Separator for lithium secondary battery and method for producing same

A porous base material with a MOF layer formed via the Langmuir-Blodgett method addresses the shuttle phenomenon in lithium-sulfur batteries, enhancing their cycle performance and stability by suppressing lithium polysulfide permeation.

JP7566140B2Active Publication Date: 2024-10-11LG ENERGY SOLUTION LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023513236
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-27
Filing Date
2022-01-27
Publication Date
2024-10-11
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Lithium-sulfur secondary batteries suffer from poor cycle characteristics due to the shuttle phenomenon caused by polysulfides eluted from the positive electrode, which is not effectively addressed by existing separation membranes.

Method used

A separation membrane for lithium secondary batteries is developed, comprising a porous base material with a metal-organic frameworks (MOF) layer formed on one or both sides, using the Langmuir-Blodgett method to create a uniform and thin coating that suppresses lithium polysulfide permeation.

Benefits of technology

The membrane effectively prevents the shuttle phenomenon, improving the cycle performance and stability of lithium-sulfur secondary batteries by controlling lithium polysulfide movement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566140000003
    Figure 0007566140000003
  • Figure 0007566140000004
    Figure 0007566140000004
  • Figure 0007566140000005
    Figure 0007566140000005
Patent Text Reader

Abstract

The present invention relates to a separator for a lithium secondary battery and a manufacturing method thereof. More specifically, the separator includes an MOF layer formed by the Langmuir-Blodgett method, and can prevent a shuttle phenomenon caused by polysulfides eluted from a cathode containing a sulfur-containing material, thereby improving the cycle stability of the lithium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 2021-0011577 filed on January 27, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a separator for a lithium secondary battery and a method for manufacturing the same. [Background technology]

[0003] The lithium-sulfur (Li-S) secondary battery, which is an energy storage device, has a theoretical energy density of 2600Wh / kg and a theoretical capacity of 1672mAh / g, which is 3 to 5 times higher than conventional lithium batteries, and is therefore attracting attention as a next-generation energy storage device. However, there is a problem that the cycle characteristics are not good enough for commercial use.

[0004] The poor cycle characteristics of lithium-sulfur secondary batteries are due to the shuttle phenomenon caused by polysulfide eluted from the positive electrode. In order to effectively suppress the shuttle phenomenon that occurs in lithium-sulfur secondary batteries, it is necessary to prevent lithium polysulfide, a reaction intermediate, from leaking to the negative electrode.

[0005] Generally, the transfer and exchange of materials between the positive and negative electrodes in a battery is carried out through a separator, and the cycle characteristics of the lithium-sulfur secondary battery can be controlled by the separator.

[0006] China Patent Publication No. 110729439 relates to a separator for lithium-ion batteries in which MOFs are coated on the surface of a polyolefin separator, and the polyolefin separator coated with MOFs can have the effect of improving the stability of the battery.

[0007] Korean Patent Publication No. 2016-0126503 relates to a composite separator for lithium secondary batteries, in which multiple metal compound layers are formed on the surface of a porous polymer substrate by atomic layer deposition (ALD).

[0008] Thus, in the past, when manufacturing a separator, a method of coating using already grown crystals was adopted, rather than coating using the Langmuir-Blodgett method. When coating using already grown crystals, the uniformity of the coating is determined by the spacing between the crystals (several hundred nanometers to several micrometers), but this has the disadvantage that it is difficult to see the influence of the pore size (several angstroms) of the crystals that form the coating. In addition, with the conventional coating method, an uneven coating can be formed when forming the separator, which can cause problems such as the thickness becoming too thick and acting as resistance when the battery is running.

[0009] As described above, existing separator manufacturing methods have limitations in forming a uniform and thin coating layer. Therefore, there is a need to develop a separator manufacturing technology that can form a uniform and thin coating layer on the separator to minimize battery resistance and prevent the shuttle phenomenon. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] China Patent Publication No. 110729439 [Patent Document 2] Korean Patent Publication No. 2016-0126503 Summary of the Invention [Problem to be solved by the invention]

[0011] Therefore, the present invention provides a separator capable of preventing the shuttle phenomenon caused by lithium polysulfide, which is an intermediate product generated by polysulfide eluted from the positive electrode of a lithium-sulfur secondary battery.

[0012] SUMMARY OF THE PRESENTLY PREFERRED EMBODIMENTS OF THE PRESENT EMBODIMENT An object of the present invention is to provide a separator for a lithium secondary battery, which has high permeability to lithium ions and can effectively inhibit the permeation of lithium polysulfide, and a method for manufacturing the same. [Means for solving the problem]

[0013] To achieve the above object, the present invention provides a separator for a lithium secondary battery, comprising: a porous substrate; and a metal organic frameworks (MOF) layer formed on one or both sides of the porous substrate, wherein the MOF layer comprises one or more MOF molecular films and has an amorphous structure.

