Preparation method of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units and its 4D printing
The ultra-high superelastic titanium-nickel shape memory alloy with sequentially configured functional units addresses the limitations of 4D printing by achieving superior superelasticity and mechanical properties, enabling the production of complex components with customized shapes for diverse applications.
Patent Information
- Application Number
- JP2022069783
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-20
- Filing Date
- 2022-04-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-04-20
AI Technical Summary
Current 4D printing of titanium-nickel shape memory alloys lacks the ability to achieve stable and large superelastic strains necessary for industrial applications, and the relationship between microstructure and functional properties is not fully understood, leading to insufficient performance in functional properties such as superelasticity.
The development of an ultra-high superelastic titanium-nickel shape memory alloy with sequentially configured functional units, comprising a cellular-grain zone, transition zone, and heat-affected zone, with gradient changes in nickel content and properties like nanohardness and Young's modulus, achieved through a 4D printing process involving powder preparation and selective laser melting.
The alloy exhibits enhanced superelasticity and mechanical properties, enabling the production of complex components with customized shapes and improved performance, suitable for various applications including aerospace, weapons, ships, and medical implants.
Smart Images

Figure 0007566232000001 
Figure 0007566232000002 
Figure 0007566232000003
Abstract
Description
[Technical field]
[0001] The present invention belongs to the field of titanium-nickel shape memory alloy, additive manufacturing and 4D printing, in particular to a preparation method and application of an ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units and its 4D printing. [Background technology]
[0002] For titanium-nickel shape memory alloys, the low thermal conductivity, strong elastic rebound, and poor processing performance result in low preparation efficiency, and traditional processes (such as casting, forging, and welding) cannot efficiently form high-precision and complex (porous structure, gradient structure, thin-walled structure, etc.) engineering parts (Prog. Mater. Sci. 57 (2012) 911-946.). As a cutting-edge new technology, additive manufacturing technology can directly prepare engineering parts with complex internal structures that are porous and formed by near-net shaping technology, which can greatly reduce the subsequent processing process. The meaning of 4D printing is 3D printing shape memory alloy (Shape Memory Alloy, SMA). It is actively designed by material properties or structural configuration, so that the shape, performance and function of the component can be controlled in time and space, realizing complex intelligent "heterogeneous" component preparation and meeting the high-end application requirements of controllable deformation, modification and function of high-end equipment (Mater. Sci. Eng., A 763 (2019) 138166; Mater. Des. 122 (2017) 42-79.). At present, 4D printing technology has greatly expanded the engineering application field of titanium-nickel shape memory alloy parts and products, but the titanium-nickel shape memory alloy prepared by 4D printing has many microscopic defects (cracks, holes, etc.) and a large number of columnar crystals, so its functional properties (such as superelasticity, shape memory effect and damping properties) cannot reach the equivalent level of titanium-nickel shape memory alloy prepared by conventional drastic plastic deformation processes (such as equal diameter angular extrusion, high pressure torsion and rolling).
[0003] Many recent studies have shown that the process of preparing titanium-nickel shape memory alloys by 4D printing is the same as the physical metallurgical process of the welding process. They have similar energy sources, microstructures, and solidification rates. Meanwhile, the difference between the two is that the 4D printing process is a cyclical, repeated single-pass laser welding process. The matrix of the 4D printed titanium-nickel shape memory alloy has specific regions that are repeated and layer-by-layer stacked. These specific regions correspond to the specific regions of the titanium-nickel shape memory alloy formed during the welding process, namely, the heat-affected zone, the transition zone, the cellular crystal zone, etc. (Prog. Mater. Sci. 88 (2017) 412-466;MRS Bull. 41(10) (2016) 765-774.) Here, the basic units consisting of the heat-affected zone, the transition zone, and the cellular crystal zone are defined as functional basic elements that realize unique functional properties, and are methodically constructed (sequentially constructed) by repeated layer-by-layer 4D printing to obtain large bulk materials. At present, researchers are gradually using these characteristic regions to describe the microstructural characteristics of titanium-nickel shape memory alloys prepared by 4D printing and establish the essential correlation of process-microstructure-performance regulation. At the same time, a literature survey shows that many studies have been conducted to improve the functional properties of 4D printed titanium-nickel shape memory alloys by adjusting process parameters, introducing heat treatment processes, adding a second phase, and so on (Prog. Mater. Sci. 83 (2016) 630-663.). However, the research results have not revealed the essential relationship between the basic element microstructure and the functional properties of 4D printed titanium-nickel shape memory alloys, and the enhancement of functional properties by controlling the overall functional basic element microstructure has not yet been achieved.
