Lithium electrode and lithium secondary battery including the same
A protective layer containing a two-dimensional material and an intrinsically porous polymer addresses dendrite formation and conductivity issues in lithium secondary batteries, enhancing their capacity and lifespan.
Patent Information
- Application Number
- JP2023502840
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-02
- Filing Date
- 2022-05-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-05-09
AI Technical Summary
Conventional lithium secondary batteries face issues with dendrite formation, reduced lithium ion conductivity, and shortened cycle life due to the reactivity of lithium metal electrodes, which affect the energy density and stability of the battery.
A protective layer comprising a two-dimensional material and an intrinsically porous polymer is applied to the lithium metal layer to suppress dendrite formation and enhance lithium ion transfer characteristics.
The protective layer effectively prevents dendrite growth, improves lithium ion conductivity, and enhances the capacity and lifespan of lithium secondary batteries.
Smart Images

Figure 0007566126000004 
Figure 0007566126000005 
Figure 0007566126000006
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2021-0071605 dated June 2, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated as part of this specification.
[0002] The present invention relates to a lithium electrode and a lithium secondary battery including the same. [Background technology]
[0003] The range of applications of lithium secondary batteries has expanded from portable electronic devices and communication devices to electric vehicles (EVs) and electric storage systems (ESSs), and there is an increasing demand for higher capacity and higher energy density of lithium secondary batteries used as power sources for these devices.
[0004] Conventional lithium secondary batteries have an energy density of 700Wh / kg, using graphite for the negative electrode and lithium cobalt oxide (LCO) for the positive electrode. However, as mentioned above, the fields requiring lithium secondary batteries with high energy density have been expanding recently, and the need to increase the energy density of lithium secondary batteries has been continuously raised. For example, an increase in energy density is also necessary to extend the driving distance of electric vehicles on a single charge to more than 500km.
[0005] In order to increase the energy density of lithium secondary batteries, the use of lithium electrodes containing lithium metal is increasing. Specifically, lithium metal has an extremely high theoretical capacity of 3,860mAh / g, and a very low standard hydrogen electrode (SHE) of -3.045V, which is advantageous in realizing batteries with high capacity and high energy density.
[0006] However, lithium metal is a highly reactive and difficult metal to handle, which makes it difficult to handle during processing. In addition, when a lithium electrode is used as the negative electrode of a lithium secondary battery, lithium metal easily reacts with electrolyte, water, or impurities in the battery, such as lithium salt, to form a solid electrolyte interface layer (SEI layer), which is a type of passivation layer, on the surface. This passivation layer promotes the formation of dendrites by lithium metal during charging by causing a difference in local current density, and gradually grows as charging and discharging proceeds, causing internal cracks between the positive and negative electrodes. In addition, dendrites have mechanically weak points (bottle necks), and form inactive lithium that loses electrical contact with the current collector during discharging, reducing the battery capacity and shortening the cycle life, adversely affecting the stability of the battery.
[0007] In order to improve the above-mentioned problems of lithium electrodes, lithium electrodes having protective layers with various compositions or morphologies have been researched.
[0008] As an example, Korean Patent Publication No. 2018-0041086 relates to a protective layer formed by applying a slurry containing fluorocarbon or metal fluoride and PVdF-based resin to a lithium metal anode. A lithium metal anode with a protective layer containing the above composition can prevent the formation of dendrites, but there is a problem that uniform lithium ion distribution and effective solid electrolyte interfacial layer formation on the surface of the anode are not smooth so that uniform plating and stripping of lithium metal can be performed during charging and discharging to improve battery performance.
[0009] In addition, Korean Patent Publication No. 2016-0052351 discloses that the growth of lithium dendrites can be suppressed by including a lithium dendrite water absorbing material in a polymer protective film formed on the surface of a lithium metal electrode, thereby improving the stability and life characteristics of a lithium secondary battery. However, the polymer protective film makes it difficult to uniformly distribute lithium ions on the electrode surface, making it difficult to apply the polymer protective film to lithium-sulfur batteries.
[0010] In addition, Qiuli Yang et al. and Gi Hyeon Moon et al. have disclosed that by forming a protective film on a lithium metal anode using polymers of intrinsic microporosity (PIM) that have inherent pores within the polymer structure, it is possible to uniformly distribute lithium ions on the surface of the lithium metal anode and suppress the formation of dendrites. However, when the protective film formed on the lithium metal anode contains only an intrinsic microporosity polymer, lithium ions can only move through the pores contained in the intrinsic microporosity polymer, which reduces the conductivity of lithium ions and causes a large overvoltage during charging and discharging.
[0011] Thus, in batteries using a lithium electrode as the negative electrode, much research has been conducted on the development of protective layers to prevent the growth of lithium metal dendrites, but the research results on protective layers that can improve the overall performance of the battery are insufficient. Therefore, there is still a need to develop a lithium electrode that can prevent the formation of dendrites on the lithium electrode and realize a lithium secondary battery with high capacity, high energy density, and long life. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Korean Patent Publication No. 2018-0041086 (April 23, 2018), Negative electrode for lithium-ion secondary battery and method for manufacturing the same [Patent Document 2] Korean Patent Publication No. 2016-0052351 (May 12, 2016), Lithium metal electrode having a stable protective layer and lithium secondary battery including the same [Non-patent literature]
[0013] [Non-Patent Document 1] Qiuli Yang et al., PIM‐1 as an artificial solid electrolyte interphase for stable lithium metal anode in high‐performance batteries, Journal of Energy Chemistry 2020, 42, 83‐90 [Non-Patent Document 2] Gi Hyeon Moon et al., An artificial solid interphase with polymers of intrinsic microporosity for highly stable Li metal anodes, Chemical Communications 2019, 55, 6313‐6316 Summary of the Invention [Problem to be solved by the invention]
[0014] Here, the present inventors have conducted extensive research to solve the above problems, and have confirmed that when a protective layer including a two-dimensional material and an intrinsic porous polymer is formed on a lithium electrode, the formation of dendrites can be prevented and at the same time, excellent lithium ion transport properties can be exhibited, thereby improving the performance of a battery including the same, and thus completed the present invention.
