Methods for Preparing Silicone for 3D Printing
Heat-enhanced radical curing and silanol condensation curing methods address the challenges of incomplete curing and mechanical inconsistency in 3D printed silicones, ensuring uniform properties and complete curing in large structures.
Patent Information
- Application Number
- JP2022580866
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-10
- Filing Date
- 2021-07-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-07-09
AI Technical Summary
Silicones, particularly polysiloxanes, are challenging to use in additive manufacturing due to high viscosity issues and lack of spatial control in crosslinking methods, leading to incomplete curing and mechanical property inconsistencies, especially in large structures.
Employing heat-enhanced radical curing or silanol condensation curing steps in the post-curing process for 3D printed silicone, ensuring uniform curing and isotropic mechanical properties.
Achieves complete curing and consistent mechanical properties across large silicone structures, with improved Young's modulus, elongation at break, tensile strength, and Shore A hardness values, reducing variability between surface and center measurements.
Smart Images

Figure 0007566055000004 
Figure 0007566055000005 
Figure 0007566055000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preparing 3D printed silicone that includes a non-light accelerated post-cure treatment step, an additive manufacturing composition for preparing 3D printed silicone, and 3D printed silicone articles prepared via this method. [Background technology]
[0002] Additive manufacturing, also commonly known as 3D printing, refers to a process used to create three-dimensional objects by depositing and solidifying material in various forms (e.g., layers, droplets, etc.) to obtain the entire object layer-by-layer or sequentially, or by simultaneously solidifying the entire volume to obtain the entire object in one piece.
[0003] Many materials are currently used for additive manufacturing, ranging from metals to synthetic resins. In one type of additive manufacturing, a device with a nozzle is used to deposit layers of a liquid crosslinkable material in a predetermined pattern. Examples of such additive manufacturing include 3D printing of elastomers and hydrogels, both of which require crosslinking. After depositing a layer of crosslinkable material (either as a layer or as multiple droplets forming a layer), the crosslinkable material can be crosslinked, for example, by exposure to radiation, temperature changes, or by contact with a chemical crosslinking agent, to obtain a self-supporting structure on which further layers can be deposited and crosslinked. Alternatively, the object can be monolithically formed from the crosslinkable material in a first step and monolithically crosslinked in a second step.
[0004] Silicones, including polysiloxanes, have not been widely used in the field of additive manufacturing so far due to some problems inherent to this class of chemical compounds: on the one hand, their high viscosity makes precise dosing difficult, and on the other hand, polysiloxanes are crosslinked by condensation or addition reactions, neither of which allows the spatial control essential for additive manufacturing.
[0005] US Patent No. 5,399,633 discloses a UV-curable silicone resin-organo mercaptan composition, in which the polysiloxane is functionalized with at least two aliphatically unsaturated radicals capable of reacting with a mercaptan having two or more mercapto groups, as well as a free radical photoinitiator and a free radical inhibitor. The composition is formed by mixing the components of the composition into a transparent, compatible mixture, which is then cast onto different substrates to form a coating.
[0006] Patent Document 2 discloses a crosslinkable composition for producing microlenses, which comprises a polysiloxane having an unsaturated bond group, a polysiloxane different from the aforementioned polysiloxane, a mercapto compound, a photoinitiator, and an organic solvent for dissolving the aforementioned compound. The composition is applied to a substrate as a film coating and crosslinked using radiation and heat.
[0007] US Patent No. 5,999,333 discloses a composition that forms a dry silicone gel that can act as a crosslinker / chain extender having two or more thiol groups, a free radical initiator, and a reinforcing agent such as fumed silica. The composition can be crosslinked by UV radiation or heat.
[0008] US Pat. No. 5,399,433 discloses a three-dimensional printable ink composition comprising polydimethylsiloxane (PDMS) microbeads, a PDMS precursor liquid that bonds to the microbeads to form a paste-like material, and an aqueous phase.
[0009] US Patent No. 5,399,633 discloses a two-part curable ink composition in which an olefin monomer is polymerized in an inkjet process to form a 3D printed polyolefin composition.
[0010] US Patent No. 6,399,633 discloses an additive manufacturing ink comprising a polysiloxane having multiple alkenyl groups and a crosslinker having multiple thiol groups, the polysiloxane having multiple alkenyl groups and the crosslinker having multiple thiol groups forming an emulsion with beneficial shear thinning properties.
[0011] US Patent No. 5,399,633 discloses a similar additive manufacturing ink that includes an alkenyl-derivatized polysiloxane and a crosslinker that is a mercapto-derivatized polysiloxane-based crosslinker.
[0012] In both of the previous two inventions, the additive manufacturing process includes a first step of generating a semi-finished product through UV-VIS controlled additive manufacturing, followed by a post-curing step involving UV treatment of the generated semi-finished product. The post-curing with UV light has the effect of ensuring that all monomers remaining after additive manufacturing are reacted to form the final cured product.
[0013] Although light post-curing is an effective process for transparent materials, it remains subject to a number of drawbacks. First, light has limited penetration through partially cured semi-finished products, especially colored objects. For large 3D printed silicone structures, e.g., 1 cm 3 At sizes above 100 mm, the center of the semi-finished product is therefore not subject to the action of light. This not only affects the properties of the final 3D printed silicone product, but can also affect its lifetime if uncured monomer escapes from the structure. Furthermore, light curing is a fast process and can weaken the material, as it freezes existing tensions in the molecular network formed during the curing step.
[0014] Therefore, there is a need for a method for preparing 3D printed silicone products with isotropic mechanical properties as a result of improved post-curing processing. Furthermore, large semi-finished products, e.g., 1 cm 3 There is a need for a post-cure process that can achieve complete cure of these semi-finished products.
[0015] The above problems are addressed in the present application whereby the use of a heat-accelerated free radical curing step and / or a silanol condensation curing step can be used to obtain 3D printed silicone products with improved mechanical properties. [Prior art documents] [Patent documents]
[0016] [Patent Document 1] European Patent Application Publication No. 0437247 [Patent Document 2] JP 2010-0185991 A [Patent Document 3] International Publication No. 2013 / 160252 [Patent Document 4] International Publication No. 2018 / 013779 [Patent Document 5] European Patent Application Publication No. 1942159 [Patent Document 6] International Publication No. 2019 / 053258 [Patent Document 7] Unpublished Swiss Patent Application No. 3612019 Summary of the Invention
[0017] The present invention is based on the discovery that when producing silicone articles via additive manufacturing processes, a post-cure step other than photocuring, such as either heat-accelerated radical curing or silanol condensation curing, results in uniform curing throughout the 3D printed silicone article, and therefore isotropic mechanical properties, especially for large articles of 1 cm or more.
[0018] The present invention is directed to a method for preparing 3D printed silicone, the method comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) at least one crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); and c) performing a post-cure treatment comprising at least one further curing step other than a light-accelerated cure, preferably either a heat-accelerated radical cure or a silanol condensation cure; Including, The ratio of thiol groups to alkenyl groups in the composition for layered manufacturing is in the range of 0.5:1 to 5:1.
[0019] In another aspect, the present invention is directed to an additive manufacturing composition, the additive manufacturing composition comprising: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) a thermally activatable free radical initiator (E) in an amount ranging from 0.1 to 5.0 parts by weight, preferably from 0.2 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1.
[0020] In a further aspect, the present invention is directed to an additive manufacturing composition, the additive manufacturing composition comprising: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) a condensation cure silicone blend (C1) in an amount preferably ranging from 1 to 90 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1.
[0021] In yet another aspect, the present invention is directed to a 3D printed silicone obtainable by the method of the present invention, the size of which is at least 1x1x1 mm, preferably at least 3x3x3 mm, most preferably at least 5x5x5 mm, and the Shore A hardness values measured according to ISO 7619-1 between samples taken from the surface of the cured composition and from the center of the cured composition vary by less than 10%, preferably by less than 5%, and most preferably the values are identical.
[0022] In yet another aspect, the present invention is directed to the use of a thermally activatable free radical initiator (E) in a process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, a ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1; c) a post-curing step including a heat-promoted radical curing step, in which the semi-finished product is heated at a constant temperature, preferably in the range of 50°C to 150°C, for a time period in the range of 1 to 24 hours; Including, The thermally activatable free radical initiator (E) is a) the Young's modulus, measured on a type 4 tensile specimen according to ISO 37, is within the range of 110 to 10,000% of the Young's modulus of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110 to 1,000% of the elongation at break of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110 to 500% of the tensile strength of 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; d) the tear strength, measured on a sample of test piece type C according to ASTM D624, is in the range of 110-400% of the tear strength of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; e) a Shore A hardness measured according to ISO 7619-1, the Shore A hardness being in the range of 110 to 2,500% of the Shore A hardness of a 3D printing silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; To produce 3D printed silicone having one or more of the properties of Preferably, it is present in the additive manufacturing composition of step b) in an amount ranging from 0.1 to 5.0 parts by weight, preferably from 0.2 to 3.0 parts by weight, relative to the total weight of the silicone building blocks having multiple alkenyl groups.
[0023] In a final aspect, the present invention is directed to the use of a condensation cured silicone blend (C1) in a process, said process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, a ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1; c) a post-curing step including a silanol condensation curing step, preferably consisting of exposing the semi-finished product to a relative humidity of more than 20%, preferably more than 50%, for a time period ranging from 30 minutes to 72 hours, preferably from 6 to 36 hours; Including, The condensation cured silicone blend (C1) is a) the Young's modulus measured on a type 4 tensile specimen according to ISO 37 is within the range of 110 to 10,000% of the Young's modulus of the condensation cured silicone blend (C1) or of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110 to 1,000% of the elongation at break of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same composition for additive manufacturing in the absence of a silanol condensation curing step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110 to 500% of the tensile strength of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; d) the tear strength measured on a sample of test piece type C according to ASTM D624 is in the range of 110-400% of the tear strength of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; e) a Shore A hardness measured according to ISO 7619-1, the Shore A hardness being in the range of 110 to 2,500% of the Shore A hardness of the condensation cured silicone blend (C1) or of a 3D printing silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; To produce 3D printed silicone having one or more of the properties of Preferably, it is present in the additive manufacturing composition of step b) in an amount ranging from 1 to 90 parts by weight, relative to the total weight of the silicone building blocks having multiple alkenyl groups. [Brief description of the drawings]
[0024] [Figure 1] The effect of thermal curing compared to UV / Vis curing is shown. [Diagram 2] A comparison of cure depth between UV-cured and thermally cured samples is shown. [Diagram 3] 1 shows a 3D printed ear prosthesis manufactured using composition 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] (definition) The term "additive manufacturing" as used herein refers to methods such as stereolithography, e.g., laser-based stereolithography (SLA) and digital light processing (DLP), material jetting, drop-on-demand, volumetric 3D printing, i.e., holographic laser 3D printing, and material extrusion, e.g., robocasting.
[0026] In a typical stereolithography process, a build platform is positioned in a vat or tank containing the additive manufacturing composition of the present invention at a distance of one layer height from the surface of the liquid, and a light source selectively polymerizes and solidifies the additive manufacturing composition to produce the next layer. While SLA printers use a laser source that moves over a predetermined area of some layer, DLP printers use a digital light projector that flashes a single image of each layer at a time, which can also raster larger areas for a larger build volume than the projection. The process steps are repeated until the 3D object is complete. Further post-treatment under UV / Vis light ensures that the object is fully crosslinked, which is especially needed when high mechanical and thermal properties are desired.
[0027] "Top-down" orientation refers to a printer in which the light source is placed above the tank and the build platform starts at the top of the tank and moves downward after each layer. Typically, the direction perpendicular to the 3D printed layers of the 3D object is called the z direction (or axis), and the direction parallel to the 3D printed layers of the 3D object (and thus perpendicular to the z axis) is called the xy plane. Objects in a top-down printer are built up from the top.
[0028] "Bottom-up" orientation refers to a printer in which the light source is located below a tank that has a suitable transparent bottom to allow the light source to pass through. After each layer, the cured additive manufacturing composition is detached from the bottom of the tank as the build platform moves upward. Objects in bottom-up printers are built upside down.
[0029] In a typical material jetting process, a print head deposits droplets of an additive manufacturing composition at desired locations on a build platform. A radiation source attached to the print head cures and solidifies the additive manufacturing composition to produce a first layer, and the build platform is moved down to allow the process steps to be repeated until the 3D object is complete. Droplet deposition can be done in a continuous manner, where droplets are generated by breaking a continuous stream of droplets, or by drop-on-demand, where droplets are generated when needed.
[0030] In a typical volumetric (i.e. holographic) printing method, a 3D object is generated simultaneously in one piece by projecting a hologram-like pattern of a light source onto a transparent tank containing the additive manufacturing composition, allowing the additive manufacturing composition to harden in one piece. After the 3D object is completed, excess additive manufacturing composition can be drained off to reveal the completed 3D object.
[0031] In a typical material extrusion printing process, an additive manufacturing composition is extruded through a nozzle onto a build platform or substrate, whereby the nozzle follows a predetermined path to build up a 3D object layer by layer.
[0032] The additive manufacturing composition can be used in any typical 3D printer. In one embodiment, the additive manufacturing composition can be used in an SLA or DLP printer, preferably a top-down SLA or DLP printer, where a build platform is positioned on top of a tank filled with liquid photopolymer resin, and a light source located above the tank selectively hardens and solidifies the additive manufacturing composition layer by layer (by moving the platform downward after each layer) to create the desired 3D product (upward). In another embodiment, the additive manufacturing composition can be used in volumetric or holographic 3D printing, where a 3D image, such as a laser-generated hologram, is flashed onto the additive manufacturing composition contained in the tank to create the desired 3D product in one piece.
[0033] The term "emulsion" as used in the context of the present invention refers to a stable mixture of two or more immiscible (e.g. polysiloxane) liquid components, in which (at least) one component (the dispersed phase) is dispersed in the form of fine droplets in (at least) another component (the continuous phase). It is also understood that the term "immiscible" includes predominantly or substantially immiscible phases, whereby the dispersed phase has a finite solubility in the continuous phase. The mixture may be further stabilized by the presence of additives such as emulsifiers or surfactants.
