Decorative material, wall structure, construction set and construction method

A decorative material with a uniformly provided magnetic layer achieves strong fixation and easy removal by optimizing magnetic flux density relative to basis weight, addressing the challenge of balancing strength and replaceability.

JP7566456B2Inactive Publication Date: 2024-10-15SUMITOMO BAKELITE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019065775
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-03-29
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing decorative materials face challenges in achieving a balance between strong fixation to a base and easy removal, leading to potential damage during replacement.

Method used

A decorative material design with a uniformly provided magnetic layer on one surface, where the magnetic flux density relative to the basis weight is within a specific range, allowing for sufficient fixation strength while enabling easy removal.

Benefits of technology

The solution enhances the balance between fixation strength and ease of removal, allowing for quick and damage-free replacement of decorative materials without the need for adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566456000002
    Figure 0007566456000002
  • Figure 0007566456000003
    Figure 0007566456000003
  • Figure 0007566456000004
    Figure 0007566456000004
Patent Text Reader

Abstract

To provide a technique to improve a balance between a fixing strength of a decorative material to a base and readiness to remove the decorative material from the base.SOLUTION: A decorative material 10 has a decorative layer 12 and a magnet layer 14 disposed uniformly on one face of the decorative layer 12. A flux density X (mT) of the decorative material 10 of a basis weight W (kg / m2) of the decorative material 10 satisfies that X / W (mT m2 / kg) equals to or more than 5.0 and equals to or less than 18.0.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative material, a wall structure, an installation set, and an installation method. [Background technology]

[0002] 2. Description of the Related Art When constructing interior and exterior walls of houses, buildings, etc., decorative materials are sometimes applied to enhance the design of the walls. Patent Documents 1 and 2 describe techniques relating to cosmetic materials having a magnetic layer.

[0003] Patent Document 1 (JP Patent Publication 2004-098296A) describes a decorative board with a magnetic layer, which is formed by applying a magnetic resin, in which magnetic powder is dispersed in the resin, to the back side of the decorative board and then magnetizing it. This document also describes that, when joining the decorative board to the underlying metal frame, a decorative board with a magnetic layer on the back side is used, so that subtle misalignment can be corrected during construction without requiring skill, and that the board can be held in place by magnetic force until the adhesive hardens.

[0004] In addition, Patent Document 2 (JP Patent Publication 2005-254544A) describes a decorative board that is lightweight, has excellent processability, does not affect the surroundings with a magnetic field, and can magnetically attract commercially available magnetic sheets, etc., and a technology related to storage using this decorative board. To solve this problem, the document describes that in a decorative board in which a magnetic layer made of a soft magnetic material and a resin is provided on at least one side of a base material, and a decorative layer is provided on the magnetic layer, the thickness of the magnetic layer and the content of the soft magnetic material in the magnetic layer are each set within a specific range.

[0005] Also, Patent Document 3 (JP Patent Publication 2002-128429A) describes an elevator interior material in which a magnetic plate is provided on the back surface of a decorative plate, and a magnetic shielding material is interposed between the decorative plate and the magnetic plate. Specifically, the document describes that a small piece of magnetic plate is adhered along the outer periphery of the edge of the decorative plate. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-098296 A [Patent Document 2] JP 2005-254544 A [Patent Document 3] JP 2002-128429 A Summary of the Invention [Problem to be solved by the invention]

[0007] By providing a magnetic layer in the decorative material, as described in Patent Documents 1 and 2 above, it is believed that the variation in fixing strength within the installation area of ​​the decorative material can be reduced compared to the case in which magnetic pieces are provided locally on the outer periphery of the edge, etc., as described in Patent Document 3. On the other hand, the techniques described in Patent Documents 1 and 2 employ a method of using an adhesive or directly coating a magnetic layer on the base when fixing the decorative material to the base. While these methods may improve the strength of the material when fixed, when replacing the decorative material, it requires a long time of work to remove the decorative material from the base, and may damage the base.

[0008] The present invention provides a technique for improving the balance between the strength of fixation of a decorative material to a substrate and the ease of removal of the decorative material from the substrate. [Means for solving the problem]

[0009] The inventors of the present invention have studied intensively the design guidelines for ensuring sufficient fixing strength of the decorative material to the substrate while easily removing the decorative material from the substrate, for example, when replacing the decorative material. As a result, they have found that a magnetic layer is uniformly provided on one side of the decorative layer, and that in such a configuration, the measure of the magnetic flux density X of the decorative material relative to the basis weight W of the decorative material is effective as the above-mentioned design guidelines, and have completed the present invention.

[0010] That is, according to the present invention, A decorative material having a decorative layer and a magnet layer uniformly provided on one surface of the decorative layer, The basis weight of the decorative material W (kg / m 2 ) for the magnetic flux density X (mT) of the decorative material, X / W (mT m 2 / kg) is 5.0 or more and 18.0 or less.

[0011] According to the present invention, A wall structure is provided, which comprises a laminate of a substrate containing a ferromagnetic material and the decorative material of the present invention.

