Induced stress for stretching EUV thin films
Inducing tensile stress in CNT membranes through electrical or magnetic means addresses the warping and sagging issues of EUV thin films, ensuring mechanical integrity and optical consistency for photomask protection in lithography tools.
Patent Information
- Application Number
- JP2019170478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-20
- Filing Date
- 2019-09-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-09-19
AI Technical Summary
Existing thin films used in EUV lithography tools face challenges in maintaining mechanical integrity and optical consistency due to warping and sagging, which can lead to contact with scanner structures and changes in light correlation, while being transparent and robust enough to handle EUV light.
A method involving carbon nanotube (CNT) membranes is used, where electrical current is induced through the free-standing portion to create tensile stress, reducing sagging and wrinkling by applying a bias or magnetic field, and optionally coated for enhanced protection.
The method achieves compliant thin films without additional materials or complex tools, maintaining EUV permeability and stability, extending the film's lifetime and ensuring optical consistency.
Smart Images

Figure 0007565679000001 
Figure 0007565679000002 
Figure 0007565679000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of photolithography, and in particular to a method for protecting a photomask by providing a free-standing pellicle over the photomask. [Background technology]
[0002] In lithography, a thin film is needed to prevent particles from falling onto the patterned surface mask. Particles may fall onto the photomask during storage, handling, and lithography exposure. A thin film mounted on the patterned photomask surface keeps particles suspended outside the store so that most particles do not create wafer pattern errors when the photomask is imaged in a lithography exposure tool. The thin film preferably includes a transparent film that does not change the light path and does not affect imaging.
[0003] State-of-the-art lithography tools expose photomasks with extreme ultraviolet (EUV) light centered at 13.5 nm, a wavelength that is readily absorbed by all materials, making it difficult to develop a thin film that is both strong enough to stand on its own and transparent enough for thin-film applications.
[0004] Carbon nanotubes (CNTs) are considered a strong candidate because they provide protection against particles and minimal changes to the exposure light. CNT films are inherently robust, repeatedly achieving transmission of about 96% or more at the exposure wavelength of 13.5 nm and maintaining transmission at other measurement wavelengths (190-500 nm). A concern with thin films is the balance of film stress so that the film is not destroyed but is tensile enough to avoid deflection. In CNT-based films, relaxation of the CNT-CNT bonds has been observed both after film formation and over time, resulting in film slack. This slack includes the mechanical integrity and optical integrity of the film. The film may come into contact with scanners, handling systems, or mask carrier components as a result of deflection. Also, if there is a correlation between light and the thin film, the correlation may change due to deflection as the light passes through the thin film at a certain angle.
[0005] Therefore, there is a need for thin films, including films that have good transparency to EUV and are resistant to bowing, and methods for forming these films in lithographic processes. Summary of the Invention
[0006] It is an object of embodiments of the present invention to provide a method for obtaining a good thin film for protecting a photomask.
[0007] The above objectives are achieved by a method and apparatus according to the present invention.
[0008] An embodiment of the present invention relates to a method for protecting a photomask, the method comprising: providing a photomask; providing a border; depositing at least two electrical contacts on the border; mounting the film including the carbon nanotubes over the border such that the film includes a free-standing portion; After the steps of mounting and depositing, electrical contacts are contacted with the film; further comprising inducing a current through the free-standing portion of the membrane by applying a bias to at least one set of electrical contacts; Mounting a border on at least one side of the photomask with a free-standing portion of the membrane on the photomask; Includes.
[0009] It is an advantage of embodiments of the present invention that compliance with the thin film requirements can be achieved without additional materials, complicated tools, or difficult procedures (thin film being a structure including a membrane and a border). In embodiments of the present invention, the free-standing CNTs forming the thin film are altered by passing an electric current to create a stretched CNT film that is deposited on the border that forms the thin film. This procedure can be repeated multiple times as needed, can be performed outside the scanner, and can be applied to a thin film already deposited on a reticle.
[0010] Strain can be induced on the CNT-based film, if desired, by passing an electric current. This may be accomplished using available equipment. The application of the electric current can be done in a clean room without the risk of adding particles.
[0011] A current generator may be connected using a set of electrical contacts to directly induce a current, or a potential difference may be applied to induce a current through a free-standing portion of the membrane.
