: Dissolve 1.06 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.89 parts of polyoxyethylene octylphenol ether-10 in 50 parts of deionized water, add 1.125 parts of lithium acrylate and 0.375 parts of lithium methacrylate, and disperse and dissolve. Then, add 40.5 parts of ethyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 1.125 parts of acrylic acid, 0.375 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order, and emulsify to obtain a shell pre-emulsion.

[0081] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0082] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0083] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 15.37 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 89.08 parts of the core pre-emulsion and 1.9 parts of the initiator solution were simultaneously added dropwise. After the addition was complete, the reaction was continued for 15 minutes, and then 135.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the system was kept at 87°C for 1 hour. After the end of the holding period, the system was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then cooled to 30°C. The pH was adjusted to 7.67 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0084] Example 3

[0085] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0086] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0087] Core pre-emulsion: Dissolve 0.90 parts of disodium nonylphenol sulfonate and 0.76 parts of polyoxyethylene octylphenol ether-10 in 25.50 parts of deionized water. Add 1.28 parts of lithium acrylate and 0.43 parts of lithium methacrylate and disperse and dissolve. Then, add 28.26 parts of ethyl methacrylate, 22.95 parts of butyl acrylate, 3.61 parts of lauric acrylate, 0.85 parts of acrylonitrile, 0.85 parts of acrylamide, 1.28 parts of acrylic acid, 0.43 parts of methacrylic acid, and 1 part of hydroxyethyl methacrylate in this order to emulsify. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0088] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 4.5 parts of deionized water, add 0.23 parts of lithium acrylate and 0.08 parts of lithium methacrylate, and disperse and dissolve. Then, add 4.99 parts of ethyl methacrylate, 4.05 parts of butyl acrylate, 0.64 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.23 parts of acrylic acid, 0.08 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0089] Shell pre-emulsion: Dissolve 1.06 parts of disodium nonylphenol sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 in 50 parts of deionized water, add 1.5 parts of lithium acrylate and 0.5 parts of lithium methacrylate, and disperse and dissolve. Then, add 40.5 parts of ethyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order, and emulsify to obtain a shell pre-emulsion.

[0090] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0091] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0092] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 15.52 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 89.93 parts of the core pre-emulsion and 1.9 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction lasted for 15 minutes, 136.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the system was kept at 87°C for 1 hour. After the end of the holding period, the system was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then cooled to 25°C. The pH was adjusted to 7.41 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0093] Example 4

[0094] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0095] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0096] Core pre-emulsion: Dissolve 0.90 parts of disodium nonylphenol sulfonate and 0.76 parts of polyoxyethylene octylphenol ether-10 in 25.50 parts of deionized water and disperse until dissolved. Then, add 28.26 parts of ethyl methacrylate, 22.95 parts of butyl acrylate, 3.61 parts of lauric acrylate, 0.85 parts of acrylonitrile, 0.85 parts of acrylamide, 1.28 parts of acrylic acid, 0.43 parts of methacrylic acid, and 0.85 parts of hydroxyethyl methacrylate in this order for emulsification. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0097] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 4.5 parts of deionized water and disperse until dissolved. Then, add 4.99 parts of ethyl methacrylate, 4.05 parts of butyl acrylate, 0.64 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.23 parts of acrylic acid, 0.08 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0098] Shell pre-emulsion: Dissolve 1.06 parts of disodium nonylphenol sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 in 50 parts of deionized water and disperse until dissolved. Then, add 40.5 parts of ethyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order and emulsify to obtain a shell pre-emulsion.

[0099] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0100] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0101] 61.25 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 15.22 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 88.23 parts of the core pre-emulsion and 1.9 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction lasted for 15 minutes, 134.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the system was kept at 87°C for 1 hour. After the end of the holding period, the system was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then cooled to below 50°C. The pH was adjusted to 7.41 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0102] Example 5

[0103] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0104] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0105] Core pre-emulsion: Dissolve 2 parts of sodium dodecylbenzenesulfonate and 2 parts of polyoxyethylene octylphenol ether-10 in 30 parts of deionized water, then add 13 parts of styrene, 17 parts of methyl methacrylate, 15 parts of butyl acrylate, 13 parts of lauric methacrylate, 4 parts of lithium crotonate, 5 parts of acrylamide, 8 parts of acrylic acid, 4 parts of methacrylic acid, and 4 parts of hydroxypropyl methacrylate in sequence for emulsification, add 6 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly;

