Microsphere surface polymer coating and functionalization method

By mixing the microspheres with Tris-HCl solution and dopamine hydrochloride aqueous solution, a polydopamine layer was formed, and then reacted with anhydrous diethylene glycol dimethyl ether and tetraglycol to obtain a double bonded polyurethane layer, and through an initiator and The functional monomer is further functionalized, solving the problems of high risk and limited applicability of microsphere surface coating and functionalization in the prior art, and achieving a gentle coating and functionalization process.

CN118955954APending Publication Date: 2024-11-15SHENZHEN JIANZHU BIOTECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410989342.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing microsphere surface polymer coating and functionalization methods have problems such as high operational risk, high cost and limited applicability, especially in the field of in vitro diagnosis, especially in the modification of organic polymer microspheres and composite microspheres. During the sexual process.

Method used

A method of coating microspheres surface polymers, including mixing the microspheres with Tris-HCl solution and aqueous dopamine hydrochloride solution, drying with anhydrous diethylene glycol dimethyl ether, tetraethylene glycol and diphenylmethane diisocyanate After mixing, centrifugation, react with hydroxyethyl methacrylate to form a double bonded polyurethane layer, and further reacts through initiator and functional monomer to obtain functional acrylate polymer-coated microspheres.

Benefits of technology

Provides a mild reaction condition, suitable for polymer coating methods for a variety of microsphere materials, avoids the use of hazardous chemical reagents, simplifies the operation process, and realizes the hydrophobic dense polyurethane layer coating and function on the surface of microspheres change.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955954A_ABST
    Figure CN118955954A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of micro-nano materials, and provides a microsphere surface polymer coating and functionalization method which comprises the following steps: mixing microspheres and a Tris-HCl solution, adding a dopamine hydrochloride aqueous solution, mixing, separating, and drying to prepare microspheres coated with a polydopamine layer on the surface; mixing the microspheres of which the surfaces are coated with the polydopamine layers with anhydrous diethylene glycol dimethyl ether, tetraethylene glycol and diphenylmethane diisocyanate to prepare a mixture, mixing the mixture with hydroxyethyl methacrylate, and centrifuging to prepare microspheres of which the surfaces are coated with double-bond polyurethane polymers; and mixing the microspheres coated with the double-bond polyurethane polymer on the surface with an initiator and a functional monomer for reaction to prepare the microspheres coated with the functional acrylate polymer. The microsphere preparation method provided by the invention is mild in reaction condition and relatively short in technological process, and can greatly improve the production quality of the microspheres and reduce the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of micro-nano material technology, and in particular relates to a method for polymer coating and functionalization of microsphere surfaces. Background Art

[0002] Microspheres are widely used as carrier materials or signal emitting materials in in vitro diagnostic reagents and are important raw materials that affect detection sensitivity and accuracy. There are many types of microspheres, including semiconductor nanoparticle microspheres, upconversion nanoparticle microspheres, dye-dyed microspheres, latex microspheres, magnetic microspheres, etc. These different microspheres need to be polymer-coated and functionalized on the surface during in vitro diagnostic applications, and then coupled with biological macromolecules such as antibodies, antigens or nucleic acids. Therefore, establishing an effective and simple surface polymer coating and functionalization method is a key condition for these microsphere materials to be used in diagnostic reagents.

[0003] Surface in-situ polymerization coating is the main method of polymer coating on the surface of microspheres. Surface in-situ polymerization coating refers to the polymerization reaction of polymer monomers on the surface or near the microspheres, and the generated polymer molecular chains are directly covalently bonded to the surface of the microspheres. This coating method requires pre-modification of functional groups on the surface of the microspheres that can trigger or capture polymer molecular chains (i.e., surface modification of the base ball). For example, as described in patent CN 112851866 A, there are residual carbon-carbon double bonds on the surface of the microspheres, and the double bonds are oxidized to epoxy groups and then modified with amino groups, and then the polyurethane molecular chains generated by the polymerization reaction in the solution are captured, thereby coating the surface of the microspheres with a polyurethane layer. Similarly, in patent US6986913B2, the nitro groups of the microspheres are reduced and converted into amino groups by ferrous ions during the magnetization process, and then the epoxy resin or polyurethane generated by polymerization in the solution is covalently bonded through the amino groups. For another example, as described in patent CN 114093586A, a silane coupling agent layer with carbon-carbon double bonds is first coated on the surface of the microspheres, and then polymer molecular chains generated by free radical polymerization in the solution are captured to modify the upper polymer layer.