[0014] The present invention further provides a method for producing a separator for a lithium secondary battery, comprising the steps of: (S1) mixing an aqueous solution containing a zinc precursor with an organic solution containing an organic ligand precursor to form a MOF molecular membrane; and (S2) depositing the MOF molecular membrane on a surface of a porous substrate, the deposition being performed by the Langmuir-Blodgett method. Effect of the Invention

[0015] The separator for a lithium secondary battery according to the present invention can prevent a shuttle phenomenon caused by polysulfides that can occur in a battery including a sulfur-containing material as a positive electrode active material, thereby improving the cycle performance of the battery. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a schematic diagram of a manufacturing process of a lithium-sulfur secondary battery according to the present invention. [Diagram 2]The following shows a photograph of a SiO2 substrate whose surface has been partially coated by the Langmuir-Blodgett technique and a scanning electron microscope (SEM) photograph. [Diagram 3] This is a graph (2-theta scale) showing the XRD analysis results of MOF layers deposited on a porous substrate of a separator by the Langmuir-Blodgett method, the XRD analysis results of MOF layers formed by deposition once (1 Layer), five times (5 Layers), and twenty times (20 Layers). [Figure 4] 1 is a graph showing the results of FT-IR analysis of terephthalic acid used as an organic ligand precursor in Example 1 and an MOF layer (Langmuir layer). [Diagram 5] 1 is a graph showing the correlation between molecular spacing and surface tension when a MOF-5 molecular film is formed at room temperature. [Figure 6A] 1 is a graph showing a vertical cross-sectional photograph and thickness of a MOF layer formed in a separation membrane of Example 1. [Figure 6B] These are AFM images showing the surface characteristics of MOF layers formed by the Langmuir-Blodgett technique depending on the number of deposition processes. [Figure 7] Photographs showing experimental results on the polysulfide filtration effect of MOF materials. [Figure 8] 1 is a graph showing the results of a long-term cycle performance experiment on the lithium-sulfur secondary batteries of Examples 1 and 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will now be described in further detail to aid in the understanding of the present invention.

[0018] The terms or words used in this specification and claims should not be interpreted in a limited manner to their ordinary or dictionary meaning, but should be interpreted in a meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to explain his / her invention in the best possible manner.

[0019] The term "Langmuir-Blodgett (LB)" used in this specification refers to a technique in which a thin film layer made of a monolayer is transferred to a support while the support passes vertically through the thin film layer, so that a thin film layer is formed on the support. According to the Langmuir-Blodgett method, a thin film layer that is densely aligned can be deposited on a support.

[0020] Separator for lithium secondary batteries The present invention relates to a separator for a lithium secondary battery, the separator comprising a porous substrate and a metal organic frameworks (MOF) layer formed on one or both sides of the porous substrate, the MOF layer including one or more MOF molecular membranes and having an amorphous structure, the MOF layer being a molecular membrane in the form of a stack of a number of uniform MOF molecular membranes.

[0021] In general, in a lithium secondary battery containing a sulfur-containing material as a positive electrode active material, polysulfide is dissolved from the positive electrode during charging and discharging, and lithium polysulfide (LiPS) is generated by a side reaction of the dissolved polysulfide. The LiPS causes a shuttle phenomenon, which reduces the cycle stability of the battery.

[0022] In order to suppress such a shuttle phenomenon, it is advantageous for the separation membrane to have physical properties that can suppress the permeation of LiPS and thus the elution of LiPS.

[0023] In the present invention, the porous substrate included in the separator for a lithium secondary battery separates or insulates the anode and cathode from each other and allows lithium ions to be transported between the cathode and anode. Therefore, the separator of the present invention may be porous and made of a non-conductive or insulating material.

[0024] Specifically, the porous substrate may be a porous polymer film alone or in a laminated state thereof, for example, a nonwoven fabric made of high melting point glass fiber, polyethylene terephthalate fiber, or the like, or a polyolefin-based porous film, but is not limited thereto.

[0025] The material of the porous substrate is not particularly limited in the present invention, and any porous substrate generally used in electrochemical devices can be used. For example, the porous substrate can be made of a material selected from the group consisting of polyolefins such as polyethylene and polypropylene, polyesters such as polyethyleneterephthalate and polybutyleneterephthalate, polyamides, polyacetals, polycarbonates, polyimides, polyetheretherketones, polyethersulfones, polyphenyleneoxides, polyphenylenesulfides, polyethylenenaphthalates, polytetrafluoroethylenes, polyvinylidene fluorides, polyvinyl chlorides, and the like. The material may include one or more materials selected from the group consisting of poly(p-phenylene benzobisoxazole), polyacrylonitrile, cellulose, nylon, poly(p-phenylene benzobisoxazole), and polyarylate.