[0106] Seed emulsion: Dissolve 0.4 parts of sodium dodecylbenzenesulfonate and 0.4 parts of polyoxyethylene octylphenol ether-10 in 7.5 parts of deionized water, and then add 3.25 parts of styrene, 4.25 parts of methyl methacrylate, 3.75 parts of butyl acrylate, 3.25 parts of lauric methacrylate, 0.8 parts of lithium crotonate, 1.25 parts of acrylamide, 2 parts of acrylic acid, 1 part of methacrylic acid, and 1 part of hydroxypropyl methacrylate in this order for emulsification to obtain a seed emulsion;

[0107] Shell pre-emulsion: dissolve 2 parts of sodium dodecylbenzenesulfonate and 2 parts of polyoxyethylene octylphenol ether-10 in 40 parts of deionized water, and then add 10 parts of styrene, 15 parts of methyl methacrylate, 30 parts of butyl acrylate, 20 parts of lauric methacrylate, 2 parts of lithium crotonate, 5 parts of acrylamide, 8 parts of acrylic acid, 4 parts of methacrylic acid, 4 parts of hydroxypropyl methacrylate, 1.5 parts of aziridine, 1 part of silane coupling agent, and 5 parts of divinylbenzene in sequence for emulsification to obtain a shell pre-emulsion;

[0108] A bottom reaction solution was prepared by dissolving 1.5 parts of sodium dodecylbenzenesulfonate and 1.5 parts of polyoxyethylene octylphenol ether-10 in 120 parts of deionized water, followed by adding 0.25 parts of sodium hydroxide to obtain a bottom reaction solution.

[0109] Initiator solution: Add 0.6 parts of ammonium persulfate to 15 parts of deionized water to obtain an initiator aqueous solution.

[0110] 123.25 parts of the bottom reaction liquid were added to a reactor at 75°C at a speed of 250 rpm. 28.85 parts of the seed emulsion were added to the reactor, the temperature was raised to 83°C, 1.4 parts of the initiator solution were added, and after reacting for 25 minutes, 123 parts of the core pre-emulsion and 12 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction was continued for 23 minutes, 149.5 parts of the shell pre-emulsion and 2.2 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the reaction was kept at 88°C for 0.5 hours. After the reaction was completed, the temperature was lowered to 60°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and the temperature was then lowered to 10°C. The pH was adjusted to 7.32 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0111] Example 6

[0112] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0113] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0114] Core pre-emulsion: Dissolve 3 parts of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 25 parts of deionized water, then add 28 parts of styrene, 18 parts of butyl acrylate, 3 parts of isooctyl acrylate, 2 parts of lithium allyl acetate, 5 parts of acrylamide, and 10 parts of hydroxyethyl methacrylate in sequence for emulsification. Add 3 parts of N-hydroxymethyl acrylamide to the core pre-emulsion and emulsify evenly.

[0115] Seed emulsion: Dissolve 0.45 parts of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 4 parts of deionized water, then add 4.2 parts of styrene, 2.7 parts of butyl acrylate, 0.45 parts of isooctyl acrylate, 0.75 parts of acrylamide, 0.3 parts of lithium allyl acetate, 0.3 parts of methacrylic acid, and 1.5 parts of hydroxyethyl methacrylate in this order for emulsification to obtain a seed emulsion;

[0116] Shell pre-emulsion: Dissolve 2.5 parts of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 25 parts of deionized water, then add 25 parts of styrene, 35 parts of butyl acrylate, 8 parts of isooctyl acrylate, 8 parts of lithium allyl acetate, 4 parts of acrylamide, 3 parts of glycidyl methacrylate, and 2 parts of N-hydroxymethyl acrylamide in this order for emulsification to obtain a shell pre-emulsion;

[0117] A bottom reaction solution was prepared by dissolving 1 part of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 90 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0118] Initiator solution: Add 0.6 parts of ammonium persulfate to 10 parts of deionized water to obtain an initiator aqueous solution.

