Method for synthesizing cerium oxide composite abrasive and chemical mechanical polishing solution
Synthesis of spherical cerium oxide composite abrasive by hydrothermal method of modifying metal salt and solid acid, the problem of poor dispersion of cerium oxide particles in the prior art is solved, efficient polishing effect and particle size uniformity are achieved, and polishing rate is improved. and surface flatness.
Patent Information
- Application Number
- CN202410901102.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-05
AI Technical Summary
It is difficult to synthesize spherical ceria composite abrasives with uniform particle size and good dispersion in the prior art, resulting in increased wafer surface roughness and unstable polishing efficiency during polishing.
The cerium oxide precursor is synthesized by hydrothermal method of modifying metal salts and solid acids, controlling the pH value and molar ratio, forming a spherical cerium oxide composite abrasive, combining organic acids, organic alkalis and surfactants to achieve good dispersible oxidation with good dispersion Synthesis of cerium particles.
Cerium oxide particles with good morphology and narrow particle size distribution were obtained, which significantly improved the dispersion and polishing rate of the polishing liquid, and was suitable for industrial-scale applications.
Smart Images

Figure CN118995136A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical mechanical polishing, and in particular to a method for producing a cerium oxide composite abrasive and a cerium dioxide polishing liquid. Background Art
[0002] Integrated circuits are one of the main high-tech technologies that promote the development of social economy and informatization. As the integration level increases, the feature size decreases, resulting in a three-dimensional structure and multi-layer wiring, which requires the surface between the layers inside the integrated circuit to have a very high flatness. Chemical mechanical polishing (CMP) is currently the last process to obtain an ultra-smooth, damage-free surface, and is a crucial step in semiconductor manufacturing technology.
[0003] Polishing liquid plays a decisive role in chemical mechanical polishing technology. The components of the polishing liquid include chemical reagents that play a role in corroding and softening the polishing body, and abrasives that can play a mechanical role. Nano-cerium oxide can be used as an excellent abrasive due to its advantages such as strong cutting ability, good chemical stability, and fast polishing speed. It is widely used in the field of chemical mechanical polishing, especially in the formation of shallow trench isolation (STI) and the flattening of dielectric layers and insulating layers. On the other hand, due to the large specific surface area, large number of surface atoms, and high surface energy of nano-cerium oxide particles, it is difficult to disperse in aqueous media, and the particles are prone to agglomeration and sedimentation. During polishing, it will lead to problems such as increased wafer surface roughness, increased scratches, and unstable polishing efficiency. Therefore, how to synthesize spherical cerium oxide with uniform particle size, good dispersibility, and stable suspension in solution is a very important research topic.
[0004] Patent CN116409809A discloses a method for synthesizing cerium oxide and a chemical mechanical polishing liquid. Cerium oxide is synthesized by controlling the ratio of cerium salt to precipitant, as well as the synthesis temperature and time. However, the morphology of the synthesized cerium oxide is not indicated. If it is not spherical cerium oxide, the surface roughness of the wafer may increase during polishing. Patent CN114790367A discloses a nano-spherical cerium oxide polishing liquid and application for single crystal silicon and polycrystalline silicon, but the morphology of cerium oxide is poor, which is not conducive to obtaining better surface roughness. Patent CN202311657264X and Patent CN2021115 76349.6 discloses a method for preparing a cerium oxide polishing liquid. When dispersing cerium oxide, the cerium oxide must first be ball-milled to activate the cerium oxide powder to enhance its dispersibility, and then ultrasonic dispersion is performed. This method involves more equipment and complicated steps, and is not suitable for large-scale industrial applications; Patent CN20221103707.3 discloses an octahedral cerium oxide abrasive polishing liquid and its preparation method and application. The patent synthesizes cerium oxide by controlling the molar ratio of cerium nitrate hexahydrate to polyvinyl pyrrolidone and the content of anhydrous ethanol in the solvent, but the cerium oxide morphology is octahedral, and a low roughness surface is not obtained during polishing. Summary of the invention
[0005] The technical problem to be solved by the present invention is: to provide a method for preparing a cerium oxide composite abrasive and a cerium dioxide polishing liquid. First, a metal salt is modified, a solid acid and a metal salt are dissolved in deionized water, the pH value of the solution is adjusted, and the obtained precipitate is aged, washed, dried and high-temperature roasted to obtain a modified metal salt powder; then, a cerium salt and the modified metal salt powder are dissolved in deionized water in a certain proportion, an organic acid, an organic base and a surfactant are added, and a modified cerium oxide precursor is synthesized by a hydrothermal method, and after washing, drying and calcining, a spherical cerium oxide composite abrasive modified by a solid acid can be obtained. The synthesized composite cerium oxide has the advantages of good dispersibility and high hardness.