[0034] As used herein, the term "transparent" refers to the property of transmitting (without diffusion) at least 70%, preferably at least 80%, and more preferably at least 90% of incident visible light. The term "semi-transparent" refers to the property of having reduced light transmission, such as less than 60% transmission, and more preferably less than 50% transmission.
[0035] The term "silicone building block" as used herein refers to a polymerizable silicone building block that is generally used to synthesize a more extended network, as opposed to the individual monomers within these polymerizable silicone building blocks. Silicone building blocks are typically in liquid to viscous form, as opposed to the solid silicone network that results from polymerization / curing. Silicone building blocks are typically polysiloxanes, but may also be silsesquioxanes or blends that include both polysiloxanes and silsesquioxanes.
[0036] The term "polysiloxane" refers to a compound having the general formula (R)Si-(O-Si(R)) n refers to linear, branched and cyclic polyorganosiloxanes characterized by the formula O-Si(R)3, where R is H or an organic group, and n is an integer, typically 1 to 10. 9 In polyorganosiloxanes, the organic moieties can be the same (such as the methyl groups in polydimethylsiloxane or PDMS) or different within a single molecule (for example, in polydimethyldiphenylsiloxane or diphenyldimethicone).
[0037] The term "silsesquioxane" refers to a compound having the chemical formula [RSiO 1.5 ] n where R=H, alkyl, aryl, or alkoxyl. In these compounds, silicon is typically bonded to three oxygen atoms (four when R=alkoxyl) as opposed to two oxygen atoms in polysiloxanes. Silsesquioxanes may exhibit cage or polymeric structures. While cage structures are more common, they can undergo rearrangement reactions to form highly crosslinked ladder-like polymeric structures such as poly(phenylsilsesquioxane).
[0038] In the following description, many amounts are given as "parts by weight, relative to the total weight of the different components (or combinations of components)". In each case, this means that the total weight of the reference component (or combination of components) is taken as 100 parts by weight, while the component in question has a relative weight in the given range.
[0039] (Method for preparing silicone for 3D printing) The method of the present invention comprises the steps of: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) at least one crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); and c) performing a post-cure treatment comprising at least one further curing step other than a light-accelerated cure, preferably either a heat-accelerated radical cure or a silanol condensation cure; Including, The ratio of thiol groups to alkenyl groups in the composition for layered manufacturing is in the range of 0.5:1 to 5:1.
[0040] It is understood that the semi-finished product is the product obtained directly by step b) before the post-curing treatment c). Typically, a 3D model of the semi-finished product is prepared as a CAD (Computer Aided Design) file or a 3D scan. The resulting CAD data can then be converted into a format suitable for or readable by the additive manufacturing device. The 3D model of the semi-finished product usually contains all relevant information required for the additive manufacturing of the actual semi-finished product in step b). For example, the 3D model may contain information about the dimensions, structure, size, color, etc. of the semi-finished product. Furthermore, the 3D model may contain information about the orientation of the semi-finished product. In particular, the 3D model of the semi-finished product may contain information about the orientation of the actual semi-finished product relative to the additive manufacturing device or to certain components of the additive manufacturing device.
[0041] The additive manufacturing apparatus preferably comprises a radiation source for irradiating at least a portion of the additive manufacturing composition.
[0042] More preferably, the radiation source may be an LED lamp. In particular, the intensity of the LED lamp is 1 to 1000 mW / cm 2 , preferably 50 to 50 mW / cm 2 It is.
[0043] It is also preferred that the additive manufacturing of step b) is carried out by photopolymerization, the additive manufacturing being carried out by VAT photopolymerization, volumetric 3D printing, holographic laser 3D printing or any other suitable method. More preferably, the additive manufacturing is carried out by DLP or SLA VAT photopolymerization. In a particularly preferred embodiment, the photopolymerization is carried out in a top-down orientation.
[0044] The additive manufacturing apparatus preferably comprises a chamber containing the additive manufacturing composition and a platform within the chamber which is moved in the z-direction during step b), such an additive manufacturing apparatus being suitable for use in a top-down or bottom-up orientation.
[0045] Furthermore, the 3D model of step a) is preferably prepared in such a way that the stability of the semi-finished product is maximized. Such stabilization, such as mechanical stabilization or positional stabilization, especially lateral stabilization, is important for 3D printing silicone, since the elastic and soft properties of silicone, in contrast to common 3D printed hard materials, lead to a greater instability of the semi-finished product appearing during additive manufacturing.
[0046] For example, in some embodiments, the center of mass of the actual workpiece is determined in step a). A 3D model of the workpiece is prepared such that the distance between the determined center of mass of the workpiece and the platform is minimized. Thus, in these embodiments, the 3D model of the workpiece includes data on the orientation of the workpiece relative to the platform. Minimizing this distance significantly improves the stability of the workpiece. In particular, the lateral stability is improved, which is typically more affected by the use of a recoater. As a result, the need to print large support structures is reduced.
[0047] It is further preferred that the 3D model of the workpiece in step a) is prepared such that the surface area of the actual workpiece in contact with the platform and / or the projected surface area of the workpiece to the build platform is maximized, thereby increasing the stability of the workpiece.
[0048] Alternatively or additionally, the stability of the workpiece may be increased by providing support structures, which may be larger than those typically used for rigid 3D printed polymers. Typically, these support structures may already be included in the 3D model of the workpiece. Such support structures are generally removed from the workpiece after additive manufacturing is completed. Thus, embodiments having support structures may include removal of the support structures before or after step c). Removal may be achieved by any suitable method, such as cutting, slicing, ripping, etc.
[0049] The additive manufacturing apparatus preferably comprises a recoater or wiper, e.g. a blade.
[0050] The use of a recoater is particularly beneficial for additive manufacturing compositions having high viscosities, as the recoater promotes shear thinning of the additive manufacturing composition, allowing the use of compositions with higher viscosities than would be possible in a typical additive manufacturing process.
[0051] Furthermore, step b) of the method according to the invention may comprise the following steps: i) immersing the platform into the additive manufacturing composition at a predefined height to apply a layer of the additive manufacturing composition to the surface of the platform or the emerging workpiece, ii) moving the platform so that at least the applied layer of the additive manufacturing composition is above the additive manufacturing composition; iii) providing a film of the additive manufacturing composition of a predefined thickness by wiping off the applied layer of the additive manufacturing composition with a recoater; iv) irradiating the film coated with the additive manufacturing composition with a radiation source; v) optionally moving the platform in the z direction; vi) Optionally, repeating steps ii), iii), iv), and / or v).
[0052] In some embodiments, the method comprises steps i) to vi).
[0053] In step i), the predefined height is typically selected such that the platform is immersed in the additive manufacturing composition below the height of the additive manufacturing layer. The height of the additive manufacturing layer is the height of the layer formed during step iv) and may preferably be in the range of 5 to 1,000 μm. Preferably, the predefined height is selected such that the additive manufacturing composition covers the entire surface of the platform or the entire surface of the emerging semi-finished product. Thereby, the predefined height is influenced by the immersion speed of the platform, the material flow behavior and the surface tension. Alternatively or additionally, the predefined height may be selected such that the distance between the platform and the surface of the additive manufacturing composition in the chamber is at least between 1,000 and 50,000 μm.
[0054] In some embodiments, self-leveling of the applied film is performed by providing a self-leveling time after step ii) and before step iii) that is sufficient for efficient self-leveling of the additive manufacturing composition, preferably 100 to 10,000 ms.
[0055] Wiping can preferably be done by mechanical wiping in a circular orbit or linear motion. In general, wiping removes excess material, leaving only the thickness of the additive manufacturing layer of raw material on the emerging object.
[0056] It will be readily understood by those skilled in the art that the emerging product surface refers to the most recently produced layer, which is then covered with additional layers by repeating steps ii) to iv).
[0057] In step iv), the z-direction refers to the printing direction. The z-direction is therefore the direction across the manufactured layers of the semi-finished product. For example, if the additive manufacturing is performed in a top-down orientation, the platform is moved downwards, i.e. towards the bottom of the chamber.
[0058] The displacement in the z-direction is carried out at least a monolayer thick, preferably between 5 and 1000 μm.
[0059] The distance from the platform to the radiation source is preferably adjusted after step ii) and before irradiating the coated film.
[0060] Also, the radiation source is preferably moved to a predefined focal distance prior to step iv), for example the predefined focal distance may be between 10 and 100 cm, preferably between 15 and 30 cm.
[0061] Furthermore, it is preferred that the irradiation of the coated film in step iv) is carried out for more than 50 ms, in particular for more than 150 ms. Preferably, the coated film is irradiated for 100 to 5,000 ms, more preferably for 150 to 4,000 ms.
[0062] Preferably, the recoater is operated at a speed of 0.1-100 mm / s, which has been found to allow high printing speeds but also has no significant effect on the lateral stability of the emerging semi-finished product.
[0063] The additive manufacturing apparatus preferably comprises a sealable housing. Preferably, the housing is hermetically sealable. Typically, the housing is oxygen-free. Preferably, the sealed housing is filled or pressurized essentially with only an inert gas, such as nitrogen or argon. Utilizing an inert atmosphere or vacuum increases the yield of the polymerization reaction, since the presence of oxygen can react with and / or quench any of the radical species formed during the thiol-ene reaction.
[0064] Additionally, the additive manufacturing composition is maintained at a predefined temperature during step b) of the method according to the invention, thereby adjusting the viscosity of the additive manufacturing composition. It has been found that the viscosity should typically not exceed 50 Pa·s. The higher the viscosity, the slower the self-leveling to provide a smooth surface before irradiation can take place. Thus, if the viscosity of the additive manufacturing composition is too high, its temperature may be increased. In some embodiments, the predefined temperature may be in the range of 0 to 250°C.
[0065] In addition, the viscosity of the layered modeling composition may be appropriately controlled by adjusting the shear thinning properties.
[0066] Typically, the irradiation intensity measured at the surface of the additive manufacturing composition and / or the applied film irradiated by the radiation source is reduced by 0-99%, preferably 50-90%, of its original value. The use of the additive manufacturing composition described herein has the advantage of its high reactivity in the polymerization reaction. Therefore, the intensity of the radiation source can be reduced, which significantly reduces overexposure due to scattering and therefore improves the printing resolution.
[0067] For example, the intensity of the irradiation is preferably reduced by digitally changing the greyscale of the projector and / or by providing a physical light filter between the radiation source and the additive manufacturing composition.
[0068] Furthermore, in step c), the post-curing treatment preferably further comprises pre-washing the semi-finished product. Pre-washing may typically be performed by pre-washing the semi-finished product with a solvent, for example an alkane such as cyclohexane, n-hexane, pentane, etc., to remove residues of the additive manufacturing composition. Additionally or alternatively, the semi-finished product is then swollen, preferably in the same solvent or alternatively in another solvent, by rinsing the semi-finished product or by immersing the semi-finished product in this other solvent. As an alternative to the preferred alkane solvent, an alcohol such as i-propanol, n-propanol or ethanol may be used to swell the semi-finished product. In a preferred embodiment, stirring, agitation, vibration, ultrasonic treatment and / or heating can be used to improve the swelling of the product. Additionally or alternatively, the semi-finished product is post-cured under light irradiation, preferably for 10 seconds to 30 minutes. Post-curing ensures complete polymerization of the components of the additive manufacturing composition.
[0069] Those skilled in the art will recognize that post-curing under light irradiation as described above results in curing of unreacted monomers close to the surface of the workpiece, whereas the heat-accelerated radical curing step and / or silanol condensation curing step results in a much deeper cure of the unreacted monomers. The optional post-curing under light irradiation may or may not be separate from the heat-accelerated radical curing step and / or silanol condensation curing step required by the process of the present invention.
[0070] If step c) comprises both a light post-curing step and a heat-promoted radical curing step, the light post-curing is preferably carried out before the heat-promoted radical curing step in order to provide dimensional stability to the semi-finished product.
[0071] When step c) includes both a light post-cure step and a silanol condensation cure step, the light post-cure can be performed before the silanol condensation step, or both steps can be performed simultaneously, preferably both steps are performed simultaneously, but the silanol condensation cure step can continue after the light post-cure is completed.
[0072] (Method for preparing 3D printing silicone composition for additive manufacturing) The composition for additive manufacturing of the method of the present invention comprises i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) at least one crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); Including, The ratio of thiol groups to alkenyl groups in the composition for layered manufacturing is in the range of 0.5:1 to 5:1.
[0073] In addition to at least one silicone building block (A) having multiple alkenyl groups, in certain circumstances it may be beneficial for the additive manufacturing composition of the present invention to comprise one or more s silicone building blocks having alkenyl groups.
[0074] The one or more further silicone building blocks having alkenyl groups are different from the first silicone building block (A) having multiple alkenyl groups.
[0075] Additional silicone building blocks with a single alkenyl group may be used as plasticizers, while additional silicone building blocks with multiple alkenyl groups may be used to tune the final properties of the 3D printed silicone product.
[0076] When the one or more further silicone building blocks has multiple alkenyl groups, it typically has a lower alkenyl group density and / or a longer chain length than the first silicone building block (A) which has multiple alkenyl groups.
[0077] The additional silicone building blocks may further differ from the first silicone building block (A) having multiple alkenyl groups in one or more of the following properties: viscosity, functional group valency, molecular mass, molecular weight, silsesquioxane resin concentration, and / or the nature of the alkenyl derivative (i.e., whether the alkenyl group is at the end of the polysiloxane / silsesquioxane chain or present as a comonomer unit within the polysiloxane / silsesquioxane chain).
[0078] When a further silicone building block having an alkenyl group is present in the additive manufacturing composition of the present invention, the weight ratio of the first silicone (A) having multiple alkenyl groups to the further silicone building block having an alkenyl group is preferably in the range of 99:1 to 10:90.
