Positive electrode active material for lithium secondary batteries
A lithium secondary battery active material with directed lithium ion diffusion paths and structured layers addresses thermal safety and energy density issues by enhancing conductivity and stability, improving battery performance.
Patent Information
- Application Number
- JP2021162233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-08-07
- Filing Date
- 2021-09-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2035-01-21
AI Technical Summary
Lithium-ion batteries face issues with thermal safety and low energy density due to unstable crystal structures during charging and discharging, and existing compositions fail to provide continuous metal composition gradients, leading to interfacial resistance and reduced lithium diffusion.
A positive electrode active material with a specific directionality of lithium ion diffusion paths within primary particles, forming a continuous concentration gradient and structured layers to enhance lithium ion conductivity and stability.
The solution improves lithium ion conduction speed, reduces crystal structure collapse, and enhances cycle characteristics, capacity, and output of lithium secondary batteries.
Smart Images

Figure 0007565896000003 
Figure 0007565896000004 
Figure 0007565896000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery and a lithium secondary battery including the same, and more particularly, to a positive electrode active material for a lithium secondary battery, characterized in that lithium ion diffusion paths in primary particles and secondary particles of the positive electrode active material having a layered structure are formed with directionality in a specific direction, and a lithium secondary battery including the same. [Background technology]
[0002] Recently, interest in energy storage technology has been increasing. As the fields of application are expanding to include mobile phones, camcorders, and notebook computers, as well as the energy of electric vehicles, efforts in the research and development of electrochemical devices are gradually being made concrete. Electrochemical devices are the field that has been attracting the most attention in this regard, and among them, the development of secondary batteries that can be charged and discharged is the focus of attention.
[0003] Among the secondary batteries currently in use, lithium-ion batteries, developed in the early 1990s, have been widely used as power sources for portable devices since their introduction in 1991 as small, lightweight, and large-capacity batteries. Lithium secondary batteries have been attracting attention due to their advantages of higher operating voltage and significantly higher energy density compared to conventional batteries that use aqueous electrolytes, such as Ni-MH, Ni-Cd, and sulfuric acid-lead batteries. In particular, research into hybrid power sources for electric vehicles that combine internal combustion engines and lithium secondary batteries has been actively conducted in the United States, Japan, Europe, and other countries recently.
[0004] However, although the use of lithium-ion batteries is being considered for large batteries for electric vehicles from the perspective of energy density, nickel-metal hydride batteries are still being used from the perspective of safety. In lithium-ion batteries used for electric vehicles, the most immediate problems are high cost and safety. In particular, cathode active materials such as LiCoO2 and LiNiO2 that are currently commercialized and in use will undergo a rapid structural change when a battery in an overcharged state is heated to 200 to 270 °C. Due to such a structural change, the reaction in which oxygen in the lattice is released proceeds, and the crystal structure is unstable due to de-lithiation during charging, and it has the disadvantage of very poor thermal properties.
[0005] To improve this, attempts have been made to partially replace nickel with transition metal elements to shift the heat generation start temperature slightly to the higher temperature side or to prevent sudden heat generation. In the case of the LiNi 1-x Co x O2 (x = 0.1 - 0.3) material, excellent charge-discharge characteristics and life characteristics were shown, but the problem of thermal safety could not be solved. Also, the composition of Li-Ni-Mn-based composite oxides in which Mn with excellent thermal safety is partially substituted at the Ni site or Li-Ni-Mn-Co-based composite oxides substituted with Mn and Co, and the technology related to their production are widely known. Recently, Japanese Patent Application No. 2000-227858 disclosed a new concept cathode active material that forms a solid solution by uniformly dispersing a compound of Mn and Ni at the atomic level, rather than the concept of partially substituting transition metals in LiNiO2 and LiMnO2.
[0006] According to European Patent No. 0918041 and US Patent No. 6,040,090 regarding the composition of Li-Ni-Mn-Co-based composite oxides in which Ni is substituted with Mn and Co, LiNi 1-x Co x Mn y O2 (0 < y ≦ 0.3) has improved thermal safety compared to existing materials composed only of Ni and Co, but still could not solve the thermal safety problem of the Ni system.