[0006] Specifically, the present invention provides a method for synthesizing composite cerium oxide, comprising: (1) Modifying the metal salt: dissolving a certain amount of solid acid and metal salt in a certain amount of deionized water, adjusting the pH value of the solution to between 9 and 11, aging, washing, drying and high-temperature calcining the resulting precipitate to obtain a modified metal salt powder; (2) Synthesis of grinding cerium oxide: Cerium salt and modified metal salt powder are dissolved in deionized water in a certain proportion, and organic acid, organic base and surfactant are added in a certain proportion. The reaction is carried out at 100-120°C for 2-4 hours. The obtained precipitate is washed, dried and calcined to obtain a spherical cerium oxide composite abrasive modified with a solid acid.
[0007] Preferably, the solid acid in step (1) is selected from one or more of sulfuric acid, phosphoric acid, silicotungstic acid, boric acid and iodic acid.
[0008] Preferably, the metal salt in step (1) is one or more of lanthanum chloride, calcium chloride, erbium chloride, zirconium chloride, ferric sulfate, aluminum sulfate, zirconium sulfate, calcium sulfate, ferric nitrate, aluminum nitrate, europium nitrate and zirconium nitrate.
[0009] Preferably, the molar ratio of the solid acid to the metal salt in step (1) is controlled between 1:1 and 20:1.
[0010] More preferably, the molar ratio of the solid acid to the metal salt in step (1) is controlled between 5:1 and 15:1.
[0011] Preferably, the precipitation aging temperature in step (1) is 80°C for 3-5 hours, and after cleaning, it is dried at 100°C for 24 hours.
[0012] Preferably, the calcination temperature in step (1) is 300-600° C. and the calcination time is 3-6 hours.
[0013] Preferably, the cerium salt in step (2) is selected from one or more of cerium nitrate, cerium sulfate, cerium chloride and cerium nitrate amine.
[0014] Preferably, the organic acid in step (2) is selected from one or more of tartaric acid, citric acid, malonic acid, succinic acid, oxalic acid, salicylic acid, benzoic acid, malic acid, diethylenetriaminepentaacetic acid and ascorbic acid.
[0015] Preferably, the organic base in step (2) is selected from one or more of ethylenediamine, piperazine, monoethanolamine, triethanolamine, isopropanolamine, tetramethylammonium hydroxide and imidazole.
[0016] Preferably, the surfactant in step (2) is selected from one or more of polyvinyl pyrrolidone, polyacrylic acid, sodium polyacrylate, fatty alcohol polyoxyethylene ether AEO-9, polymethacrylic acid, Tween-20, Tween-80, alkylphenol polyoxyethylene ether, dodecyltrimethylammonium bromide and hexadecyltrimethylammonium bromide.
[0017] Preferably, the molar ratio of the cerium salt to the modified metal salt powder in step (2) is between 20:1 and 5:1.
[0018] More preferably, the molar ratio of the cerium salt to the modified metal salt powder in step (2) is between 20:1 and 10:1.
[0019] Preferably, the molar ratio of the organic acid: organic base: surfactant: cerium salt in step (2) is controlled between 0-0.5: 0-5: 0-1: 0-5.
[0020] More preferably, the molar ratio of the organic acid: organic base: surfactant: cerium salt in step (2) is controlled within the range of 0.1-0.3: 0.5-2: 0.1-1: 0.5-3.
[0021] Preferably, the calcination temperature in step (2) is controlled between 300-500° C., and the calcination time is controlled between 1-4 h.
[0022] Another aspect of the present invention provides cerium oxide, which is prepared using any of the above methods for synthesizing composite cerium oxide.
[0023] Another aspect of the present invention provides a chemical mechanical polishing solution, comprising the cerium oxide as described above.
[0024] The composite cerium oxide synthesized by the present invention adopts a hydrothermal synthesis method, and the reaction conditions are mild and controllable. The composite cerium oxide particles finally obtained have good morphology, narrow particle size distribution, good dispersibility, are easy to disperse into a cerium oxide polishing liquid with a particle size of 100-350nm, and have a high polishing rate, and have a wide range of promotion and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the particle size distribution diagram of the product obtained in Example 1.