[0015] Therefore, an object of the present invention is to provide a lithium electrode having a protective layer formed thereon, which can suppress the generation of dendrites and have lithium ion transport properties, thereby improving the life characteristics of a lithium secondary battery.
[0016] Another object of the present invention is to provide a lithium secondary battery including the lithium electrode. [Means for solving the problem]
[0017] In order to achieve the above objective, The present invention provides a lithium electrode comprising: a lithium metal layer; and a protective layer formed on at least one surface of the lithium metal layer, The protective layer provides a lithium electrode comprising a two-dimensional material and an intrinsically porous polymer.
[0018] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: (a) dispersing a two-dimensional material in a first solvent to prepare a first solution; (b) dissolving the intrinsically porous polymer in a second solvent to prepare a second solution; (c) mixing the first solution and the second solution to prepare a coating solution; and (d) applying the coating liquid to at least one surface of a lithium metal layer.
[0019] The present invention also provides a lithium secondary battery including the lithium electrode. Effect of the Invention
[0020] The protective layer according to the present invention includes a two-dimensional material and an intrinsic porous polymer together, and is effective for dendrite formation. In addition, the protective layer can exhibit excellent lithium ion transport properties, thereby increasing the life of a lithium secondary battery including the protective layer. [Brief description of the drawings]
[0021] [Figure 1] Photographs showing the surfaces of lithium electrodes used in Examples 1 to 4 and Comparative Example 1 ((a): Example 1, (b): Example 2, (c): Example 3, (d): Example 4, (e): Comparative Example 1). [Diagram 2]3 is a photograph of the surface of the lithium electrode according to Examples 1 to 4 taken by a scanning electron microscope. [Diagram 3] 1 is a graph showing the results of evaluating the life characteristics of a lithium-sulfur battery according to Experimental Example 2. [Figure 4] 1 is a graph showing the results of evaluating the capacity retention rate of a lithium-sulfur battery according to Experimental Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will now be described in more detail.
[0023] The terms and words used in this specification and claims should not be construed in a limited manner based on their ordinary or dictionary meaning, but should be construed in a meaning and concept that corresponds to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to explain his / her invention in the best possible way.
[0024] The terms used in the present invention are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the present invention, the terms "include" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0025] When a lithium electrode containing lithium metal is used as the negative electrode of a lithium secondary battery, the following problems arise.
[0026] First, lithium metal is difficult to handle because it is highly reactive and has poor mechanical strength.
[0027] Secondly, lithium metal reacts with electrolyte, water, impurities in the battery, lithium salt, etc. to form a solid electrolyte interface layer (SEI layer) on the surface of lithium metal, which is a passive film, and this solid electrolyte interface layer creates a difference in local current density to form tree-like dendrites. Furthermore, the dendrites thus formed grow and cause an internal short circuit in the battery, forming inactive lithium, which can lead to deterioration of the battery's performance or explosion.
[0028] Third, if the positive electrode contains a sulfur-based material, lithium polysulfide (Li2S) that is generated from the positive electrode x , x=8, 6, 4, 2) undergo a side reaction with lithium metal, forming lithium sulfide (Li2S) on the lithium metal surface, immobilizing the lithium electrode and reducing the electrochemical reactivity of the lithium electrode.
[0029] For this reason, in the prior art, protective layers have been formed on lithium metal using several materials, but the problem of dendrite formation has not been effectively alleviated, resulting in problems that degrade not only the capacity and life characteristics of the battery, but also driving stability.
[0030] Here, the present invention provides a lithium electrode that can realize a lithium secondary battery having excellent capacity, life and driving stability by forming a protective layer including a two-dimensional material and a polymer of intrinsic microporosity (PIM) on the surface of lithium metal to prevent the formation of dendrites and improve the lithium ion transport properties.
[0031] Specifically, the lithium electrode according to the present invention includes a lithium metal layer; and a protective layer formed on at least one surface of the lithium metal layer, the protective layer including a two-dimensional material and an intrinsically porous polymer.
[0032] In particular, the protective layer according to the present invention includes both an intrinsic porous polymer and a two-dimensional material, thereby suppressing the formation of dendrites and at the same time ensuring a certain level of lithium ion conductivity. Such an intrinsic porous polymer includes micropores inside and can provide uniform lithium ion channels, and is therefore known as a conventional technique for using it as a protective layer for a lithium electrode to suppress the growth of dendrites. However, in the conventional technique, a satisfactory dendrite formation prevention effect cannot be ensured, and when the protective layer for a lithium electrode includes only an intrinsic porous polymer, lithium ions can only move through the micropores included in the intrinsic porous polymer, which reduces the lithium ion conductivity of the lithium electrode itself and generates a large overvoltage during the charge / discharge process, adversely affecting the overall performance of the battery. Meanwhile, as described above, in the present invention, a protective layer including both an intrinsic porous polymer and a two-dimensional material is introduced onto a lithium metal layer, thereby uniformly distributing lithium ions on the lithium metal layer, suppressing dendrite formation, and obtaining excellent lithium ion transport properties. As a result, the capacity and life characteristics of a lithium secondary battery including the same can be improved.