[0079] The alkenyl group in at least one silicone building block (A) having multiple alkenyl groups is preferably selected from vinyl, allyl, butenyl or pentenyl, most preferably vinyl.
[0080] Also, the alkenyl group in any further silicone building blocks having an alkenyl group is preferably selected from vinyl, allyl, butenyl or pentenyl, most preferably vinyl.
[0081] It is further preferred that the alkenyl groups in both the at least one silicone building block (A) having multiple alkenyl groups and in any further silicone building blocks having alkenyl groups are selected from vinyl, allyl, butenyl or pentenyl, most preferably vinyl.
[0082] It is further preferred that the at least one silicone building block (A) having multiple alkenyl groups is selected from alkenyl-derivatized poly(alkylsiloxanes), alkenyl-derivatized poly(arylsiloxanes), alkenyl-derivatized poly(alkylarylsiloxanes), and alkenyl-derivatized poly(alkyl(aryl)siloxanes), where the alkyl groups are preferably selected from C(1-6) alkyl, more preferably methyl, ethyl, propyl, or butyl, each of the options in this list may be present in the form of a polysiloxane or blended with a silsesquioxane. More preferably, the at least one silicone building block (A) having multiple alkenyl groups is selected from alkenyl-derivatized poly(dimethylsiloxanes), alkenyl-derivatized poly(diphenylsiloxanes), alkenyl-derivatized poly(methylphenylsiloxanes), alkenyl-derivatized poly(dimethyldiphenylsiloxanes), each of the options in this list may be present in the form of a polysiloxane or blended with a silsesquioxane.
[0083] It is also preferred that the optional further silicone building blocks having multiple alkenyl groups are selected from alkenyl-derivatized poly(alkylsiloxanes), alkenyl-derivatized poly(arylsiloxanes), alkenyl-derivatized poly(alkylarylsiloxanes), and alkenyl-derivatized poly(alkyl(aryl)siloxanes), where the alkyl groups are preferably selected from C(1-6) alkyl, more preferably from methyl, ethyl, propyl, or butyl. More preferably, the optional further silicone building blocks having multiple alkenyl groups are selected from alkenyl-derivatized poly(dimethylsiloxanes), alkenyl-derivatized poly(diphenylsiloxanes), alkenyl-derivatized poly(methylphenylsiloxanes), alkenyl-derivatized poly(dimethyldiphenylsiloxanes).
[0084] It is further preferred that both the at least one silicone building block (A) having multiple alkenyl groups and any further silicone building blocks having multiple alkenyl groups are selected from alkenyl-derivatized poly(alkylsiloxanes), alkenyl-derivatized poly(arylsiloxanes), alkenyl-derivatized poly(alkylarylsiloxanes), and alkenyl-derivatized poly(alkyl(aryl)siloxanes), where the alkyl groups are preferably selected from C(1-6) alkyl, more preferably from methyl, ethyl, propyl, or butyl, and each member of this list may be present in the form of a polysiloxane or blended with a silsesquioxane. More preferably, both the at least one silicone building block (A) having multiple alkenyl groups and any further silicone building blocks having multiple alkenyl groups are selected from alkenyl-derivatized poly(dimethylsiloxanes), alkenyl-derivatized poly(diphenylsiloxanes), alkenyl-derivatized poly(methylphenylsiloxanes), alkenyl-derivatized poly(dimethyldiphenylsiloxanes).
[0085] Such polymers can be prepared as described in numerous patents and publications, or are commercially available as liquid silicone rubbers (LSR), high temperature vulcanizing (HTV) silicones or room temperature vulcanizing (RTV) silicones.
[0086] Exemplary silicone resins comprising or consisting of silicone building blocks suitable for use as at least one silicone building block (A) having a plurality of alkenyl groups include Ecoflex® 00-15 (Smooth-On, USA), Ecoflex® 00-20 (Smooth-On, USA), Dragon Skin™ 30 (Smooth-On, USA), Sorta-Clear® 40 (KauPo, Germany), PlatSil® 73-15 (Mouldlife, UK), Sylgard® 184 (Sigma-Aldrich, Switzerland), Zhermack 00, Zhermack 08, Zhermack 13 (Zhermack, Germany), LS-8941 (NuSil, USA), KE-2061 (Shin-Etsu Chemical Co., Ltd., Japan), VQM-146 (Gelest Inc., Germany), VQM973 (Evonik, Germany), Ecoflex 00-50 Part A (Smooth-On, USA), Silopren™ U Base Compound P1300 (Momentive, USA), Silopren™ U Base Compound P300 (Momentive, USA), and HANSA MBA™ 37130 (CHT, Germany).
[0087] Suitable silicone resins that can be used as silicone building blocks with a single alkenyl group for application as plasticizers include Polymer VS 10000 (Evonik, Germany), Polymer MV 2000 (Evonik, Germany), and Silopren™ U 10 Base Polymer (Momentive, USA).
[0088] In both the at least one silicone building block (A) bearing multiple alkenyl groups and in any further silicone building blocks bearing alkenyl groups, the alkenyl groups can be present either as terminal groups and / or as side chains.
[0089] At least one silicone building block (A) having multiple alkenyl groups, and any additional silicone building blocks having alkenyl groups, may be a polysiloxane, a silsesquioxane, or a mixture thereof.
[0090] The polysiloxanes having multiple alkenyl groups useful in the present invention include at least one, typically 1 to 10, in the form of a homopolymer, or a random or block copolymer, preferably a homopolymer. 9 , preferably a polymer, prepolymer, oligomer or macromonomer having 100 to 10,000,000 siloxane repeat units. Optionally, polysiloxanes having multiple alkenyl groups may carry additional functional groups, for example as terminal groups or disposed on the side chains of the siloxane backbone.
[0091] The weight average molecular weight of the polysiloxane having multiple alkenyl groups that can be used in the present invention is preferably in the range of 100 to 10 9 The polysiloxane having multiple alkenyl groups may have a viscosity between 0.1 and 104 Pa·s, preferably between 1 and 102 Pa·s, measured at a shear rate of 1 / s according to standard steady-state rheological measurements.
[0092] The at least one crosslinking agent (B) having multiple thiol groups according to the present invention preferably has the formula (I): R 1 (R)2SiO((R 3 R)SiO) x Si(R)2R 2 (I) It is expressed as wherein R is independently C(1-12)alkyl, preferably methyl; R 1 , R 2 , R 3 is independently C(1-12)alkyl, preferably methyl, or mercapto-C(1-12)alkyl; R 3each instance of may be the same (i.e., a homopolymer) or different (i.e., a copolymer); x is 1 or more, preferably 1 to 100; However, R 1 , R 2 , R 3 At least one, preferably 10 to 100,000, of these is mercapto-C(1-12)alkyl.
[0093] C(1-12) alkyl is preferably C(1-8) alkyl, more preferably C(1-6) alkyl, more preferably methyl, ethyl, butyl, propyl. Thus, the mercaptoalkyl group preferably has 1 to 8 C atoms, preferably 1 to 6 C atoms, more preferably mercaptomethyl, mercaptoethyl, mercaptobutyl, mercaptopropyl, most preferably mercaptopropyl.
[0094] In some embodiments, x is in the range of 40-60.
[0095] In a preferred embodiment, at least one crosslinker (B) having multiple thiol groups useful in the present invention has the formula (I), where R, R 1 , R 2 is independently C(1-12)alkyl, preferably methyl; R 3 is independently mercapto-C(1-12)alkyl, more preferably mercapto-C(1-6)alkyl or C(1-12)alkyl, most preferably methyl; and x is 1 or more, more preferably 2 to 100,000, most preferably 5 to 1,000.
[0096] If x>1, R 3 Each instance of R may be the same (e.g., a homopolymer), and preferably 3 is mercapto-C(1-12)alkyl, more preferably mercapto-C(1-6)alkyl as defined above. Alternatively, R 3Each instance of R may be a different copolymer (e.g., an alternating or block copolymer), preferably R 3 is -(mercapto-C(1-6)alkyl)n-(C(1-12)alkyl)m- or -(C(1-12)alkyl)m-(mercapto-C(1-6)alkyl)n-, where -(mercapto-C(1-6)alkyl)n-(C(1-12)alkyl)m- is as defined above and n and m are independently 1 to 100,000, preferably n is 1 to 10,000 and m is 1 to 10,000.
[0097] It is further preferred that the at least one crosslinking agent (B) having multiple thiol groups of the present invention has the formula (I), 1 , R 2 is independently C(1-12) alkyl, more preferably methyl; R 3 are independently mercaptomethyl, mercaptobutyl, mercaptoethyl, or mercaptopropyl, and x is 1 or more, more preferably 2 to 100,000, and most preferably 2 to 10,000.
[0098] Exemplary crosslinkers (B) having multiple thiol groups according to formula (I) that are believed to be suitable for use in the present invention include SMS-022, SMS-042, SMS-992 (Gelest Inc., Germany), KF-2001, KF-2004 (Shin-Etsu Chemical Co., Japan), SIPELL® RE 61 F (Wacker Chemie AG, Germany).
[0099] The additive manufacturing composition may comprise a crosslinker (B) having multiple thiol groups, or a blend of two or more crosslinkers (B) having multiple thiol groups, preferably one crosslinker (B) having multiple thiol groups.
[0100] In a further embodiment of the additive manufacturing composition according to the invention the crosslinker (B) having multiple thiol groups has a molecular weight of less than 100,000 g / mol, preferably less than 90,000 g / mol, more preferably less than 80,000 g / mol.
[0101] In the additive manufacturing composition according to the invention, the ratio of thiol groups to alkenyl groups is in the range of 0.5:1 to 5:1. The alkenyl groups present may be present in at least one silicone building block (A) having multiple alkenyl groups or in any further silicone building block having alkenyl groups, if present. The thiol groups present may be present in at least one crosslinker (B) having multiple thiol groups.
[0102] Preferably, at least one silicone building block (A) having multiple alkenyl groups and a crosslinker (B) having multiple thiol groups form a stable emulsion.
[0103] In the context of the present invention, a stable emulsion is defined as an emulsion that does not separate (phase separate, flocculate, cream or settle) after changes in ambient conditions, such as temperature, for a period of at least 24 hours.
[0104] Furthermore, it is preferred that a stable emulsion does not exhibit any Ostwald ripening (i.e., aggregation of small droplets into larger ones) within 6 hours, more preferably within 12 hours. The presence or absence of Ostwald ripening can be determined by means well known to those skilled in the art, for example, by microscopy or dynamic light scattering (DLS).
[0105] A stable emulsion also has a minimum shelf life of one month, meaning that the reactivity does not decrease by more than 10% during this period. In the context of the present invention, reactivity is defined as the minimum critical amount of energy (Ec) required to form a solid layer, as described in Equation 1 below. Cd = Dp × ln(t × Irr) + Ec (1) where Cd is the hardening depth given in [mm], Dp is the penetration depth given in [mm] t = time (i.e. exposure time) is given in units of [s], Irr = illuminance (i.e., the power of the light source), in [W / mm 2 ], Ec is the minimum amount of energy required to form a solid layer, and its unit is [J / mm 2 ] is given by:
[0106] The stable emulsion is formed as a result of the immiscibility of at least one silicone building block having an alkenyl group (A) and a crosslinker having multiple thiol groups.
[0107] In embodiments where no further silicone building blocks having alkenyl groups are present, an emulsion is formed between at least a first silicone building block having multiple alkenyl groups (A) and a crosslinker having multiple thiol groups (B), in which the first silicone building block having alkenyl groups (A) typically forms a continuous phase, while the crosslinker having multiple thiol groups (B) forms a dispersed (discontinuous) phase.
[0108] In embodiments in which further silicone building blocks having alkenyl groups are present, an emulsion is formed between the silicone building block having multiple alkenyl groups (A) and the further silicone building block having alkenyl groups using a crosslinker having multiple thiol groups (B), in which the mixture of the silicone building block having multiple alkenyl groups (A) and the further silicone building block having alkenyl groups typically forms a continuous phase, and the crosslinker having multiple thiol groups (B) forms a dispersed (discontinuous) phase.
[0109] Preferably, the emulsion is obtained by means of mixing or shearing (e.g. effective mixing in a suitable high shear mixer) at 100 rpm or more, more preferably 500-5,000 rpm, for several minutes, e.g. at 2000 rpm for at least 2 minutes, more preferably 5-15 minutes.
[0110] Alternatively, mixing is described by the tip speed of the mixer. Thus, the emulsion is preferably obtained by mixing or shearing (e.g. effective mixing in a suitable high shear mixer) means at a tip speed of 1 m / s or more, more preferably 2-10 m / s, for several minutes, e.g. 5 m / s for at least 2 minutes, more preferably 5-15 minutes.
[0111] The emulsions may be stabilized with emulsion stabilizers such as surfactants and dispersants, and rheology modifiers such as fumed silica and nanoclays.
[0112] Within the emulsion, the discontinuous phase is mainly present as droplets with a diameter of 100 μm or less, preferably less than 10 μm, preferably 0.1-10 μm, which allows the emulsion to be sufficiently stable to prevent droplet coalescence and coarsening, and therefore exhibit good shelf life. Step-growth polymerization is expected to occur selectively near or at the emulsion interface until the crosslinker is completely exhausted. Consumption of the dispersed phase (droplets) in the polymerization process reduces the droplet size and scattering of visible light, allowing the production of transparent 3D objects. Thus, in a specific embodiment, the 3D silicone object obtained by the present invention is transparent.
[0113] The emulsions of the present invention also allow the polymerized 3D objects to distinguish themselves by exhibiting unidirectional properties (also in the z-direction) and therefore achieve a certain light penetration depth by light scattering (in the xy plane and in the z-direction), which allows printing at high resolution (such as 30 μm) due to the limited penetration depth. Thus, in a specific embodiment, the 3D silicone objects obtained according to the present invention are of high resolution.