[0012] The current may also be induced by varying a magnetic field. An alternative method according to an embodiment of the invention therefore comprises the following steps: providing a photomask; providing a border; mounting a film including carbon nanotubes over the edge such that the film includes a free-standing portion; inducing a current through the free-standing portion of the membrane by varying a magnetic field within the free-standing portion of the membrane; Mounting a border on at least one side of the photomask with a free-standing portion of the membrane on the photomask; Includes.
[0013] This method provides an alternative solution to the same problem, and aims to protect the photomask by providing a free-standing portion of film over the photomask.
[0014] Tension is induced on the CNT-based film by inducing an electric current through the free-standing portion of the film.
[0015] Sagging and wrinkling of the membrane can be reduced or completely eliminated by inducing an electric current through a free-standing portion of the membrane.
[0016] In an embodiment of the present invention, a current is induced by applying a bias to at least two sets of electrical contacts.
[0017] It is an advantage of embodiments of the present invention that better distribution of current is obtained when a voltage is applied to at least two contact pairs. The more uniform the electric field applied to the free-standing portion of the membrane, the more uniform the tensile strength of the membrane.
[0018] In an embodiment of the invention, a current pulse is induced through the free-standing portion of the film, which may be achieved by applying a bias pulse to at least one set of electrical contacts to bias at least one set of electrical contacts, or by applying a magnetic field pulse to the free-standing portion of the film.
[0019] In an embodiment of the invention, a current pulse train with a predetermined determined cycle is induced through the free-standing portion of the film, which may be achieved by biasing at least one set of electrical contacts with a pulse train, or by applying a magnetic field pulse train to the free-standing portion of the film to bias at least one set of electrical contacts.
[0020] In an embodiment of the present invention, the border provided is a silicon border.
[0021] In an embodiment of the present invention the border is provided by providing a silicon based material and partially removing the silicon based material.
[0022] In embodiments of the present invention, electrical contact is achieved by depositing a titanium seed layer followed by deposition of palladium.
[0023] In an embodiment of the present invention, the film is preferably prepared by dry transfer of carbon nanotubes.
[0024] Carbon nanotubes may be grown by floating catalytic chemical vapor deposition or extracted from a solution using vacuum filtration onto filter paper, methods known to those skilled in the art, such as floating aerosol CVD reactors deposited onto filter paper, CVD forests drawn into a film, vacuum filtration of CNT solutions, spin coating onto intermediate substrates, etc. In an embodiment of the invention, the step of mounting the film comprises placing carbon nanotubes onto filter paper or pulling a sheet from a carbon nanotube forest, the film being mounted by pressing the filter paper against the edges or by pulling the sheet off.
[0025] It is an advantage of embodiments of the present invention that the process of drawing CNT sheets from vertically oriented CNT forests grown by fixed catalyst CVD produces more aligned films.
[0026] In an embodiment of the invention, the method includes the step of providing isopropyl alcohol on top of the film after deposition of the film.
[0027] It is an advantage of embodiments of the present invention that increased densification and / or increased adhesion can be obtained by providing isopropyl alcohol (vapor, spray, or wet) onto the membrane.
[0028] In an embodiment of the invention, the method includes the step of providing a coating on the membrane.
[0029] The extended lifetime of CNT films in halogen radical environments is an advantage of embodiments of the present invention: even though they have a finite etch rate in halogen radicals, CNTs are inexpensive to produce and therefore can have thin films with a finite lifetime.
[0030] In embodiments of the present invention, one or more layers may be coated onto the CNT film. In embodiments of the present invention, a coating may be formed on both sides of the film.
[0031] The coating may be applied before or after the application of the voltage or current.
[0032] In embodiments of the present invention, a partial coating may be provided on the membrane.
[0033] By reducing the amount of coating material, the EUV transmission of the resulting CNT film is improved.
[0034] According to embodiments of the present invention, the partial coating may be provided by deposition or by decoration of defects in the film containing nanocarbon.
[0035] In embodiments of the present invention, a complete coating may be provided on top of the membrane.
[0036] It is an advantage of embodiments of the present invention that due to such controlled complete coating, the life span of the CNT film is longer (compared to partial coating).
[0037] According to embodiments of the present invention, a conformal coating is provided. In embodiments of the present invention, the complete coating may be deposited using physical vapour deposition, or atomic layer deposition, or chemical vapour deposition, or electrochemical deposition.
[0038] In an embodiment of the present invention, the method comprises the step of applying lithography on a photomask protected by a loaded film comprising carbon nanotubes.