[0119] 91.5 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 300 rpm. 14.35 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 0.742 parts of the initiator solution were added, and after reacting for 15 minutes, 97 parts of the core pre-emulsion and 6 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction was continued for 10 minutes, 112.5 parts of the shell pre-emulsion and 3.858 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the reaction was kept at 87°C for 1 hour. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and the temperature was then lowered to 35°C. The pH was adjusted to 7.24 with lithium carbonate, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0120] Example 7

[0121] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0122] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0123] Core pre-emulsion: Dissolve 2.5 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 20 parts of deionized water, then add 25 parts of methyl methacrylate, 14 parts of isooctyl acrylate, 2 parts of lithium isovalerate, 5 parts of acrylamide, 4 parts of acrylic acid, and 8 parts of hydroxyethyl methacrylate in sequence for emulsification. Add 4 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0124] Seed emulsion: Dissolve 0.45 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 2.5 parts of deionized water, then add 5 parts of methyl methacrylate, 2.8 parts of isooctyl acrylate, 0.4 parts of lithium isovalerate, 1 part of acrylamide, 0.8 parts of acrylic acid, and 1.6 parts of hydroxyethyl methacrylate in this order for emulsification to obtain a seed emulsion;

[0125] Shell pre-emulsion: dissolve 2.5 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 30 parts of deionized water, then add 10 parts of styrene, 30 parts of lauric acid methacrylate, 4 parts of lithium isovalerate, 4 parts of acrylonitrile, 8 parts of methacrylic acid, 2 parts of diacetone acrylamide, and 2 parts of silane coupling agent in sequence for emulsification to obtain a shell pre-emulsion;

[0126] A bottom reaction solution was prepared by dissolving 1 part of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 70 parts of deionized water, followed by adding 1 part of aqueous ammonia to obtain a bottom reaction solution.

[0127] Initiator solution: Add 0.6 parts of ammonium persulfate to 8 parts of deionized water to obtain an initiator aqueous solution.

[0128] 72 parts of the bottom reaction liquid were added to a reactor at 55°C at a speed of 350 rpm. 14.55 parts of the seed emulsion were added to the reactor, the temperature was raised to 82°C, 0.43 parts of the initiator solution were added, and after reacting for 15 minutes, 84.5 parts of the core pre-emulsion and 3 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction was continued for 10 minutes, 92.5 parts of the shell pre-emulsion and 5.17 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the reaction was kept at 86°C for 1.5 hours. After the reaction was completed, the temperature was lowered to 67°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and the temperature was then lowered to 40°C. The pH was adjusted to 7.34 using lithium bicarbonate, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0129] Example 8

[0130] In this embodiment, a method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive is provided, the preparation method comprising the following steps:

[0131] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0132] Core pre-emulsion: Dissolve 2 parts of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 30 parts of deionized water, then add 10 parts of methyl methacrylate, 18 parts of butyl acrylate, 3 parts of lithium 5-hexanoate, 10 parts of acrylonitrile, 5 parts of acrylic acid, and 6 parts of hydroxyethyl methacrylate in sequence for emulsification. Add 3 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0133] Seed emulsion: Dissolve 0.5 parts of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 3 parts of deionized water, then add 1 part of methyl methacrylate, 1.8 parts of butyl acrylate, 0.3 parts of lithium 5-hexanoate, 1 part of acrylonitrile, 0.5 parts of acrylic acid, and 0.6 parts of hydroxyethyl methacrylate in this order for emulsification to obtain a seed emulsion;

[0134] Shell pre-emulsion: dissolve 2 parts of disodium nonylphenol polyoxyethylene ether succinate sulfonate in 35 parts of deionized water, and then add 10 parts of styrene, 30 parts of isooctyl acrylate, 4 parts of lithium 5-hexanoate, 4 parts of acrylamide, 8 parts of methacrylic acid, 2 parts of 4-hydroxybutyl acrylate, and 5 parts of glycidyl methacrylate in this order for emulsification to obtain a shell pre-emulsion;

[0135] A bottom reaction solution was prepared by dissolving 0.5 parts of disodium nonylphenol polyoxyethylene ether sulfonate succinate in 60 parts of deionized water, followed by adding 1 part of aqueous ammonia to obtain a bottom reaction solution.

[0136] Initiator solution: Add 0.6 parts of ammonium persulfate to 9 parts of deionized water to obtain an initiator aqueous solution.

[0137] 61.5 parts of the bottom reaction liquid were added to a reactor at 50°C at a speed of 150 rpm. 8.7 parts of the seed emulsion were added to the reactor, the temperature was raised to 81°C, 0.5 parts of the initiator solution were added, and after reacting for 15 minutes, 129 parts of the core pre-emulsion and 4.5 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction was continued for 10 minutes, 99 parts of the shell pre-emulsion and 4.6 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the reaction was kept at 85°C for 1.2 hours. After the reaction was completed, the temperature was lowered to 67°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and the temperature was then lowered to 30°C. The pH was adjusted to 7.11 using lithium carbonate and lithium bicarbonate, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0138] Comparative Example 1

[0139] In this comparative example, what is different from Example 4 is that the traditional seed emulsion polymerization is not prepared into core-shell emulsion polymerization.