[0004] According to current research results, 4D printed titanium-nickel shape memory alloys have not yet been able to obtain stable large superelastic strain to meet their industrial applications. Moreover, the existing research on the microstructural evolution and functional realization of 4D printed titanium-nickel shape memory alloys is not deep and systematic enough. The present invention obtains ultra-high elastic titanium-nickel shape memory alloys by adjusting the functional units in a sequential configuration, revealing the essential relationship between microstructure and the realization of functional properties. Summary of the Invention [Problem to be solved by the invention]
[0005] To overcome the shortcomings and drawbacks of the prior art, the primary objective of the present invention is to provide an ultra-high superelastic titanium-nickel shape memory alloy having ordered functional units.
[0006] The second object of the present invention is to provide a 4D printing preparation method for an ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units.
[0007] The third object of the present invention is to provide a use of the super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units prepared by the above-mentioned preparation method. [Means for solving the problem]
[0008] The main object of the present invention is achieved by the following technical solutions: The super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units has (1) microstructural characteristics, (2) compositional characteristics, and (3) functional characteristics, (1) Microstructural characteristics: The ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units includes a cellular-grain zone (CGZ), a transition zone (TZ), and a heat-affected zone (HAZ), and these three characteristic zones constitute the functional basic elements (Figures 1 and 2). (2) Composition characteristics: The cellular crystal zone, transition zone and heat-affected zone of the super-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units have different nickel contents and have the characteristics of gradient change; (3) Functional properties: The nanohardness, Young's modulus, and critical stress of stress-induced martensitic transformation in the cellular crystal zone, transition zone, and heat-affected zone in the ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units are different, and have gradient change characteristics.
[0009] Preferably, the crystal grains in the cellular crystal zone of the characteristic (1) have a grain size of 600 to 1000 nm, Ti2Ni nanoprecipitates having a size of 40 to 100 nm are distributed at the grain boundaries, Ti2Ni nanoprecipitates having a size of 20 to 60 nm are diffusely distributed within the crystal grains in the transition zone, and a large number of Ni4Ti3 clusters having a size of 1 to 5 nm are distributed in the heat-affected zone.
[0010] Preferably, the functional basic element consisting of the three characteristic zones of the above characteristic (1) appears periodically in the titanium-nickel shape memory alloy, and the matrices of the three characteristic zones are all austenitic phase, while the proportion of the cellular crystalline zone is 20-25%, the proportion of the transition zone is 20-25%, and the proportion of the heat-affected zone is 50-60%.
[0011] Preferably, in the characteristic (2), the matrix nickel content in the cellular crystalline zone, the transition zone and the heat affected zone decreases gradually, with the nickel atomic ratio varying in the range of 50% to 53% (at.%).
[0012] Preferably, in the characteristic (3), the nanohardness, Young's modulus, and critical stress gradient for stress-induced martensitic transformation in the cellular crystalline zone, the transition zone, and the heat affected zone are changed, where the nanohardness and Young's modulus gradient increase, the critical stress gradient for stress-induced martensitic transformation decreases, the nanohardness changes from 3.5 to 5.5 GPa, and the Young's modulus changes from 50 to 66 GPa.
[0013] The second object of the present invention is achieved through the following technical solution. The preparation method of 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units includes a grinding step (1), a powder mixing and powder modification step (2), and a 4D printing molding step (3); (1) Grinding: Pure titanium and pure nickel are separately refined to obtain single titanium rods and nickel rods, and then single titanium powder and nickel powder are obtained by plasma atomization (PA), electrode induction gas melting atomization (EIGA) or plasma rotating electrode atomization (PREP), and the particle size of the powder is in the range of 100-1000nm or 15-53μm.ppm, the oxygen content of the titanium powder is 510-650ppm, and the oxygen content of the nickel powder is 700-800ppm; (2) Powder mixing and powder modification: The elemental titanium powder and nickel powder obtained in step (1) are put into a discharge plasma-assisted ball mill and discharge treated to modify the surface of the powder mixture, and the atomic ratio of nickel in the powder mixture is 50-53%; (3) 4D printing molding: The powder blended and powder modified in step (2) are mixed and molded by selective laser melting (SLM) to obtain a titanium-nickel shape memory alloy.
