Resin member for plating and its manufacturing method

The resin member with laser-formed grooves and burrs addresses adhesion issues in plating, enhancing adhesion and maintaining functionality in portable devices.

JP7565807B2Active Publication Date: 2024-10-11POLYPLASTICS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021008134
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-21
Publication Date
2024-10-11
Estimated Expiration
2041-01-21

AI Technical Summary

Technical Problem

The adhesion between plating and resin members in portable devices is inadequate, leading to potential peeling and device malfunction, despite surface roughening methods like laser treatment and chemical treatment.

Method used

A resin member with grooves of 1 to 15 μm depth and 10 to 500 μm interval, featuring a burr height related to groove interval by formula (b≦35a-24, formed using laser irradiation, made from polybutylene terephthalate, polyphenylene sulfide, or liquid crystal polymer, enhances adhesion.

Benefits of technology

Improves plating adhesion and maintains electromagnetic shielding properties, preventing peeling and ensuring device functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565807000002
    Figure 0007565807000002
  • Figure 0007565807000003
    Figure 0007565807000003
  • Figure 0007565807000001
    Figure 0007565807000001
Patent Text Reader

Abstract

To provide a resin member plated with good adhesion; and to provide a production method thereof.SOLUTION: In a resin member for plating, the resin member has multiple grooves each having a depth of 1-15 μm on a surface to be plated, and the groove has burr having a height a of 5 μm or more around an opening, and the height a of the burr has a relation of following formula (1) with an interval b of the multiple grooves: formula (1) b≤35a-24. A production method thereof is also provided.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin member for plating treatment and a method for producing the same. [Background technology]

[0002] In recent years, the number of applications in which metal is plated onto resin members has increased, and the requirements for adhesion between the plating and the resin member have become stricter. For example, in mobile devices such as smartphones, electrodes are formed directly on the resin member by plating to reduce its weight (Patent Document 1), and plated resin members are used as electromagnetic shields (Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-184090 A [Patent Document 2] JP 2020-195105 A [Patent Document 3] JP 2019-131839 A Summary of the Invention [Problem to be solved by the invention]

[0004] These mobile devices are handled in a variety of ways, and so the plating can peel off from the resin parts, which can be a direct cause of malfunction of the mobile devices. Prior to plating, the surface of the resin part to be plated was roughened with a laser and then treated with a chemical, but this alone was not sufficient (Patent Document 3).

[0005] An object of the present invention is to provide a resin member for use in plating with good adhesion, and a method for manufacturing the same. [Means for solving the problem]

[0006] The object of the present invention has been achieved by the following.

[0007] 1. aluminum A resin member for plating treatment, the resin member having a plurality of grooves having a depth of 1 to 15 μm on a surface to be plated, The interval b between the plurality of grooves is 10 to 500 μm; The groove is 5 mm around the opening. ~30 μ m The grooves have a burr having a height a, and the height a of the burr and the interval b between the grooves are related by the following formula (1): death, Formula (1) b≦35a-24 The resin member is formed from any resin selected from the group consisting of polybutylene terephthalate, polyphenylene sulfide, and liquid crystal polymer. 2. before The width c of the opening of the recording groove is 50 to 200 μm. 1 to The resin member described above. 3 For resin parts aluminum A method for producing a plated resin member, the method comprising forming a plurality of grooves having a depth of 1 to 15 μm on a surface of the resin member to be plated, The interval b between the plurality of grooves is 10 to 500 μm; The groove is 5 mm around the opening ~30 μ m A groove has a burr having a height a, and the height a of the burr and the interval b of the plurality of grooves have the following formula (1): By irradiating laser light Forming a death, Formula (1) b≦35a-24 The method for producing a plated resin member, wherein the resin member is made of any resin selected from the group consisting of polybutylene terephthalate, polyphenylene sulfide, and liquid crystal polymer. Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin member for applying plating with good adhesion and a method for manufacturing the same. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a cross-sectional schematic diagram showing multiple grooves of the present invention. [Diagram 2] 1 is a graph showing the experimental results obtained by calculating formula (1) of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described in detail.

[0011] <Resin materials> The resin member of the present invention is a resin member for plating treatment, characterized in that the resin member has a plurality of grooves with a depth of 1 to 15 μm on a surface to be plated, the grooves have burrs with a height a of 5 μm or more around openings, and the height a of the burrs and the interval b between the plurality of grooves satisfy the following formula (1): Formula (1) b≦35a-24

[0012] <Resin> The resin forming the resin member of the present invention is not particularly limited as long as it can be plated. For example, thermoplastic resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), aliphatic polyamide, aromatic polyamide, polyphenylene sulfide (PPS), liquid crystal polymer (LCP), polyether ether ketone (PEEK), polyimide, polyacetal (POM), ABS resin, and cyclic polyolefin (COC) can be used.