[0033] In the present invention, the lithium metal layer includes lithium metal and may include a lithium metal thin film in the form of a foil or sheet, or a lithium metal powder in which lithium metal particles are collected. The lithium metal layer may be in the form of a lithium sheet metal having a lithium metal thin film formed on at least one surface of a current collector.
[0034] The current collector is for supporting the lithium metal layer and is not particularly limited as long as it has high conductivity without causing chemical changes in the lithium secondary battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, or the like, aluminum-cadmium alloy, or the like.
[0035] The current collector may have fine irregularities on its surface to strengthen the bonding force with the lithium metal, and may be in various forms such as a film, sheet, foil, mesh, net, porous body, foam, nonwoven fabric, etc.
[0036] The method for forming the lithium metal thin film on the current collector is not particularly limited, and may be a layer or film forming method commonly used in the art, such as squeezing, coating, deposition, etc.
[0037] As described above, when the lithium metal layer is formed on one surface of the current collector, a protective layer (described later) may be formed on the entire surface of the lithium metal thin film except for the surface of the lithium metal thin film in contact with the current collector.
[0038] In addition, when the current collector is a porous current collector, lithium metal may be contained in pores in the porous current collector. In this case, a protective layer, which will be described later, may be provided on the entire surface of the porous current collector except for a terminal connected to the porous current collector and extended to the outside.
[0039] The lithium metal layer has a thickness of 20 to 200 μm, preferably 25 to 100 μm, and more preferably 30 to 80 μm. If the lithium metal layer is less than this range, the capacity and life characteristics of the battery may be reduced, and conversely, if it exceeds this range, the lithium electrode becomes too thick, which is disadvantageous for commercialization.
[0040] In the present invention, the protective layer comprises a two-dimensional material and an intrinsic porosity polymer.
[0041] The two-dimensional material has the shape of a plate, flake, or sheet with a thickness, as a material in which atoms form a crystal structure on a two-dimensional plane with the thickness of a single atomic layer, and can be classified as a conductor, semiconductor, or non-conductor according to its electrical properties. The two-dimensional material maximizes the Li ion transfer number of the protective layer formed on the lithium metal, thereby improving the lithium ion transfer properties of the protective layer as well as increasing the mechanical strength of the protective layer.
[0042] The two-dimensional material may include at least one selected from the group consisting of graphene, graphene oxide (GO), transition metal dichalcogenides, hexagonal boron nitride (h-BN), and graphitic carbon nitride (g-C3N4). The transition metal dichalcogenides are compounds having a two-dimensional layer structure formed by bonding transition metal elements such as tungsten (W) or molybdenum (Mo) with chalcogen elements such as sulfur (S), specifically, molybdenum disulfide (MoS2), tungsten disulfide (WS2), etc. Preferably, the two-dimensional material may include at least one selected from the group consisting of graphene oxide and graphitic carbon nitride.
[0043] The polymers of intrinsic microporosity (PIM) are very rigid, but have a twisted structure of the backbone, which disrupts the arrangement of polymer chains through strong intermolecular interactions and forms free volume formed by the connection of functional groups, resulting in microporosity within the structure. As a result, the intrinsic porous polymer contains micropores of less than 2 nm, and the 300 mm diameter polymer formed from these micropores. 2 / g or more.
[0044] As described above, the intrinsically porous polymer has a microporous structure, and therefore when used as a protective layer for a lithium electrode, it forms uniform lithium ion channels and uniformizes the current density distribution on the surface of the lithium metal layer, thereby suppressing the formation of dendrites.
[0045] Specifically, the intrinsically porous polymer is a polymer (PIM-1) having a repeating structure represented by the following formula 1:
[0046] [ka]
[0047] The weight average molecular weight (Mw) of the polymer (PIM-1) having the repeating structure represented by Formula 1 is 1,000 to 100,000 g / mol, preferably 3,000 to 60,000 g / mol, and more preferably 5,000 to 50,000 g / mol.
[0048] The protective layer may contain the two-dimensional material and the intrinsic porous polymer in a weight ratio of 1:1 to 1:20, preferably 1:5 to 1:18, and more preferably 1:7 to 1:12. In the present invention, the weight ratio corresponds to the ratio of "weight % of the two-dimensional material": "weight % of the intrinsic porous polymer". When the weight ratio of the two-dimensional material and the intrinsic porous polymer falls within the above-mentioned range, the battery exhibits excellent lithium ion conductive properties while exhibiting excellent dendrite generation suppression effects. When the weight ratio of the two-dimensional material and the intrinsic porous polymer is less than the above-mentioned range, coating imbalance may occur, resulting in a decrease in battery performance, and conversely, when the weight ratio exceeds the above-mentioned range, a problem of increased resistance may occur.
[0049] The thickness of the protective layer is 0.1 to less than 5 μm, preferably 0.2 to 3 μm, and more preferably 0.5 to 1.5 μm. The protective layer can be formed to an appropriate thickness in consideration of the intended battery performance. If the thickness of the protective layer is less than the above range, it may not be possible to perform the intended function as a protective layer, and conversely, if the thickness exceeds the above range, the battery capacity may decrease due to overvoltage, making it impossible to operate the battery at a high rate.
[0050] The lithium ion conductivity of the protective layer according to the present invention having the above-mentioned composition is 10 ‐20 or 10 ‐4 S / cm, preferably 10 ‐10 or 10 ‐5 The lithium electrode according to the present invention includes a protective layer including the two-dimensional material and an intrinsic porosity polymer, and thus exhibits superior lithium ion conduction characteristics compared to a conventional lithium electrode including a protective layer made only of an intrinsic porosity polymer.