[0014] The ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units of the present invention strictly controls the oxygen content of titanium powder and nickel powder in the preparation process to reduce the formation of oxide particles in the 4D printed titanium-nickel alloy, thereby weakening the titanium-nickel alloy.
[0015] Preferably, at least one of the elemental titanium powder and nickel powder in step (2) has a particle size range of 15-53 μm, and the mixed powder is modified using a plasma-BM-S plasma ball mill, and the control parameters are: voltage is 130-150 V, current is 1-1.4 A, electrode rotation speed is 400-800 r / min, each discharge treatment time is 0.5-2 hours, the interval between two adjacent discharge treatments is 15-45 minutes, and the number of discharge treatments is 2-8.
[0016] Preferably, the selective laser melting molding equipment in step (3) includes CONCEPT LASER M2, EOS M280 / 290, SLM solution 125 / 250 / 280 2.0 / 500, RENISHAW 400, BLT-S320, etc., and the equipment for the 4D printing preparation process can be single laser, dual laser, multi-laser, etc.
[0017] Preferably, the process parameters of the 4D printing preparation method are: laser power of 70-150 W, laser scanning speed of 80-200 mm / s, powder layer thickness of 30 μm, and scanning interval of 100 μm.
[0018] The third object of the present invention is achieved by the following technical proposal. The ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units is applied in components such as prepared eyeglass frames, orthodontic wires, compression bone plates, spinal orthopedic rods, drive units, executive components, complex dampers, intelligent temperature control devices, self-expanding trusses, self-expanding communication satellite components, and variant aircraft.
[0019] The ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units is applied in adjusted joint implants (hip, knee joint implants), spinal implants (internal fixation implants, minimally invasive implants, etc.), shoulder implants (scapula implants, etc.), craniomaxillofacial implants (mandibular implants, cranial implants, etc.), ankle implants (ankle joint implants, toe bone implants, etc.) and other implants (sternum implants, etc.), etc.
[0020] The principle of the present invention is as follows. The 4D printing preparation method of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units according to the present invention is formed based on layer-by-layer accumulation in the 4D printing process, and when there is an overlap rate between the laser passes, the first formed laser pass will be heat-treated by the subsequent laser pass. In the 4D printing process, by controlling the overlap rate, the temperature and heat treatment time of the heat treatment area can be effectively controlled, and a 4D printed titanium-nickel shape memory alloy with a periodic distribution of three characteristic zone sequences, namely, the cellular crystal zone, the transition zone and the heat-affected zone, can be obtained.
[0021] The super-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units prepared according to the present invention exhibits gradient change mechanical properties in the compositional domain of the sequentially constructed functional units (Figure 3). Specifically, the Young's modulus and nanohardness gradually decrease from the heat-affected zone to the transition zone and then to the cellular crystal zone. In addition, the Ni content of the sequentially constructed functional units and the critical stress of the stress-induced martensitic transformation show opposite trends in the three zones. At the same time, the stress-induced phase transition occurs preferentially in the heat-affected zone, but the B2 matrix phase contains a large number of Ni4Ti3 clusters, which inhibits the generation of dislocations, and furthermore, during the phase transition, the strain generated around the Ni4Ti3 clusters inhibits the formation of dislocations and the occurrence of plastic deformation, thereby further enhancing the superelasticity of the 4D printed titanium-nickel shape memory alloy. Effect of the Invention
[0022] Compared with the prior art, the present invention has the following advantages and effects: (1) The super-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units prepared by the present invention has three characteristic zones, namely, cellular crystal zone, transition zone and heat-affected zone, and the precipitated phase (Ti2Ni and Ni4Ti3) precipitation situation, distribution position and amount in the three characteristic zones are greatly different. At the same time, the nickel content between the three characteristic zones is different, and has the characteristics of gradient change. In addition, the nano-hardness, Young's modulus and critical stress of stress-induced martensitic transformation between the characteristic zones are different, and