[0007] In order to overcome these shortcomings, a patent for lithium transition metal oxides having a concentration gradient of metal composition has been proposed in Korean Patent Application No. 10-2005-7007548. However, this method can synthesize different metal compositions in the inner layer and the outer layer during synthesis, but the metal composition does not change continuously and gradually in the produced positive electrode active material. Although a gradual gradient of the metal composition can be achieved by the heat treatment process, an interface resistance occurs between the inner layer and the outer layer, which can act as a resistance that inhibits the diffusion of lithium within the particles, and this can lead to a decrease in life characteristics. In addition, since the composition of the inner layer is LCO, Corich NCM, or NCM with a nickel content of 60% or less, and the total nickel content is also low, it is difficult to realize high capacity.
[0008] In addition, since the powder synthesized by this invention does not use ammonia as a chelating agent, the tap density of the powder is low, and it is not suitable for use as a positive electrode active material for lithium secondary batteries, which require high energy density. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] US Patent Application Publication No. 2014 / 0158932 [Patent Document 2] JP 2002-279985 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0010] In order to solve the above problems, the present invention aims to provide a new structure of a positive electrode active material for a lithium secondary battery, in which the lithium ion diffusion path in the primary particles and the secondary particles of the positive electrode active material having a layered structure shows a specific direction. Another object of the present invention is to provide a lithium secondary battery including the positive electrode active material for lithium secondary batteries according to the present invention. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides a lithium-ion-diffusion battery comprising spherical secondary particles formed by agglomeration of primary particles, and a lithium ion diffusion path in the primary particles, i.e., a layered structure. a-axis The present invention provides a positive electrode active material for a lithium secondary battery, characterized in that a secondary particle is formed in the central direction.
[0012] 6 and 7 are schematic diagrams showing the structures of the primary particles and secondary particles of the positive electrode active material for lithium secondary batteries according to the present invention. As shown in FIG. 6 and FIG. 7, the positive electrode active material for lithium secondary batteries according to the present invention has a lithium ion diffusion path in the primary particles, that is, a in the layer structure. The axis They are characterized by being formed in parallel and exhibiting directionality toward the center of the secondary particles.
[0013] The positive electrode active material for a lithium secondary battery according to the present invention is characterized in that the aspect ratio of the primary particles is 1 or more, and the lithium ion diffusion path within the primary particles is formed in the long axis direction of the particles. That is, in the positive electrode active material for a lithium secondary battery according to the present invention, the lithium ion diffusion path is formed in the long axis direction, and when lithium ions move within the primary particles of the positive electrode active material during charging and discharging, they move within the primary particles in the horizontal axis direction, which has a relatively narrow area, so that the area where the crystal structure collapses due to continued charging and discharging is relatively small, resulting in structural stability.
[0014] The positive electrode active material for a lithium secondary battery according to the present invention is characterized in that the aspect ratio is 1 or more, and the area occupied by primary particles in which a lithium ion diffusion path within the particle is formed in the longitudinal direction of the particle is 20% or more of the total area.
[0015] In the positive electrode active material for a lithium secondary battery according to the present invention, the aspect ratio is defined as L / W (L major axis, W shortened axis) when the particles are rectangular as shown in FIG. 6, and is defined as L / (W1+W2) / 2 when the horizontal axis length is W1, W2.
[0016] The positive electrode active material for a lithium secondary battery according to the present invention is characterized in that the area occupied by the primary particles, in which the lithium ion diffusion path is directed toward the center of the secondary particle, is 40% or more of the total particle area. The positive electrode active material for a lithium secondary battery according to the present invention is characterized in that the lithium ion diffusion path in the primary particle is inclined within ±45° from the center of the secondary particle. That is, in the positive electrode active material for a lithium secondary battery according to the present invention, the lithium ion diffusion path in the primary particle is directed toward the center of the secondary particle, but is not mechanically arranged toward the center of the secondary particle, but shows a degree of freedom of arrangement within ±45° from the center of the secondary particle.
[0017] In the positive electrode active material for a lithium secondary battery according to the present invention, the primary particles are formed with a directionality toward the center of the entire particle, a lithium ion diffusion path within the primary particles is formed toward the center of the entire particle, and the lithium ion diffusion path from the surface to the center of the secondary particle has a one-dimensional or two-dimensional tunnel structure.