[0026] In addition, the thickness of the porous substrate is not particularly limited, but may be 1 μm to 100 μm, specifically, 1 μm or more, 5 μm or more, or 10 μm or more, and may be 50 μm or less, 60 μm or less, 70 μm or less, 80 μm or less, or 100 μm or less. The thickness range of the porous substrate is not limited to the above range, but if the thickness is less than the above lower limit, the mechanical properties are reduced and the separator is easily damaged during use of the battery.

[0027] In the present invention, the MOF layer included in the separator for lithium secondary batteries can physically suppress the dissolution of LiPS by adjusting the pore size, and when the MOF is doped with a foreign atom, it can adsorb LiPS or electrically suppress the dissolution of LiPS through electrical repulsion between the separator and LiPS.

[0028] When the MOF is doped with a heteroatom, the heteroatom may include one or more selected from N, S, and O. The N, S, or O may have a high adsorption efficiency for LiPS.

[0029] The MOF layer may include one or more MOF molecular films, and more specifically, may be a laminate of the one or more MOF molecular films.

[0030] The thickness of the MOF layer can be 0.5 nm to 20 nm, specifically, 0.5 nm or more, 0.8 nm or more, or 1 nm or more, and may be 10 nm or less, 15 nm or less, or 20 nm or less. If the thickness of the MOF layer is less than 0.5 nm, it may be difficult to form the MOF layer itself, and if it exceeds 20 nm, the resistance of the battery may increase, the time required for MOF synthesis may increase, and the uniformity of the MOF layer may decrease.

[0031] In addition, the MOF layer may have an amorphous structure, which has the advantage of being more resistant to physical deformation than a MOF layer having a crystalline structure.

[0032] In addition, the MOF layer may have a uniform surface. Specifically, the surface roughness Rq may be 0 nm to 1.0 nm, and Rq may be 0 nm to 1.0 nm. Specifically, the Ra may be 0 nm or more, 0.1 nm or more, or 0.3 nm or more, and 0.4 nm or less, 0.7 nm or less, or 1.0 nm or less, and the Ra may be 0 nm or more, 0.2 nm or more, or 0.3 nm or more, and 0.6 nm or less, 0.8 nm or less, or 1.0 nm or less. If the Rq or Ra is out of the above range, the surface characteristics of the MOF layer are poor, which may adversely affect the battery life. In the case of the Ra and Rq, the lower the numerical value, the higher the uniformity.

[0033] The Rq is the mean square surface roughness and the Ra is the arithmetic surface roughness, which can be measured by an AFM (Atomic Force Microscope) using a specimen of the MOF layer.

[0034] Method for manufacturing separator for lithium secondary battery The present invention further relates to a method for producing a separator for a lithium secondary battery, comprising: (S1) mixing an aqueous solution containing a zinc precursor with an organic solution containing an organic ligand precursor to form an MOF molecular membrane; and (S2) depositing the MOF molecular membrane on a surface of a porous substrate, the deposition being performed by a Langmuir-Blodgett (LB) method.

[0035] Hereinafter, each step of the method for preparing a separator for a lithium secondary battery according to the present invention will be described in detail.

[0036] In the step (S1), an aqueous solution containing a zinc precursor and an organic solution containing an organic ligand precursor can be mixed to form a MOF molecular membrane.

[0037] When the organic solution containing the organic ligand precursor is mixed into the aqueous solution containing the zinc precursor in a dropwise manner, it may be more advantageous for the formation of the MOF molecular film. If the simple mixing is performed instead of the dropwise method, a three-dimensional crystalline MOF may be formed instead of a two-dimensional molecular film on the surface of the aqueous solution, which may make coating via Langmuir-Blodgett (LB) difficult.

[0038] When an organic ligand dissolved in a volatile organic solvent is dropped into the aqueous solution containing the zinc precursor, the organic solvent evaporates and the ligand is synthesized only on the surface of the aqueous solution, thereby restricting the reaction to only the two-dimensional phase to form a molecular film.

[0039] The zinc precursor may be one or more selected from the group consisting of zinc acetate and zinc nitrate, and may be zinc acetate in terms of the efficiency of forming the MOF molecular film. When zinc nitrate is used, it may be used in the form of an aqueous solution containing zinc nitrate and trimethylamine.

[0040] The concentration of the aqueous zinc precursor solution may be 0.002 M to 0.01 M, specifically, 0.002 M or more or 0.003 M or more, and may be 0.006 M or less, 0.008 M or less, or 0.01 M or less. If the concentration of the aqueous zinc precursor solution is less than 0.002 M, the MOF layer may not be sufficiently formed, and if it is more than 0.01 M, the surface roughness characteristics may be reduced.

[0041] In addition, the organic ligand precursor may include one selected from the group consisting of terephthalic acid, 2-aminoterephthalic acid, 2-hydroxyterephthalic acid, and 2,5-mercaptoterephthalic acid. In terms of the efficiency of forming the MOF molecular film, the organic ligand precursor may be terephthalic acid or 2-aminoterephthalic acid.