have the characteristics of gradient change. Due to the synergistic strengthening between different regions in the sequentially constructed functional units, the titanium-nickel shape memory alloy with sequentially constructed functional units can obtain super-high superelasticity. (2) Compared with the titanium-nickel alloy prepared by the conventional process, the titanium-nickel shape memory alloy prepared by the present invention proposes a new microstructural design idea that can effectively improve the superelasticity of high titanium-nickel shape memory alloy, and obtains sequentially constructed functional units with performance gradient at the microscopic scale. (3) The present invention adopts 4D printing to realize the formation of super-high super-elastic titanium-nickel shape memory alloy with sequentially constructed functional units, which can prepare various complex-shaped parts compared with the traditional casting method and rapid plastic deformation method, and can truly be used to prepare components for individual applications to meet customized requirements. At the same time, the super-high super-elastic titanium-nickel shape memory alloy with sequentially constructed functional units of the present invention can complete the formation of titanium-nickel alloy parts with a wide range of complex shapes, complete the rapid manufacturing of complex structure titanium-nickel alloy parts, and have super-high elastic performance, which can be used to prepare various functional components in many fields such as aerospace, weapons, ships, medical care, and architecture. (4) In the present invention, 4D printing molding technology is used to prepare an ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units, which realizes near-net shape and personalized customization, improves material utilization, and saves costs. [Brief description of the drawings]
[0023] [Figure 1] 1A-1C are scanning electron microscope microstructure views of sequentially constructed functional units. [Diagram 2] FIG. 13 Transmission electron microscope microstructure images of the cellular crystalline zone, transition zone and heat affected zone. [Diagram 3] 1 is a graph showing the change in nano hardness and Young's modulus of sequentially constructed functional units. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described in more detail below with reference to embodiments and the accompanying drawings, to which however the embodiments of the invention are not limited.
[0025] Example 1: 1.Microstructure of ultra-highly superelastic titanium-nickel shape memory alloy with sequentially constructed functional units The sequentially constructed functional units consist of a cellular crystalline zone, a transition zone, and a heat-affected zone. The grain size of the cellular crystalline zone is 800 nm, and Ti2Ni precipitates with a size of 55 nm are distributed at the grain boundaries. In the transition zone, Ti2Ni precipitates with a size of 40 nm are diffusely distributed. In the heat-affected zone, Ni4Ti3 clusters with a size of 3 nm (see Figures 1 and 2) are distributed.
[0026] 2. Functional properties of ultra-highly superelastic titanium-nickel shape memory alloy with sequentially constructed functional units The nanohardness of the cellular crystal zone, transition zone and heat affected zone in the sequentially constructed functional units are 3.7 GPa, 4.2 GPa and 4.9 GPa, respectively, the Young's modulus is 50 GPa, 57 GPa and 63 GPa (see Fig. 3), and the matrix nickel content is 50.6%, 51.0% and 51.3% (at.%), respectively.
[0027] 3. Preparation method of 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units (1) Grinding: Pure titanium and pure nickel are separately refined to obtain single titanium rods and nickel rods, and then prepared single titanium powder and nickel powder by plasma spraying (PA). The particle size range of the powders is 15-53 μm, the oxygen content of the titanium powder is 650 ppm, and the oxygen content of the nickel powder is 700 ppm. (2) Powder mixing and powder modification: The obtained single titanium powder (powder particle size: 15-53 μm) and nickel powder (powder particle size: 15-53 μm) are put into the Plasma-BM-S plasma ball mill to carry out surface modification, and the atomic ratio of nickel in the mixed powder is 51.3%, the voltage is 130 V, the current is 1 A, the electrode rotation speed is 400 r / min, and each discharge treatment time is 0.5 hours. The interval between two adjacent discharge treatments is 15 minutes, and the number of discharge treatments is 8 times. (3) 4D printing molding: The powder blended and powder modified powders are mixed and molded by CONCEPT LASER M2, and the titanium-nickel shape memory alloy is prepared and obtained using the process parameters of laser power 70 W, laser scanning speed 80 mm / s, powder layer thickness 30 μm, and scanning interval 100 μm.