[0026] Figure 2 This is the particle size distribution diagram of the product obtained in Example 2.
[0027] Figure 3 This is the particle size distribution diagram of the product obtained in Example 3.
[0028] Figure 4 This is the particle size distribution diagram of the product obtained in Example 4.
[0029] Figure 5 This is the particle size distribution diagram of the product obtained in Example 5.
[0030] Figure 6 This is the particle size distribution diagram of the product obtained in Example 6.
[0031] Figure 7 This is the particle size distribution diagram of the product obtained in Example 7.
[0032] Figure 8 This is the particle size distribution diagram of the product obtained in Example 8.
[0033] Fig. 9 This is the particle size distribution diagram of the product obtained in Comparative Example 1.
[0034] Fig.10 This is the particle size distribution diagram of the product obtained in Comparative Example 2. DETAILED DESCRIPTION
[0035] The advantages of the present invention are further illustrated below in conjunction with specific embodiments. Figure 1 shown.
[0036] Example 1 At room temperature, 85% solid phosphoric acid and zirconium chloride were dissolved in 200 mL of deionized water at a ratio of 8:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain zirconium phosphate powder.
[0037] Then, cerium nitrate and zirconium phosphate were dissolved in deionized water, the solubility of cerium sulfate was controlled to be 3.5 g / L, cerium sulfate: zirconium phosphate = 10:1, malonic acid, monoethanolamine and dodecyl trimethyl ammonium bromide were added in sequence after dissolution, malonic acid: monoethanolamine: dodecyl trimethyl ammonium bromide: cerium sulfate = 0.25:1:0.25:0.5, and the reaction was carried out at 120°C for 4 hours. Then, the solid was washed with deionized water and anhydrous ethanol, dried at 80°C for 12 hours, and then calcined at 500°C for 3 hours to obtain the modified composite cerium oxide.
[0038] Example 2 At room temperature, 85% solid phosphoric acid and lanthanum chloride were dissolved in 200 mL of deionized water at a ratio of 8:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain lanthanum phosphate powder.
[0039] Then, cerium nitrate and lanthanum phosphate are dissolved in deionized water, the solubility of cerium nitrate is controlled to be 2g / L, cerium nitrate: lanthanum phosphate = 12:1, malonic acid, monoethanolamine and dodecyl trimethyl ammonium bromide are added in sequence after dissolution, malonic acid: monoethanolamine: dodecyl trimethyl ammonium bromide: cerium nitrate = 0.25:1:0.25:0.5, and react at 120°C for 4h. Then, the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0040] Example 3 At room temperature, silicic acid and zirconium chloride were dissolved in 200 mL of deionized water at a ratio of 10:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain zirconium silicate powder.
[0041] Then, cerium chloride and zirconium silicate are dissolved in deionized water, the solubility of cerium nitrate is controlled to be 2g / L, cerium chloride: zirconium silicate = 15:1, ascorbic acid, triethanolamine and Tween-20 are added in sequence after dissolution, ascorbic acid: triethanolamine: Tween-20: cerium chloride = 0.3: 0.5: 0.25: 0.75, and the reaction is carried out at 120°C for 4h. Then, the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0042] Example 4 At room temperature, silicic acid and europium chloride were dissolved in 200 mL of deionized water at a ratio of 10:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain europium silicate powder.
[0043] Then, cerium nitrate and europium silicate were dissolved in deionized water, the solubility of cerium nitrate was controlled to be 5.5g / L, cerium nitrate: europium silicate = 12:1, malic acid, isopropanolamine and polyvinyl pyrrolidone were added in sequence after dissolution, malic acid: isopropanolamine: polyvinyl pyrrolidone: cerium nitrate = 0.25: 0.8: 0.1: 0.5, and the reaction was carried out at 120°C for 4h. Then, the solid was washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0044] Example 5 At room temperature, iodic acid and erbium chloride were dissolved in 200 mL of deionized water in a ratio of 8:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain erbium iodate powder.