[0004] The surface modification methods of base balls vary depending on the microsphere matrix materials. In the field of in vitro diagnosis, the modification conditions of the matrix materials of some microspheres are more stringent or involve the use of hazardous chemical reagents, resulting in high modification costs or greater operational risks. For example, the modification of common polystyrene microspheres involves Friedel-Crafts acylation or nitration. The former involves the use of volatile corrosive reagents such as acyl chlorides, anhydrous aluminum chloride, and anhydrous organic reagents, which requires strict protection and produces a large amount of corrosive waste. The latter uses concentrated sulfuric acid and concentrated nitric acid, which are highly dangerous to operate and produce a large amount of waste acid. The use of silane coupling agents is a common surface modification method, but it is generally applied to inorganic oxide surfaces and has limited application in the field of in vitro diagnosis where the base ball contains many organic polymer microspheres or composite microspheres. Therefore, a method for polymer coating and functionalization of microsphere surfaces with high safety, wide applicability, and simple operation is needed. Summary of the invention

[0005] The embodiments of the present application provide a method for polymer coating and functionalization of microsphere surfaces to solve the above problems.

[0006] The technical solutions adopted in this application are as follows:

[0007] A method for coating the surface of microspheres with polymers, comprising the following steps:

[0008] (1) mixing the microspheres with a Tris-HCl solution, adding a dopamine hydrochloride aqueous solution, mixing, separating, and drying to obtain microspheres coated with a polydopamine layer;

[0009] (2) mixing microspheres coated with a polydopamine layer with anhydrous diethylene glycol dimethyl ether, tetraethylene glycol, and diphenylmethane diisocyanate to obtain a mixture, mixing the mixture with hydroxyethyl methacrylate, and centrifuging to obtain microspheres coated with a double-bonded polyurethane polymer;

[0010] (3) The microspheres coated with double-bonded polyurethane polymer are mixed with an initiator and a functional monomer to obtain microspheres coated with a functionalized acrylate polymer.

[0011] Furthermore, in step (1), the mass ratio of the microspheres to the Tris-HCl solution is 1-6 g:950-1050 mL, and the mass ratio of the microspheres to the Tris-HCl solution is 1-6 g:35-45 mL.

[0012] Furthermore, in step (1), the concentration of the Tris-HCl solution is 9.5-10.5 mM, the pH value is 8.3-8.7, and the concentration of the dopamine hydrochloride aqueous solution is 0.1-0.15 g / mL.

[0013] Furthermore, in step (1), the microspheres are mixed with a Tris-HCl solution, an aqueous dopamine hydrochloride solution is added and stirred for 12 to 18 hours, the microspheres are collected by centrifugation or magnetic separation, and the collected microspheres are dried at 35 to 45° C. to obtain microspheres coated with a polydopamine layer.

[0014] Furthermore, in step (2), the ratio of the microspheres coated with the polydopamine layer to anhydrous diethylene glycol dimethyl ether, tetraethylene glycol, and diphenylmethane diisocyanate is 0.9-1.1 g: 130-170 mL: 3.7-3.9 g: 9.5-10.5 g.

[0015] Furthermore, the mass ratio of the hydroxyethyl methacrylate to the microspheres coated with a polydopamine layer is 9.5-10.5:1.

[0016] Furthermore, the functionalized acrylate polymer-coated microspheres are one of carboxyl-functionalized acrylate polymer-coated microspheres, epoxy-functionalized acrylate polymer-coated microspheres, amino-functionalized acrylate polymer-coated microspheres, and hydroxyl-functionalized acrylate polymer-coated microspheres.

[0017] Furthermore, the microspheres are one of polystyrene microspheres, polystyrene-iron oxide composite magnetic microspheres, and iron oxide nanomagnetic microspheres.