[0039] Particular and preferred aspects of the invention are set out in the accompanying independent and dependent claims. Features from the dependent claims may be combined with features of the independent claims as appropriate and not merely as set out in the claims.
[0040] These and other aspects of the invention will be apparent from and elucidated with reference to the embodiments described hereinafter. [Brief description of the drawings]
[0041] [Figure 1] 1 shows a flow chart of an exemplary method according to an embodiment of the present invention. [Diagram 2] 2 shows a schematic side view of a thin film on a photomask obtained using a method according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic plan view of a CNT film mounted on a border, the CNT film having a rectangular free-standing portion outlined by the border, and electrical contacts present on the border according to an embodiment of the present invention. [Figure 4] FIG. 2 shows a schematic plan view of a CNT film having a rectangular free-standing portion mounted on an edge with a contact on the edge according to an embodiment of the present invention. [Diagram 5] 4 illustrates a biasing procedure in which a set of electrical contacts is biased according to an embodiment of the present invention. [Figure 6] 4 illustrates a biasing procedure in which two sets of electrical contacts are biased according to an embodiment of the present invention. [Figure 7] 1 shows a scanning electron microscope (SEM) image of the membrane before a current is applied through the free-standing portion of the membrane. [Figure 8] 1 shows a scanning electron microscope (SEM) image of a membrane after a current has been applied through a free-standing portion of the membrane according to an embodiment of the present invention.
[0042] Reference signs in the claims shall not be construed as limiting the scope. The same reference signs in different drawings indicate the same or similar elements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] The present invention will be described with reference to certain embodiments and certain drawings but the invention is not limited thereto but only by the claims. The drawings described are merely schematic and are non-limiting. In the drawings, for illustrative purposes, the size of elements may be exaggerated and not drawn to scale. The dimensions and relative dimensions do not correspond to actual scales in the practice of the invention.
[0044] The terms first, second, etc., in the description and claims are used to distinguish between similar elements and do not necessarily denote an order in time, space, precedence, or in any other manner. The terms so used are interchangeable under appropriate circumstances, and it is to be understood that the embodiments of the invention described herein can be operated in different orders than those described or illustrated herein.
[0045] Moreover, terms such as above, below, and the like in the description and claims are used for descriptive purposes only and do not denote relative positions. It is to be understood that the terms so used are interchangeable under appropriate circumstances and that the embodiments of the invention described herein can be operated in positions other than those described or illustrated herein.
[0046] The term "comprising" used in the claims should not be interpreted as being limited to the means listed thereafter, nor excluding other elements or steps. Thus, any recited feature, number, step or component should be interpreted accordingly, and should not exclude the presence or addition of one or more other features, numbers, steps or components, or any combination thereof. Thus, the scope of the expression "a device comprising means A and B" should not be limited to a device that includes only components A and B. In the present invention, it simply means that the components associated with the device are A and B.
[0047] References throughout this specification to "one embodiment" or "an embodiment" mean that a particular advantage, structure, or feature described in connection with that embodiment is included in at least one embodiment of the invention. Thus, appearances of the phrases "one embodiment" or "an embodiment" in various places throughout this specification do not necessarily refer to the same embodiment, but may. Furthermore, the particular advantages, structures, or features may be combined in any suitable manner in one or more embodiments, as will be apparent to one of ordinary skill in the art from this description.
[0048] Similarly, in the description of the illustrative aspects of the present invention, it should be appreciated that, for the purposes of efficiently disclosing and facilitating understanding of one or more of the inventive aspects, the numerous advantages of the invention are sometimes grouped together in a single embodiment, drawing, or description thereof. However, this method of disclosure should not be construed as representing an intention that the claimed invention requires more features than are recited in each claim. Rather, as the following claims reflect, inventive aspects amount to less than all advantages of a single described embodiment. Thus, the claims following the detailed description are hereby expressly incorporated into the detailed description, with each claim standing on its own as a separate embodiment of this invention.
[0049] Furthermore, some embodiments described herein may include some features that are not included in other embodiments, and the combination of advantages of different embodiments is meant to fall within the scope of the present invention and forms different embodiments as would be understood by one skilled in the art. For example, in the following claims, some of the claimed embodiments may also be used in other combinations.
[0050] In the description provided herein, numerous specific details are set forth. However, it should be understood that embodiments of the present invention may be practiced without those specific details. In other instances, well-known methods, structures and techniques have not been shown in detail in order not to obscure an understanding of this description.