[0045] Then, cerium nitrate and erbium iodate are dissolved in deionized water, the solubility of cerium nitrate is controlled to be 2g / L, cerium nitrate: erbium iodate = 16:1, malonic acid, monoethanolamine and dodecyl trimethyl ammonium bromide are added in sequence after dissolution, malonic acid: monoethanolamine: dodecyl trimethyl ammonium bromide: cerium nitrate = 0.25:1:0.25:0.5, and react at 120°C for 4h. Then, the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0046] Example 6 At room temperature, solid sulfuric acid and zirconium nitrate were dissolved in 200 mL of deionized water at a ratio of 8:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain zirconium sulfate powder.
[0047] Then, cerium nitrate and zirconium sulfate were dissolved in deionized water, the solubility of cerium nitrate was controlled to be 5.5g / L, cerium nitrate: zirconium sulfate = 14:1, tartaric acid, monoethanolamine and decanyl trimethyl ammonium bromide were added in sequence after dissolution, tartaric acid: isopropanolamine: decanyl trimethyl ammonium bromide: cerium nitrate = 0.15:1.2:0.55:1.1, and the reaction was carried out at 120°C for 4h. Then, the solid was washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0048] Example 7 Under room temperature, boric acid and lanthanum chloride were dissolved in 200 mL of deionized water at a ratio of 10:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain zirconium phosphate powder.
[0049] Then, cerium chloride and lanthanum borate are dissolved in deionized water, the solubility of cerium nitrate is controlled to be 3g / L, cerium chloride: lanthanum borate = 10:1, succinic acid, imidazole and octadecyl trimethyl ammonium bromide are added in sequence after dissolution, succinic acid: imidazole: octadecyl trimethyl ammonium bromide: cerium nitrate = 0.3:1.2:0.3:0.6, and the reaction is carried out at 120°C for 4h. Then, the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0050] Example 8 At room temperature, iodic acid and aluminum sulfate were dissolved in 200 mL of deionized water at a ratio of 10:1, stirred at a speed of 2000 r / min, and then ammonia water was uniformly added to the solution until the pH of the mixed solution was 9. The solution was then aged at 80°C for 4 hours, cleaned, and dried at 100°C for 24 hours to obtain aluminum iodate powder.
[0051] Then, cerium nitrate and aluminum iodate are dissolved in deionized water, the solubility of cerium nitrate is controlled to be 4.5g / L, cerium nitrate: aluminum iodate = 10:1, citric acid, ethylenediamine and polyacrylic acid are added in sequence after dissolution, citric acid: ethylenediamine: polyacrylic acid: cerium nitrate = 0.25:1.5:0.5:1, and the reaction is carried out at 120°C for 4h. Then, the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain the modified composite cerium oxide.
[0052] Comparative Example 1 Under room temperature, the solubility of cerium nitrate is controlled to be 2g / L, and after dissolution, malonic acid, monoethanolamine and dodecyltrimethylammonium bromide are added in sequence, and the ratio of malonic acid: monoethanolamine: dodecyltrimethylammonium bromide: cerium nitrate is controlled to be 0.25:1:0.25:0.5, and the reaction is carried out at 120°C for 4h. Then the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain cerium oxide.
[0053] Comparative Example 2 Under room temperature, the solubility of cerium nitrate is controlled to be 2g / L, and after dissolution, citric acid, imidazole and dodecyltrimethylammonium bromide are added in sequence, and the ratio of citric acid: imidazole: dodecyltrimethylammonium bromide: cerium nitrate is controlled to be 0.3:1.5:0.5:0.8, and the reaction is carried out at 120°C for 4h. Then the solid is washed with deionized water and anhydrous ethanol, dried at 80°C for 12h, and then calcined at 500°C for 3h to obtain cerium oxide.
[0054] In order to further characterize the scenario of using the composite cerium oxide synthesized in the present invention, the composite cerium oxide in the above Examples 1-8 was used to prepare a chemical mechanical polishing solution, and the polishing rate of the polishing solution on a silicon carbide wafer was further measured. The specific test conditions are as follows: The cerium oxide solid content of the dispersion prepared in Examples 1-8 and Comparative Examples 1-2 was 1 wt%, and the system pH was adjusted to about 3 (1% dilute nitric acid was used as a pH regulator). The polishing removal rate (RR) of each group of polishing liquids on the silicon surface of the silicon carbide wafer was evaluated under different test pressures. The polishing conditions were: the polishing machine was a Fangda grinder, the Sbua800 polishing pad, the upper and lower disc speeds were both 50 rpm, the pressure was 7.5 psi, the polishing liquid flow rate was 100 mL / min, and the polishing time was 30 min.