[0018] Furthermore, the preparation method of the microspheres coated with the carboxyl functionalized acrylate polymer is as follows: 1.0 g of microspheres coated with a double-bonded polyurethane polymer on the surface is weighed, dispersed into 100 mL of a sodium dodecyl sulfate aqueous solution with a concentration of 0.25% w / v, 100 mg of potassium persulfate, 0.80 mL of ethylene glycol dimethacrylate, and 5.0 mL of methacrylic acid, nitrogen is introduced for deoxygenation, and mechanical stirring is performed at 180 rpm for dispersion, and then the temperature is raised to 70° C. for reaction for 24 hours. After the reaction is completed, the temperature is lowered to room temperature, the microspheres are separated by centrifugation, and then dispersed into purified water, the microspheres are separated by centrifugation again, and the centrifugal washing step is repeated 5 times to obtain microspheres coated with the carboxyl functionalized acrylate polymer.

[0019] Furthermore, the preparation method of the microspheres coated with epoxy functionalized acrylate polymer is as follows: 2.0 g of microspheres coated with double bonded polyurethane polymer on the surface are weighed, dispersed into 200 mL of 0.25% w / v sodium dodecyl sulfate aqueous solution, 200 mg of potassium persulfate, 0.50 mL of ethylene glycol dimethacrylate, and 2.0 mL of glycidyl methacrylate, nitrogen is introduced for deoxygenation, and mechanical stirring is performed at 180 rpm for dispersion, and then the temperature is raised to 70° C. for reaction for 24 hours. After the temperature is lowered to room temperature, the microspheres are separated by centrifugation, and then dispersed into purified water, and the microspheres are washed by centrifugation for 5 times to obtain microspheres coated with epoxy functionalized acrylate polymer.

[0020] Furthermore, the preparation method of the amino-functionalized acrylate polymer-coated microspheres is as follows: 1.0 g of epoxy-functionalized acrylate polymer-coated microspheres are weighed, dispersed into 50 mL of N,N-dimethylformamide after centrifugation, 200 mg of ethylenediamine is added, nitrogen is introduced after stirring, and the temperature is raised to 60° C. for reaction for 6 hours. After the temperature drops to room temperature, the microspheres are centrifuged, then dispersed into ethanol, and the microspheres are centrifuged again, and this step is repeated 5 times to obtain amino-functionalized acrylate polymer-coated microspheres.

[0021] Furthermore, the preparation method of the microspheres coated with the hydroxyl-functionalized acrylate polymer is as follows: 1.0 g of microspheres coated with a double-bonded polyurethane polymer on the surface is weighed, dispersed into 100 mL of a 0.25% w / v sodium dodecyl sulfate aqueous solution, 100 mg of potassium persulfate, 0.50 mL of ethylene glycol dimethacrylate, and 3.0 mL of hydroxyethyl methacrylate, nitrogen is introduced for deoxygenation, and mechanical stirring is performed at 180 rpm for dispersion, and then the temperature is raised to 70° C. for reaction for 18 hours. After the reaction is completed, the temperature is lowered to room temperature, the microspheres are separated by centrifugation, and then the microspheres are washed by centrifugation for 5 times to obtain microspheres coated with the hydroxyl-functionalized acrylate polymer.

[0022] The beneficial effects of the embodiments of the present application compared with the prior art are:

[0023] The present application provides a polymer coating method with mild reaction conditions and applicable to most microsphere material matrices. The polydopamine layer can be coated on the surface of microsphere materials including organic polymer microspheres, inorganic material microspheres, composite material microspheres, etc. at room temperature and with water as a solvent, providing a non-covalent activation layer, which allows the surfaces of these different materials to continue to be coated with a hydrophobic and dense polyurethane layer, and by functionalizing the polyurethane layer with double bonds, the polyurethane layer can continue to be grafted with different chemically active functional groups through conventional free radical polymerization reactions. The overall reaction conditions of the process are mild, and there is no need to use highly dangerous chemical reagents or reaction conditions, and the process is simple and easy. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Example 1 is an electron microscope image of microspheres coated with double-bonded polyurethane polymers, which are prepared using polystyrene microspheres as raw materials. The left side is the polystyrene microspheres before polyurethane coating, and the right side is the polystyrene microspheres after polyurethane coating.