[0018] Such particles may have a primary needle-like, plate-like, rectangular, inclined rectangular or cylindrical shape with different aspect ratios.
[0019] Such lithium ion diffusion pathways not only increase the lithium ion conduction rate and provide high lithium ion conductivity, but also improve cycle characteristics by preventing the crystal structure from being easily destroyed even after repeated charging and discharging.
[0020] In addition, the positive electrode active material for a lithium secondary battery according to the present invention has low charge transfer resistance, diffusion, migration, and convection between the active material particles and the lithium ions or electrolyte due to the lithium ion diffusion path formed in a one-dimensional or planar tunnel structure in a linear path, and therefore the impedance inside the battery can be significantly reduced.
[0021] In the positive electrode active material for a lithium secondary battery according to the present invention, The secondary particles are A core layer represented by the following chemical formula 1 and having a constant transition metal concentration; a concentration gradient layer formed on the outer periphery of the core layer, in which the concentration of one or more transition metals changes continuously to show a concentration gradient; and a surface layer, which is represented by the following Chemical Formula 2 and is formed on the outer periphery of the concentration gradient layer and has a constant transition metal concentration.
[0022] <Chemical formula 1>Li x Ni 1-a-b-c Co a Mn b Me c O 2-y X y (In the above formula 1, 0.9≦x≦1.15, 0≦a≦0.20, 0≦b≦0.20, 0≦c≦0.1, 0≦y≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof, and X is at least one element or molecule selected from anions such as F, BO3, PO4, etc.) <Chemical formula 2>Li x Ni 1-a-b-c Co a Mn b Me c O 2-y X y (In the above formula 2, 0.9≦x≦1.15, 0≦a≦0.50, 0≦b≦0.6, 0≦c≦0.2, 0≦y≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof, and X is at least one element or molecule selected from anions such as F, BO3, PO4, etc.) In the positive electrode active material for a lithium secondary battery according to the present invention, the surface layer has a thickness of 0.05 to 2.0 μm.
[0023] In the positive electrode active material for a lithium secondary battery according to the present invention, the primary particles of the concentration gradient layer are characterized in that the lithium ion diffusion path is directed toward the center of the secondary particles.
[0024] The present invention also provides a lithium secondary battery including the positive electrode active material for lithium secondary batteries according to the present invention. Effect of the Invention
[0025] In the positive electrode active material for a lithium secondary battery according to the present invention, the lithium ion diffusion path within the primary particles is formed with directionality such that it faces the center of the particle, and therefore, the absorption and release of lithium ions into the primary particles is facilitated, and the capacity, output, and life characteristics of a battery including the positive electrode active material for a lithium secondary battery according to the present invention are greatly improved. [Brief description of the drawings]
[0026] [Figure 1] 1 shows SEM photographs of positive electrode active material particles produced in Examples 1 to 5 of the present invention and Comparative Example 1. [Diagram 2] 1 shows the results of measuring SEM photographs of fracture surfaces of positive electrode active material particles produced in Examples 1 to 5 of the present invention and Comparative Example 1. [Diagram 3] 1 shows the results of measuring the pattern and structure of primary particles in a particle of Example 5 of the present invention using a TEM. [Figure 4] 1 shows the results of measuring the pattern and structure of primary particles in a particle of Comparative Example 1 of the present invention using a TEM. [Diagram 5] 1 shows the results of measuring the internal composition of the particles produced in Example 3 of the present invention using EDX. [Figure 6] 1A is a schematic diagram showing the layered structure of a positive electrode active material for a lithium secondary battery according to the present invention, and FIG. 1B is a schematic diagram showing the cross-sectional pattern of a secondary particle and the lithium ion diffusion path of a primary particle. [Figure 7] 1 shows a schematic cross-sectional view of a secondary particle according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0028] <Example 1> In the first step, 20 L of distilled water and 1000 g of ammonia as a chelating agent were added to a co-precipitation reactor (rotating motor output of 80 W or more) having an internal volume of 100 L, and the temperature inside the reactor was maintained at 40°C to 50°C while stirring at a motor speed of 300 rpm to 1000 rpm.