[0140] Preparation of pre-emulsion, seed emulsion, bottom reaction liquid and initiator solution.

[0141] Pre-emulsion: Dissolve 1.96 parts of disodium nonylphenol sulfonate and 1.65 parts of polyoxyethylene octylphenol ether-10 in 75.50 parts of deionized water and disperse until dissolved. Then, add 68.76 parts of ethyl methacrylate, 42.95 parts of butyl acrylate, 18.61 parts of lauric acrylate, 1.85 parts of acrylonitrile, 1.85 parts of acrylamide, 2.78 parts of acrylic acid, 0.93 parts of methacrylic acid, 1.85 parts of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order to emulsify. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0142] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 4.5 parts of deionized water and disperse until dissolved. Then, add 4.99 parts of ethyl methacrylate, 4.05 parts of butyl acrylate, 0.64 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.23 parts of acrylic acid, 0.08 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0143] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0144] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0145] 61.25 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 15.22 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and the reaction was continued for 20 minutes. 222.68 parts of the core pre-emulsion and 3.85 parts of the initiator solution were then added dropwise. After the addition was complete, the temperature was maintained at 87°C for 1 hour. After the temperature was maintained at 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then lowered to below 50°C. The pH was adjusted to 7.40 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0146] Comparative Example 2

[0147] In this comparative example, the difference from Example 4 is that a core-shell emulsion polymerization with a soft inner layer and a hard outer layer is provided.

[0148] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0149] Core pre-emulsion: Dissolve 0.90 parts of disodium nonylphenol sulfonate and 0.76 parts of polyoxyethylene octylphenol ether-10 in 42.5 parts of deionized water and disperse until dissolved. Then, add 34.43 parts of ethyl methacrylate, 17 parts of butyl acrylate, 12.75 parts of lauric acrylate, 0.85 parts of acrylonitrile, 0.85 parts of acrylamide, 1.28 parts of acrylic acid, 0.43 parts of methacrylic acid, and 0.85 parts of hydroxyethyl methacrylate in this order for emulsification. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0150] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 7.5 parts of deionized water and disperse until dissolved. Then, add 6.08 parts of ethyl methacrylate, 3 parts of butyl acrylate, 2.25 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.23 parts of acrylic acid, 0.08 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0151] Shell pre-emulsion: Dissolve 1.06 parts of disodium nonylphenol sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 in 30 parts of deionized water and disperse until dissolved. Then, add 33.25 parts of ethyl methacrylate, 27.00 parts of butyl acrylate, 4.25 parts of lauric acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 1.5 parts of acrylic acid, 0.5 part of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order and emulsify to obtain a shell pre-emulsion.

[0152] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0153] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0154] 61.25 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 19.87 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 114.58 parts of the core pre-emulsion and 1.9 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction lasted for 15 minutes, 103.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the system was kept at 87°C for 1 hour. After the end of the holding period, the system was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then cooled to below 50°C. The pH was adjusted to 7.36 using lithium hydroxide, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0155] Comparative Example 3

[0156] In this comparative example, unlike Example 4, an ammonia-neutralized core-shell emulsion polymerization was provided.

[0157] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, bottom reaction liquid and initiator solution.

[0158] Core pre-emulsion: Dissolve 0.90 parts of disodium nonylphenol sulfonate and 0.76 parts of polyoxyethylene octylphenol ether-10 in 25.50 parts of deionized water and disperse until dissolved. Then, add 28.26 parts of ethyl methacrylate, 22.95 parts of butyl acrylate, 3.61 parts of lauric acrylate, 0.85 parts of acrylonitrile, 0.85 parts of acrylamide, 1.28 parts of acrylic acid, 0.43 parts of methacrylic acid, and 0.85 parts of hydroxyethyl methacrylate in this order for emulsification. Add 2 parts of ethoxylated trimethylolpropane triacrylate to the core pre-emulsion and emulsify evenly.