[0114] In an alternative embodiment, at least one silicone building block (A) having multiple alkenyl groups and a crosslinker (B) having multiple thiol groups form a continuous phase, therefore there is no phase separation.
[0115] In such embodiments, no stability issues arise since no phase separation is observed. An important feature to avoid in either emulsions or homogeneous mixtures is the formation of multiphase systems having two or more continuous phases.
[0116] The composition for additive manufacturing according to the present invention preferably has a viscosity in the range of 1 to 2,000 Pa·s, more preferably in the range of 30 to 700 Pa·s, and most preferably in the range of 50 to 300 Pa·s.
[0117] The additive manufacturing composition further comprises at least one free radical photoinitiator, which can be activated by exposure to radiation, i.e. UV A, UV B, UV C and the full visible range, preferably UVA and the visible range, more preferably the visible range from 355 to 420 nm.
[0118] Exemplary free radical photoinitiators suitable for the additive manufacturing composition according to the present invention include: (i) Acylphosphine oxides and bisacylphosphine oxides, such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide; (ii) anisoin; (iii) Benzoin and benzoin alkyl ethers, such as benzoin ethyl ether, benzoin isobutyl ether, and benzoin methyl ether; (iv) benzyl and benzyl dialkyl ketals, such as benzyl dimethyl ketal; (v) Acetophenone; hydroxyacetophenones such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)-phenyl]-2-methyl-1-propanone, 3'-hydroxyacetophenone, 4'-hydroxyacetophenone, 2-hydroxy-2-methylpropiophenone; (di)alkoxyacetophenones such as 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 4'-ethoxyacetophenone; aminoacetophenones such as 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)-phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)-phenyl]-2-(4-morpholinyl)-1-propanone; aryloxyacetophenones such as 4'-phenoxyacetophenone; (vi) (di)hydroxybenzophenones such as benzophenone, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, benzoylbiphenyl, 4'-dihydroxybenzophenone, 3-hydroxybenzophenone, and 4-hydroxybenzophenone; and (di)alkylbenzophenones such as 4-(dimethylamino)benzophenone, 2-methylbenzophenone, 3-methylbenzophenone, 2,5-dimethylbenzophenone, and 3,4-dimethylbenzophenone, (di)aminobenzophenones such as 4,4'-bis(dimethylamino)benzophenone, and 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone and 2-methyl-4'-(methylthio)-2-morpholinopropiophenone; (vii) Anthraquinones and alkylanthraquinones, such as 2-ethylanthraquinone; (viii) Thioxanthones; alkylthioxanthones such as i-propylthioxanthone; and thioxanthen-9-ones such as 2-chlorothioxanthen-9-one; (ix) dibenzosuberenone; (x) a-diketones or derivatives thereof, such as camphorquinone, 9,10-phenanthrenequinone, 1-phenyl-propane-1,2-dione, 4,4'-dichlorobenzil, methylbenzoylformate, etc.; (xi) monoacylgermanium compounds and diacylgermanium compounds, such as benzoyltrimethylgermanium, dibenzoyldiethylgermanium, and bis-(4-methoxybenzoyl)-diethylgermanium; (xii) Titanocenes, such as bis-(etha5-2,4-cyclopentadien-1-yl)-bis-[2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl]-titanium.
[0119] Specific examples are acetophenone, anisoin, anthraquinone, benzil, benzoin, benzoin ethyl ether, benzoin isobutyl ether, benzoin methyl ether, benzophenone, 1-hydroxycyclohexyl phenyl ketone, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, benzoylbiphenyl, 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, camphorquinone, 2-chlorothioxanthen-9-one, dibenzosuberenone, 2,2-diethoxyacetophenone, 4,4'-dihydroxybenzophenone, 2,2-dimethoxy-2-phenylacetophenone, 4-(dimethylamino)benzophenone, 4 , 4'-dimethylbenzyl, 2,5-dimethylbenzophenone, 3,4-dimethylbenzophenone, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide / 2-hydroxy-2-methylpropiophenone, 4'-ethoxyacetophenone, 2-ethylanthraquinone, 3'-hydroxyacetophenone, 4'-hydroxyacetophenone, 3-hydroxybenzophenone, 4-hydroxybenzophenone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methylpropiophenone, 2-methylbenzophenone, 3-methylbenzophenone, methylbenzoyl formate, 2-methyl-4'-(methylthio)-2-morpholinopropiophenone, phenanthrenequinone, 4'-phenoxyacetophenone, and thioxanthen-9-one.
[0120] In a specific embodiment, the additive manufacturing composition comprises 1-hydroxycyclohexyl phenyl ketone (98%, Alfa Aesar, USA) and / or 2,2-dimethoxy-2-phenylacetophenone as free radical photoinitiators.
[0121] Typically, the at least one photoinitiator (D) is present in an amount ranging from 0.01 to 3.0 parts by weight, preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
[0122] In one embodiment, the additive manufacturing composition comprises a single free radical photoinitiator.
[0123] In alternative embodiments, the additive manufacturing composition comprises a first free radical photoinitiator and a second free radical photoinitiator, for example, the first free radical photoinitiator and the second free radical photoinitiator have the same, overlapping or different absorption behaviors. In one embodiment, the additive manufacturing composition comprises a first free radical photoinitiator and a second free radical photoinitiator that have overlapping absorption behaviors. In another embodiment, the additive manufacturing composition comprises a first free radical photoinitiator and a second free radical photoinitiator that have different absorption behaviors.
[0124] It is understood that the absorption spectra of the first and second photoinitiators may overlap to some extent. For example, the difference between the longest wavelength absorption maxima of the first and second photoinitiators may be at least 5 nm, preferably at least 10 nm, and more preferably at least 15 nm.
[0125] In a specific embodiment, the longest wavelength absorption maximum of the first photopolymerization initiator is less than 400 nm, for example, less than 300 to 400 nm, preferably less than 330 to 400 nm, more preferably 340 to 380 nm. The longest wavelength absorption maximum of the second photopolymerization initiator is at least 380 nm, for example, 380 to 600 nm, preferably 400 to 500 nm, more preferably 400 to 480 nm.
[0126] A preferred embodiment includes a combination of a germanium compound and a hydroxyacetophenone, preferably bis(4-methoxybenzoyl)diethylgermanium and 1-hydroxycyclohexylphenylketone. The germanium compound, preferably bis(4-methoxybenzoyl)diethylgermanium, and the hydroxyacetophenone are preferably present in a ratio ranging from 1:1 to 3:1, more preferably in a ratio ranging from 1:1 to 2:5, and most preferably in a ratio of 2:1.
[0127] The additive manufacturing composition also preferably contains at least one light blocker so that the photocatalytic reaction is limited to the area of direct exposure and is not initiated prematurely, ensuring a suitable shelf life. Suitable light blockers include, for example, light blockers with an absorption maximum in the range of the beam wavelength of the light source used for photopolymerization, or colorants, such as (inorganic or organic) color pigments (e.g. carbon black, blue, red), organic dyes, etc., that absorb light and do not retransmit it. Other suitable blockers (especially for transparent compositions) include fluorescent / optical brighteners, photochromic and thermochromic dyes, leuco dyes, or absorbers that absorb light and emit light at a different frequency.
[0128] Commercially available light blockers suitable for use in the additive manufacturing composition include avobenzone, coumarin, 1-(4-tert-butylphenyl)-3-(4-methoxyphenyl)-1,3-propanedione (TCI, Germany), 5-tert-butyl-2-hydroxybenzaldehyde (Sigma-Aldrich, Switzerland), 2,2'-(2,5-thiophenediyl)bis(5-tert-butylbenzoxazole (Sigma-Aldrich, Switzerland), 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid (Alfa Aesar, USA), 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole (Mayzo, USA) or 2-hydroxy-4-methoxybenzophenone (Alfa Aesar, USA).
[0129] The light blocker is preferably present in an amount of 0.01 to 0.50 parts by weight, preferably 0.10 to 0.30 parts by weight, based on the total weight of the silicone building block having multiple alkenyl groups.
[0130] Determination of the wavelength of absorption maximum and molar extinction coefficient of the photoinitiator and photoblocker is typically performed by UV-VIS spectroscopy, such as a conventional double beam UV-VIS spectrometer, at room temperature using solutions in a suitable solvent, such as acetonitrile, preferably at a concentration of 1 mM. For example, a conventional double beam UV-VIS spectrometer can be used for the measurements.
[0131] It is further preferred that the additive manufacturing composition comprises at least one radical inhibitor so that the photocatalytic reaction proceeds in a controlled manner and the propagation of radical chain reactions beyond the area of direct exposure is avoided. Furthermore, the radical inhibitor prevents premature curing of the additive manufacturing composition, thus increasing its shelf life and the window of operability in the additive manufacturing process of the invention. Suitable radical inhibitors include TEMPO, 2,6-di-tert-butylphenol, hydroquinone, phenothiazine, 2,6-di-tert-butyl-p-cresol, tert-butylhydroquinone, 2-tert-butyl-1,4-benzoquinone, 1,4-benzoquinone. When present, the at least one radical inhibitor is preferably present in an amount of 0.001 to 1 part by weight, preferably 0.01 to 0.5 parts by weight, relative to the total weight of the silicone building blocks having multiple alkenyl groups.
[0132] Depending on the application of the 3D printed silicone product, the presence of further components in the additive manufacturing composition may be important.
[0133] One such further component may be a pigment, to achieve the production of colored 3D printed silicone parts. If present, the pigment is preferably present in an amount of 0.01 to 5 parts by weight, preferably 0.01 to 1 part by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
[0134] Another such further component may be a shear-thinning filler, which is preferably selected from pyrogenic silica and silicone powder. If present, the shear-thinning filler is preferably present in an amount of 1 to 60 parts by weight, preferably 1 to 50 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
[0135] Shear thinning fillers become essential components when the shear thinning properties of the additive manufacturing composition are important, and as such depend on the exact method of additive manufacturing.
[0136] Such shear thinning fillers are also beneficial for stabilizing emulsions, as discussed above.
[0137] Yet another such additional component may be silicone rubber powder, a reinforcing filler for increasing Shore hardness and tear strength. When present, the silicone rubber powder is preferably present in an amount of 1 to 30 parts by weight based on the total weight of the silicone building blocks having multiple alkenyl groups.
[0138] In particular, it is preferred that the only polymer present in the additive manufacturing composition is silicone, and it is also preferred that the only polymer present in the 3D printed silicone part obtained by the method of the invention is silicone.
[0139] (Heat-accelerated radical curing step) In one embodiment, the at least one further curing step of step c) of the present invention is a heat-accelerated radical curing step.
[0140] In the context of the present invention, the term heat-promoted radical curing step refers to any step in which a radical reaction is promoted by heating the semi-finished product for a sustained period of time, where the radical reaction is promoted by a heat-activatable free radical initiator (E).
[0141] Thus, if the at least one further curing step of step c) is a heat-accelerated radical curing step, the additive manufacturing composition of step b) must comprise a heat-activatable free-radical initiator.
[0142] The thermally activatable free radical initiator (E) is preferably present in an amount ranging from 0.1 to 5.0 parts by weight, more preferably from 0.2 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
[0143] The thermally activatable free radical initiator (E) according to the present invention is preferably selected from diazo compounds and peroxides, more preferably from 2,4-dichlorobenzoyl peroxide, 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane and 2,2'-azobis(N-butyl-2-methylpropionamide).
[0144] The heat-accelerated radical curing step preferably consists of heating the semi-finished product at a constant temperature in the range of 30-200°C, preferably 40°C-200°C, for a time in the range of 1 second to 24 hours, preferably 1 minute to 24 hours.
[0145] In one embodiment, heating may be carried out at a relatively low temperature for a relatively long time, preferably at a constant temperature in the range of 30-90°C, more preferably in the range of 40-80°C, and most preferably in the range of 50-70°C, for a time in the range of 12-24 hours, more preferably in the range of 14-21 hours, and most preferably in the range of 15-18 hours.
[0146] In alternative embodiments, heating may be carried out at a relatively high temperature for a relatively short time, preferably at a constant temperature in the range of 90-200°C, more preferably in the range of 100-150°C, and most preferably in the range of 110-130°C, for a time in the range of 1 minute to 6.0 hours, more preferably in the range of 0.5-4.5 hours, and most preferably in the range of 1.0 hour to 3.0 hours.
[0147] The present invention is therefore further directed to an additive manufacturing composition, which comprises i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) a thermally activatable free radical initiator (E) in an amount ranging from 0.1 to 5.0 parts by weight, preferably from 0.2 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1.
[0148] All preferred embodiments and features of the additive manufacturing composition given in the above and following sections are equally applicable to the additive manufacturing composition of this aspect.
[0149] Preferably, the additive manufacturing composition of this embodiment is suitable for the method of preparing 3D printed silicone of the present invention.
[0150] (Silanol condensation curing step) In a further embodiment, the at least one further curing step of step c) of the present invention is a silanol condensation curing step.
[0151] In the context of the present invention, the term silanol condensation cure step refers to any step of forming an extended polysiloxane from polysiloxane monomers (C1a) and silanol crosslinkers (C1b) that react with each other through a silanol condensation reaction. In the context of the present invention, a blend of polysiloxane monomers and silanol crosslinkers suitable for undergoing a silanol condensation reaction to form an extended polysiloxane is referred to as a condensation cure silicone blend.
[0152] Thus, if the at least one further curing step of step c) is a silanol condensation curing step, the additive manufacturing composition of step b) must comprise a condensation curing silicone blend (C1).
[0153] The condensation cured silicone blend (C1) is preferably present in an amount ranging from 1 to 90 parts by weight, more preferably ranging from 5 to 75 parts by weight, and most preferably ranging from 10 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. The inventors have found that the above ranges provide optimal mechanical performance of the final product. In particular, high amounts of the condensation cured silicone blend (C1) tend to produce mechanically unstable semi-finished products.