[0029] In the second stage, a first precursor aqueous solution of 2.5M concentration, in which nickel sulfate, cobalt sulfate, and manganese sulfate were mixed in a molar ratio of 80:20:0, was continuously fed into the reactor at 2.2L / hr, and ammonia aqueous solution of 28% concentration was continuously fed into the reactor at 0.15L / hr. In addition, a sodium hydroxide aqueous solution of 25% concentration was fed to adjust the pH so that the pH was maintained at 11.3 to 11.4. The impeller speed was adjusted to 300 rpm to 1000 rpm. 38 L of the first precursor aqueous solution, ammonia aqueous solution, and sodium hydroxide solution were continuously fed into the reactor.
[0030] In the third step, a 2.5M concentration aqueous solution for forming a concentration gradient layer was prepared by mixing nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 35:20:45, and the volume of the first precursor aqueous solution of 2.5M concentration prepared in the second step by mixing nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 80:20:0 was fixed to 10L in another agitator other than the reactor, and then the second precursor aqueous solution was prepared by stirring while being added at a rate of 2.2L / hr, and was simultaneously introduced into the reactor. The aqueous solution for forming the concentration gradient layer was introduced into the reactor while being mixed until the nickel sulfate, cobalt sulfate, and manganese sulfate molar ratio in the second precursor aqueous solution became the shell layer concentration of 40:20:40, and a 28% concentration aqueous ammonia solution was added at a rate of 0.08L / hr, and the sodium hydroxide solution was maintained so that the pH was 11.3 to 11.4. At this time, the second aqueous precursor solution, the aqueous ammonia solution, and the sodium hydroxide solution were added in a total volume of 24 L.
[0031] Next, in the fourth step, the third precursor aqueous solution, which was a mixture of nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 40:20:40, was added to the reactor until the reactor volume reached 8 L. After the reaction was completed, a spherical nickel manganese cobalt composite hydroxide precipitate was obtained from the reactor.
[0032] The precipitated composite metal hydroxide was filtered, washed with pure water, and then dried in a hot air dryer at 100° C. for 12 hours. The inner core layer was (Ni 0.8 Co 0.20 )(OH)2, and the outer shell layer is (Ni 0.80 Co 0.20 )(OH)2 to (Ni 0.4 Co 0.2 Mn 0.4 The precursor powder was obtained in the form of a metal composite oxide having a continuous concentration gradient from 0.1 to 1.0.
[0033] The precursor metal composite hydroxide and lithium hydroxide (LiOH.HO) were mixed in a molar ratio of 1:1.00 to 1.10, and then heated at a temperature increasing rate of 2°C / min. The mixture was then heat-treated at 550°C for 10 hours and then sintered at 750°C for 20 hours. The inner core layer was formed of Li(Ni 0.80 Co 0.20 )O2, and the outer shell layer is Li(Ni 0.80 Co 0.20 )O2 to Li(Ni 0.4 Co 0.2 Mn 0.4 )O2.
[0034] <Example 2> The composition of the inner core layer is Li(Ni 0.70 Co 0.30 )O2, and the composition of the outer shell layer is Li(Ni 0.70 Co 0.30 )O2 to Li(Ni 0.4 Co 0.2 Mn 0.4 A positive electrode was prepared in the same manner as in Example 1, except that the positive electrode had a constant concentration gradient continuously from 0 to 100.
[0035] <Example 3> The composition of the inner core layer is Li(Ni 0.80 Co 0.20 )O2, and the composition of the outer shell layer is Li(Ni 0.80 Co 0.20 )O2 to Li(Ni 0.35 Co 0.35 Mn 0.30 A positive electrode was prepared in the same manner as in Example 1, except that the positive electrode had a constant concentration gradient continuously from 0 to 100.
[0036] <Example 4> The composition of the inner core layer is Li(Ni 0.90 Co 0.10 )O2, and the composition of the outer shell layer is Li(Ni 0.90 Co 0.10 )O2 to Li(Ni 0.33 Co 0.33 Mn 0.33A positive electrode was prepared in the same manner as in Example 1, except that the positive electrode had a constant concentration gradient continuously from 0 to 100.
[0037] <Example 5> Composition of the inner core layer Li(Ni 0.97 Co 0.03 )O2 and the composition of the outer shell layer Li(Ni 0.97 Co 0.03 )O2 to Li(Ni 0.5 Co 0.2 Mn 0.3 A positive electrode was prepared in the same manner as in Example 1, except that the positive electrode had a constant concentration gradient continuously from 0 to 100.