[0028] 4. Superelastic behavior of superelastic titanium-nickel shape memory alloy with sequentially constructed functional units: The superelastic recovery strain of titanium-nickel alloy under compression (maximum stress is 800MPa) is 6.22%, which is compared with the related literature descriptions, such as 4.6% recovery strain (Acta Mater. 194 (2020) 178-189.), 5.62% recovery strain (Sci. Rep. 9(1) (2019) 41), and 5.77% recovery strain (Acta Mater. 144 (2018) 552-560.), and the present invention has superior overall performance (Prog. Mater. Sci. 83 (2016) 630-663.).
[0029] Example 2: 1.Microstructure of ultra-highly superelastic titanium-nickel shape memory alloy with sequentially constructed functional units The sequentially constructed functional units are composed of a cellular crystalline zone, a transition zone, and a heat-affected zone. The grain size of the cellular crystalline zone is 1000 nm, and Ti2Ni precipitates with a size of 100 nm are distributed at the grain boundaries. Ti2Ni precipitates with a size of 60 nm are diffusely distributed in the transition zone. Ni4Ti3 clusters with a size of 5 nm (see Figures 1 and 2) are distributed in the heat-affected zone.
[0030] 2. Functional properties of ultra-highly superelastic titanium-nickel shape memory alloy with sequentially constructed functional units The nanohardness of the cellular crystal zone, transition zone and heat-affected zone in the sequentially constructed functional units are 3.5 GPa, 4.7 GPa and 5.2 GPa, respectively, the Young's modulus is 55 GPa, 59 GPa and 66 GPa, respectively (see Fig. 3), and the matrix nickel content is 551.1%, 51.8% and 52.1% (at.%), respectively.
[0031] 3. Preparation method of 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units (1) Grinding: Pure titanium and pure nickel are separately refined to obtain single titanium rods and nickel rods, and then prepared into single titanium powders and nickel powders by electrode induction melting gas atomization (EIGA), the particle size of the powders is in the range of 100-1000 nm or 15-53 μm. The oxygen content of the titanium powder is 580 ppm, and the oxygen content of the nickel powder is 800 ppm. (2) Powder mixing and powder modification: The obtained elemental titanium powder (powder particle size: 15-53 μm) and nickel powder (powder particle size: 100-1000 nm) are put into a Plasma-BM-S plasma ball mill to perform surface modification. The atomic ratio of nickel in the mixed powder is 52.1%, and the voltage is 150 V, the current is 1.2 A, the electrode rotation speed is 600 r / min, the duration of each discharge treatment is 1 h, the interval between two adjacent discharge treatments is 30 min, and the number of discharge treatments is 4. (3) 4D printing molding: The powder blended and powder modified powders are mixed and molded by EOS M280, and the titanium-nickel shape memory alloy is prepared and obtained using the process parameters of laser power 100 W, laser scanning speed 150 mm / s, powder layer thickness 30 μm, and scanning interval 100 μm.
[0032] 4. Superelastic behavior of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units: The superelastic recovery strain of the titanium-nickel alloy under compression (maximum stress is 800 MPa) is 6.3%, which is superior to the recovery strain of 4.6% in the related literature (Acta Mater. 194 (2020) 178-189.), 5.62% (Sci. Rep. 9(1) (2019) 41), and 5.77% (Acta Mater. 144 (2018) 552-560.) (Prog. Mater. Sci. 83 (2016) 630-663.).
[0033] Example 3: 1. Microstructure of ultra-highly superelastic titanium-nickel shape memory alloy with sequentially constructed functional units The sequentially constructed functional units are composed of a cellular crystalline zone, a transition zone, and a heat-affected zone. The grain size of the crystal grains in the cellular crystalline zone is 600 nm, and Ti2Ni precipitate phases with a size of 40 nm are distributed at the grain boundaries. Ti2Ni precipitate phases with a size of 20 nm are diffusely distributed in the transition zone. Ni4Ti3 clusters with a size of 1-3 nm (see Figures 1 and 2) are distributed in the heat-affected zone.
[0034] 2. Functional properties of super-elastic titanium-nickel shape memory alloy with sequentially constructed functional units: The nanohardness of the cellular crystal zone, transition zone and heat affected zone in the sequentially constructed functional units are 3.5 GPa, 4.7 GPa and 5.5 GPa, respectively; Young's modulus is: 50 GPa, 56 GPa and 66 GPa, respectively (see Figure 3), and the matrix nickel content is 51.9%, 52.4% and 53.0% (at.%), respectively.