[0051] When referring to a film in an embodiment of the present invention, the reference is to a cover that protects the photomask. This film may also be referred to as a "dust cover."
[0052] When referring to thin films in embodiments of the present invention, reference may be made to the mounted film and border used in a scanner for exposure.
[0053] An embodiment of the present invention relates to a method 100 for protecting a photomask 210. The method comprises: Step 110 of providing a photomask 210; Step 120 of providing a border 220; depositing 130 at least two electrical contacts 230 on the border 220; mounting 140 a film 240 including carbon nanotubes on the border 220 such that the film 240 includes a free-standing portion; After the loading step 140 and the deposition step 130, electrical contacts 230 contact the film 240; and obtaining 150 a current through the free-standing portion of the membrane by applying a bias to at least one set of electrical contacts 230; Step 170 of mounting a border 220 on at least one side of the photomask 210 with a free-standing portion of the membrane; Includes.
[0054] The border 220 and membrane 240 are attached to the photomask 210. This can be done directly or through the use of an additional spacer frame. The border may be mounted on both sides of the photomask.
[0055] The steps do not have to be in the order as described above. Step 130 of depositing at least two electrical contacts 230 may, for example, be performed before or after step 140 of depositing the carbon nanotube-containing film 240. The photomask may, for example, be provided immediately after step 170 of depositing the border 120 onto the photomask 210.
[0056] The current may be induced by varying a magnetic field in the free-standing portion of the film. In this case, electrical contacts are not strictly required. The variation in the magnetic field may induce eddy currents in the film. The variation in the magnetic field in the film may be produced, for example, by an alternating current transformer or an electromagnet arranged to produce a variation in the magnetic field in the free-standing portion of the film during operation.
[0057] The tension in the free-standing part of the membrane is increased by applying a bias to one contact pair such that a current is obtained through the free-standing part of the membrane. This results in a stretched mesh of CNTs that meets, for example, scanner conditions, e.g., a maximum deflection of 0.7 mm at a pressure difference of 2 Pa. In an embodiment of the invention, a bulge test measurement may be performed to qualify the tension of the membrane. A bulge tester may be used, for example, to qualify the maximum deflection of the membrane. The tension on the membrane may be tested using different types of equipment.
[0058] A flow chart of an exemplary method according to an embodiment of the present invention is shown in Figure 1. Figure 2 is a schematic diagram of a photomask protected with a film containing carbon nanotubes obtained using a method according to an embodiment of the present invention.
[0059] In an exemplary method, a border is formed 120. This border 220 may be obtained, for example, from a Si wafer.
[0060] The border 220 may be formed, for example, by providing a substrate material (e.g., a silicon wafer) on which a mask material, e.g., SiN, is deposited, and then partially removing the substrate material. For example, between 30 nm and 50 nm of a mask material (e.g., SiN) may be deposited on the substrate. The partial removal may be achieved by laser cutting or a patterning / etching process (e.g., etching in KOH 20%, 70° C., 8 hours, and rinsing with DI water / IPA). Other borders 220 may be used. The border may include, for example, a high temperature ceramic.
[0061] In accordance with an embodiment of the present invention, at least two electrical contacts 230 (also called pads) are deposited on the border 220. This may be done before or after the application step 140 of the membrane 240 containing carbon nanotubes. The pads 230 may have different dimensions, may be made of different conductive materials and may be formed separately depending on the desired effect. In accordance with an embodiment of the present invention, the electrical contacts 230 may be obtained by forming metal contacts, for example by a deposition step 130 of a titanium adhesion layer followed by a deposition step of palladium. For example, a 50 nm palladium contact may be grown and then a 0.3-2 nm titanium layer may be deposited (Ti / Pd). In accordance with an embodiment of the present invention, the material of the electrical contacts is selected for a number of reasons, preferably to obtain a low resistance. For example, palladium (Pd), gold (Au) and platinum (Pt) all have low resistance.
[0062] The carbon nanotube (CNT) containing film is assembled into a free-standing film 240 whose morphology depends on the fabrication process.
[0063] The CNTs in film 240 are randomly positioned when prepared either by wet transfer of CNTs grown by floating catalyst chemical vapor deposition (CVD) or by vacuum filtration of CNTs dispersed in solution followed by removal of the filter membrane.
[0064] The process of drawing CNT sheets from vertically aligned CNT forests grown by stationary catalytic CVD produces more aligned CNTs in films arranged in one or multiple layers.