[0038] <Comparative Example 1> After adding 60 L of distilled water and 1000 g of ammonia as a chelating agent to a coprecipitation reactor (volume 70 L), the temperature in the reactor was maintained at 40-50°C, and the motor speed was set to 6000 rpm to stir. Nitrogen gas was continuously supplied to the reactor at a flow rate of 3 L / min. Next, a 1M concentration precursor aqueous solution in which nickel sulfate, cobalt sulfate, and manganese sulfate were mixed in a molar ratio of 8:1:1 was continuously fed into the reactor at 6.5 L / hr, and a 28% concentration ammonia aqueous solution was continuously fed into the reactor at 0.6 L / hr. In addition, a 25% concentration sodium hydroxide aqueous solution was continuously fed to the liquid surface in the reaction tank at 1.5-2.0 L / hr to adjust the pH to 11-12. The temperature of the reaction solution was maintained at 50±2°C. After 30 hours had passed since the inside of the reactor had returned to normal, the hydroxide particles discharged from the overflow pipe were continuously collected and washed with water, then dried in a hot air dryer at 100°C for 12 hours to obtain (Ni 0.8 Co 0.1 Mn 0.1 A precursor powder in the form of a metal complex hydroxide having the formula (III)(OH)2 was obtained.
[0039] The metal composite hydroxide and lithium hydroxide (LiOH.H2O) were mixed in a molar ratio of 1:1.00 to 1.10, and then heated at a temperature increasing rate of 2°C / min. Then, the mixture was heat-treated at 550°C for 10 hours, and then calcined at 750°C for 20 hours to obtain a positive electrode active material powder.
[0040] <Experimental example: SEM photo measurement> The positive electrode active material particles and their fracture surfaces prepared in Examples 1 to 5 and Comparative Example 1 were photographed using SEM, and the results are shown in FIGS.
[0041] It can be seen from FIG. 1 that the positive electrode active material particles prepared in Examples 1 to 5 and Comparative Example 1 are spherical secondary particles formed by agglomeration of primary particles.
[0042] In FIG. 2, which is an SEM photograph of a fracture surface of a particle, it can be seen that in the case of the particles produced in Examples 1 to 5 of the present invention, the aspect ratio of the primary particles is 1 or more, and the primary particles grow with a directionality toward the center of the particle in the long axis, i.e., the long direction, and a lithium conduction path is formed from the particle surface to the particle center in a one-dimensional or two-dimensional tunnel structure, whereas in the case of the comparative example, the aspect ratio of the primary particles is much shorter than that of the Examples, and no directionality of the primary particles is observed inside the secondary particles in an irregular (random) form.
[0043] <Experimental example: TEM photo measurement> The patterns and structures of the primary particles in the particles of Example 5 and Comparative Example 1 were measured using TEM, and the results are shown in FIG. 3 and FIG.
[0044] In FIG. 3, it can be seen that the primary particles of the particles prepared in Example 5 of the present invention are formed with directionality toward the center, and the lithium ion conduction paths within the primary particles are formed parallel to the center of the secondary particles.
[0045] On the other hand, in the case of the particles prepared in Comparative Example 1 of the present invention, as shown in FIG. 4, it can be seen that the lithium ion conductive paths in the primary particles are irregularly formed without directionality.
[0046] <Experimental example: EDX photo measurement> The composition inside the particles produced in Example 3 was measured using EDX, and the results are shown in FIG.
[0047] In FIG. 5, it can be seen that the particles produced according to the embodiment of the present invention show a concentration gradient of nickel, cobalt, and manganese from the center to the surface.
[0048] <Experimental example: Particle characteristic measurement> The compositions and particle size distributions of the lithium metal composite oxides prepared in Examples 1 to 5 and Comparative Example 1 were measured using a particle size analyzer and are shown in Table 1 below.
[0049] For composition analysis, a certain amount (about 2 g) of the produced lithium metal composite oxide was accurately weighed (to the nearest 0.1 mg), transferred to a glass beaker, and completely decomposed on a hot plate after adding aqua regia (HCl:HNO3=3:1).