[0154] When the condensation cured silicone blend (C1) is employed, two interwoven networks are formed, the first one originating from components (A) and (B) and the second one originating from the condensation cured silicone blend (C1). Preferably, the condensation cured silicone blend (C1) is present in an amount ranging from 1.0 to 50.0% by weight, more preferably ranging from 10.0 to 45.0% by weight, even more preferably ranging from 20.0 to 40.0% by weight, and most preferably ranging from 20.0 to 39.0% by weight, relative to the total weight of (A)+(B)+(C1), i.e., relative to the total weight of the silicone building blocks having multiple alkenyl groups, the total weight of the crosslinker having multiple thiol groups, and the total weight of the condensation cured silicone blend. As well as the ranges expressed in parts by weight, the ranges expressed in weight percent are also important for improving the mechanical performance of the final product. Furthermore, the mechanical properties of the mid-section cured semi-finished product have significantly improved mechanical properties and stability, which means that particularly complex 3D shapes requiring high resolution can be produced.
[0155] The condensation-cured silicone building blocks (C1a) are preferably selected from silanol (Si-OH)-terminated polysiloxanes.
[0156] The condensation-cured silicone building block (C1a) preferably has a viscosity of less than 1,000 Pa·s, preferably less than 100 Pa·s, more preferably less than 50 Pa·s.
[0157] The condensation-cured silicone building blocks (C1a) preferably have a weight average molecular weight (Mw) in the range of 100 to 500,000, more preferably in the range of 2,000 to 50,000.
[0158] An exemplary condensation-cured silicone building block (C1a) can be selected from the Polymer OH portfolio available from Evonik, or DMS-S27 available from Gelest.
[0159] In a broad sense, the silanol crosslinker (C1b) of the present invention will be understood to be any molecule capable of crosslinking the condensation-cured silicone building block (C1a). It will be well understood by those skilled in the art that if the condensation-cured silicone building block contains silanol functionality, the silanol crosslinker (C1b) only needs to contain a suitable leaving group to achieve crosslinking, whereas if the condensation-cured silicone building block (C1a) consists of a leaving group, the silanol crosslinker (C1b) will contain silanol functionality. The term "silanol crosslinker" does not necessarily require that the crosslinker contain silanol functionality, but rather that the crosslinker has a functionality suitable for forming silanol bridges. Suitable functionality will be well understood by those skilled in the art.
[0160] The silanol crosslinkers (C1b) according to the present invention are preferably selected from low molecular weight silanol crosslinkers and polymeric / oligomeric silanol crosslinkers.
[0161] The low molecular weight silanol crosslinker is preferably represented by the following formula (II): (R') m Si(R) n (II) and wherein the compound is selected from the group consisting of wherein R is selected from H, alkyl, alkenyl, cycloalkyl, aryl, and heteroaryl; R' may be any group capable of acting as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkoxy group, especially a C(1-6)alkoxy group, and most preferably ethoxy; each instance of R and R' may be the same or different; m is either 3 or 4, n is either 0 or 1, and m+n=4.
[0162] In an alternative embodiment, the low molecular weight silanol crosslinker is preferably of formula (IIa): (R') m Si(R) n (IIa) and wherein the compound is selected from the group consisting of compounds according to the formula: wherein R is selected from H, alkyl, alkenyl, cycloalkyl, aryl, and heteroaryl; R' may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkenoxy group, and most preferably isopropenoxy; each instance of R and R' may be the same or different; m is either 3 or 4, n is either 0 or 1, and m+n=4.
[0163] The polymeric / oligomeric silanol crosslinker typically has the formula (III): R 1 O((R 3 O)R 4 SiO) x R 2 (III) is a polyalkylsilicate polymer / oligomer according to In the formula, R1 , R 2 , and R 3 is independently C(1-6) alkyl, preferably R 1 , R 2 , and R 3 are identical and are most preferably ethyl, R 4 is selected from C(1-6) alkyl, and C(1-6) alkenyl, preferably methyl, ethyl, vinyl, and isopropenyl; x is preferably 2 to 100.
[0164] Commercially available polyalkylsilicates are typically supplied as mixtures of monomeric, dimeric, trimeric and cyclic polysiloxanes, which correspond to combinations of compounds according to formulas (II) and (III).
[0165] A crosslinker group (i.e., R′ for low molecular weight silanol crosslinkers, OR for polymeric / oligomeric silanol crosslinkers) for the silanol (Si—OH) groups of the condensation-cured silicone building blocks (C1a) in the additive manufacturing composition. 1 , OR 2 and OR 3 ) is preferably in the range of 0.5:1 to 50:1.
[0166] The silanol condensation curing step preferably consists of exposing the semi-finished product to a relative humidity of greater than 20%, preferably greater than 50%, for a time period ranging from 30 minutes to 72 hours, preferably from 6 to 36 hours.
[0167] Particularly preferred are conditions where the relative humidity is greater than 50% for a period in the range of 12 to 36 hours, more preferably 18 to 30 hours, and most preferably 22 to 26 hours.
[0168] Although the silanol condensation reaction can take place in the presence of moisture alone, it is sometimes beneficial for the additive manufacturing composition of step b) to further comprise a silanol condensation catalyst. In the context of the present invention, a silanol condensation catalyst is any species capable of catalyzing a silanol condensation reaction.
[0169] The silanol condensation catalyst of the present invention is preferably selected from the group of complexes of tin, titanium, zinc, iron, lead or cobalt, or aromatic organic sulfonic acids.
[0170] Most preferably, the silanol condensation catalyst is selected from complexes of tin and titanium. Exemplary silanol condensation catalysts suitable for the present invention include dimethylhydroxy(oleate)tin, dibutyltin dilaurate, and diisopropoxybis(ethylacetoacetate)titanium.
[0171] The silanol condensation catalyst of the present invention is preferably present in an amount of 0.1 to 5.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
[0172] The 3D printed silicone product of this embodiment is best visualized as an interwoven network of silicone cured via thiol-ene reaction in step b) and extended polysiloxane formed in silanol condensation curing step c). These two interwoven silicone networks complement each other and contribute to improved mechanical properties of the 3D printed silicone product, but the two networks are not chemically bonded to each other.
[0173] In certain circumstances it may be advantageous to further improve the mechanical properties by introducing a chemical bond between the two interwoven silicone networks.
[0174] One strategy to achieve this cross-linking is to use a condensation-cured silicone building block (C1a) that bears thiol (-SH) functionality.
[0175] Another method is to incorporate a small molecule silane coupling agent that has both a silanol bridging functionality (similar to silanol crosslinker (C1b)) and an alkenyl or thiol functionality.
[0176] These small molecules are incorporated into the matrix formed in step b) by thiol-ene reactions. During the silanol condensation cure step, the matrix thus contains reactive functional groups that can react with the condensation cure silicone blend (C1), resulting in a crosslinked structure in which the two interwoven silicone networks are crosslinked to each other.
[0177] Suitable low molecular weight silanol coupling agents are selected from alkenyl silane coupling agents (C2) and thiol-containing silane coupling agents (C3).
[0178] The alkenyl silane coupling agent (C2) of the present invention is preferably represented by formula (IV): (R') m Si(R'') n R (IV) It is expressed as wherein R is a vinyl, allyl, butenyl or pentenyl group, preferably a vinyl group; R' may be any group capable of acting as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkoxy group, especially a C(1-6)alkoxy group, and most preferably ethoxy; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; m is either 2 or 3, n is either 0 or 1, and m+n=3.
[0179] In an alternative embodiment, the alkenyl silane coupling agent (C2) of the present invention has the following formula (IVa): (R') m Si(R'') n R (IVa) It is expressed as wherein R is a vinyl, allyl, butenyl or pentenyl group, preferably a vinyl group; R' may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkenoxy group, in particular a C(1-6)alkenoxy group, and most preferably isopropenoxy; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; m is either 2 or 3, n is either 0 or 1, and m+n=3.
[0180] The thiol-containing silane coupling agent (C3) of the present invention is preferably represented by the formula (V): (R a ) m Si(R b ) n R (V) It is expressed as wherein R is mercapto-C(1-12)alkyl, preferably mercapto-C(1-6)alkyl, most preferably mercaptopropyl; R a may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkoxy group, in particular a C(1-6)alkoxy group, and most preferably an ethoxy group; R b is selected from C(1-6) alkyl, and C(1-6) alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; m is either 2 or 3, n is either 0 or 1, and m+n=3.
[0181] In an alternative embodiment, the thiol-containing silane coupling agent (C3) of the present invention is preferably represented by the following formula (Va): (R a ) m Si(R b ) n R (Va) It is expressed as wherein R is mercapto-C(1-12)alkyl, preferably mercapto-C(1-6)alkyl, most preferably mercaptopropyl; R a may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkenoxy group, in particular a C(1-6)alkenoxy group, and most preferably isopropenoxy; R b is selected from C(1-6) alkyl, and C(1-6) alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; m is either 2 or 3, n is either 0 or 1, and m+n=3.
[0182] In one embodiment, R′ (for (C2)) or R a It is preferred to select either R' (for (C3)) as ethoxy. In another embodiment, either R' (for (C2)) or R a It is preferred to select either of the leaving groups (for (C3)) as isopropenoxy. These particular leaving groups are preferred because they allow the silanol moieties to be reactive enough to efficiently undergo a silanol condensation reaction during step c), but not so reactive that a silanol condensation reaction occurs either in step b) or in the preparation of the additive manufacturing composition.
[0183] The layered manufacturing composition of the present invention may contain either an alkenyl silane coupling agent (C2) or a thiol-containing silane coupling agent (C3), or a mixture thereof.
[0184] The total amount of the alkenyl silane coupling agent (C2) and the thiol-containing silane coupling agent (C3) in the additive manufacturing composition is preferably in the range of 1 to 60 parts by weight, more preferably 1 to 30 parts by weight, and most preferably 1 to 20 parts by weight, relative to the total weight of the silicone building blocks having multiple alkenyl groups.
[0185] Alternatively, it is preferred that the combined amount of the condensation cured silicone blend (C1), the alkenyl silane coupling agent (C2) and the thiol-containing silane coupling agent (C3) is in the range of 1.0 to 50.0 wt. %, more preferably 10.0 to 45.0 wt. %, even more preferably 20.0 to 40.0 wt. %, and most preferably 20.0 to 39.0 wt. %, based on the total weight of (A)+(B)+(C1)+(C2)+(C3), i.e., based on the total weight of the silicone building blocks having multiple alkenyl groups, the total weight of the crosslinker having multiple thiol groups and the total weight of the condensation cured silicone blend including any alkenyl and / or thiol-containing silane coupling agents ([(C1)+(C2)+(C3)] / [(A)+(B)+(C1)+(C2)+(C3)]).
[0186] The ratio of the alkenyl silane coupling agent (C2) to the thiol-containing silane coupling agent (C3) in the additive manufacturing composition of the present invention is not critical, provided that the overall ratio of thiol groups to alkenyl groups in the additive manufacturing composition is in the range of 0.5:1 to 5:1 and the ratio of crosslinker groups present in the silanol crosslinker (C1b), the alkenyl silane coupling agent (C2) and the thiol-containing silane coupling agent (C3) to silanol (Si-OH) groups of the condensation-cured silicone building block (C1a) is in the range of 0.5:1 to 50:1.
[0187] The present invention is therefore further directed to an additive manufacturing composition, which comprises i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) a condensation cure silicone blend (C1) in an amount preferably ranging from 1 to 90 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1.
[0188] All preferred embodiments and features of the additive manufacturing composition given in the above and following sections are equally applicable to the additive manufacturing composition of this aspect.
[0189] Preferably, the additive manufacturing composition of this embodiment is suitable for the method of preparing 3D printed silicone of the present invention.
[0190] (Combination of a heat-promoted radical curing step and a silanol condensation curing step) In a particularly preferred embodiment, step c) of the method for preparing 3D printed silicone comprises both a heat-promoted radical curing step and a silanol condensation curing step.
[0191] The heat-promoted radical curing step and the silanol condensation curing step may be performed sequentially, but it is preferred that the two steps are performed simultaneously. Conditions for combining the two steps simultaneously include heating the semi-finished product at a constant temperature in the range of 50-150° C., for a time in the range of 1-24 hours, and at a relative humidity of more than 50%.
[0192] In one embodiment, heating may be carried out at a relatively low temperature for a relatively long time, preferably at a constant temperature in the range of 50-80°C, more preferably in the range of 53-70°C, and most preferably in the range of 55-65°C, for a time in the range of 12-24 hours, more preferably in the range of 14-21 hours, and most preferably in the range of 15-18 hours, at a relative humidity of greater than 50%.
[0193] In an alternative embodiment, heating may be carried out at a relatively high temperature for a relatively short time, preferably at a constant temperature in the range of 90-150°C, more preferably in the range of 100-140°C, and most preferably in the range of 110-130°C, for a time in the range of 1-6.0 hours, more preferably in the range of 1.5-4.5 hours, and most preferably in the range of 1.5 hours to 3.0 hours, at a relative humidity of greater than 50%.
[0194] When step c) of the method for preparing 3D printed silicone according to the invention comprises both a heat-promoted radical curing step and a silanol condensation curing step, the additive manufacturing composition of step b) is i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) a condensation cured silicone blend (C1) in an amount preferably ranging from 1 to 90 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; v) a thermally activatable free radical initiator (E) in an amount ranging from 0.1 to 5.0 parts by weight, preferably from 0.2 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1.
[0195] All of the preferred embodiments of the composition for additive manufacturing described in the previous sections are similarly applicable to the composition for additive manufacturing of this aspect.
[0196] (Items and Use) The present invention is further directed to a 3D printed silicone product obtainable by the method of the present invention.
[0197] One of the major advantages of the present invention over methods using only UV / visible light curing is the depth of cure, resulting in a homogeneous cure with isotropic material properties, even in relatively large volumes of semi-finished products.