[0013] These resins may contain inorganic fillers such as glass fillers and mineral fillers. These resins may be used alone or in combination of two or more.

[0014] <groove> The surface to be plated of the resin member of the present invention has a plurality of grooves having a depth of 1 to 15 μm.

[0015] A surface of the resin member of the present invention to be plated has multiple grooves with a depth of 1 to 15 μm formed thereon. In Fig. 1, a indicates the height of burrs formed around the openings of the grooves from the flat portion of the resin member. b indicates the distance between the multiple grooves, c indicates the width of the grooves, and d indicates the pitch between the multiple grooves.

[0016] The periphery of the groove opening refers to a range of about 30 μm from the groove opening toward the flat portion. The height a of the burr refers to the highest point within a range of about 30 μm from the groove opening toward the flat portion. The burr does not have to be formed all around the periphery of the groove opening, but good plating adhesion can be obtained by forming the burr on at least 60% or more of the periphery of the opening, more preferably 70% or more, and particularly preferably 80% or more.

[0017] The height a of the burr is 5 μm or more, preferably 5 to 30 μm, and more preferably 5 to 20 μm. The grooves are formed at intervals b, and the number of grooves is determined appropriately depending on the area to be plated. The intervals b do not have to be the same on all the surfaces to be plated. If the height a of the burr exceeds 30 μm, in addition to poor appearance, the electromagnetic shielding properties may be reduced due to poor adhesion of the plating to the side of the burr.

[0018] The grooves may be arranged in a line like contour lines with both ends connected, or in stripes without intersecting, or in a lattice pattern with intersecting grooves, or in polka dots. When the grooves are arranged in a lattice pattern, they may be rhombic.

[0019] The length of the groove is not particularly limited, and when the groove is short, the shape of the opening may be rectangular, round, or elliptical. In order to obtain an anchor effect, the longer the groove, the better.

[0020] The spacing b between adjacent grooves in the present invention is preferably 0.5 to 4 times the groove width c, i.e., if the groove width c is 100 μm, then 50 μm to 400 μm, and more preferably 1 to 2 times the groove width, i.e., if the groove width c is 100 μm, then 100 μm to 200 μm.

[0021] The distance b between adjacent grooves is preferably 600 μm or less, more preferably 500 μm or less, and particularly preferably 300 μm or less. In the present invention, the burr height a and the groove interval b have the relationship represented by formula (1). Formula (1) b≦35a-24 Equation (1) is the relationship between the burr height a and the groove spacing b obtained from the experimental data shown in FIG.

[0022] <How to form grooves> The grooves in the resin member of the present invention are preferably formed by irradiating the surface of the resin member before the grooves are formed with a laser beam to partially remove the resin. The conditions such as the type, wavelength, output, and irradiation time of the laser beam may be appropriately selected according to the resin composition constituting the target resin member, and it is preferable to adjust the burrs to 5 μm or more from the flat portion and the groove depth to 1 to 15 μm.

[0023] In order to ensure image quality and adhesive strength, the area of ​​the grooves to be formed is preferably 20% or more of the area of ​​the plating, more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more. Since the formation of burrs improves adhesiveness, the upper limit is preferably 90% or less, more preferably 80% or less, and particularly preferably 70% or less.

[0024] In particular, when grooves are formed over the entire surface of a plated resin member that contains inorganic fibers, the inorganic fibers are exposed by the laser treatment, and when plating is performed, the inorganic fibers may peel off from the exposed inorganic fiber portion. Also, in order to shorten the laser treatment time, treatment of the entire surface of the plated portion should be avoided.

[0025] If the presence of a carbonized resin layer can be confirmed by Raman spectroscopic analysis of the groove portion, it can be determined that the groove has been formed by irradiation with laser light.

[0026] It is also preferable to add a colorant (light absorbent) such as a dye or pigment to the resin workpiece of the present invention in order to efficiently absorb laser light, or a transparent near-infrared absorbent that does not affect the hue of the resin, and it is more preferable to add an inorganic colorant (e.g., carbon black) rather than an organic colorant. EXAMPLES

[0027] The present invention will be described in detail below with reference to examples. The evaluations were carried out in an atmosphere of 23° C. and 50% RH unless otherwise specified.