[0050] Using an inductively coupled plasma atomic emission spectroscope (ICP-AES, Perkin-Elmer7300), the intensity of three types of standard solutions prepared using a standard solution (Inorganic Venture, 1000mg / kg) at element-specific wavelengths of Li / Ni / Co / Mn was measured to create a calibration curve, and then the pretreated sample solution and a blank sample were introduced into the instrument, and the intensity of each was measured to calculate the actual intensity. The concentration of each component was calculated in comparison with the created calibration curve, and normalized so that the total was a theoretical value, thereby analyzing the composition of the prepared lithium metal composite oxide.
[0051] [Table 1]
[0052] <Manufacturing example: Battery manufacturing> The positive electrode active materials prepared in Examples 1 to 5 and Comparative Example 1 were mixed with Super-P as a conductive agent and polyvinylidene fluoride (PVdF) as a binder in a weight ratio of 92:5:3 to prepare a slurry. The slurry was uniformly coated on an aluminum foil having a thickness of 15 μm and dried in a vacuum at 135° C. to prepare a positive electrode for a lithium secondary battery.
[0053] A coin-type battery was manufactured by a known manufacturing process using the positive electrode, lithium foil as a counter electrode, a porous polyethylene film (Celgard, LLC., Celgard 2300 (registered trademark), thickness: 25 μm) as a separator, and a liquid electrolyte in which LiPF6 was dissolved at a concentration of 1.15 M in a solvent in which ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7.
[0054] <Experimental example: Battery characteristic measurement> The initial capacity, initial efficiency, rate characteristics and life characteristics of the batteries prepared using the active materials prepared in Examples 1 to 5 and Comparative Example 1 were measured, and the results are shown in Table 2 below.
[0055] In Table 2 below, it can be seen that in the case of the battery containing the active material produced in the embodiment of the present invention, the battery characteristics are significantly improved compared to the comparative example.
[0056] [Table 2] [Industrial Applicability]
[0057] As described above, the positive electrode active material for a lithium secondary battery according to the present invention is formed with a directionality such that the lithium ion diffusion path in the primary particles is oriented toward the center of the particles, and therefore, the lithium ions can be easily absorbed and released into the primary particles, and the capacity, output, and life characteristics of a battery including the positive electrode active material for a lithium secondary battery according to the present invention are greatly improved, which can be said to be very useful. Hereinafter, embodiments of the present invention will be described. Article 1. The secondary particles are formed by agglomeration of primary particles, A lithium ion diffusion path formed inside the primary particle as measured by TEM is formed toward the center of the secondary particle, and The secondary particles are a core layer having a constant transition metal concentration; a concentration gradient layer formed on the outer periphery of the core layer, in which the concentration of one or more transition metals changes continuously to show a concentration gradient; a surface layer formed on the outer periphery of the concentration gradient layer and having a constant concentration of the transition metal; The aspect ratio of the primary particles is 1 or more, and a lithium ion diffusion path formed inside the primary particles is formed in a major axis direction of the primary particles, the primary particles are formed with a directionality toward the center of the entire secondary particle, a lithium ion diffusion path formed inside the primary particle is formed toward the center of the entire secondary particle, and the lithium ion diffusion path from the surface to the center of the secondary particle has a one-dimensional or two-dimensional tunnel structure; The core layer of the secondary particle is represented by the following chemical formula (1): The surface layer of the secondary particle is represented by the following chemical formula (2): <Chemical formula 1>Li x1 Ni 1-a1-b1-c1 Co a1 Mn b1 Me c1 O 2-y1 X y1 (wherein, in the formula 1, 0.9≦x1≦1.15, 0≦a1≦0.20, b1=0, 0≦c1≦0.1, 0≦y1≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba, and combinations thereof, and X is at least one element or molecule selected from the group consisting of anions of F, BO3, and PO4), and <Chemical formula 2>Li x2 Ni 1-a2-b2-c2 Co a2 Mn b2 Me c2 O 2-y2 X y2 (wherein in the above formula 2, 0.9≦x2≦1.15, 0≦a2≦0.50, 0.3≦b2≦0.6, 0≦c2≦0.2, 0≦y2≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof, and X is at least one element or molecule selected from the group consisting of anions of F, BO3, and PO4). In the formula, a1+b1+c1 <a2+b2+c2であり、 The thickness of the surface layer is 0.05 to 2.0 μm. A positive electrode active material for a lithium secondary battery. Article 2. Item 1. The positive electrode active material for a lithium secondary battery according to item 1, characterized in that the aspect ratio is 1 or more, and the area occupied by the primary particles in which the lithium ion diffusion paths formed inside the primary particles are formed in the major axis direction of the primary particles is 20% to 100% of the total surface area of the secondary particles. Article 3. Item 1. A positive electrode active material for a lithium secondary battery, characterized in that the lithium ion diffusion