[0051] In addition, the surface resistance of the lithium electrode having the protective layer according to the present invention in the electrolyte is 50 to 300Ω, preferably 100 to 200Ω, more preferably 120 to 150Ω, and the resistance does not change for 1 to 72 hours, preferably 24 to 65 hours, more preferably 36 to 60 hours, which means that the protective layer including the two-dimensional material and the intrinsic porosity polymer does not react with the electrolyte and is maintained in a stable state.
[0052] In the present invention, the method for manufacturing the lithium electrode is not particularly limited, and any method known to those skilled in the art or various modified methods thereof may be used.
[0053] As an example, the method for producing the lithium electrode includes the steps of: (a) dispersing a two-dimensional material in a first solvent to prepare a first solution; (b) dissolving the intrinsically porous polymer in a second solvent to prepare a second solution; (c) mixing the first solution and the second solution to prepare a coating solution; and (d) applying the coating solution to at least one surface of the lithium metal layer.
[0054] Specific examples of the two-dimensional material and the intrinsically porous polymer are as described above.
[0055] The first and second solvents used in preparing the coating solution are at least one selected from the group consisting of tetrahydrofuran (THF), toluene, cyclohexane, N-methyl-2-pyrrolidone (NMP), dimethyl formamide (DMF), dimethyl acetamide (DMAc), tetramethyl urea, dimethyl sulfoxide (DMSO) and triethyl phosphate. Tetrahydrofuran is preferably used as the first and second solvents because it has high solubility for the two-dimensional material and the inherently porous polymer, which is advantageous for forming a protective layer by a coating process.
[0056] The first and second solvents may be contained at a concentration level that allows easy coating, and the specific content varies depending on the coating method and device.
[0057] When preparing the first and second solutions, the respective contents of the two-dimensional material and the intrinsic porosity polymer are appropriately adjusted in consideration of their weight ratio in the above-mentioned protective layer.
[0058] The coating method for forming the protective layer may be a method selected from the group consisting of dip coating, spray coating, spin coating, die coating, roll coating, slot-die coating, bar coating, gravure coating, comma coating, curtain coating, and micro-gravure coating, but is not limited thereto, and various coating methods available in the art for forming a coating layer may be used.
[0059] After the coating, a drying process may be performed to remove the solvent. The drying process is performed at a temperature and time level that allows the solvent to be sufficiently removed, and the conditions may vary depending on the type of solvent, and are not particularly limited in the present invention. Examples include drying with warm air, hot air, or low humidity air, vacuum drying, and drying by irradiation with (far) infrared rays and electron beams. The drying speed is usually adjusted so that the solvent can be removed as quickly as possible within a speed range that does not cause cracks in the protective layer due to stress concentration or peel off the lithium metal layer from the current collector.
[0060] The protective layer formed by the above-mentioned manufacturing method has a thickness of 0.1 to less than 5 μm, preferably 0.2 to 3 μm, and more preferably 0.5 to 1.5 μm. The protective layer can suppress the formation of dendrites, improve the lithium ion transport characteristics, and increase the life characteristics of a lithium secondary battery including the same.
[0061] The present invention also provides a lithium secondary battery including the lithium electrode.
[0062] The lithium secondary battery includes a positive electrode, a negative electrode, and an electrolyte interposed therebetween, and the negative electrode includes the lithium electrode according to the present invention.
[0063] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on one or both sides of the positive electrode current collector.
[0064] The positive electrode current collector is for supporting the positive electrode active material, as described above.
[0065] The positive electrode active material layer includes a positive electrode active material, and may further include a conductive material, a binder, or an additive.
[0066] The positive electrode active material is not particularly limited as long as it can be applied to a lithium secondary battery, reduce lithium ions during discharge, and oxidize during charge. For example, the positive electrode active material is a transition metal oxide or a compound based on sulfur (S). Specifically, the positive electrode active material is a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; 1+x Mn 2‐x O4 (0≦x≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1‐x M x Lithium nickel oxide with Ni site represented by O2 (M=Co, Mn, Al, Cu, Fe, Mg, B or Ga; 0.01≦x≦0.3); chemical formula LiMn 2‐x M x Lithium manganese composite oxide represented by Li2Mn3MO8 (M=Fe, Co, Ni, Cu, or Zn) or LiNi x Mn 2‐xLithium manganese oxides with spinel structure represented by O4; LiCoPO4; LiFePO4; and elemental sulfur (S8); Li2S n (n≧1), organic sulfur compounds or carbon-sulfur polymers (C2S x ) n The compound may include at least one of sulfur-containing compounds such as: x=2.5 to 50, n≧2.
[0067] When the positive electrode active material is a compound containing sulfur, the lithium secondary battery may be a lithium-sulfur battery.
[0068] In addition, when the positive electrode active material is sulfur element, since it does not have electrical conductivity by itself, it is used in combination with a conductive material such as a porous carbon material. In this case, the positive electrode active material may be a sulfur-carbon composite.
[0069] The porous carbon material provides a framework to which sulfur, a positive electrode active material, can be uniformly and stably fixed, and compensates for the low electrical conductivity of sulfur, allowing the electrochemical reaction to proceed smoothly.
[0070] The porous carbon material may be any material commonly used in the art that has a porous structure or a high specific surface area. For example, the porous carbon material may be at least one selected from the group consisting of graphite, graphene, carbon black such as denka black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, carbon nanotubes (CNTs) such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs), carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs), graphite such as natural graphite, artificial graphite, and expanded graphite, and activated carbon.