[0035] 3. Preparation method of 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units (1) Grinding: Pure titanium and pure nickel are separately refined to obtain single titanium rods and nickel rods, and then elemental titanium powder and nickel powder are prepared by plasma rotating electrode atomization powder process (PREP). The particle size range of the powders is 100-1000nm or 15-53μm, the oxygen content of the titanium powder is 510ppm, and the oxygen content of the nickel powder is 780ppm. (2) Powder mixing and powder modification: The obtained titanium powder (powder particle size: 100-1000 nm) and nickel powder (powder particle size: 15-53 μm) are put into a Plasma-BM-S plasma ball mill to perform surface modification. The atomic ratio of nickel in the mixed powder is 53%, and the voltage is 140 V, the current is 1.4 A, the electrode rotation speed is 800 r / min, the duration of each discharge treatment is 2 h, the interval between two adjacent discharge treatments is 40 min, and the number of discharge treatments is two. (3) 4D printing molding: The powder blended and powder modified powders are mixed and molded by EOS M290, and the titanium-nickel shape memory alloy is prepared and obtained using the process parameters of laser power 150 W, laser scanning speed 200 mm / s, powder layer thickness 30 μm, and scanning interval 100 μm.
[0036] 4. Superelastic behavior of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units: The superelastic recovery strain of the titanium-nickel alloy under compression (maximum stress is 800 MPa) is 6.5%, which is superior to the recovery strain of 4.6% in the related literature (Acta Mater. 194 (2020) 178-189.), 5.62% (Sci. Rep. 9(1) (2019) 41), and 5.77% (Acta Mater. 144 (2018) 552-560.) (Prog. Mater. Sci. 83 (2016) 630-663.).
[0037] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above examples. Other changes, modifications, substitutions, combinations, and simplifications that do not depart from the spirit and principle of the present invention are equivalent replacement methods and fall within the protection scope of the present invention.
[0038] (Additional Note) (Appendix 1) A super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units, (1) microstructural properties; (2) compositional properties; and (3) functional properties; (1) Microstructural characteristics: The super-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units includes three characteristic zones, namely, the cellular crystal zone, the transition zone and the heat-affected zone, and the above three characteristic zones constitute the functional basic elements; (2) Composition characteristics: The cellular crystal zone, transition zone and heat-affected zone in the super-high super-elastic titanium-nickel shape memory alloy with sequentially constructed functional units have different nickel contents and have the characteristics of gradient change; (3) Functional properties: The ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units is characterized in that the nano-hardness, Young's modulus, and critical stress for stress-induced martensitic transformation of the cellular crystal zone, transition zone, and heat-affected zone in the ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units are different and have gradient change properties.
[0039] (Appendix 2) The ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units according to appended claim 1, characterized in that the crystal grains in the cellular crystal zone of the characteristic (1) have a grain size of 600 to 1000 nm, Ti2Ni nanoprecipitates having a size of 40 to 100 nm are distributed at the grain boundaries, Ti2Ni nanoprecipitates having a size of 20 to 60 nm are diffusely distributed within the crystal grains in the transition zone, and a large number of Ni4Ti3 clusters are distributed in the heat affected zone and have a size of 1 to 5 nm.
[0040] (Appendix 3) The ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units described in Appendix 1, characterized in that the sequentially constructed functional units consisting of the three characteristic zones of the characteristic (1) appear periodically in the titanium-nickel shape memory alloy, and the matrices of the three characteristic zones are all austenite phase, while the ratio of the cellular crystal zone is 20 to 25%, the ratio of the transition zone is 20 to 25%, and the ratio of the heat-affected zone is 50 to 60%.
[0041] (Appendix 4) The ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units as described in Appendix 1, characterized in that, in the characteristic (2), the matrix nickel content in the cellular crystal zone, the transition zone and the heat affected zone decreases gradually, and the atomic ratio of nickel is in the range of 50% to 53%.
[0042] (Appendix 5) The ultrahigh superelastic titanium-nickel shape memory alloy having sequentially constructed functional units as described in Appendix 1, characterized in that, in the property (3), the nanohardness, Young's modulus, and critical stress gradient for stress-induced martensitic transformation in the cellular crystalline zone, the transition zone, and the heat affected zone change, the nanohardness and Young's modulus gradient increase, the critical stress gradient for stress-induced martensitic transformation decreases, the nanohardness changes from 3.5 to 5.5 GPa, and the Young's modulus changes from 50 to 66 GPa.