[0065] In an embodiment, the CNT films are mounted by placing them onto a supporting border 220 to form a free-standing film 240. For example, filter paper (aerosol collection method) or drawn sheets (vertical forest growth) may be pressed onto the border for adhesion.
[0066] Optionally, IPA (gas, spray, or wet) may be applied for densification and / or adhesion. The border may have a thin layer (5-50 nm) of SiN, TiN, or other material deposited for a number of reasons, such as improving the chemical stability of the CNT or pad, balancing the stress, or improving adhesion.
[0067] The free-standing membrane can be further processed, i.e., washed, coated, or stretched.
[0068] Due to van der Waals forces between the CNTs, which predominate at the nanoscale, the CNTs form a film. Over time, a sagging is observed which raises two concerns: a compromise between print quality and the risk of reflections and many optical effects during pressure fluctuations in the scanner.
[0069] Therefore, in an embodiment of the present invention, an electric current is forced through the membrane 240 mounted at the border 220. This process of applying an electric current results in a macroscopically visible change that greatly reduces or even eliminates sagging and wrinkling.
[0070] In embodiments of the invention, at least two, and typically four or more, electrical contacts 230 (also called pads) are disposed on the border 220 and a current is applied directly or a voltage difference is applied to induce a current through the membrane. In embodiments of the invention, the pads 230 may be distributed at different positions along the border. The pads 230 may be elongated contacts (e.g., with a length / width ratio limited only by the dimensions of the border and the need to separate one pad from the other). The pads 230 are formed such that when a current is applied through the membrane by applying a bias to at least two pads 230, a desired tension is induced across the membrane.
[0071] The borders 220 are mounted 170 on the photomask 210, with the free-standing portion of the membrane 240 on top of the photomask. In the example of Figure 2, a schematic drawing of the resulting stack is shown. Here, the photomask 210 is shown with a pattern drawn on it. On top of the photomask is a thin film with its borders 220 attached to the photomask 210 and with the membrane 240 on top of the photomask 210. Although not drawn in this schematic, a thin film may be on both sides of the photomask. Also shown in this schematic are electrical contacts 230. Those electrical contacts 230 are drawn on top of the borders.
[0072] Examples of pads 230 on borders of different sizes are shown in Figures 3 and 4, respectively. Figure 3 shows a 3x3 cm outer dimension pad for a test sample with four pads 230 deposited on the edge of the border 220. 2 FIG. 2 shows a border 220 of 120×150 cm with outer dimensions, with eight deposited pads, two on each edge of the silicon-based border 220. The border 220 is located between the outer and inner rectangles. A CNT film 240 (indicated by a pattern) is free-standing in the center 250 and supported on the border 220. FIG. 4 is a schematic of a larger sample, with outer dimensions of 120×150 cm with eight deposited pads, two on each edge of the silicon-based border 220. 22. The CNT film 240 is free-standing at the center 250 and rests on the border 220 at the edges.
[0073] In an embodiment of the invention, the border has an open volume. By providing a membrane on this border, the membrane on this volume becomes a free-standing membrane. The shape of the free-standing area of the membrane is defined by the border surrounding this area. In the examples of figures 3 and 4, square or rectangular free-standing parts of the membrane are shown. However, the invention is not limited to this. Other shapes are also possible, for example circular. They are defined by the border 220.
[0074] In an embodiment of the invention, a bias is applied on one or more pairs of electrical contacts 230. In the example of FIG. 3, if a current is applied from contact 2 to contact 4, the current application process will deform the membrane such that it becomes more tensile in the direction 2-4. If a current is applied to 2-1, only a limited portion between contact 2 and contact 1 will become more tensile as a result of the current application. A single current may be induced along a single path, or multiple currents may be induced between multiple contact pads. For example, a first voltage may be applied on contact 1 and contact 3, and simultaneously a second voltage may be applied on contact 2 and contact 4. By doing so, a first current is obtained between node 1 and node 3, and a second current is obtained between node 2 and node 4. The first voltage may be different from the second voltage, and additionally the first current may be different from the second current.