[0071] The sulfur-carbon composite may contain 60 to 90 parts by weight, preferably 65 to 85 parts by weight, more preferably 70 to 80 parts by weight of sulfur based on 100 parts by weight of the sulfur-carbon composite. If the sulfur content is less than the above range, the content of the porous carbon material in the sulfur-carbon composite is relatively high, so that the specific surface area increases and the binder content increases during the preparation of the positive electrode. This increase in the amount of binder used may ultimately increase the surface resistance of the positive electrode and act as an insulator that prevents electron pass, thereby reducing the battery performance. On the other hand, if the sulfur content exceeds the above range, the sulfur that could not be bonded to the porous carbon material may gather together or be re-sprouted on the surface of the porous carbon material, making it difficult for it to receive electrons and therefore unable to participate in the electrochemical reaction, resulting in a loss of battery capacity.
[0072] In addition, in the sulfur-carbon composite, the sulfur is located at least in one of the inner and outer surfaces of the porous carbon material, and may be present in an area of less than 100%, preferably 1 to 95%, more preferably 60 to 90% of the entire inner and outer surfaces of the porous carbon material. When the sulfur is present in the inner and outer surfaces of the porous carbon material within the above range, it can exhibit the maximum effect in terms of electron transfer area and wettability with the electrolyte. Specifically, in the above range, the sulfur is thinly and uniformly impregnated in the inner and outer surfaces of the porous carbon material, so that the electron transfer contact area during charging and discharging can be increased. If the sulfur is located in 100% of the entire inner and outer surfaces of the porous carbon material, the carbon material is completely covered with sulfur, which reduces wettability with the electrolyte and reduces contact with the conductive material contained in the electrode, making it unable to transfer electrons and unable to participate in the electrochemical reaction.
[0073] The method for producing the sulfur-carbon composite is not particularly limited in the present invention, and may be a method commonly used in the art. For example, the sulfur and the porous carbon material may be simply mixed and then heat-treated to form a composite.
[0074] The positive electrode active material may be included in an amount of 40 to 95 wt%, preferably 50 to 90 wt%, and more preferably 60 to 85 wt%, based on 100 wt% of the entire positive electrode active material layer constituting the positive electrode. If the content of the positive electrode active material is less than the above range, the electrochemical reaction of the positive electrode is difficult to fully exhibit, and conversely, if it exceeds the above range, the contents of the conductive material and binder described below are relatively insufficient, causing an increase in the resistance of the positive electrode and a deterioration in the physical properties of the positive electrode.
[0075] The positive electrode active material layer may further include a conductive material for allowing electrons to move smoothly within the positive electrode and a binder for better adhesion of the positive electrode active material to a current collector.
[0076] The conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path through which electrons move from a current collector to the positive electrode active material, and can be used without limitation as long as it has electrical conductivity.
[0077] For example, the conductive material may be graphite such as natural graphite or artificial graphite; carbon black such as Super-P, Denka Black, acetylene black, Ketjen Black, channel black, furnace black, lamp black, thermal black, or carbon black; carbon derivatives such as carbon nanotubes or fullerene; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorinated carbon, aluminum powder, or nickel powder; or conductive polymers such as polyaniline, polythiophene, polyacetylene, or polypyrrole, which may be used alone or in combination.
[0078] The conductive material may be included in an amount of 0.01 to 30 wt % based on 100 wt % of the entire positive active material layer. If the conductive material content is less than this range, the electron transfer between the positive active material and the current collector is not easy, resulting in a decrease in voltage and capacity. On the other hand, if the conductive material content exceeds this range, the proportion of the positive active material is relatively decreased, resulting in a decrease in the total energy (charge) of the battery, so it is preferable to determine the appropriate content within the above range.
[0079] The binder supports the positive electrode active material on the positive electrode current collector and organically connects the positive electrode active material to enhance the binding strength therebetween, and any binder known in the art may be used.
[0080] For example, the binder may be one or a mixture or copolymer of two or more selected from the group consisting of fluororesin-based binders including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.
[0081] The binder may be included in an amount of 0.5 to 30 wt % based on 100 wt % of the entire positive electrode active material layer. If the content of the binder is less than this range, the physical properties of the positive electrode may be deteriorated and the positive electrode active material, additives or conductive material in the positive electrode may fall off, and if the content exceeds this range, the ratio of the positive electrode active material and conductive material in the positive electrode may relatively decrease, resulting in a decrease in battery capacity, so it is preferable to determine the appropriate content within the above range.
[0082] In the present invention, the method for manufacturing the positive electrode for the lithium-sulfur battery is not particularly limited, and any method known to those skilled in the art or various methods modified therefrom may be used.
[0083] For example, the positive electrode for the lithium-sulfur battery is manufactured by preparing a positive electrode slurry composition including the above-mentioned composition, and then coating the positive electrode slurry composition on at least one surface of the positive electrode current collector to form the positive electrode active material layer.
[0084] The positive electrode slurry composition includes the positive electrode active material, the conductive material, the binder, and the additives, and may further include a solvent.
[0085] The solvent is one that can uniformly disperse the positive electrode active material, additives, conductive material, and binder. As such a solvent, water is most preferred as an aqueous solvent, and the water is distilled water or deionized water. However, the solvent is not necessarily limited thereto, and if necessary, a lower alcohol that can be easily mixed with water can be used. Examples of the lower alcohol include methanol, ethanol, propanol, isopropanol, and butanol, and these can be preferably mixed with water before use.
[0086] The content of the solvent may be at a level having a concentration that allows easy coating, and the specific content varies depending on the coating method and device.
[0087] The positive electrode slurry composition may further include, as necessary, a substance commonly used in the relevant technical field for the purpose of improving its function, etc., such as a viscosity modifier, a fluidizing agent, a filler, etc.
[0088] The method of applying the positive electrode slurry composition is not particularly limited in the present invention, and examples of the method include doctor blade, die casting, comma coating, screen printing, etc. In addition, the positive electrode slurry may be applied onto the positive electrode current collector by a pressing or lamination method after forming the positive electrode slurry on a substrate separately.