[0042] The organic solution containing the organic ligand precursor may be prepared by dissolving the organic ligand precursor in an organic solvent.

[0043] The organic solvent may be one or more non-polar solvents selected from the group consisting of chloroform, cyclohexane, n-hexane, and toluene, but is not limited thereto. A wide range of non-polar solvents that allow a two-dimensional MOF molecular film to be synthesized on the surface of the zinc precursor aqueous solution can be used.

[0044] In the case of the organic ligand precursor organic solution, it is preferable to use a saturated solution since the ligand exhibits the characteristic of being almost insoluble in the organic solvent. If the concentration is lower than the saturated solution, it may be difficult to form a MOF layer, and if the concentration is higher than the saturated solution, it may be impossible to achieve due to physical limitations.

[0045] In the step (S2), the MOF molecular film can be deposited on the surface of a porous substrate using a Langmuir-Blodgett method, where the type and properties of the porous substrate are as described above.

[0046] The MOF molecular membrane formed in step (S1) is in a state of being suspended on the surface of the solution, and the suspended MOF molecular membrane can be deposited on the surface of a porous substrate.

[0047] According to the Langmuir-Blodgett method, an MOF layer may be formed on the surface of an aqueous solution by immediately bonding an organic ligand precipitated after evaporation of an aqueous solution containing metal ions and a volatile organic solvent that is not miscible with the aqueous solution with the metal ions on the aqueous solution. In this case, the organic ligand must have good reactivity, and the types of the organic solvent and the ligand are specified in consideration of this point as described above.

[0048] When the MOF molecular membrane formed in the step (S1) is passed through a porous substrate in a direction perpendicular to the substrate, the MOF molecular membrane is transferred to the porous substrate, and a MOF layer can be formed on the cross section of the porous substrate.

[0049] The MOF molecular membrane formed by the Langmuir-Blodgett method can be formed to a thin thickness. Generally, self-assembled membranes are thick with a minimum thickness of several micrometers, but the MOF molecular membrane formed by the Langmuir-Blodgett method can form a thin layer with a thickness of several nanometers. Therefore, a separator including the MOF molecular membrane formed by the Langmuir-Blodgett method can contribute to the miniaturization and weight reduction of batteries.

[0050] In addition, in MOF molecular membranes, physical adsorption characteristics are determined by the spacing between molecules rather than the pore characteristics of the molecules. For example, the density of coating on the surface of the substrate may change depending on the crystal size and shape of the MOF, which may cause performance differences in batteries (Electrochim.Acta, 2014, 129, 55-61; J.Power Sources, 2018, 389, 169-177; ACS Energy Letters, 2017, 2, 2362-2367). Therefore, the crystal size and shape of MOFs that can be applied to the Langmuir-Blodgett method can be easily controlled, which is advantageous for controlling battery performance.

[0051] In addition, the general ALD (Atomic Layer Deposition) method mainly synthesizes metal oxides, making it difficult to use it to synthesize MOF molecular films for use in separation membranes. Because ALD requires a high-temperature process, it is difficult to apply it to plastic separation membranes, which undergo thermal shrinkage at high temperatures, whereas the Langmuir-Blodgett method does not require a high-temperature process and can be applied to the manufacture of separation membranes.

[0052] Lithium secondary battery The present invention also relates to a lithium secondary battery comprising the separator described above.

[0053] The lithium secondary battery according to the present invention may include a positive electrode, a negative electrode, a separator interposed therebetween, and an electrolyte.

[0054] In the present invention, the positive electrode of the lithium secondary battery may include a positive electrode current collector and a positive electrode mixture layer formed on the positive electrode current collector and having a positive electrode active material.

[0055] As the positive electrode active material, a lithium-containing transition metal oxide is preferably used, for example, LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , Li(Ni a Co b Mn c )O 2 (0 <a<1、0<b<1、0<c<1、a+b+c=1)、LiNI 1-y Co y O 2 , LiCo 1-y Mn y O 2 , LiNi 1-y Mn y O 2 (O≦y<1), Li(Ni a Co b Mn c )O 4 (0 <a<2、0<b<2、0<c<2、a+b+c=2)、LiMn 2-z Ni z O 4 , LiMn 2-z Co z O 4 (0 <z<2)、LiCoPO 4 and LiFePO 4 Any one selected from the group consisting of or a mixture of two or more of these can be used. In addition to these oxides, sulfides, selenides, halides, etc. can also be used.

[0056] The positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and can be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc. In this case, the positive electrode current collector can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc., with fine irregularities formed on the surface so as to enhance adhesion to the positive electrode active material.

[0057] In the present invention, the negative electrode of the lithium secondary battery may include a negative electrode current collector and a negative electrode mixture layer having a negative electrode active material formed on the negative electrode current collector.