[0075] In an embodiment of the invention, the electrical resistance of the membrane 240 is measured using the van der Pauw method to measure the changes in the membrane. To quantify the process, the resistance is measured before, during and after tensioning. The sample procedure may include measuring the resistance followed by applying a current or voltage between two contacts (I24 / V24 in FIG. 5). During this, the resistance is measured and the membrane is visually inspected for a straight and wrinkle-free appearance. The tension may be measured (e.g. indirectly with a dilation test, measuring the value of the deflection while applying pressure to the membrane). If additional tension is required, an additional set of contacts may be used to apply the current or voltage, e.g. I13 / V13. This procedure may be repeated on different sets of contacts (I12 / V12, I34 / V34, I41 / V41, I23 / V23, I24 / V24 or I13 / V13) while measuring the resistance and checking for a flat, wrinkle-free tension on the membrane. The application of bias to different sets of electrical contacts 230 may be repeated until a uniform strain is achieved, the membrane is flat and wrinkle-free, and the resistance saturates to a constant value. The goal is to use electrical current to strategically induce a tensile stress uniformly across the membrane.
[0076] As mentioned above, in embodiments of the invention, the resistance of the membrane may be detected by changing using the Van der Pauw method. This is the reference resistance. Current or voltage may be applied simultaneously to multiple electrical contacts. An example of such a configuration is shown diagrammatically in FIG. 6, which shows a voltage or current source on contact sets 1 and 3 (I13 or V13) and contact sets 2 and 4 (I24 or V24). For example, I24 or V24 and I13 or V13 are contacted simultaneously to form a dual channel configuration. In embodiments of the invention, multiple sets of electrical contacts are biased, and this multiple channel approach may be expanded to complex contact and current / voltage sets for the configuration shown in FIG. 6, or for configurations with more contact pads.
[0077] In embodiments of the invention, this method is suitable for thin films consisting of uncoated CNT films or for thin films formed from CNT films coated with different materials. In embodiments of the invention, the CNT film coating 160 is performed after placing 130 the contact pads on the edging and mounting the uncoated CNT film.
[0078] In embodiments of the present invention, the amount of time for which a bias is applied to a set of electrical contacts such that a current is obtained through the free-standing portion of the membrane may range, for example, from a few milliseconds to a few minutes, the applied current may range, for example, from a few milliamps to 200 mA or more, the applied voltage may vary, for example, from zero to 40 V, and the applied voltage may be, for example, greater than 20 V, or greater than 40 V, although these are not necessary limitations of this procedure.
[0079] In embodiments of the invention, the application of a pulse train (current or voltage) may be used to induce such stress. The on / off ratio of such a pulse train may for example be adjustable. The on / off ratio may for example be greater than 20%, such as 40%, 60%, 80%. However, this is not strictly required.
[0080] In embodiments of the invention, the electrical current may be provided such that heating of the free-standing parts of the membrane is limited. During application, the temperature of the membrane may for example be less than 200° C., or less than 30° C. This may for example be achieved by controlling the convective gas flow and the duty cycle of the applied current or voltage. Hence, the current may be limited to a maximum value and / or the duration of the pulses may be limited to a maximum value and / or in the case of a pulse train the on / off ratio may be limited to a maximum value.
[0081] It is specifically noted by the inventors that the resistance of the CNT film increases with the applied current. Without wishing to be bound by a particular theory, it is believed that this relationship between resistance and current suggests a nanoscale change in the film itself. Figure 7 shows a scanning electron microscope (SEM) image of the film before applying a current through the free-standing portion of the film. Figure 8 shows an SEM image after applying a current so that increased tension is obtained. As can be seen, there is no difference in the SEM. Therefore, the inventors speculate that the change is that the nanomorphology (healing bonds) or volatilizing contaminants must be dealt with more.
[0082] In an embodiment of the invention, a coating is applied 160 onto the membrane. This is an optional step and may be performed, for example, prior to applying a bias 150 to at least one pair of electrical contacts, thereby forcing a current through the free-standing portion of the membrane. However, the invention is not so limited and the coating may be performed after biasing the contact pair.
[0083] The CNT film 240 may be partially or completely coated. Partial coatings may be obtained by depositing very thin (e.g., less than 3 nm) or decorating CNT defects. Complete coatings are achieved, for example, by physical vapor deposition (PVD), i.e., electron beam or thermal evaporation, remote plasma sputtering, atomic layer deposition (ALD), chemical vapor deposition (CVD), electrochemical deposition (ECD), and sol-gel techniques, or a combination of several methods. Coatings include, for example, the following materials: Zr, Y, B, Ti, Ru, Mo, and related compounds, nitrides or oxides. However, this list is not limited to these materials.