[0089] After the coating, a drying process may be performed to remove the solvent. The drying process is performed at a temperature and time level that allows the solvent to be sufficiently removed, and the conditions may vary depending on the type of solvent, and are not particularly limited in the present invention. Examples include drying with warm air, hot air, or low humidity air, vacuum drying, and drying by irradiation with (far) infrared rays and electron beams. The drying speed is usually adjusted so that the solvent can be removed as quickly as possible within a speed range that does not cause cracks in the positive electrode active material layer due to stress concentration or the positive electrode active material layer to peel off from the positive electrode current collector.
[0090] Furthermore, after the drying, the current collector can be pressed to increase the density of the positive electrode active material in the positive electrode. Examples of the pressing method include die pressing and roll pressing.
[0091] The positive electrode manufactured by the above-mentioned composition and manufacturing method, specifically the porosity of the positive electrode active material layer, is 50 to 80%, preferably 60 to 75%. If the porosity of the positive electrode is less than 50%, the filling degree of the positive electrode slurry composition including the positive electrode active material, the conductive material and the binder is too high, and sufficient electrolyte capable of showing ionic conduction and / or electrical conduction between the positive electrode active material is not maintained, so that the output characteristics and cycle characteristics of the battery may be reduced, and the overvoltage and discharge capacity reduction of the battery may become severe. On the other hand, if the porosity of the positive electrode is too high, exceeding 80%, there is a problem that the physical and electrical connection with the current collector is reduced, the adhesion is reduced, and the reaction is difficult, and the high porosity is filled with electrolyte, so that the energy density of the battery may be reduced, so it is appropriately adjusted within the above range.
[0092] In addition, the sulfur loading amount of the positive electrode according to the present invention, i.e., the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode, is 0.5 to 15 mg / cm. 2 , preferably 1 to 10 mg / cm 2 It is.
[0093] The negative electrode is as described above.
[0094] The electrolyte is disposed between the positive and negative electrodes and serves to cause an electrochemical oxidation or reduction reaction between the positive and negative electrodes through the electrolyte, and includes a lithium salt and a non-aqueous organic solvent.
[0095] The lithium salt can be used without any limitation as long as it is one that can be generally used in lithium secondary batteries.
[0096] Specific examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10, LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2 (lithium bis(trifluoromethanesulfonyl)imide; LiTFSI), LiN(C2F5SO2)2, LiN(SO2F)2 (lithium bis(fluorosulfonyl)imide; LiFSI), lithium chloroborane, lithium lower aliphatic carboxylates, lithium tetraphenylborate, and lithium imide.
[0097] The concentration of the lithium salt is 0.2 to 4 M, specifically 0.6 to 2 M, more specifically 0.7 to 1.7 M, depending on several factors such as the composition of the electrolyte, the solubility of the lithium salt, the conductivity of the dissolved lithium salt, the charging and discharging conditions of the battery, the operating temperature, and other factors known in the field of lithium secondary batteries. If the lithium salt is used at a concentration of less than 0.2 M, the conductivity of the electrolyte may be reduced, resulting in a decrease in electrolyte performance, and if the lithium salt is used at a concentration of more than 4 M, the viscosity of the electrolyte may increase, resulting in a decrease in the mobility of lithium ions.
[0098] The non-aqueous organic solvent may be any organic solvent commonly used in electrolytes for lithium secondary batteries, without any limitation. For example, the organic solvent may be ether, ester, amide, linear carbonate, cyclic carbonate, etc., which may be used alone or in combination of two or more. Among them, a representative example may include an ether-based compound.
[0099] The ether-based compound may include acyclic ethers and cyclic ethers.
[0100] For example, the acyclic ether may be at least one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, dimethoxyethane, diethoxyethane, ethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, and polyethylene glycol methyl ethyl ether, but is not limited thereto.
[0101] As an example, the cyclic ethers include 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, 2,5-dimethoxytetrahydrofuran, 2-ethoxytetrahydrofuran, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, 2-ethyl-2-methyl-1,3-dioxolane, tetrahydropyran, 1,4-dioxane, 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4-dimethoxybenzene, isosorbide dimethyl ether, ether), but is not limited thereto.
[0102] The ester compound may be any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, or a mixture of two or more of these may be used, but is not limited thereto.
[0103] Specific examples of the linear carbonate compound include, but are not limited to, any one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, or a mixture of two or more of these.
[0104] Specific examples of the cyclic carbonate compound include any one or mixtures of two or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halides thereof. Examples of halides thereof include, but are not limited to, fluoroethylene carbonate (FEC).
[0105] In addition to the above-mentioned non-aqueous organic solvents, the solvent may contain one or more selected from the group consisting of N-methylpyrrolidone, dimethyl sulfoxide, sulfolane furan, 2-methylfuran, 3-methylfuran, 2-ethylfuran, 2-propylfuran, 2-butylfuran, 2,3-dimethylfuran, 2,4-dimethylfuran, 2,5-dimethylfuran, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzofuran, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene, and 2,5-dimethylthiophene.
[0106] In addition to the above-mentioned composition, the electrolyte may further include a nitrate-based compound commonly used in the relevant technical field, such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), magnesium nitrate (Mg(NO3)2), barium nitrate (BaNO3)2), lithium nitrite (LiNO2), potassium nitrite (KNO2), and cesium nitrite (CsNO2).
[0107] The electrolyte injection may be performed at a suitable stage during the battery manufacturing process depending on the manufacturing process and required properties of the final product, i.e., before or at the final assembly stage of the battery.
[0108] A separator may further be included between the positive electrode and the negative electrode.