[0159] Seed emulsion: Dissolve 0.16 parts of disodium nonylphenol sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 in 4.5 parts of deionized water and disperse until dissolved. Then, add 4.99 parts of ethyl methacrylate, 4.05 parts of butyl acrylate, 0.64 parts of lauric acrylate, 0.15 parts of acrylonitrile, 0.15 parts of acrylamide, 0.23 parts of acrylic acid, 0.08 parts of methacrylic acid, and 0.15 parts of hydroxyethyl methacrylate in this order and emulsify to obtain a seed emulsion.

[0160] Shell pre-emulsion: Dissolve 1.06 parts of disodium nonylphenol sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 in 50 parts of deionized water and disperse until dissolved. Then, add 40.5 parts of ethyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate in this order and emulsify to obtain a shell pre-emulsion.

[0161] A bottom reaction solution was prepared by dissolving 0.54 parts of disodium nonylphenol polyoxyethylene ether sulfonate monohydrate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, followed by adding 0.5 parts of sodium bicarbonate to obtain a bottom reaction solution.

[0162] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.

[0163] 61.25 parts of the bottom reaction liquid were added to a reactor at 40°C at a speed of 120 rpm. 15.22 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 88.23 parts of the core pre-emulsion and 1.9 parts of the initiator solution were simultaneously added dropwise. After the addition was complete and the reaction lasted for 15 minutes, 134.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were simultaneously added dropwise to the system. After the addition was complete, the system was kept at 87°C for 1 hour. After the end of the holding period, the system was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and the temperature was then cooled to below 50°C. The pH was adjusted to 7.28 with aqueous ammonia, and the material was filtered to obtain the core-shell lithium-containing polyacrylic acid aqueous adhesive.

[0164] The adhesives obtained in the examples and comparative examples were subjected to performance tests, and the test methods were as follows:

[0165] (1) Take graphite slurry without adding adhesive, then add adhesive in an amount of 2% of the solid component of the graphite slurry to the solid component of the adhesive, stir evenly to obtain a mixed slurry. Take 8g of the mixed slurry, apply it evenly on the copper foil with a 200um thick applicator, and then bake it in a 75℃ oven for 20 minutes to obtain an electrode. Cut the electrode into 30mm wide strips, use 3M tape to stick the strips to the plywood, use a 2kg standard rolling wheel to roll the strips back and forth 3 times to compact them, and then stretch the strips at a stretching speed of 50mm / min to obtain the peel strength;

[0166] (2) After the adhesive solution is dried at 65°C to form a film, 1.5 g of the film sample is cut and immersed in an electrolyte at 65°C for 3 days. The film is weighed and the swelling ratio is calculated as follows: swelling ratio = (weight after swelling - weight before swelling) / weight before swelling × 100%;

[0167] The test results are shown in Table 1.

[0168] Table 1

[0169] As can be seen from Table 1, the present invention prepares a core-shell lithium-containing polyacrylic acid aqueous adhesive by designing the monomer types and mass ratios in the core and shell pre-emulsions. By introducing lithium ions, carboxylates, and ester groups into the adhesive, it has good flexibility, low swelling properties, and good adhesion, thereby reducing the loss of lithium ions during the charge and discharge process.

[0170] The applicant states that while the present invention uses the above-described embodiments to illustrate the core-shell lithium-containing aqueous polyacrylic acid adhesive and its preparation method, the present invention is not limited to these embodiments, nor does it necessarily rely on these embodiments for implementation. Those skilled in the art will appreciate that any improvements to the present invention, equivalent substitutions for raw materials in the present invention, addition of auxiliary components, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present invention.

Claims

1. A core-shell type lithium-containing polyacrylic acid aqueous adhesive, characterized in that: The core-shell type lithium-containing polyacrylic acid aqueous adhesive comprises a core-shell structure polymer and lithium ions, and the polymerization monomers of the core-shell structure polymer comprise a basic monomer, an optional first functional monomer, a second functional monomer and a cross-linking monomer; The basic monomer is selected from any one or a combination of at least two of acrylate monomers, vinyl acetate or styrene; the first functional monomer is selected from any one or a combination of at least two of lithium acrylate, lithium methacrylate, lithium crotonate, lithium allyl acetate, lithium isovalerate, lithium 5-hexanoate, lithium hexadienedioate, lithium 6-heptanoate, lithium isoheptanoate, lithium (E)-2-octenoate or lithium acetylacetonate; the second functional monomer is selected from any one or a combination of at least two of acrylic acid, methacrylic acid, acrylonitrile, 2-hydroxyethyl acrylate, acrylamide, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate, 4-hydroxybutyl acrylate; the crosslinking monomer is selected from any one or a combination of at least two of diacetone acrylamide, N-hydroxymethyl acrylamide, divinylbenzene, aziridine, glycidyl methacrylate, ethoxylated trimethylolpropane triacrylate or silane coupling agent.