[0025] Figure 2 Example 2 is an electron microscope image of microspheres coated with double-bonded polyurethane polymer on the surface, which are prepared using polystyrene-iron oxide composite magnetic microspheres as raw materials. The left side is the polystyrene-iron oxide composite magnetic microspheres before polyurethane coating, and the right side is the polystyrene-iron oxide composite magnetic microspheres after polyurethane coating.

[0026] Figure 3 Example 3 is an electron microscope image of microspheres coated with double-bonded polyurethane polymers, which are prepared using iron oxide nanospheres as raw materials. The left side is the iron oxide nanospheres before polyurethane coating, and the right side is the iron oxide nanospheres after polyurethane coating. DETAILED DESCRIPTION

[0027] It should be understood that the present application is not limited to the specific compositions, methods or schemes described herein. In addition, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present application belongs. It should also be understood that the terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the scope of the present application, which is limited only by the claims. The test methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can all be obtained from commercial sources.

[0028] The room temperature in this application is 25-35°C.

[0029] Determination method of functional groups of functionalized polymer layer on microsphere surface

[0030] The carboxyl content on the surface of functionalized microspheres was determined by conductivity titration. The specific steps are:

[0031] Take 10mg of carboxyl microspheres in a 200mL beaker, add 100g of purified water, and insert the conductivity meter electrode. Take 0.1mL of 0.15M hydrochloric acid solution and add it to the reaction solution, and record the initial conductivity. Add 100μL of 0.01M NaOH solution every 1min, record the corresponding conductivity value, and stop the titration after recording about 30 points. Perform data fitting processing, and calculate the content of carboxyl groups on the surface of the microspheres based on the volume of NaOH solution consumed.

[0032] The functional group determination of epoxy microspheres, amino microspheres and hydroxyl microspheres is to convert the corresponding groups into carboxyl groups through chemical reactions, and then convert the carboxyl content into the content of the corresponding groups after determining it through the above-mentioned conductivity titration.

[0033] The method for converting amino microspheres and hydroxyl microspheres into carboxyl microspheres is as follows: 1.0 g of microspheres are dispersed in 50 mL of N, N-dimethylformamide, 1.0 g of succinic anhydride and 0.5 mL of triethylamine are added, and the reaction is carried out at 60°C for 20 hours. The microspheres are separated by centrifugation (4000 rpm, 10 minutes), and then dispersed into 20 mL of N, N-dimethylformamide, and the centrifugation-dispersion washing step is repeated 5 times, and then N, N-dimethylformamide is replaced with ethanol and then centrifuged-dispersion washed 3 times, and finally the microspheres are placed in a 40°C oven for drying for 48 hours. To convert epoxy microspheres into carboxyl microspheres, mercaptopropionic acid is used to replace the above succinic anhydride, and the other conditions and processes are the same.

[0034] Example 1: Polystyrene microspheres coated with a polydopamine layer and a polyurethane layer

[0035] (1) Take polystyrene microspheres (average particle size of 2 microns, 40 mL, containing 1.2 g of microspheres), disperse them into 1000 mL of Tris-HCl solution (pH 8.5, 10 mM), add 40 mL of dopamine hydrochloride aqueous solution (containing 5.0 g of dopamine hydrochloride), and react at room temperature (25-35° C.) with mechanical stirring (100-500 rpm) for 18 hours. Then centrifuge to separate the microspheres (4000 rpm, 10 minutes) and remove the aqueous solution. Add 100 mL of anhydrous ethanol to the separated microspheres for ultrasonic dispersion (240 W, 40 Hz, 10 minutes), and then centrifuge to separate the microspheres (4000 rpm, 10 minutes). Repeat the ethanol ultrasonic dispersion-centrifugation step 5 times, and finally place the microspheres in a 40° C. vacuum drying oven to dry until the microspheres become solid powder.