[0028] <Formation of test specimen> <Formation of resin member for forming groove> Using the following resin manufactured by Polyplastics Co., Ltd., a test specimen of a flat resin member having dimensions of 100 mm x 100 mm x 3 mm was formed by injection molding. 1. LCP resin LAPEROS (product name) LCP E130i (glass fiber 30%) 2. PPS resin DURAFIDE (product name) PPS 1140A6 (glass fiber 40%) 3. PBT resin DURANEX (product name) PBT 733LD (glass fiber 30%) [Molding conditions] ·LCP resin Cylinder temperature CT350℃ Mold temperature 100℃ Injection speed 1m / min PPS resin, cylinder temperature CT320℃, mold temperature 140℃, injection speed 1m / min PBT resin Cylinder temperature CT260℃ Mold temperature 80℃ Injection speed 1m / min

[0029] <Formation of burrs on resin components: Laser processing> Using a Keyence laser marker: MD-X1520, laser light with a wavelength of 1064 nm was irradiated onto any 20 mm x 20 mm area of ​​the surface to be plated of the injection-molded test specimen, forming grid-like grooves with a width of 80 μm, length of 20 mm, depth of 10 μm, and pitches of 200, 300, and 500 μm.

[0030] <Measurement of burr height a and spacing b> The measurements were made using a laser microscope. <Test specimen preparation: plating process> The resin member with the grooves formed therein was plated by vacuum deposition (aluminum plating) to form a plated test piece. The plating thickness was 80 nm.

[0031] <Adhesion test: Cross-cut peel test (cross-cut method)> In accordance with JIS K-5600-5-6, a cutter knife was used to make six scratches at 1 mm intervals in the vertical and horizontal directions on the plated surface of the plated specimen. 25 A grid of 1 mm squares was created, and commercially available cellophane tape was attached to the grid and rubbed well with a finger to adhere it to the painted surface. One end of the cellophane tape was then pinched with the fingers and peeled off in one go, and the peeling condition of the plated surface was observed. The test was carried out in an atmosphere of 23°C and 50% RH. Of the JIS K-5600-5-6 classification of 0 to 5 points, a score of 2 or less was considered to be a pass. The results are shown in Table 1.

[0032] [Table 1]

[0033] The results of Table 1 are graphed in Figure 2. The relationship between a (horizontal axis, unit μm) and b (vertical axis, unit μm) is shown in the graph, with pass marked with a and fail marked with an x. The straight line in Figure 2 is the equal sign mathematical expression in formula (1). As can be seen from these results, adhesion is good within the range that satisfies the relationship in formula (1).

[0034] Equation (1) is a regression equation derived from five critical points from experimental data, and the correlation coefficient is greater than 85%. [Explanation of symbols]

[0035] a Burr height b Groove spacing c Width of groove opening d Groove pitch

Claims

1. A resin member for aluminum plating, the resin member having a surface to be plated with a plurality of grooves having a depth of 1 to 15 μm, a spacing b between the plurality of grooves being 10 to 500 μm, the grooves having burrs around openings with a height a of 5 to 30 μm, and the height a of the burrs and the spacing b between the plurality of grooves being related by the following formula (1): Formula (1) b≦35a-24 The resin member is formed from any resin selected from the group consisting of polybutylene terephthalate, polyphenylene sulfide, and liquid crystal polymer.

2. 2. The resin member according to claim 1, wherein the width c of the opening of the groove is 50 to 200 μm.

3. A method for producing a plated resin member by plating a resin member with aluminum, the method comprising the steps of: forming, on a surface to be plated of the resin member, a plurality of grooves each having a depth of 1 to 15 μm, the plurality of grooves having a spacing b of 10 to 500 μm, the grooves having burrs with a height a of 5 to 30 μm around openings, and the height a of the burrs satisfying the relationship between the spacing b of the plurality of grooves and the following formula (1) by irradiating the surface with laser light; Formula (1) b≦35a-24 The method for producing a plated resin member, wherein the resin member is made of any resin selected from the group consisting of polybutylene terephthalate, polyphenylene sulfide, and liquid crystal polymer.

Citation Information

Patent Citations

  • Plastic film with metallic gloss and its manufacture

    JP1990150344A

  • Metal vapor deposition plastic film

    JP2005007738A

  • Grooved resin molded article

    JP2015091642A

  • Metallic material joined with dissimilar material having airtightness in phase boundary between dissimilar material and metallic material, material joined with dissimilar material having airtightness in phase boundary between dissimilar materials

    JP2016132131A

  • Method of manufacturing plating film coated body, and pretreatment liquid

    JP2019131839A