[0198] Thus, the present invention is directed to a 3D printed silicone obtainable by the method of the present invention, the size of which is at least 1x1x1 mm, preferably at least 3x3x3 mm, most preferably at least 5x5x5 mm, and the Shore A hardness values measured according to ISO 7619-1 between samples taken from the surface of the cured composition and from the center of the cured composition vary by less than 10%, preferably by less than 5%, and most preferably the values are identical.
[0199] The present invention is further directed to the use of a thermally activatable free radical initiator (E), the process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1. c) a post-curing step including a heat-promoted radical curing step, in which the semi-finished product is heated at a constant temperature preferably in the range of 50°C to 150°C for a time in the range of 1 to 24 hours; Including, The thermally activatable free radical initiator (E) is a) the Young's modulus, measured on a type 4 tensile specimen according to ISO 37, is within the range of 110 to 10,000% of the Young's modulus of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110 to 1,000% of the elongation at break of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110-500% of the tensile strength of 3D printed silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; d) the tear strength, measured on a sample of test piece type C according to ASTM D624, is in the range of 110-400% of the tear strength of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; e) a Shore A hardness measured according to ISO 7619-1, the Shore A hardness being in the range of 110 to 2,500% of the Shore A hardness of a 3D printing silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; To produce 3D printed silicone having one or more of the properties of It is preferably present in the additive manufacturing composition of step b) in an amount ranging from 0.1 to 5.0 parts by weight, preferably from 0.2 to 3.0 parts by weight, relative to the total weight of the silicone building blocks having multiple alkenyl groups.
[0200] In a final aspect, the present invention is directed to the use of a condensation cured silicone blend (C1), the process of which comprises a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, The ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1. c) a post-curing step including a silanol condensation curing step, preferably consisting of exposing the semi-finished product to a relative humidity of more than 20%, preferably more than 50%, for a time period ranging from 30 minutes to 72 hours, preferably from 6 to 36 hours; Including, The condensation cured silicone blend (C1) is a) the Young's modulus measured on a type 4 tensile specimen according to ISO 37 is within the range of 110 to 10,000% of the Young's modulus of the condensation cured silicone blend (C1) or of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110 to 1,000% of the elongation at break of the condensation cured silicone blend (C1) or of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110-500% of the tensile strength of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; d) the tear strength measured on a sample of test specimen type C according to ASTM D624 is in the range of 110 to 400% of the tear strength of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation cure step; e) a Shore A hardness measured according to ISO 7619-1, the Shore A hardness being in the range of 110 to 2,500% of the Shore A hardness of the condensation cured silicone blend (C1) or of a 3D printing silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; To produce 3D printed silicone having one or more of the properties of Preferably, it is present in the additive manufacturing composition of step b) in an amount ranging from 1 to 90 parts by weight, relative to the total weight of the silicone building blocks having multiple alkenyl groups.
[0201] All preferred embodiments and features of both the method and the additive manufacturing composition given in the sections above are equally applicable to both the articles and uses discussed in this section.
[0202] The present invention can also be explained by the following items. (Item 1) 1. A method for preparing 3D printed silicone, comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) at least one crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); and c) performing a post-cure treatment comprising at least one further curing step other than a light-accelerated cure, preferably either a heat-accelerated radical cure or a silanol condensation cure; Including, The method, wherein the ratio of thiol groups to alkenyl groups in the composition for additive manufacturing is in the range of 0.5:1 to 5:1. (Item 2) Item 13. The method of claim 1, wherein the at least one silicone building block (A) having a plurality of alkenyl groups and the crosslinker (B) having a plurality of thiol groups form a stable emulsion. (Item 3) Item 2. The method according to item 1, wherein the at least one silicone building block (A) having a plurality of alkenyl groups and the crosslinker (B) having a plurality of thiol groups form a continuous phase. (Item 4) The method according to any one of items 1 to 3, wherein the additive manufacturing composition preferably has a viscosity in the range of 1 to 2,000 Pa·s, more preferably in the range of 30 to 700 Pa·s, and most preferably in the range of 50 to 300 Pa·s. (Item 5) 5. The method according to any one of items 1 to 4, wherein the alkenyl groups in the at least one silicone building block (A) having a plurality of alkenyl groups are selected from vinyl, allyl, butenyl or pentenyl. (Item 6) 5. The method according to any one of items 1 to 4, wherein the alkenyl group in the at least one silicone building block (A) having multiple alkenyl groups is vinyl. (Item 7) The at least one crosslinking agent (B) having a plurality of thiol groups has the formula (I): R 1 (R)2SiO((R 3 R)SiO) x Si(R)2R 2 (I) It is expressed as wherein R is independently C(1-12)alkyl, preferably methyl; R 1 , R 2 , R 3 is independently C(1-12)alkyl, preferably methyl, or mercapto-C(1-12)alkyl; R 3 each instance of may be the same (i.e., a homopolymer) or different (i.e., a copolymer); x is 1 or more, preferably 1 to 100; However, R 1 , R 2 , R 3 The method according to any one of items 1 to 6, wherein at least one, preferably 10 to 100,000, of is mercapto-C(1-12)alkyl. (Item 8) The composition for additive manufacturing, iv) a shear-thinning filler, preferably selected from pyrogenic silica and silicone powder, in an amount ranging from 1 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; The method according to any one of items 1 to 7, further comprising: (Item 9) 9. The method according to any one of items 1 to 8, wherein the at least one free radical photoinitiator (D) is present in an amount ranging from 0.01 to 3.0 parts by weight, preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. (Item 10) The composition for additive manufacturing, v) a thermally activatable free radical initiator (E), preferably present in an amount ranging from 0.1 to 5.0 parts by weight, more preferably from 0.2 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Further comprising: 10. The method according to any one of the preceding claims, wherein said at least one further curing step of step c) is a heat-promoted radical curing step. (Item 11) 11. The method according to item 10, wherein the heat-promoted radical curing step comprises heating the semi-finished product at a constant temperature in the range of 30° C. to 200° C. for a time in the range of 1 second to 24 hours. (Item 12) 12. The method according to item 10 or 11, wherein the thermally activatable free radical initiator (E) is selected from diazo compounds and peroxides, more preferably from 2,4-dichlorobenzoyl peroxide, 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane and 2,2′-azobis(N-butyl-2-methylpropionamide). (Item 13) The composition for additive manufacturing, vi) a condensation-cured silicone blend (C1), preferably present in an amount ranging from 1 to 90 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. Further comprising: said at least one further curing step of step c) is a silanol condensation curing step; 13. The method according to any one of items 1 to 12, wherein the condensation cured silicone blend (C1) is a blend of condensation cured silicone building blocks (C1a), preferably selected from silanol terminated polysiloxanes, and silanol crosslinkers (C1b), preferably selected from low molecular weight silanol crosslinkers and polymeric / oligomeric silanol crosslinkers. (Item 14) The silanol crosslinker (C1b) has the formula (II): (R') m Si(R) n (II) is a low molecular weight silanol crosslinker selected from compounds according to wherein R is selected from H, alkyl, alkenyl, cycloalkyl, aryl, and heteroaryl; R' may be any group capable of acting as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkoxy group, especially a C(1-6)alkoxy group, and most preferably ethoxy; each instance of R and R' may be the same or different; 14. The method according to item 13, wherein m is either 3 or 4, n is either 0 or 1, and m+n=4. (Item 15) The silanol crosslinker (C1b) has the formula (IIa): (R') m Si(R) n (IIa) is a low molecular weight silanol crosslinker selected from compounds according to wherein R is selected from H, alkyl, alkenyl, cycloalkyl, aryl, and heteroaryl; R' may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkenoxy group, and most preferably isopropenoxy; each instance of R and R' may be the same or different; 13. The method according to item 12, wherein m is either 3 or 4, n is either 0 or 1, and m+n=4. (Item 16) 16. The method according to any one of items 12 to 15, wherein the silanol condensation curing step consists of exposing the semi-finished product to a relative humidity of more than 20%, preferably more than 50%, for a time in the range of 30 minutes to 72 hours, preferably 6 to 36 hours. (Item 17) 17. The method according to any one of items 12 to 16, wherein the ratio of crosslinker groups to silanol groups of the condensation-cured silicone building blocks (C1a) in the additive manufacturing composition is in the range of 0.5:1 to 50:1. (Item 18) 18. The method according to any one of items 12 to 17, wherein the condensation cured silicone blend (C1) is present in an amount in the range of 1 to 90 parts by weight, more preferably in the range of 5 to 75 parts by weight, and most preferably in the range of 10 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. (Item 19) 18. The method according to any one of items 12 to 17, wherein the condensation cured silicone blend (C1) is present in an amount in the range of 1.0 to 50.0 wt.%, more preferably 10.0 to 45.0 wt.%, even more preferably in the range of 20.0 to 40.0 wt.%, and most preferably in the range of 20.0 to 39.0 wt.%, based on the sum of the total weight of the silicone building blocks having multiple alkenyl groups, the total weight of the crosslinker having multiple thiol groups and the total weight of the condensation cured silicone blend. (Item 20) The composition for additive manufacturing, vii) alkenyl silane coupling agents (C2), and / or viii) Thiol-containing silane coupling agents (C3) Further comprising: 20. The method according to any one of items 12 to 19, wherein the combined amount is preferably 1 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. (Item 21) The composition for additive manufacturing, vii) an alkenyl silane coupling agent (C2) having the formula (IV): (R') m Si(R'') n R (IV) It is expressed as wherein R is a vinyl, allyl, butenyl or pentenyl group, preferably a vinyl group; R' may be any group capable of acting as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkoxy group, especially a C(1-6)alkoxy group, and most preferably ethoxy; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; an alkenyl silane coupling agent (C2), in which m is either 2 or 3, n is either 0 or 1, and m+n=3; and / or viii) a thiol-containing silane coupling agent (C3) having the formula (V): (R a ) m Si(R b ) n R (V) It is expressed as wherein R is mercapto-C(1-12)alkyl, preferably mercapto-C(1-6)alkyl, most preferably mercaptopropyl; R a may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkoxy group, especially a C(1-6)alkoxy group, and most preferably ethoxy; R b is selected from C(1-6) alkyl, and C(1-6) alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; Thiol-containing silane coupling agent (C3), in which m is either 2 or 3, n is either 0 or 1, and m+n=3. Further comprising: 20. The method according to any one of items 12 to 19, wherein the combined amount is preferably 1 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. (Item 22) The composition for additive manufacturing, vii) an alkenyl silane coupling agent (C2) having the formula (IVa): (R') m Si(R'') n R (IVa) It is expressed as wherein R is a vinyl, allyl, butenyl or pentenyl group, preferably a vinyl group; R' may be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkenoxy group, in particular a C(1-6)alkenoxy group, and most preferably isopropenoxy; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; an alkenyl silane coupling agent (C2), in which m is either 2 or 3, n is either 0 or 1, and m+n=3; and / or viii) Thiol-containing silane coupling agents (C3) having the formula (Va): (R a ) m Si(R b ) n R (Va) It is expressed as wherein R is mercapto-C(1-12)alkyl, preferably mercapto-C(1-6)alkyl, most preferably mercaptopropyl; R amay be any group capable of behaving as a leaving group in a silanol condensation reaction, more preferably selected from carboxylate, alkenyloxy, oxime, alkoxy and dialkylamino groups, even more preferably an alkenoxy group, in particular a C(1-6)alkenoxy group, and most preferably isopropenoxy; R b is selected from C(1-6) alkyl, and C(1-6) alkenyl, preferably selected from methyl, ethyl, vinyl and isopropenyl, most preferably methyl; Thiol-containing silane coupling agent (C3), in which m is either 2 or 3, n is either 0 or 1, and m+n=3. Further comprising: 20. The method according to any one of items 12 to 19, wherein the combined amount is preferably 1 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. (Item 23) 23. The method according to any one of items 20 to 22, wherein the combined amount of the condensation cured silicone blend (C1), the alkenyl silane coupling agent (C2) and the thiol-containing silane coupling agent (C3), based on the total weight of (A)+(B)+(C1)+(C2)+(C3), i.e. based on the total weight of the silicone building blocks having multiple alkenyl groups, the total weight of the crosslinker having multiple thiol groups and the total weight of the condensation cured silicone blend including any alkenyl and / or thiol-containing silane coupling agent ([(C1)+(C2)+(C3)] / [(A)+(B)+(C1)+(C2)+(C3)]), is in the range of 1.0 to 50.0% by weight, more preferably 10.0 to 45.0% by weight, even more preferably in the range of 20.0 to 40.0% by weight, and most preferably in the range of 20.0 to 39.0% by weight. (Item 24) The composition for additive manufacturing, ix) a silanol condensation catalyst (F), preferably in an amount of 0.1 to 5.