path formed inside the primary particle is inclined within ±45° toward the center of the secondary particle. Article 4. Item 1. The positive electrode active material for a lithium secondary battery according to item 1, characterized in that the area occupied by the primary particles in which the lithium ion diffusion path is directed toward the center of the secondary particles is 40% to 100% of the surface area of the secondary particles. Article 5. Item 1. A positive electrode active material for a lithium secondary battery, characterized in that the lithium ion diffusion path formed inside the primary particles in the concentration gradient layer is directed toward the center of the secondary particles. Article 6. Item 1. The positive electrode active material for a lithium secondary battery according to item 1, wherein the primary particles are needle-like, plate-like, rectangular, inclined rectangular, or cylindrical. Article 7. Item 1. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to item 1. Article 8. Item 2. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries. Article 9. Item 3. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to item 3. Article 10. Item 4. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries. Article 11. Item 6. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to item 5. Article 12. Item 7. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to item 6. Further embodiments of the present invention are described below. Article A-1. The secondary particles are formed by agglomeration of primary particles, A lithium ion diffusion path formed inside the primary particle as measured by TEM is formed toward the center of the secondary particle, and The secondary particles are a core layer having a constant transition metal concentration; a concentration gradient layer formed on the outer periphery of the core layer, in which the concentration of one or more transition metals changes continuously to show a concentration gradient; a surface layer formed on the outer periphery of the concentration gradient layer and having a constant concentration of the transition metal; The aspect ratio of the primary particles is 1 or more, and a lithium ion diffusion path formed inside the primary particles is formed in a major axis direction of the primary particles, the primary particles are formed with a directionality toward the center of the entire secondary particle, a lithium ion diffusion path formed inside the primary particle is formed toward the center of the entire secondary particle, and the lithium ion diffusion path from the surface to the center of the secondary particle has a one-dimensional or two-dimensional tunnel structure; The core layer of the secondary particle is represented by the following chemical formula (1): The surface layer of the secondary particle is represented by the following chemical formula (2): <Chemical formula 1>Li x1 Ni 1-a1-b1-c1 Co a1Mn b1 Me c1 O 2-y1 X y1 (wherein, in the formula 1, 0.9≦x1≦1.15, 0≦a1≦0.20, b1=0, 0≦c1≦0.1, 0≦y1≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba, and combinations thereof, and X is at least one element or molecule selected from the group consisting of anions of F, BO3, and PO4), and <Chemical formula 2>Li x2 Ni 1-a2-b2-c2 Co a2 Mn b2 Me c2 O 2-y2 X y2 (wherein in the above formula 2, 0.9≦x2≦1.15, 0≦a2≦0.50, 0≦b2≦0.60, 0≦c2≦0.2, 0≦y2≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof, and X is at least one element or molecule selected from the group consisting of anions of F, BO3, and PO4), The thickness of the surface layer is 0.05 to 2.0 μm. A positive electrode active material for a lithium secondary battery. Article A-2. The positive electrode active material for lithium secondary batteries according to clause A-1, characterized in that the aspect ratio is 1 or more, and the area occupied by the primary particles in which the lithium ion diffusion paths formed inside the primary particles are formed in the major axis direction of the primary particles is 20% or more of the total surface area of the secondary particles. Article A-3. The positive electrode active material for a lithium secondary battery described in clause A-1, characterized in that the lithium ion diffusion path formed inside the primary particle is inclined within ±45° toward the center of the secondary particle. Article A-4. The positive electrode active material for lithium secondary batteries according to clause A-1, characterized in that the area occupied by the primary particles in which the lithium ion diffusion path is directed toward the center of the secondary particles is 40% or more of the surface area of the secondary particles. Article A-5. The positive electrode active material for a lithium secondary battery described in clause A-1, characterized in that the lithium ion diffusion path formed inside the primary particle in the concentration gradient layer is directed toward the center of the secondary particle. Article A-6. The positive electrode active material for a lithium secondary battery according to clause A-1, characterized in that the primary particles are needle-shaped, plate-shaped, rectangular, inclined rectangular, or cylindrical. Article A-7. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to clause A-1. Article A-8. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to clause A-2. Article A-9. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to clause A-3. Article A-10. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to clause A-4. Article A-11. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to clause A-5. Article A-12. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to clause A-6.