[0043] (Appendix 6) A method for preparing 4D printing of ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units, comprising: The method includes a grinding step (1), a powder mixing and powder modification step (2), and a 4D printing molding step (3). (1) Grinding: Pure titanium and pure nickel are separately refined to obtain single titanium rods and nickel rods, and then prepared single titanium powders and nickel powders by plasma spraying, electrode induction melting gas spraying or plasma rotating electrode spraying powder method, the particle size of the powders is in the range of 100-1000nm or 15-53μm.ppm, the oxygen content of the titanium powder is 510-650ppm, and the oxygen content of the nickel powder is 700-800ppm; (2) Powder mixing and powder modification: The elemental titanium powder and nickel powder (at least one of the powders has a particle size range of 15-53 μm) obtained in step (1) are put into a discharge plasma-assisted ball mill to carry out discharge treatment, and the surface of the powder mixture is modified, and the atomic ratio of nickel in the powder mixture is 50-53%; (3) 4D printing molding: A method for preparing 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units, characterized in that the powder mixed and powder modified in step (2) are mixed and molded by selective laser melting to obtain a titanium-nickel shape memory alloy.
[0044] (Appendix 7) The method for preparing 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units described in Appendix 6, characterized in that when the plasma ball mill in step (2) performs discharge treatment on the mixed powder, the control parameters are: voltage: 130-150 V, current: 1-1.4 A, electrode rotation speed: 400-800 r / min, duration of each discharge treatment time: 0.5-2 h, interval between two adjacent discharge treatments: 15-45 minutes, and number of discharge treatments: 2-8.
[0045] (Appendix 8) The method for preparing a 4D printing of an ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units as described in Appendix 6, characterized in that the process parameters of the 4D printing preparation method in step (3) are a laser power of 70 to 150 W, a laser scanning speed of 80 to 200 mm / s, a powder layer thickness of 30 μm, and a scanning interval of 100 μm.
[0046] (Appendix 9) Applications of ultra-high superelastic titanium-nickel shape memory alloys with sequentially constructed functional units in components such as prepared eyeglass frames, orthodontic wires, compression bone plates, spinal orthopedic rods, drive units, executive components, complex dampers, intelligent temperature control devices, self-expanding trusses, self-expanding communication satellite components and variant aircraft.
[0047] (Appendix 10) The use of ultra-high superelastic titanium-nickel shape memory alloys having sequentially constructed functional units in prepared joint implants, spinal implants, shoulder implants, craniomaxillofacial implants, ankle implants and other implants.
Claims
1. A super-highly super-elastic titanium-nickel shape memory alloy having sequentially configured functional units, (1) microstructural properties; (2) compositional properties; and (3) functional properties; (1) Microstructural characteristics: The super-elastic titanium-nickel shape memory alloy with sequentially constructed functional units includes three characteristic zones, namely, a cellular crystal zone, a transition zone and a heat-affected zone, and the above three characteristic zones constitute functional building blocks; (2) composition characteristics: the cellular crystal zone, the transition zone and the heat-affected zone in the super-high super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units have different nickel contents and have the characteristics of gradient change of nickel content; (3) Functional properties: The super-high super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units is characterized in that the nano-hardness, Young's modulus, and critical stress for stress-induced martensitic transformation of the cellular crystal zone, transition zone, and heat-affected zone in the super-high super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units are different, and the nano-hardness, Young's modulus, and critical stress for stress-induced martensitic transformation of the cellular crystal zone, transition zone, and heat-affected zone have gradient change properties.
2. The grain size of the cellular crystalline zone of the characteristic (1) is 600 to 1000 nm, and the size of Ti is 40 to 100 nm. 2 Ni nano-precipitates are distributed at the grain boundaries, and Ti nano-precipitates with sizes of 20 to 60 nm are present within the crystal grains in the transition zone. 2 Ni nano-precipitates are distributed diffusely, and many Ni particles are present in the heat-affected zone. 4 Ti 3 The super-elastic titanium-nickel shape memory alloy with sequentially constructed functional units as claimed in claim 1, characterized in that the clusters are distributed and the size is 1-5 nm.