[0058] The negative electrode active material may be a carbon material capable of absorbing and releasing lithium ions, lithium metal, silicon, or tin. A carbon material may be preferably used, and low-crystalline carbon and high-crystalline carbon may be used. Typical low-crystalline carbons include soft carbon and hard carbon, and typical high-crystalline carbons include natural graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, mesocarbon microbeads, mesophase pitches, and high-temperature fired carbons such as petroleum or coal tar pitch derived cokes. In this case, the negative electrode may contain a binder, and various types of binder polymers such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, and polymethylmethacrylate may be used as the binder.

[0059] The negative electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and examples of the negative electrode current collector that can be used include copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, aluminum-cadmium alloy, etc. Similarly to the positive electrode current collector, the negative electrode current collector can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc., with fine irregularities formed on the surface.

[0060] In this case, the positive electrode mixture layer or the negative electrode mixture layer may further include a binder resin, a conductive material, a filler, and other additives.

[0061] The binder resin is used to bind the electrode active material and the conductive material and to bind the electrode active material to the current collector. Examples of such binder resins include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0062] The conductive material is used to further improve the conductivity of the electrode active material. Such a conductive material is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and summer black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.

[0063] The filler is selectively used as a component that suppresses the expansion of the electrode, and is not particularly limited as long as it is a fibrous material that does not induce chemical changes in the battery. For example, olefin polymers such as polyethylene and polypropylene; glass fiber, carbon fiber, and other fibrous substances are used.

[0064] In the present invention, the electrolyte may be a non-aqueous electrolyte, and the electrolyte salt contained in the non-aqueous electrolyte is a lithium salt. The lithium salt may be any of those commonly used in electrolytes for lithium secondary batteries without any restrictions. For example, the lithium salt may be LiFSI, LiPF 6 , LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 Cl 10 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiPF 6 , LiAlCl 4 , C.H. 3 SO 3 Li, C.F. 3 SO 3 Li, (CF 3 SO 2 ) 2 It may be one or more selected from the group consisting of NLi, lithium chloroborane, and lithium 4-phenylborate.

[0065] The organic solvent contained in the non-aqueous electrolyte can be any organic solvent commonly used in electrolytes for lithium secondary batteries, and can be used without limitation, for example, ethers, esters, amides, linear carbonates, cyclic carbonates, etc., each of which can be used alone or in combination of two or more. Among these, representative examples include cyclic carbonates, linear carbonates, or carbonate compounds that are slurries thereof.

[0066] Specific examples of the cyclic carbonate compound include ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halides thereof, or slurries of two or more of these. Examples of these halides include, but are not limited to, fluoroethylene carbonate (FEC).

[0067] In addition, specific examples of the linear carbonate compound include, but are not limited to, any one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, or a slurry of two or more of these. In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, are high-viscosity organic solvents with high dielectric constants, and can dissociate lithium salts in the electrolyte better. When such cyclic carbonates are mixed with linear carbonates with low viscosity and low dielectric constants, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte solution with higher electrical conductivity can be prepared.

[0068] The ether in the organic solvent may be any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, and ethyl propyl ether, or a slurry of two or more of these ethers, but is not limited thereto.

[0069] In addition, the ester in the organic solvent may be any one or two or more selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, but is not limited thereto.

[0070] The injection of the non-aqueous electrolyte may be performed at an appropriate stage during the manufacturing process of the electrochemical device depending on the manufacturing process and required properties of the final product, i.e., before assembly of the electrochemical device or at the final stage of assembly of the electrochemical device.

[0071] The lithium secondary battery according to the present invention can be manufactured by laminating (stack) and folding the separator and electrodes in addition to the general winding process.

[0072] The shape of the battery case is not particularly limited, and may be various shapes such as a cylindrical type, a laminated type, a square type, a pouch type, a coin type, etc. The structure and manufacturing method of these batteries are widely known in the art, so a detailed description will be omitted.

[0073] In addition, the lithium secondary batteries can be classified into various types of batteries, such as lithium-sulfur secondary batteries, lithium-air batteries, lithium-oxide batteries, and lithium solid-state batteries, depending on the positive and negative electrode materials used.

[0074] The present invention also provides a battery module including lithium secondary batteries as unit cells.

[0075] The battery module can be used as a power source for medium to large devices that require high temperature stability, long cycle characteristics, and high capacity characteristics.

[0076] Examples of the medium- to large-sized devices include, but are not limited to, power tools that are powered by battery-powered motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PLEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems.

[0077] Lithium-sulfur secondary battery The separator according to the present invention can be used as a separator for a lithium-sulfur secondary battery among lithium secondary batteries, for example, in the positive electrode of a lithium-sulfur secondary battery in a form in which a positive electrode active material is supported inside the porous carbon structure.