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Further comprising: 24. The method according to any one of items 12 to 23, wherein the silanol condensation catalyst (F) is preferably selected from the group of complexes of tin, titanium, zinc, iron, lead or cobalt, or aromatic organic sulfonic acids, most preferably selected from the group of complexes of tin and titanium. (Item 25) 25. The method according to any one of items 1 to 24, wherein step c) comprises both a heat-promoted radical curing step and a silanol condensation curing step, the heat-promoted radical curing step and the silanol condensation curing step being carried out separately or simultaneously, and when the heat-promoted radical curing step and the silanol condensation curing step are carried out simultaneously, the combined heating / silanol condensation curing step consists of heating the semi-finished product at a constant temperature in the range of 40° C. to 200° C. and at a relative humidity of more than 50% for a time in the range of 1 min to 24 h. (Item 26) 26. The method according to any one of items 1 to 25, wherein the additive manufacturing apparatus comprises a recoater. (Item 27) Step b) additive manufacturing, i) immersing a platform into the additive manufacturing composition at a predefined height to apply a layer of the additive manufacturing composition to the surface of the platform or the emerging workpiece; ii) moving the platform so that at least the applied layer of the additive manufacturing composition is above the additive manufacturing composition; iii) wiping off the applied layer of the additive manufacturing composition with the recoater to provide a film of the additive manufacturing composition of a predefined thickness; iv) irradiating the film coated with the additive manufacturing composition with a radiation source; v) optionally moving said platform in the z direction; vi) optionally repeating steps ii), iii), iv), and / or v); and 27. The method according to item 26, comprising: (Item 28) A composition for additive manufacturing, comprising: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) a thermally activatable free radical initiator (E) in an amount ranging from 0.1 to 5.0 parts by weight, more preferably from 0.2 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, A composition for additive manufacturing, wherein the ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1. (Item 29) A composition for additive manufacturing, comprising: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) a condensation cured silicone blend (C1) in an amount preferably ranging from 1 to 90 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; iv) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, A composition for additive manufacturing, wherein the ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1. (Item 30) 28. A cured composition obtainable by the method according to any one of items 1 to 27, the cured composition having a size of at least 1 x 1 x 1 mm, preferably at least 3 x 3 x 3 mm, most preferably at least 5 x 5 x 5 mm, and wherein the Shore A hardness values, measured according to ISO 7619-1, between samples taken from the surface of the cured composition and from the center of the cured composition vary by less than 10%, preferably by less than 5%, most preferably the values are identical. (Item 31) Use of a thermally activatable free radical initiator (E) in a process, said process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, a ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1; c) a post-curing step including a heat-promoted radical curing step, in which the semi-finished product is heated at a constant temperature, preferably in the range of 50°C to 150°C, for a time period in the range of 1 to 24 hours; Including, The thermally activatable free radical initiator (E) is a) the Young's modulus, measured on a type 4 tensile specimen according to ISO 37, is within the range of 110 to 10,000% of the Young's modulus of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a free radical initiator (E) or a heat-accelerated radical curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110 to 1,000% of the elongation at break of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; c) the tensile strength, measured on a type 4 tensile test specimen according to ISO 37, is in the range of 110 to 500% of the tensile strength of 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; d) the tear strength measured on a sample of test piece type C according to ASTM D624 is in the range of 110-400% of the tear strength of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; e) the Shore A hardness, measured according to ISO 7619-1, is in the range of 110 to 2,500% of the Shore A hardness value of a 3D printing silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; To produce 3D printed silicone having one or more of the properties of Preferably, the silicone building blocks having a plurality of alkenyl groups are present in the additive manufacturing composition of step b) in an amount ranging from 0.1 to 5.0 parts by weight, preferably from 0.2 to 3.0 parts by weight, relative to the total weight of the silicone building blocks having a plurality of alkenyl groups. (Item 32) Use of a condensation cured silicone blend (C1) in a process comprising the step of an additive manufacturing composition, said process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, the additive manufacturing composition being: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D), preferably in an amount ranging from 0.01 to 3.0 parts by weight, more preferably from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, a ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:1; c) a post-curing step including a silanol condensation curing step, preferably consisting of exposing the semi-finished product to a relative humidity of more than 20%, preferably more than 50%, for a period ranging from 30 minutes to 72 hours, preferably from 6 to 36 hours; Including, The condensation cured silicone blend (C1) is a) the Young's modulus measured on a type 4 tensile specimen according to ISO 37 is within the range of 110 to 10,000% of the Young's modulus of the condensation cured silicone blend (C1) or of a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110 to 1,000% of the elongation at break of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same composition for additive manufacturing in the absence of a silanol condensation curing step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110 to 500% of the tensile strength of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation curing step; d) the tear strength, measured on a sample of test piece type C according to ASTM D624, is in the range of 110-400% of the tear strength of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; e) the Shore A hardness, measured according to ISO 7619-1, is in the range of 110 to 2,500% of the Shore A hardness value of the condensation cured silicone blend (C1) or a 3D printing silicone produced from the same composition for additive manufacturing in the absence of a silanol condensation curing step; To produce 3D printed silicone having one or more of the properties of Preferably, the silicone building blocks having a plurality of alkenyl groups are present in the additive manufacturing composition of step b) in an amount ranging from 1 to 90 parts by weight, relative to the total weight of the silicone building blocks having a plurality of alkenyl groups. EXAMPLES
[0203] 1.Measurement method (Young's Modulus) Young's modulus was measured using type 4 tensile specimens according to ISO 37. The specimens were obtained as follows. a) Printing an article according to the present invention. b) If the article is thicker than 1 mm, slice the article into 1 mm thick sheets. c) Type 4 tensile specimens are punched out from this 1 mm sheet. In this way, the Young's modulus at different points within the article can be measured. Measurements were performed with a UTM equipped with a 100 N load cell, and Young's modulus was calculated between 10 and 50% elongation.
[0204] (Tensile strength) Tensile strength was measured using type 4 tensile specimens according to ISO 37. The specimens were obtained as follows: a) Printing an article according to the present invention. b) If the article is thicker than 1 mm, slice the article into 1 mm thick sheets. c) Type 4 tensile specimens are punched out from this 1 mm sheet. In this way, the tensile strength at different points within the article can be measured. Measurements were taken with a UTM equipped with a 100N load cell.
[0205] (Elongation at break) The elongation at break was measured using type 4 tensile specimens according to ISO 37. The specimens were obtained as follows. a) Printing an article according to the present invention. b) If the article is thicker than 1 mm, slice the article into 1 mm thick sheets. c) Type 4 tensile specimens are punched out from this 1 mm sheet. In this way, the elongation at break at different points within the article can be measured. Measurements were taken with a UTM equipped with a 100N load cell.
[0206] (tear strength) Tear strength was measured according to ASTM D624 using Type C test specimens, which were obtained as follows. a) Printing an article according to the present invention. b) If the article is thicker than 2 mm, slice the article into 2 mm thick sheets. c) Type C test specimens are punched out from this 2 mm sheet. In this way, the tear elongation at different points within the article can be measured. Measurements were taken with a UTM equipped with a 100N load cell.
[0207] (Shore A hardness) Shore A hardness was measured according to ISO7619-1. All tests were performed with a Type A durometer. Measurements were performed directly on printed samples of all sizes. To obtain the Shore A hardness values of the internal areas of the article, the article was sliced at a given height and the Shore A hardness was measured at the center of the cut surface and at the edge of the cut surface.
[0208] 2. Experimental results: a) Preparation of 3D printed silicone including a heat-accelerated radical curing step [Table 1] A: Silopren* U Base Compound P300, available from Momentive, and Polymer VS200, available from Evonik, in a 100:35 ratio. B: (Mercaptopropyl)methylsiloxane-dimethylsiloxane copolymer (CAS: 101810-99-5), available from GPC Silicones under the trade name GP-800. D: 2,2-Dimethoxy-2-phenylacetophenone (CAS: 24650-42-8) commercially available from Merck Sigma Aldrich UV Blocker: Avobenzone (CAS: 70356-09-1) commercially available from Merck Sigma Aldrich E: 1-Hydroxycyclohexyl phenyl ketone (CAS: 947-19-3) commercially available from Alfa Aesar
[0209] Pre-blending: Component B was added to a blend of Component A with pyrogenic silica and mixed with a sawtooth propeller at 2000 rpm for 10 minutes. Component D and UV blocker were then dissolved in 5.0 mL of dichloromethane (DCM) and added to the silicone mixture. Component E was then added to the mixture and mixed for an additional 10 minutes.
[0210] Formulation: The mixed ink is passed through a three-roll mill operating at 600 rpm with slit widths of 30 μm and 5 μm, respectively. The resulting 3D printing ink is degassed for 15 min in a vacuum of 3 mbar. The resulting 3D printing ink has a measured viscosity of 85 Pa s.
[0211] 3D printing: Next, this additive manufacturing composition is used to print a 3D image using a DLP light source (385 nm, 1-10 mW / cm 2 3D silicone articles were printed using a printer using a 3000 W laser. Each layer was exposed for 5 seconds (5–50 mW / cm 2 of illumination).
[0212] Post-curing: Post-curing is necessary to obtain the final mechanical properties and is done in a light chamber (385 nm, 20 mW / cm) that ensures that the printed object is homogenously exposed to light from all angles. 2 After UV curing, a second step is performed in an oven at 120°C for 2 hours.
[0213] Figure 1 shows the effect of thermal curing compared to UV / Vis curing. A single cylindrical blank, 10 mm in diameter and 12 mm in height, was printed using the procedure described above. Prior to the thermal curing step, this article was sliced into two cylindrical articles, 10 mm in diameter and 6 mm in height. One of these articles was tested for Shore A hardness at the cut surface, while the other article was subjected to a 2 hour thermal cure in a 120°C oven before being tested for Shore A hardness at the cut surface.
[0214] Shore A hardness measurements were taken at three locations on the cut surface of each article: two locations 1 mm away from the outer wall and one location at the centre of the circular cut surface.
[0215] As can be seen from FIG. 1, the Shore A hardness of the first article that was only UV cured was non-uniform, with higher values closer to the outer wall and lower values at the center of the cut surface (which corresponds to the center of the uncured product before slicing).
[0216] In contrast, the Shore A hardness values of the heat-set article were much higher than those of the first article and were completely isotropic, with values of A61 observed in both the core and the outer wall.
[0217] b) Comparison of penetration depth between UV curing and heat-promoted radical curing To compare the efficiency of UV curing and heat-accelerated radical curing, tubes of the additive manufacturing composition were subjected to either UV curing and heat-accelerated radical curing, or UV curing only.
[0218] [Table 2] A: A blend of polysiloxane and silsesquioxane available from Evonik under the trade name VQM 973. B: (Mercaptopropyl)methylsiloxane-dimethylsiloxane copolymer (CAS: 101810-99-5), available from GPC Silicones under the trade name GP-800. D: 2,2-Dimethoxy-2-phenylacetophenone (CAS: 24650-42-8) commercially available from Merck Sigma Aldrich UV Blocker: Avobenzone (CAS: 70356-09-1) commercially available from Merck Sigma Aldrich E: 1-Hydroxycyclohexyl phenyl ketone (CAS: 947-19-3) commercially available from Alfa Aesar Pigment: Silc Pig™ blue available from Smooth-On
[0219] Premix: Component B was added to Component A and mixed with a sawtooth propeller at 2000 rpm for 10 minutes. Component D and UB blocker were then dissolved in 1.5 mL of dichloromethane (DCM) and added to the silicone mixture. 3 g of 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane and 1 g of Silc Pig™ blue pigment (Smooth-On) were then added to the mixture and mixed for an additional 10 minutes.
[0220] Formulation: The silicone mixture is then passed through a three-roll mill operating at 600 rpm with slit widths of 30 μm and 5 μm, respectively. The resulting 3D printing ink is degassed for 15 min in a vacuum of 3 mbar. The resulting 3D printing ink has a measured viscosity of 250 Pa·s.
[0221] Casting: The 3D printing ink was then poured into a 50mL Flacon tube and cast into a cylindrical shape. To remove any air bubbles formed during casting, the ink was centrifuged in the Flacon tube at 2000 rpm (650 cfm) for 1 minute. Two cylinders were cast for comparison.
[0222] UV curing: Both inks were cured in a UV chamber (385 nm, 20 mW / cm) under nitrogen atmosphere. 2 The plate was then UV cured for 20 minutes on a rotating stage in a UV-curable plastic container.
[0223] Thermal curing: After UV curing, one sample was further cured at 180°C for 20 minutes under normal atmosphere.
[0224] Testing: UV-cured and heat-cured samples were cut to obtain cross sections to observe the depth of cure.
[0225] As can be seen in Figure 2, the heat-cured sample was entirely solid, whereas the tube that was only UV-cured had a liquid core and only the outer few millimeters were cured.
[0226] For compositions prepared according to the present invention, the core region is not completely liquid, however, if the interior region of the 3D printed article is not cured, the mechanical properties of this region will be reduced, reducing the mechanical performance of the entire article (see, e.g., FIG. 1).
[0227] c) Preparation of 3D printed silicone including a silanol condensation step [Table 3] A: Silopren* U Base Compound P1300, available from Momentive, and Polymer RV100, available from Evonik, in a ratio of 83:17. B: (Mercaptopropyl)methylsiloxane-dimethylsiloxane copolymer (CAS: 101810-99-5), available from GPC Silicones under the trade name GP-800. C1a: a silanol-terminated polysiloxane having a viscosity of 700 mPa·s (commercially available from Gelest Inc. under the trade name DMS-S27). C1b: Tetraethyl orthosilicate (CAS: 78-10-4) commercially available from Merck Sigma Aldrich C2: Vinyltrimethoxysilane (CAS: 2768-02-7) commercially available from Merck Sigma Aldrich D: 2,2-Dimethoxy-2-phenylacetophenone (CAS: 24650-42-8) commercially available from Merck Sigma Aldrich F: Dimethylhydroxy(oleate)tin (CAS: 43136-18-1) available from Gelest Inc. UV Blocker: Avobenzone (CAS: 70356-09-1) commercially available from Merck Sigma Aldrich Silica: pyrogenic silica (Aerosil R8200, Evonik)
[0228] Preblending: Component A was added to Component B and mixed with a sawtooth propeller at 2000 rpm for 10 minutes. Next, Component D, Component F, and the UV blocker were dissolved in 5.0 mL of dichloromethane (DCM) and added to the silicone mixture to form Component Blend 1, which was mixed for 5 minutes.
[0229] In a separate step, components C1a, C1b, C2 and silica were mixed in a planetary mixer equipped with a disperser head rotating at a tip speed of 10 m / s and passed through a three-roll mill with slide widths of 30 μm and 5 μm operating at a speed of 600 rpm to obtain a 3D printing silicone ink with a viscosity of 250 Pa s to form component blend 2, which was stirred for 5 min. Mixing and storage were performed under dry and inert conditions.
[0230] Component Blend 1 and Component Blend 2 were mixed prior to compounding in a planetary mixer rotating the disperser head at a tip speed of 10 m / s.
[0231] Formulation: The mixed ink is then passed through a three-roll mill operating at 600 rpm with slit widths of 30 μm and 5 μm, respectively. The resulting 3D printing ink is degassed for 15 min in a vacuum of 3 mbar. The resulting 3D printing ink had a measured viscosity of 250 Pa s.