[0055]
[0056] According to the above experimental results, the composite cerium oxide synthesized in the present invention can significantly improve its polishing rate. By comparing Example 2 with Comparative Example 1, it is shown that the composite running-in abrasive can significantly improve the polishing rate of the polishing liquid on the wafer.
[0057] It should be noted that the embodiments of the present invention have better practicability and do not impose any form of limitation on the present invention. Any technician familiar with the field may use the technical content disclosed above to change or modify it into an equivalent effective embodiment. However, any modification or equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for synthesizing cerium oxide composite abrasive, characterized in that: The steps include: (1) Modified metal salt: a certain amount of solid acid and metal salt are dissolved in a certain amount of water, the pH value of the solution is adjusted to between 9 and 11, and the resulting precipitate is aged, washed, dried and calcined at high temperature to obtain a modified metal salt powder; (2) Synthesis of running-in abrasive: Cerium salt and modified metal salt powder are dissolved in water in a certain proportion, and organic acid, organic base and surfactant are added in a certain proportion. The mixture is reacted at 100-120°C for 2-4 hours. The resulting precipitate is washed, dried and calcined to obtain a spherical cerium oxide composite abrasive modified with a solid acid.
2. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The solid acid described in step (1) is one or more selected from sulfuric acid, phosphoric acid, silicotungstic acid, adipic acid, boric acid or iodic acid.
3. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The metal salt described in step (1) is one or more selected from lanthanum chloride, calcium chloride, erbium chloride, zirconium chloride, ferric sulfate, aluminum sulfate, zirconium sulfate, calcium sulfate, ferric nitrate, aluminum nitrate, europium nitrate or zirconium nitrate.
4. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The molar ratio of the solid acid to the metal salt in step (1) is controlled between 1:1 and 20:
1.
5. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The cerium salt described in step (2) is selected from one or more of cerium nitrate, cerium sulfate, cerium chloride and cerium nitrate ammonium; the organic acid is selected from one or more of tartaric acid, citric acid, malonic acid, succinic acid, oxalic acid, salicylic acid, benzoic acid, malic acid, diethylenetriaminepentaacetic acid or ascorbic acid; the organic base is selected from one or more of ethylenediamine, piperazine, monoethanolamine, triethanolamine, isopropanolamine, tetramethylammonium hydroxide or imidazole; the surfactant is selected from one or more of polyvinyl pyrrolidone, polyacrylic acid, sodium polyacrylate, fatty alcohol polyoxyethylene ether AEO-9, polymethacrylic acid, Tween-20, Tween-80, alkylphenol polyoxyethylene ether, decanyltrimethylammonium bromide or hexadecyltrimethylammonium bromide.
6. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The molar ratio of the cerium salt to the modified metal salt powder in step (2) is between 20:1 and 5:
1.
7. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The molar ratio of the organic acid: organic base: surfactant: cerium salt in step (2) is controlled between 0-0.5: 0-5: 0-1: 0-5.
8. The method for synthesizing cerium oxide composite abrasive according to claim 1, characterized in that: The calcination temperature in step (2) is controlled between 300-500° C., and the calcination time is controlled between 1-4 hours.
9. A spherical cerium oxide composite abrasive, characterized in that: The composite cerium oxide abrasive is prepared by the method for synthesizing the cerium oxide composite abrasive according to any one of claims 1 to 8.
10. A chemical mechanical polishing liquid, characterized in that: The invention comprises the cerium oxide composite abrasive as claimed in claim 9.
Citation Information
Patent Citations
Method for preparing cerium dioxide suspension, cerium dioxide suspension and polishing solution
CN114045153A
Nanometer sphere-like cerium oxide polishing solution for monocrystalline silicon and polycrystalline silicon and application of nanometer sphere-like cerium oxide polishing solution
CN114790367A
Nano-drug carrier, drug loading system containing nano-drug carrier and preparation method of drug loading system
CN115364242A
Method for synthesizing cerium oxide, cerium oxide and chemical mechanical polishing solution
CN116409809A
Preparation method of cerium oxide polishing solution
CN117887356A
Cited By
Scratch-resistant super-hard glass polishing method
CN120901837A
Modified nano rare earth oxide compound as well as preparation method and application thereof
CN121045963A
Modified nanometer rare earth oxide composite, and preparation method and application thereof
CN121045963B