[0078] In this case, the lithium-sulfur secondary battery may be a battery containing sulfur as a positive electrode active material. Specifically, the positive electrode active material may include elemental sulfur (S8), a sulfur-based compound, or a mixture thereof. Specifically, the sulfur-based compound may be Li 2 Sn (n ≥ 1), organic sulfur compounds or carbon-sulfur polymers ((C 2 S x )n:x=2.5 to 50, n≧2), etc.

[0079] These sulfur substances are not electrically conductive by themselves, so they are sometimes combined with carbon materials to form sulfur-carbon composites and used in the positive electrodes of lithium-sulfur secondary batteries.

[0080] FIG. 1 is a schematic diagram of a manufacturing process of a lithium-sulfur secondary battery according to the present invention.

[0081] Referring to FIG. 1, after forming the MOF molecular membrane (Langmuir-Blodgett film), MOF layers are formed on both sides of a porous substrate, and a cell is assembled to manufacture a lithium-sulfur dual-cell battery.

[0082] Hereinafter, preferred examples will be presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present invention. It is to be understood that such changes and modifications fall within the scope of the appended claims.

[0083] Preliminary experiment example 1: Confirmation of coating layer formation using the Langmuir-Blodgett method An experiment was conducted to confirm whether a coating layer could be formed on a substrate using the Langmuir-Blodgett technique.

[0084] Terephthalic acid, which is an organic ligand precursor, was dissolved in chloroform solvent to prepare a saturated solution of the organic ligand precursor.

[0085] Zinc acetate, a zinc precursor, was dissolved in water to prepare an aqueous zinc precursor solution with a concentration of 0.002M.

[0086] The organic ligand precursor solution was added dropwise to the zinc precursor aqueous solution to form a MOF-5 molecular membrane.

[0087] Using a Langmuir-Blodgett instrument (KSV NIMA, KN2002), SIO 2 A portion of the surface of the substrate was coated with MOF-5 material.

[0088] Figure 2 shows a SiO 2The photographs show the substrate and SEM (Scanning Electron Microscope) images, and show that the coating layer can be formed by the Langmuir-Blodgett method. The SEM images were taken using a scanning electron microscope (JEOL Ltd., JSM-7100F).

[0089] It was confirmed that a coating layer can be formed on a porous substrate using the Langmuir-Blodgett method from the results of Preliminary Experimental Example 1. Therefore, in the following Examples and Comparative Examples, various types of separators were prepared using the Langmuir-Blodgett method according to the compositions shown in Table 1 below.

[0090] [Table 1]

[0091] Example 1 (1) Separation membrane production (1-1) Formation of MOF molecular membrane Terephthalic acid, which is an organic ligand precursor, was dissolved in chloroform solvent to prepare a saturated solution of the organic ligand precursor.

[0092] Zinc acetate, a zinc precursor, was dissolved in water to prepare an aqueous zinc precursor solution with a concentration of 0.002M.

[0093] The organic ligand precursor solution was added dropwise to the zinc precursor aqueous solution to form a MOF-5 molecular membrane.

[0094] (1-2) Deposition of MOF layer on porous substrate As a porous substrate, a polypropylene (PP) porous substrate with a porosity of 50% was prepared as a separation membrane.

[0095] Using a Langmuir-Blodgett apparatus (KSV NIMA, KN2002), the MOF-5 molecular film was passed through the PP separation membrane in a vertical direction to deposit the MOF molecular film.

[0096] This deposition process was repeated five times to produce a separation membrane having MOF-5 molecular membranes formed on both sides of the PP separation membrane.

[0097] (2) Manufacturing of lithium-sulfur secondary batteries A separator was placed between the positive and negative electrodes and placed inside the case, and an electrolyte was then injected into the case to fabricate a lithium-sulfur secondary battery in the form of a CR-2032 coin cell. The positive electrode was fabricated by coating, drying, and rolling a positive electrode slurry, which was a mixture of a positive electrode active material, a conductive material (Super P), and a binder (styrene-butadiene rubber, SBR) in a weight ratio of 80:10:10, on an Al foil. The positive electrode active material was an S / MOF-5 composite obtained by mixing sulfur (manufactured by Sigma-Aldrich) with carbonized MOF-5 using a ball mill and then heat-treating at 155°C. The negative electrode was a lithium foil, and the electrolyte was a mixture of DOL and DME (DOL:DME=1:1 (v / v)) with 0.3M LiNO 3 and 1M LiTFSi (DOL: Dioxolane, DME: Dimethoxyethane).

[0098] Example 2 A separator and a lithium-sulfur secondary battery were prepared in the same manner as in Example 1, except that 2-aminoterephthalic acid was used instead of terephthalic acid as the organic ligand precursor.

[0099] Comparative Example 1 A separator and a lithium-sulfur secondary battery were manufactured in the same manner as in Example 1, except that a PP separator without a MOF layer was used as the separator.

[0100] Comparative Example 2 A separator and a lithium-sulfur secondary battery were manufactured in the same manner as in Example 1, except that a MOF layer was formed on a porous substrate by coating a mixed solution of MOF, PVDF binder, and NMP using a doctor blade instead of Langmuir-Blodgett.