[0036] (2) Take 1.0 g of solid powder, disperse it into 150 mL of anhydrous diethylene glycol dimethyl ether, add 3.88 g of tetraethylene glycol and 10.0 g of diphenylmethane diisocyanate, stir and mix at room temperature, then heat to 80°C for reaction for 18 hours, then cool to room temperature, add 10.0 g of hydroxyethyl methacrylate and stir at room temperature for 30 minutes, then heat to 60°C for reaction for 5 hours. After the temperature drops to room temperature, add 150 mL of N,N-dimethylformamide to dilute and reduce the viscosity, centrifuge to separate microspheres, then use 50 mL of N,N-dimethylformamide for ultrasonic dispersion (240 W, 40 Hz, 10 minutes), centrifuge (4000 rpm, 10 minutes), repeat the ultrasonic dispersion-centrifuge washing steps 5 times, and obtain microspheres coated with double-bonded polyurethane polymer on the surface.

[0037] See also Figure 1 , the surface of the microspheres coated with double-bonded polyurethane polymer was scanned by electron microscope, and the surface of the polystyrene microspheres was coated with a layer of polyurethane.

[0038] Example 2 Polystyrene-iron oxide composite magnetic microspheres coated with polydopamine layer and polyurethane layer

[0039] The synthesis of polystyrene-iron oxide composite magnetic microspheres refers to the method in patent CN 114093586 A. Sulfonated porous polystyrene microspheres are formed by a coprecipitation reaction of ferric chloride / ferrous chloride in an alkaline solution.

[0040] Take 5.0g of composite magnetic microspheres, disperse them into 1000mL of Tris-HCl solution (pH 8.5, 10mM), add 40mL of dopamine hydrochloride aqueous solution (containing 5.0g of dopamine hydrochloride), and react for 18 hours at room temperature using 300rpm mechanical stirring. Then, separate the microspheres magnetically and remove the aqueous solution. Add 100mL of anhydrous ethanol to disperse the separated microspheres, separate the microspheres again, repeat this step 5 times, and finally dry the microspheres in a 40°C vacuum drying oven until the microspheres become solid powder.

[0041] Take 1.0g of the above microsphere powder, disperse it into 150mL of anhydrous diethylene glycol dimethyl ether, add 3.88g of tetraethylene glycol and 10.0g of diphenylmethane diisocyanate, stir and mix at room temperature, heat to 80°C and react for 16 hours, then reduce the temperature to 60°C, add 10.0g of hydroxyethyl methacrylate and continue to react for 5 hours. After the temperature drops to room temperature, add 150mL of N,N-dimethylformamide to dilute, separate the microspheres magnetically, and then use 50mL of N,N-dimethylformamide for ultrasonic dispersion and magnetic separation of the microspheres. Repeat the ultrasonic dispersion-magnetic separation and cleaning steps 5 times to obtain microspheres coated with double-bonded polyurethane polymer on the surface.

[0042] See also Figure 2 The surface of the microspheres coated with double-bonded polyurethane polymer was detected by electron microscope. The surface of the polystyrene-iron oxide composite magnetic microspheres was coated with a layer of polyurethane.

[0043] Example 3: Iron oxide nano-magnetic microspheres coated with polydopamine layer and polyurethane layer

[0044] Iron oxide nano-magnetic microspheres were synthesized by solvothermal method. The specific process is as follows: 1.08g of ferric chloride hexahydrate, 1.0g of trisodium citrate dihydrate, 1.20g of anhydrous sodium acetate, and 20mL of ethylene glycol were added to a 100mL hydrothermal kettle, stirred for 1 hour, moved into an oven, heated to 200°C and reacted for 10 hours. After cooling to room temperature, the black solid obtained by magnetic separation was washed with water 5 times to obtain iron oxide nano-magnetic microspheres with an average particle size of 300 nanometers.

[0045] Take 3.0g of iron oxide nanomagnetic microspheres, disperse them into 500mL of Tris-HCl solution (pH 8.5, 10mM), add 40mL of dopamine hydrochloride aqueous solution (containing 5.0g of dopamine hydrochloride), and react for 18 hours at room temperature with 300rpm mechanical stirring. Then separate the microspheres by magnetic separation, add 100mL of anhydrous ethanol to disperse, separate the microspheres by magnetic separation again, repeat this step 5 times, and finally dry the solid in a vacuum drying oven at 40℃.