Claims
1. The secondary particles are formed by agglomeration of primary particles, A lithium ion diffusion path inside the primary particle is formed toward the center of the secondary particle, the secondary particles include a core layer having a constant concentration of a transition metal, a concentration gradient layer formed around the core layer and having one or more transition metals whose concentrations change continuously to exhibit a concentration gradient, and a surface layer formed on the outer periphery of the concentration gradient layer and having a constant concentration of the transition metal, The aspect ratio of the primary particles is 1 or more, and a lithium ion diffusion path inside the primary particles is formed in a major axis direction of the primary particles, an area occupied by the primary particle, in which a lithium ion diffusion path inside the primary particle is formed in a major axis direction of the primary particle, is 20% or more of a cross-sectional area passing through a center of the secondary particle, an area occupied by the primary particle along which the lithium ion diffusion path extends toward the center of the secondary particle is 40% or more of a cross-sectional area passing through the center of the secondary particle; the primary particles are formed with a directionality toward the center of the entire particle, a lithium ion diffusion path inside the primary particles is formed toward the center of the entire secondary particle, and the lithium ion diffusion path from the surface to the center of the secondary particle has a one-dimensional or two-dimensional tunnel structure; The secondary particles are The following chemical formula 1 <Chemical formula 1> Li x1 Ni 1-a1-b1-c1 Co a1 Mn b1 Me c1 O 2-y1 X y1 (wherein, in Chemical Formula 1, 0.9≦x1≦1.15, 0≦a1≦0.20, b1=0, 0≦c1≦0.1, 0≦y1≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof, and X is at least one element or molecule selected from the group consisting of anions of F, BO3, and PO4), and the concentration of the transition metal is constant; a concentration gradient layer formed on the outer periphery of the core layer, the concentration of one or more transition metals being continuously changed to exhibit a concentration gradient; The following chemical formula 2 <Chemical formula 2> Li x2 Ni 1-a2-b2-c2 Co a2 Mn b2 Me c2 O 2-y2 X y2 (wherein in Formula 2, 0.9≦x2≦1.15, 0≦a2≦0.50, 0≦b2≦0.6, 0≦c2≦0.2, 0≦y2≦0.1, Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof, and X is at least one element or molecule selected from the group consisting of anions of F, BO3, and PO4), and the transition metal concentration is constant in a surface layer formed on the outer periphery of the concentration gradient layer, A positive electrode active material for a lithium secondary battery, characterized in that, in Chemical Formula 1 and Chemical Formula 2, the difference between the Ni content of the core layer and the Ni content of the surface layer of the secondary particle is 0.3 or more.
2. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the lithium ion diffusion path inside the primary particle is inclined within ±45° from the center direction of the secondary particle.
3. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the surface layer has a thickness of 0.05 to 2.0 μm.
4. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein a lithium ion diffusion path inside the primary particle in the concentration gradient layer is directed toward the center of the secondary particle.
5. The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the primary particles are needle-like, plate-like, rectangular, inclined rectangular, or cylindrical.
6. A lithium secondary battery comprising the positive electrode active material for lithium secondary batteries according to any one of claims 1 to 5.
Citation Information
Patent Citations
Positive electrode active material for non-aqueous lithium secondary battery and the non-aqueous lithium secondary battery using the active material
JP2002279985A
Positive electrode active material of lithium secondary battery, and lithium secondary battery
JP2014067546A
Positive electrode active material precursor for lithium secondary battery, positive electrode active material manufactured by using thereof, and lithium secondary battery including same
US20140158932A1