[0101] Experimental Example 1: Structural analysis of MOF layers In order to confirm the crystal structure of the MOF layer formed on the porous substrate of the separation membrane, XRD (X-ray diffraction) analysis and FT-IR (Fourier-transform infrared spectroscopy) analysis were performed.

[0102] 1-1. XRD (X-ray Diffraction) analysis As in Example 1, a separator was prepared by depositing an MOF molecular film on a porous substrate by the Langmuir-Blodgett method, but the deposition times were 1, 5, and 20 times to prepare a separator and a lithium-sulfur secondary battery.

[0103] FIG. 3 is a graph (2-theta-scale) showing the XRD analysis results of the MOF layers deposited on the porous substrate of the separator by the Langmuir-Blodgett method, the XRD analysis results of the MOF layers formed by deposition once (1 Layer), five (5 Layers), and twenty (20 Layers).

[0104] As shown in FIG. 3, no crystallinity was observed in the MOF layer deposited on the porous substrate by the Langmuir-Blodgett technique, indicating that the MOF layer was amorphous.

[0105] 1-2.FT-IR analysis 4 is a graph showing the results of FT-IR analysis of terephthalic acid used as an organic ligand precursor and the MOF layer (Langmuir layer) in Example 1. The results were measured in the wavelength range of 700 to 3600 nm.

[0106] As shown in FIG. 4, the carboxylic acid spectrum (3300-2500 cm) of terephalic acid used as the organic ligand precursor in Example 1 was -1 :OH telescopic, 1760-1960cm -1 The peak shape is different, indicating that a new molecule different from that before the reaction was synthesized.

[0107] From these results, it can be seen that the MOF layer has a similar molecular structure to general MOFs, but has a non-crystalline two-dimensional structure because no XRD peak appears.

[0108] Experimental Example 2: Analysis of MOF layer formation conditions To determine the surface tension conditions under which a MOF layer can be uniformly formed, an isotherm analysis was performed on MOF-5 at room temperature.

[0109] FIG. 5 is a graph showing the correlation between molecular spacing and surface tension when a MOF-5 molecular film is formed at room temperature.

[0110] As shown in Figure 5, when forming a MOF-5 molecular film, the surface tension increased as the intermolecular spacing became narrower. At a surface tension of about 33 mN / m, the molecules began to overlap, and the surface tension showed a tendency to not increase any further. In the graph, Mma (mean molecular area) means the average area occupied by one molecule, and as Mma becomes smaller, the area occupied decreases, meaning that the intermolecular spacing decreases.

[0111] These results indicate that in order to form a uniform MOF-5 molecular film, it is appropriate to form the MOF layer under a surface tension of 30 mN / m, which is the surface tension before the molecules overlap.

[0112] As the distance between the Langmuir-Blodgett troughs narrows, the distance between the monomolecules on the surface of the aqueous solution narrows, forming a monolayer. As the distance between the monomolecules narrows, the surface tension of the Isotherm graph increases, and if the monolayers are too close and begin to overlap, the surface tension does not increase, so coating can be carried out under surface tension conditions just before saturation.

[0113] Experimental Example 3: Analysis of the surface properties of the MOF layer To analyze the surface characteristics of the MOF layer, the surface roughness was analyzed using AFM (Atomic Force Microscope, Bruker, Multimode IVa) photography. FIG. 6A is a vertical cross-sectional photograph and a graph showing the thickness of the MOF layer formed in the separation membrane of Example 1.

[0114] Referring to FIG. 6A, it can be seen that the MOF layer formed by performing five deposition processes using the Langmuir-Blodgett method has a maximum thickness of 4.76 nm.

[0115] FIG. 6B is an AFM image showing the surface characteristics of the MOF layer formed by the Langmuir-Blodgett method depending on the number of deposition processes. (i) shows the surface roughness of the MOF layer formed by performing five deposition processes by the Langmuir-Blodgett method when the organic solvent was confirmed to have evaporated visually (condition 1), and (ii) shows the surface roughness of the MOF layer formed by performing one, three, and five deposition processes by the Langmuir-Blodgett method for a reaction time of 30 minutes for sufficient reaction (condition 2) (Ra: arithmetic surface roughness, Rq: mean square surface roughness).

[0116] Referring to FIG. 6B (i) and (ii) and Table 2 below, it can be seen that the surface roughness characteristics of the MOF layer formed by the Langmuir-Blodgett technique were significantly improved by performing deposition once, three or five times under condition 2 compared to performing the deposition process five times under condition 1.

[0117] [Table 2]

[0118] Experimental example 4: Filtration test A filtration test was conducted to confirm the polysulfide filtration effect of the MOF material.

[0119] Through doctor blade coating, separation membranes were prepared in which MOF-5 and IRMOF-3 were uniformly coated to thicknesses of 20 μm and 40 μm, respectively.