[0046] Take 1.0g of the dried microspheres, disperse them into 150mL of anhydrous diethylene glycol dimethyl ether, add 3.88g of tetraethylene glycol and 10.0g of diphenylmethane diisocyanate, stir and mix at room temperature, heat to 80°C and react for 16 hours, then lower the temperature to 50°C, add 10.0g of hydroxyethyl methacrylate and continue to react for 8 hours. After the temperature drops to room temperature, add 150mL of N,N-dimethylformamide to dilute, separate the microspheres magnetically, and then use 50mL of N,N-dimethylformamide for ultrasonic dispersion (240W, 40Hz, 10 minutes), separate the microspheres magnetically, repeat the ultrasonic dispersion-magnetic separation and cleaning steps 5 times, and obtain microspheres with double bond-modified polyurethane polymers coated on the surface.

[0047] See also Figure 3 The microspheres coated with double-bonded polyurethane polymer were detected using electron microscope images, and the surface of the iron oxide nano-microspheres was coated with a layer of polyurethane.

[0048] In Examples 1-3, polystyrene microspheres, polystyrene-iron oxide composite magnetic microspheres, and iron oxide nanomagnetic microspheres were used as raw materials to prepare microspheres coated with double-bonded polyurethane polymers, and the polyurethane layer was successfully coated on the surface of the microspheres.

[0049] Example 4: Carboxyl functional polymer layer coated on the polyurethane layer on the surface of polystyrene microspheres

[0050] 1.0 g of the microspheres coated with double-bonded polyurethane polymer prepared in Example 1 were dispersed into 100 mL of sodium dodecyl sulfate aqueous solution with a concentration of 0.25% w / v, 100 mg of potassium persulfate, 0.80 mL of ethylene glycol dimethacrylate, and 5.0 mL of methacrylic acid, nitrogen was introduced for deoxygenation, and mechanical stirring was performed at 180 rpm for dispersion, and then the temperature was raised to 70° C. for reaction for 24 hours. After the reaction was completed, the temperature was lowered to room temperature, and the microspheres were separated by centrifugation (4000 rpm, 10 minutes), and then dispersed into 100 mL of purified water, and the microspheres were separated by centrifugation again (4000 rpm, 10 minutes), and the centrifugation-water washing step was repeated 5 times to obtain microspheres coated with carboxyl functionalized acrylate polymer.

[0051] The carboxyl content of the microspheres coated with carboxyl functionalized acrylate polymer was determined by conductometric titration, and the group content in the microspheres was 463 μmol / g.

[0052] Example 5: Polyurethane layer on the surface of polystyrene microspheres coated with epoxy functional polymer layer

[0053] Take 2.0 g of the microspheres coated with double-bonded polyurethane polymer prepared in Example 1, disperse them into 200 mL of 0.25% w / v sodium dodecyl sulfate aqueous solution, add 200 mg of potassium persulfate, 0.50 mL of ethylene glycol dimethacrylate, and 2.0 mL of glycidyl methacrylate, pass nitrogen to deoxygenate and disperse with mechanical stirring at 180 rpm, then heat to 70°C and react for 24 hours. After the temperature drops to room temperature, centrifuge (4000 rpm, 10 minutes) to obtain microspheres, which are then dispersed into 100 mL of purified water, and the centrifugation-water washing of the microspheres is repeated 5 times to obtain microspheres coated with epoxy functionalized acrylate polymer.

[0054] The carboxyl content of the epoxy-functionalized acrylate polymer coated microspheres was determined by conductometric titration, and the group content in the microspheres was 381 μmol / g.

[0055] Example 6: Polyurethane layer on the surface of polystyrene microspheres coated with amino functional polymer layer

[0056] Take 1.0 g of the epoxy functional polymer layer coated microspheres obtained in Example 5, centrifuge (4000 rpm, 10 minutes), disperse into 50 mL of N, N-dimethylformamide, add 200 mg of ethylenediamine, stir evenly, introduce nitrogen, heat to 60°C and react for 6 hours. After the temperature drops to room temperature, centrifuge (4000 rpm, 10 minutes) the microspheres, then disperse into 100 mL of ethanol, centrifuge the microspheres again, repeat this step 5 times, and obtain amino functional acrylate polymer coated microspheres.