[0109] The separator separates or insulates the positive electrode and the negative electrode from each other and allows lithium ions to be transported between the positive electrode and the negative electrode. The separator may be made of a porous non-conductive or insulating material, and may be any material that is generally used as a separator in a lithium secondary battery without any particular limitations. The separator may be an independent member such as a film, or may be a coating layer added to the positive electrode and / or the negative electrode.
[0110] The separation membrane is preferably one that has low resistance to the ion migration of the electrolyte and has excellent moisture-absorbing capacity for the electrolyte.
[0111] The separator may be made of a porous substrate. The porous substrate may be any porous substrate typically used in secondary batteries. A porous polymer film may be used alone or in combination. For example, a nonwoven fabric or a polyolefin-based porous membrane made of high-melting-point glass fiber, polyethylene terephthalate fiber, or the like may be used, but is not limited thereto.
[0112] The material of the porous substrate is not particularly limited in the present invention, and any porous substrate generally used in electrochemical devices may be used. For example, the porous substrate may be a polyolefin such as polyethylene or polypropylene, a polyester such as polyethyleneterephthalate or polybutyleneterephthalate, a polyamide, a polyacetal, a polycarbonate, a polyimide, a polyetheretherketone, a polyethersulfone, a polyphenyleneoxide, a polyphenylenesulfide, a polyethylenenaphthalate, a polytetrafluoroethylene, a polyvinylidene fluoride, a polyvinyl chloride, or the like. The material may include one or more materials selected from the group consisting of poly(p-phenylene benzobisoxazole), polyacrylonitrile, cellulose, nylon, poly(p-phenylene benzobisoxazole), and polyarylate.
[0113] The thickness of the porous substrate is not particularly limited, but is 1 to 100 μm, preferably 5 to 50 μm. The thickness range of the porous substrate is not limited to the above range, but if the thickness is smaller than the above lower limit, the mechanical properties may be deteriorated and the separator may be easily damaged during use of the battery.
[0114] The average diameter and porosity of the pores in the porous substrate are not particularly limited, but are in the range of 0.001 to 50 μm and 10 to 95%, respectively.
[0115] The lithium secondary battery of the present invention can be classified into cylindrical, square, coin, pouch, etc. according to shape, and into bulk type and thin film type according to size. The structure and manufacturing method of these batteries are widely known in this field, so detailed description will be omitted.
[0116] The present invention also provides a battery module including the lithium secondary battery as a unit cell.
[0117] The battery module can be used as a power source for medium to large-sized devices that require high temperature stability, long cycle characteristics, and high capacity characteristics.
[0118] Examples of the medium- to large-sized devices include, but are not limited to, power tools that are powered by battery-powered motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems.
[0119] In the following, preferred examples are presented to facilitate understanding of the present invention. However, the following examples are merely illustrative of the present invention, and it will be obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present invention. It is natural that such changes and modifications fall within the scope of the accompanying claims.
[0120] Examples and Comparative Examples [Example 1] (1) Lithium electrode manufacturing In one reactor, 0.1 g of hexagonal boron nitride was dispersed in 100 ml of tetrahydrofuran using an ultrasonic dispersion device to prepare a first solution.
[0121] In another reactor, 1.0 g of PIM-1 (Mw: 10,000 g / mol) was dissolved in 50 ml of tetrahydrofuran to prepare a second solution.
[0122] The first and second solutions prepared above were mixed to prepare a coating solution for forming a protective layer.
[0123] The coating solution was applied to the surface of a 30 μm-thick lithium metal layer using a bar coating process, and then dried for 12 hours in a vacuum oven at 80° C. to prepare a lithium electrode including a 0.5 μm-thick protective layer. At this time, the weight ratio of hexagonal boron nitride and PIM-1 included in the protective layer was 1:10.
[0124] (2) Lithium-sulfur battery manufacturing A positive electrode slurry composition was prepared by mixing 90 wt% of sulfur-carbon composite (S:C = 75:25 (weight ratio)) as a positive electrode active material, 5.0 wt% of Denkaburlec as a conductive material, and 5.0 wt% of styrene butadiene rubber / carboxymethyl cellulose (SBR:CMC = 70:30 (weight ratio)) as a binder.
[0125] The positive electrode slurry composition was applied onto an aluminum collector having a thickness of 20 μm, dried at 50° C. for 12 hours, and pressed using a roll press to prepare a positive electrode. At this time, the loading amount of the positive electrode active material was 5.4 mAh / cm 2 and the porosity of the positive electrode was 68%.
[0126] The prepared positive electrode and the lithium electrode (negative electrode) prepared in (1) were placed facing each other, a polyethylene separator having a thickness of 20 μm and a porosity of 68% was interposed between them, and 0.1 ml of electrolyte was injected to prepare a lithium-sulfur battery.
[0127] The electrolyte used was a mixture of 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1% by weight lithium nitrate (LiNO3) dissolved in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME = 1:1 (volume ratio)).
[0128] [Example 2] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that in the preparation of the first solution, 0.1 g of molybdenum disulfide was used instead of 0.1 g of hexagonal boron nitride, and thus the weight ratio of molybdenum disulfide to PIM-1 contained in the protective layer was 1:10.
[0129] [Example 3] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that in preparing the first solution, 0.1 g of graphene oxide was used instead of 0.1 g of hexagonal boron nitride, and thus the weight ratio of graphene oxide to PIM-1 contained in the protective layer was 1:10.
[0130] [Example 4] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that in the preparation of the first solution, 0.1 g of graphite carbon nitride was used instead of 0.1 g of hexagonal boron nitride, and thus the weight ratio of graphite carbon nitride to PIM-1 contained in the protective layer was 1:10.
[0131] [Comparative Example 1] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that a 30 μm-thick lithium metal thin film without a protective layer was used as the negative electrode.