2. The core-shell lithium-containing polyacrylic acid aqueous adhesive according to claim 1, characterized in that: The core-shell type lithium-containing polyacrylic acid aqueous adhesive is obtained by emulsion polymerization.

3. The core-shell lithium-containing polyacrylic acid aqueous adhesive according to claim 1 or 2, characterized in that: The lithium ions in the core-shell type lithium-containing polyacrylic acid aqueous adhesive are introduced through the first functional monomer, or through the pH regulator containing lithium in the emulsion polymerization, or can be introduced through the first functional monomer and the pH regulator containing lithium in the emulsion polymerization at the same time; Preferably, the pH regulator containing lithium is selected from any one of lithium hydroxide, lithium carbonate or lithium bicarbonate, or a combination of at least two thereof.

4. The core-shell lithium-containing polyacrylic acid aqueous adhesive according to any one of claims 1 to 3, characterized in that: The polymerized monomers of the core include the following components in parts by weight: 12.5-80 parts of basic monomers, 0.25-55 parts of optional first functional monomers, 0.25-30 parts of second functional monomers and 0.25-15 parts of crosslinking monomers. Preferably, the polymerized monomers of the shell include the following components in percentage by mass: 10-75 parts of basic monomers, 0.25-55 parts of optional first functional monomers, 0.25-30 parts of second functional monomers and 0.1-15 parts of crosslinking monomers.

5. The method for preparing a core-shell lithium-containing polyacrylic acid aqueous adhesive according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) preparing a core pre-emulsified liquid, a core pre-emulsified seed emulsion, a shell pre-emulsified liquid, a kettle bottom reaction liquid and an initiator solution; (2) adding the pre-emulsified seed emulsion to the reaction liquid at the bottom of the kettle, heating it, adding the initiator solution, and reacting; (3) adding the core pre-emulsion and the initiator solution to the reaction solution obtained in step (2) to react; (4) adding the shell pre-emulsion and the initiator solution to the reaction solution obtained in step (3), reacting to obtain the core-shell type lithium-containing polyacrylic acid aqueous adhesive.

6. The preparation method according to claim 5, characterized in that: The core pre-emulsion comprises basic monomers, optional first functional monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water; Preferably, the core pre-emulsion comprises 12.25-65 parts of basic monomers, 0.245-50 parts of optional first functional monomers, 0.245-25 parts of second functional monomers and 0.25-15 parts of cross-linking monomers; Preferably, the amount of the emulsifier in the core pre-emulsion is 0.25%-4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion. Preferably, the amount of deionized water in the core pre-emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion. Preferably, the core pre-emulsified seed emulsion comprises a base monomer, an optional first functional monomer and a second functional monomer; Preferably, the core pre-emulsified seed emulsion comprises 0.05-30 parts of basic monomers, 0.05-25 parts of optional first functional monomers and 0.05-8 parts of second functional monomers; Preferably, the amount of the emulsifier in the core pre-emulsified seed emulsion is 0.005%-4% of the total weight of the basic monomer, the first functional monomer, and the second functional monomer in the seed emulsion; Preferably, the amount of deionized water in the core pre-emulsified seed emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the seed emulsion; Preferably, the shell pre-emulsion comprises a basic monomer, a second functional monomer, a cross-linking monomer, an emulsifier and deionized water; Preferably, the shell pre-emulsion comprises 10-75 parts of basic monomers, 0.2-55 parts of optional first functional monomers, 0.2-30 parts of second functional monomers and 0.1-15 parts of cross-linking monomers; Preferably, the amount of the emulsifier in the shell pre-emulsion is 0.2% to 4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the amount of deionized water in the shell pre-emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the shell pre-emulsion. Preferably, the reaction liquid at the bottom of the kettle comprises an emulsifier, deionized water and a buffer; Preferably, the content of each component in the bottom reaction liquid is 0.1 to 3 parts of emulsifier, 70 to 120 parts of Deionized water, 0.25-1 parts of buffer. Preferably, the emulsifiers in the core pre-emulsified liquid, the core pre-emulsified seed emulsion, the shell pre-emulsified liquid and the bottom reaction liquid are independently selected from any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene octylphenol ether-10, allyloxy fatty alcohol oxyethylene ether ammonium sulfate or disodium succinic acid nonylphenol polyoxyethylene ether monoester sulfonate or a combination of at least two thereof; Preferably, the buffer is sodium bicarbonate, ammonia water, ammonium bicarbonate, or sodium hydroxide; Preferably, the initiator solution comprises an initiator and deionized water; Preferably, the amount of deionized water in the initiator solution is 1-20 parts relative to 1 part by weight of the initiator. Preferably, the initiator is selected from inorganic peroxide initiators; Preferably, the initiator is selected from any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof.