[0057] The carboxyl content of the amino-functionalized acrylate polymer coated microspheres was determined by conductometric titration, and the group content in the microspheres was 422 μmol / g.

[0058] Example 7: Hydroxyl functional polymer layer coated on the polyurethane layer on the surface of polystyrene microspheres

[0059] Take 1.0 g of the microspheres coated with double-bonded polyurethane polymer prepared in Example 1, disperse them into 100 mL of 0.25% w / v sodium dodecyl sulfate aqueous solution, add 100 mg of potassium persulfate, 0.50 mL of ethylene glycol dimethacrylate, and 3.0 mL of hydroxyethyl methacrylate, introduce nitrogen to deoxygenate, and disperse them with mechanical stirring at 180 rpm, then heat to 70° C. and react for 18 hours. After the reaction is completed, cool to room temperature, centrifuge (4000 rpm, 10 minutes) to separate the microspheres, and then disperse them into 100 mL of pure water, repeat the centrifugal washing step 5 times, and obtain microspheres coated with hydroxyl functionalized acrylate polymer.

[0060] The carboxyl content of the microspheres coated with hydroxyl-functionalized acrylate polymer was determined by conductometric titration, and the group content in the microspheres was 438 μmol / g.

[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for coating the surface of microspheres with polymers, characterized in that: The following steps are involved: (1) mixing the microspheres with a Tris-HCl solution, adding a dopamine hydrochloride aqueous solution, mixing, separating, and drying to obtain microspheres coated with a polydopamine layer; (2) mixing microspheres coated with a polydopamine layer with anhydrous diethylene glycol dimethyl ether, tetraethylene glycol, and diphenylmethane diisocyanate to obtain a mixture, mixing the mixture with hydroxyethyl methacrylate, and centrifuging to obtain microspheres coated with a double-bonded polyurethane polymer; (3) The microspheres coated with double-bonded polyurethane polymer are mixed with an initiator and a functional monomer to obtain microspheres coated with a functionalized acrylate polymer.

2. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: In step (1), the mass ratio of the microspheres to the Tris-HCl solution is 1-6 g:950-1050 mL, and the mass ratio of the microspheres to the Tris-HCl solution is 1-6 g:35-45 mL.

3. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: In step (1), the concentration of the Tris-HCl solution is 9.5-10.5 mM, the pH value is 8.3-8.7, and the concentration of the dopamine hydrochloride aqueous solution is 0.1-0.15 g / mL.

4. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: In step (1), the microspheres are mixed with a Tris-HCl solution, an aqueous dopamine hydrochloride solution is added and stirred for 12 to 18 hours, the microspheres are collected by centrifugation or magnetic separation, and the collected microspheres are dried at 35 to 45° C. to obtain microspheres coated with a polydopamine layer.

5. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: In step (2), the ratio of the microspheres coated with the polydopamine layer to anhydrous diethylene glycol dimethyl ether, tetraethylene glycol, and diphenylmethane diisocyanate is 0.9-1.1 g: 130-170 mL: 3.7-3.9 g: 9.5-10.5 g.

6. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: The mass ratio of the hydroxyethyl methacrylate to the microspheres coated with a polydopamine layer is 9.5-10.5:

1.

7. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: The functionalized acrylate polymer-coated microspheres are one of carboxyl-functionalized acrylate polymer-coated microspheres, epoxy-functionalized acrylate polymer-coated microspheres, amino-functionalized acrylate polymer-coated microspheres, and hydroxyl-functionalized acrylate polymer-coated microspheres.

8. The method for coating the surface of microspheres with polymers according to claim 1, characterized in that: The microsphere is one of polystyrene microspheres, polystyrene-iron oxide composite magnetic microspheres and iron oxide nano magnetic microspheres.

Citation Information

Cited By

  • High-loading porous hollow magnetic microsphere as well as preparation method and application thereof

    CN119391045A

  • Self-antifouling super-hydrophilic immunomagnetic microsphere and application thereof

    CN120479321A

  • Self-antifouling super-hydrophilic immunomagnetic microspheres and application thereof

    CN120479321B