[0084] The process flow shown in Figure 1 is an exemplary process flow according to an embodiment of the present invention. However, the present invention is not limited thereto. Steps can be skipped if not required (e.g., a coating step). The order of steps can also be changed (e.g., coating the film after applying an electric current).
[0085] The coating may include a multi-layer coating of free-standing carbon nanotube (CNT) membranes (preferably two layers, but multiple layers are also possible). This coating protects the membrane from aggressive environments, such as hydrogen radicals when used as an EUV membrane. The coating can increase the emissivity for radiative cooling.
[0086] When used as an EUV thin film, the free-standing CNT film can effectively suppress the emission of halogen radicals (H * The CNT structure in the film (also called the film structure) is * The thin film is damaged by the attack of the CNTs, which are then removed by vaporization of carbon to hydrocarbon molecules. To avoid film degradation, the CNT film structure is heated to 1000°C. * To reduce or eliminate damage, the CNT membrane must be protected. This can be done by coating (e.g., on both sides) the CNT membrane with a thin film of one or more layers. Protection can also be achieved by targeted deposition over weak spots along the CNT tubes in the membrane.
[0087] Atomic layer deposition (ALD) may be used to deposit conformal thin films on complex structures, but conformal, pinhole-free coatings on CNTs are challenging due to the inertness of the CNT surface, which has few active sites for ALD nucleation at the beginning of film growth.
[0088] According to embodiments of the present invention, the first coating may be a partial coating layer. This may be achieved by selective coating of defects by atomic layer deposition (ALD) or chemical vapor deposition (CVD). * Etching may begin at defect sites in the CNT and then proceed along the tube length. ALD / CVD begins with nucleation on the defect sites and then H * It is known that coating of CNT defects can selectively protect CNT defects from oxidation. The partial coating of CNT defects extends the lifetime of the coated CNT thin film compared to the uncoated case.
[0089] Optionally, a second coating layer may be applied on one or both sides of the CNT film on top of the partial ALD / CVD coating to improve emissivity. The coating may be provided by various thin film deposition techniques already mentioned above, e.g. thermal or electron beam evaporation, sputtering, etc.
[0090] In embodiments of the present invention, a complete coating may be provided on top of the CNT film 240 for protection. This layer may be achieved by a conformal coating process.
[0091] Conformal coating may be achieved by providing a seed (adhesion) layer deposited by thermal or e-beam evaporation prior to the ALD coating. This seed layer deposition approach is gentle on the CNT structures and preserves the initial CNT properties. For uniformity of the seed layer, the evaporation is performed at an angle of, for example, 15°, but this angle can be from 1° to 89°, and the substrate is rotated during deposition. ALD on top of the seed CNT structures is uniform and conformal.
[0092] It is an advantage of embodiments of the present invention that the above-described seed layer is provided as protection for the CNT film structure during deposition of subsequent layers, which may involve exposure of the CNTs to harsh reactive conditions (e.g., plasma-based sputtering) or strong oxidizing agents (e.g., certain ALD processes) that are known to damage CNTs during the process.
[0093] In embodiments of the present invention, an intermediate flexible thin coating can be added between the hard coating films, for example carbon, to reduce stress in the multi-layer coating.
[0094] In an embodiment, two layers may be applied using a conformal coating. Since the total stress is a combination of the compressive or tensile stresses induced by each layer, by applying two layers, the stresses may be balanced. This results in a uniform tensile film and a film with reduced or no wrinkles.
[0095] In an embodiment of the present invention, a conformal coating イ The CNT thin film tectonics may provide a CNT structure favorable for ALD or CVD nucleation. CNT thin film tectonics may include, for example, N-doped CNTs. The process of doping the CNT film with other atoms makes the CNT film more favorable for ALD or CVD nucleation due to the introduction of reactive surface species.
[0096] The CNT film may contain multi-walled CNTs to better facilitate conformal coating, in which case one of the walls may be used as a sacrificial CNT wall that serves to enable ALD seeding.
[0097] In embodiments of the present invention, the number of ALD cycles required to obtain a continuous conformal ALD coating may be reduced by coating onto seeded CNTs, for example, a very thin layer (e.g., a ruthenium coating) may be formed by ALD.
[0098] In embodiments, a dry approach may be applied to the conformal coating, where no solution is used to deposit the coating.
[0099] It is an advantage of embodiments of the present invention that the intrinsic structural, mechanical and electrical properties of the CNTs can be preserved by avoiding damage to the CNTs during seed layer growth.