3. The super-elastic titanium-nickel shape memory alloy having sequentially configured functional units according to claim 1, characterized in that the sequentially configured functional units consisting of the three characteristic zones of the characteristic (1) appear periodically in the titanium-nickel shape memory alloy, and the matrices of the three characteristic zones are all austenite phase, while the ratio of the cellular crystal zone is 20-25 volume %, the ratio of the transition zone is 20-25 volume %, and the ratio of the heat-affected zone is 50-60 volume %.
4. The super-elastic titanium-nickel shape memory alloy having sequentially constructed functional units according to claim 1, characterized in that, in the characteristic (2), the matrix nickel content in the cellular crystal zone, the transition zone and the heat affected zone decreases gradually, and the atomic ratio of nickel is in the range of 50% to 53%.
5. The ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units as claimed in claim 1, characterized in that, in the characteristic (3), the nano-hardness, Young's modulus, and critical stress gradient for stress-induced martensitic transformation in the cellular crystalline zone, the transition zone, and the heat affected zone change, the nano-hardness and Young's modulus gradient increase, the critical stress gradient for stress-induced martensitic transformation decreases, and the nano-hardness changes from 3.5 to 5.5 GPa and the Young's modulus changes from 50 to 66 GPa.
6. A method for preparing 4D printing of ultra-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units, comprising: The method includes a grinding step (1), a powder mixing and powder modification step (2), and a 4D printing molding step (3). (1) Grinding: Pure titanium and pure nickel are separately refined to obtain a single titanium rod and a single nickel rod, and then prepared by plasma spraying, electrode induction melting gas spraying or plasma rotating electrode spray powder method to produce elemental titanium powder and nickel powder; (i) the particle size of the elemental titanium powder and the nickel powder are respectively in the range of 15-53 μm; (ii) the particle size of the elemental titanium powder is in the range of 15-53 μm, and the particle size of the nickel powder is in the range of 100-1000 nm; (iii) the particle size of the elemental titanium powder is in the range of 100-1000 nm, and the particle size of the nickel powder is in the range of 15-53 μm, the oxygen content of the titanium powder is 510-650 ppm, and the oxygen content of the nickel powder is 700-800 ppm; (2) Powder mixing and powder modification: the elemental titanium powder and nickel powder obtained in step (1) are put into a discharge plasma-assisted ball mill to carry out discharge treatment, and the surface of the powder mixture is modified, and the atomic ratio of nickel in the powder mixture is 50-53%; (3) 4D printing molding: Mixing the powder mixed and powder modified in step (2), and molding by selective laser melting to obtain a titanium-nickel shape memory alloy. A method for preparing a 4D printing ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units.
7. The method for preparing 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially configured functional units according to claim 6, characterized in that, when the discharge plasma-assisted ball mill in step (2) performs discharge treatment on the mixed powder, the control parameters are: voltage 130-150V, current 1-1.4A, electrode rotation speed 400-800 r / min, duration of each discharge treatment time 0.5-2h, interval between two adjacent discharge treatments 15-45 minutes, and number of discharge treatments 2-8.
8. The method for preparing 4D printing of ultra-high superelastic titanium-nickel shape memory alloy with sequentially constructed functional units as described in claim 6, characterized in that the process parameters of the 4D printing preparation method in step (3) are: laser power of 70-150W, laser scanning speed of 80-200mm / s, powder layer thickness of 30μm, and scanning interval of 100μm.
9. The ultra-high superelastic titanium-nickel shape memory alloy having sequentially configured functional units according to any one of claims 1 to 5 in prepared eyeglass frames, orthodontic wires, compression bone plates, spinal orthopedic rods, drives, dampers, intelligent temperature control devices, self-expanding trusses, self-expanding communication satellite components and aircraft components.
10. The super-high superelastic titanium-nickel shape memory alloy having sequentially constructed functional units according to any one of claims 1 to 5 in prepared joint implants, spinal implants, shoulder implants, craniomaxillofacial implants, ankle implants and other implants.
Citation Information
Patent Citations
4D printing method and application of titanium-nickel shape memory alloy
CN109648082A
4D printing method of in-situ regulation of functional characteristics of nickel-titanium alloy and application
CN110465662A
Thermal response element
JP1985059054A
Wires of superelastic nickel-titanium alloy and methods of forming the same
WO2021062191A1