[0120] FIG. 7 is a photograph showing the experimental results on the polysulfide filtration effect of the MOF material.

[0121] Figure 7 shows the filtration test results for a membrane not coated with MOF material (Ref, PP membrane), a membrane coated with MOFs (MOF-5, IRMOF-3) prepared by doctor blade coating, and a membrane coated with MOFs (MOF-5, IRMOF-3) prepared by the Langmuir-Blodgett method. The filtration test was carried out for 24 hours.

[0122] It was confirmed that the separation membrane coated with MOFs produced through doctor blade coating had a polysulfide filtering effect over time.The separation membrane coated with MOF layers produced through the Langmuir-Blodgett method also showed no visible color change due to polysulfides up to 12 hours, and it was confirmed that the membrane still had a filtering effect compared to conventional separation membranes even after 24 hours.

[0123] Experimental Example 5: Comparison of long-term cycle performance of lithium-sulfur secondary batteries In order to compare the long-term cycle performance of the lithium-sulfur secondary batteries of Examples 1 and 2 and Comparative Example 1, charge and discharge were carried out for 20 cycles under 1C conditions.

[0124] FIG. 8 is a graph showing the experimental results of the long-term cycle performance of the lithium-sulfur secondary batteries of Examples 1 and 2 and Comparative Example 1.

[0125] As shown in FIG. 8, the discharge capacities of Comparative Example 1, Examples 1 and 2 after 20 cycles were 6.9%, 15.08% and 27.47%, respectively. It was confirmed that Examples 1 and 2 in which an MOF layer was formed on the separator also had good long-term cycle performance.

[0126] In Example 1, a MOF-5 layer was formed on the separation membrane, filtering out polysulfides with large molecular sizes so that they would not move from the positive electrode to the negative electrode, while in Example 2, an IRMOF-3 layer was formed on the separation membrane, allowing nitrogen to electrically adsorb polysulfides well, improving cycle performance.

[0127] Although the present invention has been described above using limited examples and drawings, the present invention is not limited thereto, and it is of course possible for a person having ordinary knowledge in the technical field to which the present invention pertains to make various modifications and variations within the technical spirit of the present invention and the equivalent scope of the claims described below.

Claims

1. A separator for a lithium secondary battery, comprising: a porous substrate; and a MOF (metal organic framework) layer formed on one or both sides of the porous substrate, The separator for a lithium secondary battery, wherein the MOF layer comprises one or more MOF molecular membranes and has an amorphous structure.

2. The separator for a lithium secondary battery according to claim 1, wherein the MOF is doped with at least one different element selected from the group consisting of N, S and O.

3. 3. The separator for a lithium secondary battery according to claim 1, wherein the MOF layer has a thickness of 0.5 nm to 20 nm.

4. The porous substrate may be selected from the group consisting of polyolefin, polyester, polyamide, polyacetal, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, polyethylenenaphthalate, polytetrafluoroethylene, polyvinylidene fluoride, and the like. The separator for a lithium secondary battery according to any one of claims 1 to 3, comprising at least one selected from the group consisting of polyvinyl chloride, polyacrylonitrile, cellulose, nylon, poly(p-phenylene benzobisoxazole) and polyarylate.

5. (S1) mixing an aqueous solution containing a zinc precursor with an organic solution containing an organic ligand precursor to form a MOF molecular membrane; and (S2) depositing the MOF molecular membrane on a surface of a porous substrate; The deposition is performed by a Langmuir-Blodgett method.

6. The method for producing a separator for a lithium secondary battery according to claim 5, wherein the zinc precursor comprises one selected from the group consisting of zinc acetate and zinc nitrate.

7. 7. The method for producing a separator for a lithium secondary battery according to claim 5 or 6, wherein the organic ligand precursor comprises at least one selected from the group consisting of terephthalic acid, 2-aminoterephthalic acid, 2-hydroxyterephthalic acid, and 2,5-dimercaptoterephthalic acid.

8. The method for producing a separator for a lithium secondary battery according to any one of claims 5 to 7, wherein the mixing is performed by dropping a solution in which the organic ligand precursor is dissolved in an organic solvent into the aqueous solution of the zinc precursor.

9. A lithium secondary battery comprising a positive electrode, a negative electrode, and the separator according to any one of claims 1 to 4 and an electrolyte interposed between the positive electrode and the negative electrode.

10. 10. The lithium secondary battery according to claim 9, wherein the lithium secondary battery is a lithium-sulfur secondary battery.

Citation Information

Patent Citations

  • Preparation method of porous composite nanofilm material

    CN108467502A

  • Battery diaphragm with high-temperature-resistant metal-organic frame material coating, and preparation method and application thereof

    CN109461873A

  • Preparation method of coating type MOFs / organic composite diaphragm

    CN110729439A

  • Method for producing a compound containing a carbon dioxide