[0132] [Comparative Example 2] The same procedure as in Example 1 was carried out, except that 1.0 g of PIM-1 (Mw: 10,000 g / mol) was dissolved in 50 ml of tetrahydrofuran, and the resulting solution was used as a coating solution for forming a protective layer. A lithium-sulfur battery was manufactured using a lithium electrode on which a protective layer containing only PIM-1 was formed.
[0133] [Comparative Example 3] A lithium-sulfur battery was manufactured using a lithium electrode having a protective layer formed thereon, which was prepared by dissolving 0.1 g of hexagonal boron nitride and 1.0 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-co-HFP) polymer in 150 ml of tetrahydrofuran as a coating solution for forming a protective layer, in the same manner as in Example 1.
[0134] Experimental example 1. Surface evaluation of lithium electrodes The surfaces of the lithium electrodes prepared in Examples 1 to 4 and the lithium metal thin film of Comparative Example 1 were observed with the naked eye and with a scanning electron microscope (SEM). The scanning electron microscope used was Hitachi S-4800, and the results are shown in Figures 1 and 2.
[0135] As shown in FIG. 1, in the case of the lithium electrodes according to Examples 1 to 4, it can be seen that a yellow coating layer was formed compared to Comparative Example 1 due to the intrinsic porous polymer.
[0136] Also, referring to FIG. 2, it can be seen that the surface of the lithium metal layer is coated with a two-dimensional material and an intrinsic porous polymer in the form of a film.
[0137] Experimental Example 2. Battery performance evaluation The performance of the batteries manufactured in the examples and comparative examples was evaluated using a charge / discharge measuring device (model: LAND CT-2001A, manufactured by Wuhan Co., Ltd.).
[0138] Specifically, the battery was discharged at 25°C at a current density of 0.1C to 1.8V, and then charged at a current density of 0.1C to 2.5V for three cycles, and then charged and discharged at a current density of 0.2C for three cycles in the same voltage range, discharged at a current density of 0.5C, and charged at a current density of 0.3C to evaluate the capacity and life characteristics of the battery. The results are shown in Table 1 and Figures 3 and 4.
[0139] [Table 1]
[0140] As shown in FIGS. 3 and 4 and Table 1, it can be seen that the life characteristics of the batteries according to the embodiments are superior to those of the comparative examples.
[0141] 3 and 4, the batteries according to Comparative Examples 1 to 3 are relatively inferior in discharge capacity to the batteries according to Examples 1 to 4, and also have poor capacity retention, i.e., poor life characteristics.
[0142] In particular, referring to FIG. 4 and Table 1, Comparative Example 2 is a case where a protective layer is formed on a lithium metal layer using only an intrinsic porous polymer, PIM-1, and it can be seen that the discharge capacity is lower than that of Comparative Example 1 where no protective layer is formed, and the capacity retention rate is also at a similar level to that of Comparative Example 1. This shows that in order to improve the capacity and life characteristics of a battery, the protective layer of the lithium electrode must contain both an intrinsic porous polymer and a two-dimensional material. In addition, Examples 3 and 4 show superior capacity retention rates compared to Examples 1 and 2, and therefore it can be seen that the two-dimensional materials, graphene oxide and graphite carbon nitride, are effective in improving the life characteristics of a battery.
Claims
1. A lithium electrode comprising: a lithium metal layer; and a protective layer formed on at least one surface of the lithium metal layer, The protective layer is made of a two-dimensional material and an intrinsically porous polymer, The intrinsic porosity polymer is represented by the following formula 1: 【Chemistry 1】 A lithium electrode comprising a repeating structure represented by:
2. 2. The lithium electrode of claim 1, wherein the two-dimensional material comprises at least one selected from the group consisting of graphene, graphene oxide, molybdenum disulfide, hexagonal boron nitride, and graphitic carbon nitride.
3. 3. The lithium electrode of claim 2, wherein the two-dimensional material comprises at least one selected from the group consisting of graphene oxide and graphitic carbon nitride.
4. 2. The lithium electrode of claim 1, wherein the weight ratio of the two-dimensional material to the intrinsic porosity polymer is 1:1 to 1:
20.
5. 2. The lithium electrode according to claim 1, wherein the protective layer has a thickness of 0.1 to less than 5 μm.
6. 2. The lithium electrode of claim 1, wherein the lithium metal layer has a thickness of 20 μm to 200 μm.
7. (a) dispersing a two-dimensional material in a first solvent to prepare a first solution; (b) dissolving an intrinsic porosity polymer in a second solvent to prepare a second solution; (c) mixing the first solution and the second solution to prepare a coating liquid; and 2. The method for producing a lithium electrode according to claim 1, further comprising: (d) applying the coating liquid to at least one surface of the lithium metal layer.
8. 8. The method of claim 7, wherein the first solvent and the second solvent are the same or different and include at least one selected from the group consisting of tetrahydrofuran, toluene, cyclohexane, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, tetramethylurea, dimethylsulfoxide, and triethylphosphate.
9. a positive electrode comprising a positive electrode active material; A negative electrode comprising the lithium electrode of claim 1; and A lithium secondary battery comprising an electrolyte interposed between the positive electrode and the negative electrode.
10. The lithium secondary battery according to claim 9 , wherein the positive electrode active material comprises a compound containing sulfur.
11. The lithium secondary battery of claim 10, wherein the lithium secondary battery is a lithium-sulfur battery.
Citation Information
Patent Citations
Lithium sulfur battery and manufacturing method thereof
JP2020013731A
Heat dissipation element
JP2020535241A
Lithium metal secondary battery with improved extended performances
KR1020190117275A
KR2016‐0052351
KR2018‐0041086