7. The preparation method according to claim 5 or 6, characterized in that: Before adding the pre-emulsified seed emulsion in step (2), the reaction liquid at the bottom of the kettle is first added into the reaction kettle at 40-75°C; Preferably, the temperature in step (2) is increased to 75-85°C; Preferably, the mass of the reaction liquid at the bottom of the kettle in step (2) is 3-85 times that of the seed emulsion pre-emulsified with the core; Preferably, the amount of the initiator solution added in step (2) is 0.06%-25% of the weight of the core pre-emulsified seed emulsion. Preferably, the reaction time in step (2) is 10-30 min; Preferably, the weight ratio of the nuclear pre-emulsion in step (3) to the bottom reaction liquid in step (2) is 0.184-1; Preferably, the amount of the initiator solution added in step (3) is 0.0045%-25% of the weight of the core pre-emulsion. Preferably, the reaction temperature in step (3) is 75-85°C; Preferably, the reaction time in step (3) is 10-30 min; Preferably, the weight ratio of the core pre-emulsion in step (3) to the shell pre-emulsion in step (4) is 1:0.25-3; Preferably, the amount of the initiator solution added in step (4) is 0.06%-15% of the weight of the shell pre-emulsion. Preferably, the reaction temperature in step (4) is 80-90°C; Preferably, the reaction time in step (4) is 0.5-2.5 h.

8. The preparation method according to any one of claims 4 to 7, characterized in that: After the reaction in step (4) is completed, the temperature is lowered to 60-70° C., a residual monomer eliminator is added, and then the temperature is lowered to below 50° C., the pH is adjusted to 7-8, and the material is filtered to obtain the core-shell type lithium-containing polyacrylic acid aqueous adhesive; Preferably, the residual monomer eliminator is bleaching powder and tert-butyl peroxide; Preferably, the reagent used to adjust the pH is any one of ammonia, sodium hydroxide, lithium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof; Preferably, when the core pre-emulsion and the shell pre-emulsion include the first functional monomer, the reagent used to adjust the pH is any one of ammonia water, lithium hydroxide, lithium carbonate, lithium bicarbonate, sodium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two of them; when the core pre-emulsion and the shell pre-emulsion do not include the first functional monomer, the reagent used to adjust the pH is a lithium-containing pH adjuster selected from any one of lithium hydroxide, lithium carbonate or lithium bicarbonate, or a combination of at least two of them.

9. A negative electrode plate for a lithium ion battery, characterized in that: The negative electrode plate of the lithium-ion battery comprises the core-shell lithium-containing polyacrylic acid aqueous adhesive according to any one of claims 1 to 4.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-ion battery negative electrode sheet as claimed in claim 9.

Citation Information

Patent Citations

  • Binder composition for secondary battery

    CN114342124A

  • Core-shell resin material and preparation method thereof, water-based polymer coating, battery diaphragm and secondary battery

    CN114716696A

  • Silicon-based negative electrode binder with three-dimensional network structure, preparation method of silicon-based negative electrode binder, negative electrode plate and battery

    CN115566193A

  • Polymer emulsion for battery diaphragm as well as preparation method and application of polymer emulsion

    CN115806647A

  • Lithium battery ceramic diaphragm binder, preparation method and lithium battery ceramic diaphragm

    CN115810871A

Cited By

  • Large-particle emulsion type binder and preparation method thereof, battery diaphragm and lithium ion battery

    CN119119925A

  • Negative electrode binder, negative electrode plate and electrochemical energy storage device

    CN119307207A

  • High-viscosity SBR (Styrene Butadiene Rubber)-based battery gel for negative electrode of lithium ion battery and preparation method thereof

    CN122011981A