[0232] 3D printing: Next, this additive manufacturing composition is used to print a 3D image using a DLP light source (385 nm, 1-10 mW / cm 2 3D silicone articles were printed using a printer using a 3000 W laser. Each layer was exposed for 5 seconds (5–50 mW / cm 2 of illumination).
[0233] Post-curing: Post-curing is necessary to obtain the final mechanical properties and is done in a light chamber (385 nm, 20 mW / cm) that ensures that the printed object is homogenously exposed to light from all angles. 2 After UV curing, the second step is carried out in an oven at 60° C. and 50% relative humidity for 24 hours.
[0234] 3 shows an ear-shaped prosthesis manufactured using the additive manufacturing composition 3. As can be seen, the method of the present invention can achieve highly detailed shapes with extremely high resolution.
[0235] The mechanical properties are significantly improved compared to a similar additive manufacturing composition with more component blend 2 / less component blend 1. Similarly, the link between the two networks improves the mechanical properties and stability when compared to a similar additive manufacturing composition in which component C2 is omitted. In particular, improvements in tear strength, tensile strength and tensile modulus are observed.
Claims
1. 1. A method for preparing 3D printed silicone, comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, wherein the additive manufacturing composition is i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) at least one crosslinker (B) having a plurality of thiol groups; iii) at least one free radical photoinitiator (D); and and c) performing a post-cure treatment including heat-accelerated radical curing; Including, The ratio of thiol groups to alkenyl groups in the composition for additive manufacturing is in the range of 0.5:1 to 5:1; The additive manufacturing composition comprises a thermally activatable free radical initiator (E). The method further comprising:
2. 10. The method of claim 1, wherein the at least one silicone building block (A) having multiple alkenyl groups and the crosslinker (B) having multiple thiol groups form a stable emulsion.
3. The at least one crosslinking agent (B) having a plurality of thiol groups has the formula (I): R 1 (R) 2 SiO((R 3 R)SiO) x Si(R)2R 2 (I) It is expressed as wherein R is independently C(1-12)alkyl; R 1 , R 2 , R 3 is independently C(1-12)alkyl; R 3 each instance of may be the same (i.e., a homopolymer) or different (i.e., a copolymer); x is 1 or more, However, R 1 , R 2 , R 3 The method according to claim 1 or 2, wherein the at least one of
4. wherein R is independently methyl; 1 , R 2 , R 3 are independently a methyl group or a mercapto-C(1-12)alkyl group, x is 1 to 100, R 1 , R 2 , R 3 The method of claim 3, wherein at least 10 to 100,000 of the groups are mercapto-C(1-12)alkyl groups.
5. The composition for additive manufacturing, iv) a shear-thinning filler in an amount ranging from 1 to 60 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups. The method of any one of claims 1 to 3, further comprising:
6. 6. The method according to claim 1, wherein the at least one free radical photoinitiator (D) is present in an amount ranging from 0.01 to 3.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
7. The method of claim 6, wherein the at least one free radical photoinitiator (D) is present in an amount ranging from 0.1 to 2.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups.
8. The composition for additive manufacturing, a thermally activatable free radical initiator (E) present in an amount ranging from 0.1 to 5.0 parts by weight based on the total weight of the silicone building blocks having multiple alkenyl groups; The method of any one of claims 1 to 7, further comprising:
9. 9. The method according to any one of claims 1 to 8, wherein the heat-promoted radical curing step consists of heating the semi-finished product at a constant temperature in the range of 30°C to 200°C for a time in the range of 1 second to 24 hours.
10. The process according to any one of claims 1 to 9, wherein the thermally activatable free radical initiator (E) is selected from diazo compounds and peroxides.
11. 11. The method of claim 10, wherein the thermally activatable free radical initiator (E) is selected from 2,4-dichlorobenzoyl peroxide, 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane and 2,2'-azobis(N-butyl-2-methylpropionamide).
12. 1. A method for preparing 3D printed silicone, comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, wherein the additive manufacturing composition is i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) at least one crosslinker (B) having a plurality of thiol groups; iii) at least one free radical photoinitiator (D); and and c) performing a post-cure treatment including a silanol condensation cure; Including, The ratio of thiol groups to alkenyl groups in the composition for additive manufacturing is in the range of 0.5:1 to 5:1; The composition for additive manufacturing, vi) Condensation Cured Silicone Blend (C1) Further comprising: the condensation cured silicone blend (C1) is a blend of condensation cured silicone building blocks (C1a) and silanol crosslinkers (C1b); The composition for additive manufacturing, vii) an alkenyl silane coupling agent (C2) having the formula (IVa): (R’) m Si(R’’) n R (IVa) It is expressed as where R is a vinyl, allyl, butenyl or pentenyl group. R' may be any group capable of behaving as a leaving group in a silanol condensation reaction; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl; an alkenyl silane coupling agent (C2), in which m is either 2 or 3, n is either 0 or 1, and m+n=3; and / or viii) a thiol-containing silane coupling agent (C3) having the formula (Va): (R) a ) m Yes (R) b ) n R (Va) It is expressed as wherein R is mercapto-C(1-12)alkyl; R a may be any group capable of behaving as a leaving group in a silanol condensation reaction; R b is selected from C(1-6)alkyl, and C(1-6)alkenyl; Thiol-containing silane coupling agent (C3), in which m is either 2 or 3, n is either 0 or 1, and m+n=3. The method further comprising:
13. The composition for additive manufacturing, vii) an alkenyl silane coupling agent (C2), and / or viii) Thiol-containing silane coupling agents (C3) Further comprising: The method according to claim 12, wherein the combined amount of the alkenyl silane coupling agent (C2) and / or the thiol-containing silane coupling agent (C3) is 1 to 60 parts by weight based on the total weight of the silicone building blocks having multiple alkenyl groups.
14. 14. The method of claim 12 or 13, wherein the silanol condensation curing step comprises exposing the workpiece to a relative humidity of greater than 20% for a period of time ranging from 30 minutes to 72 hours.
15. 15. The method according to any one of claims 12 to 14, wherein the ratio of crosslinker groups to silanol groups of the condensation-cured silicone building blocks (C1a) in the additive manufacturing composition is in the range of 0.5:1 to 50:
1.
16. The composition for additive manufacturing, ix) a silanol condensation catalyst (F) in an amount of 0.1 to 5.0 parts by weight based on the total weight of the silicone building blocks having multiple alkenyl groups. The method of any one of claims 12 to 15, further comprising:
17. 17. The method of claim 16, wherein the silanol condensation catalyst (F) is selected from the group of complexes of tin, titanium, zinc, iron, lead or cobalt, or aromatic organic sulfonic acids.
18. 18. The method of claim 16 or 17, wherein the silanol condensation catalyst (F) is selected from the group of tin and titanium complexes.
19. 19. The method according to any one of claims 1 to 18, wherein step c) comprises both a heat promoted radical curing and a silanol condensation curing, said heat promoted radical curing and said silanol condensation curing being carried out separately or simultaneously, and in the case where said heat promoted radical curing and said silanol condensation curing are carried out simultaneously, said heat promoted radical curing and said silanol condensation curing consists of heating said semi-finished product at a constant temperature in the range of 40°C to 200°C, at a relative humidity of more than 50%, for a time in the range of 1 minute to 24 hours.
20. A composition for additive manufacturing, comprising: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); and iv) a thermally activatable free radical initiator (E) in an amount ranging from 0.1 to 5.0 parts by weight, based on the total weight of the silicone building blocks having multiple alkenyl groups; Including, A composition for additive manufacturing, wherein the ratio of thiol groups to alkenyl groups in the composition is in the range of 0.5:1 to 5:
1.
21. A composition for additive manufacturing, comprising: i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) a condensation cured silicone blend (C1); and iv) at least one free radical photoinitiator (D); and Including, the ratio of thiol groups to alkenyl groups in the composition ranges from 0.5:1 to 5:1; the condensation cured silicone blend (C1) comprises a condensation cured silicone building block (C1a) and a silanol crosslinker (C1b); The composition for additive manufacturing, vii) an alkenyl silane coupling agent (C2) having the formula (IVa): (R’) m Si(R’’) n R (IVa) It is expressed as wherein R is a vinyl, allyl, butenyl or pentenyl group; R' may be any group capable of behaving as a leaving group in a silanol condensation reaction; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl; an alkenyl silane coupling agent (C2), in which m is either 2 or 3, n is either 0 or 1, and m+n=3; and / or viii) a thiol-containing silane coupling agent (C3) having the formula (Va): (R) a ) m Yes (R) b ) n R (Va) It is expressed as wherein R is mercapto-C(1-12)alkyl; R a may be any group capable of behaving as a leaving group in a silanol condensation reaction. R b is selected from C(1-6)alkyl, and C(1-6)alkenyl; Thiol-containing silane coupling agent (C3), in which m is either 2 or 3, n is either 0 or 1, and m+n=3. The additive manufacturing composition further comprises:
22. The composition for additive manufacturing, vi) a condensation cured silicone blend (C1) present in an amount ranging from 1 to 90 parts by weight based on the total weight of the silicone building blocks having multiple alkenyl groups; The additive manufacturing composition of claim 21 .
23. Use of a thermally activatable free radical initiator (E) in a process, said process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, wherein the additive manufacturing composition is i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); and Including, a ratio of thiol groups to alkenyl groups in the composition ranges from 0.5:1 to 5:1; c) a post-curing step including a heat-accelerated radical curing step; Including, a) the Young's modulus, measured on a Type 4 tensile specimen according to ISO 37, is within the range of 110-10,000% of the Young's modulus of 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110-1,000% of the elongation at break of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110-500% of the tensile strength of 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; d) the tear strength, measured on specimen type C samples according to ASTM D624, is in the range of 110-400% of the tear strength of 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; e) a Shore A hardness measured according to ISO 7619-1 in the range of 110-2,500% of the Shore A hardness value of a 3D printed silicone produced from the same additive manufacturing composition in the absence of the free radical initiator (E) or a heat-accelerated radical curing step; The use of the method for producing 3D printed silicone having one or more of the following properties:
24. The use according to claim 23, wherein during the post-curing treatment of step c), the semi-finished product is heated at a constant temperature in the range of 50° C. to 150° C. for a time in the range of 1 to 24 hours.
25. Use of a condensation cured silicone blend (C1) in a process, said process comprising: a) preparing a 3D model of a semi-finished product; b) additively manufacturing the semi-finished product according to the 3D model of the semi-finished product using an additive manufacturing apparatus and an additive manufacturing composition, wherein the additive manufacturing composition is i) at least one silicone building block (A) having a plurality of alkenyl groups; ii) a crosslinker (B) having multiple thiol groups; iii) at least one free radical photoinitiator (D); and Including, a ratio of thiol groups to alkenyl groups in the composition ranges from 0.5:1 to 5:1; The composition for additive manufacturing, vi) Condensation Cured Silicone Blend (C1) Further comprising: the condensation cured silicone blend (C1) is a blend of condensation cured silicone building blocks (C1a) and silanol crosslinkers (C1b); The composition for additive manufacturing, vii) an alkenyl silane coupling agent (C2) having the formula (IVa): (R’) m Si(R’’) n R (IVa) It is expressed as where R is a vinyl, allyl, butenyl or pentenyl group. R' may be any group capable of behaving as a leaving group in a silanol condensation reaction; R″ is selected from C(1-6)alkyl, and C(1-6)alkenyl; an alkenyl silane coupling agent (C2), in which m is either 2 or 3, n is either 0 or 1, and m+n=3; and / or viii) a thiol-containing silane coupling agent (C3) having the formula (Va): (R) a ) m Yes (R) b ) n R (Va) It is expressed as wherein R is mercapto-C(1-12)alkyl; R a may be any group capable of behaving as a leaving group in a silanol condensation reaction. R b is selected from C(1-6)alkyl, and C(1-6)alkenyl; Thiol-containing silane coupling agent (C3), in which m is either 2 or 3, n is either 0 or 1, and m+n=3. Further comprising: c) a post-curing step including a silanol condensation curing step; Including, a) the Young's modulus, measured on a type 4 tensile specimen according to ISO 37, is within the range of 110-10,000% of the Young's modulus of said condensation cured silicone blend (C1) or a 3D printed silicone produced from the same said additive manufacturing composition in the absence of a silanol condensation cure step; b) the elongation at break measured on a type 4 tensile specimen according to ISO 37 is in the range of 110-1,000% of the elongation at break of the condensation cured silicone blend (C1) or a 3D printed silicone produced from the same additive manufacturing composition in the absence of a silanol condensation cure step; c) the tensile strength, measured on a type 4 tensile specimen according to ISO 37, is in the range of 110-500% of the tensile strength of said condensation cured silicone blend (C1) or a 3D printed silicone produced from the same said additive manufacturing composition in the absence of a silanol condensation curing step; d) the tear strength measured on a sample of test specimen type C according to ASTM D624 is in the range of 110-400% of the tear strength of said condensation cured silicone blend (C1) or 3D printed silicone produced from the same said additive manufacturing composition in the absence of a silanol condensation cure step; e) a Shore A hardness measured according to ISO 7619-1 in the range of 110-2,500% of the Shore A hardness value of said condensation cured silicone blend (C1) or a 3D printing silicone produced from the same said additive manufacturing composition in the absence of a silanol condensation cure step; 3D printing silicone having one or more of the following properties:
26. 26. The use according to claim 25, wherein the silanol condensation curing step consists of exposing the semi-finished product to a relative humidity of greater than 20% for a period of time ranging from 30 minutes to 72 hours.
Citation Information
Patent Citations
CH3612019
UV curable silicone resin-organic mercaptan composition
EP0437247A2
Two-part curable ink composition set and ink jet recording method, ink jet recording apparatus, and printed product using the same
EP1942159A1
JP2010-0185991A
Methods of 3d printing using photocurable silicone compositions
JP2018500192A