[0100] It is an advantage of embodiments of the present invention that a variety of coating approaches are possible, as long as the CNTs are protected by a seed layer, for example from ion bombardment during the coating process.
[0101] An advantage of the embodiments of the present invention is that they can be applied to highly transparent free-standing films of single-walled CNTs, which are known to have fewer defects than multi-walled CNTs.
[0102] It is an advantage of embodiments of the present invention that the CNT structure is favorable for conformal coating because it allows defect engineering of the CNT surface for controlled coating by ALD while preserving free-standing CNT film morphology.
[0103] A method according to embodiments of the present invention may include a lithography step on a photomask protected by a loaded film containing carbon nanotubes.
[0104] In embodiments of the present invention, a CNT film may be mounted between raised edges and an electric current applied to a free-standing portion of the film to form a CNT thin film, which is a solution for reticle protection in lithography.
[0105] In embodiments of the invention, the lithography may be extreme ultraviolet lithography using a wavelength of 13.5 nm. However, the invention is not limited to this wavelength. The wavelength may range, for example, between 3 nm and 248 nm. When using carbon nanotubes, the membrane can be made so thin that it does not affect the passage of EUV light through the membrane. Furthermore, it is advantageous that the method according to embodiments of the invention increases the tensile stress, which is maintained for a long time. The tensile stress is maintained stably, for example, permanently.
Claims
1. A method (100) for protecting a photomask (210), the method comprising: Providing (110) a photomask (210); Providing (120) a border (220); Depositing (130) at least two electrical contacts (230) on the border (220); and mounting (140) a film (240) comprising carbon nanotubes onto the border (220) such that the film (240) comprises a free-standing portion; After the mounting step (140) and the depositing step (130), electrical contacts (230) contact the membrane (240); and applying a bias between at least two sets of electrical contacts (230) to induce a current through the free-standing portion of the membrane (240) to pull the membrane in the direction of the current supply such that the temperature of the membrane is limited to less than 30° C. (150). Mounting (170) a border (220) on at least one side of the photomask (210) with a free-standing portion of the membrane; The method includes:
2. A method (100) for protecting a photomask (210), the method comprising: Providing (110) a photomask (210); Providing (120) a border (220); Mounting (140) a film (240) comprising carbon nanotubes on a border (220) such that the film (240) comprises a free-standing portion; Inducing a current through the free-standing portion of the membrane (240) and pulling the membrane in the direction of the current supply (150) such that the temperature of the membrane is limited to a temperature below 30° C. by varying a magnetic field within the free-standing portion of the membrane; Mounting (170) a border (220) on at least one side of the photomask (210) with a free-standing portion of the membrane; The method includes:
3. The method (100) of claim 1 or 2, wherein a current pulse is induced (150) through a free-standing portion of the membrane (240).
4. The method (100) of claim 1 or 2, wherein a train of current pulses having a predetermined cycle is induced through the free-standing portion of the membrane (240).
5. The method (100) according to any of the preceding claims, wherein the border (220) provided is a silicon border.
6. The method (100) of claim 5, wherein the border (220) is provided by providing a silicon-based material and partially removing the silicon-based material.
7. The method (100) of claim 1, wherein the electrical contact (230) is obtained by depositing a titanium seed layer, followed by deposition of palladium.
8. The method (100) according to any of claims 1 to 7, wherein the membrane (240) is prepared by dry transfer of the carbon nanotubes or by extraction from a solution using vacuum filtration onto filter paper.
9. The method (100) according to any of the preceding claims, comprising the step of providing isopropyl alcohol on the film after deposition of the film.
10. The method (100) of any of the preceding claims, comprising the step (160) of providing a coating on the membrane (240).
11. The method (100) of claim 10, wherein a partial coating is provided on the membrane (240) covering a portion of the membrane (240).
12. The method (100) of claim 10, wherein a complete coating is provided on the membrane (240) to cover the entire membrane (240).
13. The method (100) according to any of the preceding claims, comprising the step of applying lithography on a photomask protected by a mounted film comprising carbon nanotubes.
Citation Information
Patent Citations
Method for forming pellicle
JP2018194838A
Method for manufacturing a pellicle for a lithographic apparatus, Pellicle for a lithographic apparatus, Lithographic apparatus, Device manufacturing method, Apparatus for processing a pellicle, and Method for processing a pellicle
JP2018531426A
Film for manufacturing semiconductor
KR1020190118455A
Pellicle and photomask assembly including the same
US20170038676A1