[0012] According to the present invention, There is provided an interior or exterior application set comprising a base material containing a ferromagnetic material and the decorative material of the present invention.

[0013] Further, according to the present invention, There is provided an interior or exterior application method, which comprises a step of attaching the decorative material of the present invention to a substrate containing a ferromagnetic material. Effect of the Invention

[0014] According to the present invention, it is possible to improve the balance between the strength of fixation of the decorative material to the base and the ease of removal of the decorative material from the base. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a cross-sectional view showing the configuration of a decorative material in an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing the configuration of a decorative material in an embodiment. [Diagram 3] FIG. 2 is a cross-sectional view showing the configuration of a decorative material in an embodiment. [Figure 4] FIG. 2 is a cross-sectional view showing the configuration of a decorative material in an embodiment. [Diagram 5] FIG. 2 is a diagram for explaining a construction method in the embodiment. [Figure 6] FIG. 2 is a diagram for explaining a construction method in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given the same reference numerals, and the description will be omitted as appropriate. In addition, "~" indicates "above" to "below" unless otherwise specified.

[0017] (First embodiment) FIG. 1 is a cross-sectional view showing the configuration of a decorative material in this embodiment. The decorative material 10 in this embodiment has a decorative layer 12 and a magnet layer 14 uniformly provided on one surface of the decorative layer 12. The basis weight W (kg / m 2 ) is the magnetic flux density X (mT) of the decorative material 10, where X / W(mT m 2 / kg) is greater than or equal to 5.0 and less than or equal to 18.0.

[0018] Above X / W(mT m 2 / kg) is 5.0 or more, preferably 7.0 or more, more preferably 9.0 or more, and even more preferably 10.0 or more, from the viewpoint of increasing the fixing strength of the decorative material 10 to the base. In addition, from the viewpoint of increasing the ease of removing the decorative material 10 from the base, the above X / W(mT m 2 / kg) is 18.0 or less, preferably 14.0 or less, and more preferably 12.0 or less. In decorative material 10, a magnet layer 14 is uniformly provided on one side of decorative layer 12, and the magnetic flux density X of decorative material 10 relative to the basis weight W of decorative material 10 is within the above-mentioned range, so that the fixing strength of decorative material 10 to the base is sufficiently ensured, while the decorative material 10 can be easily removed from the base, for example when replacing decorative material 10. Here, by selecting the combination of materials used for the decorative layer 12 and the magnet layer 14, it is possible to set the above-mentioned X / W within the above-mentioned range.

[0019] The basis weight W (kg / m 2 ) is preferably 1.0 or more, more preferably 2.0 or more, and even more preferably 3.0 or more, from the viewpoint of increasing the strength of the decorative material 10. In addition, from the viewpoint of reducing the weight of the decorative material 10 and increasing ease of transportation, the basis weight W (kg / m 2 ) is preferably 10.0 or less, more preferably 8.0 or less, even more preferably 6.0 or less, and even more preferably 4.0 or less.

[0020] The magnetic flux density X (mT) of the decorative material 10 is preferably 20 mT or more, more preferably 30 mT or more, and even more preferably 35 mT or more, from the viewpoint of improving the fixing strength to the base. Furthermore, from the standpoint of increasing the ease with which the decorative material 10 can be removed from the base, the magnetic flux density X (mT) of the decorative material 10 is preferably 80 mT or less, more preferably 60 mT or less, and even more preferably 40 mT or less. Here, the magnetic flux density X (mT) of the decorative material 10 is specifically the surface magnetic flux density on the side of the decorative material 10 facing the base, and more specifically, the surface magnetic flux density on the side of the magnetic layer 14 of the decorative material 10.

[0021] From the viewpoint of weight reduction or ease of transport, the shape of the decorative material 10 is preferably a sheet, more preferably a long sheet material. From the viewpoint of improving adhesion of the decorative material 10 to the base, the decorative material 10 is preferably a sheet having a uniform thickness, more preferably a long sheet material, and has a uniform thickness in cross section in the length direction, i.e., the lamination direction of the decorative layer 12 and the magnet layer 14.

[0022] The overall thickness of the decorative material 10 (also referred to simply as the "thickness" of the decorative material 10 in this specification) is preferably 0.5 mm or more, more preferably 0.8 mm or more, and even more preferably 1.0 mm or more, from the viewpoint of making the decorative material 10 lightweight and easier to transport. Furthermore, from the viewpoint of improving the fixing strength to the base, the thickness of the decorative material 10 is preferably 3.0 mm or less, more preferably 2.0 mm or less, and even more preferably 1.5 mm or less.

[0023] From the viewpoint of improving adhesion to the substrate, for example, to enable fixing to a curved substrate, and from the viewpoint of increasing the ease of removing the decorative material 10 from the substrate, the decorative material 10 is preferably flexible overall. Specifically, the decorative material 10 is preferably flexible enough to not crack when bent at a bending radius of 10 mm at 25°C.

[0024] The magnetic flux density X (mT) relative to the flexural modulus E (MPa) of the decorative material 10, i.e., X / E (mT / MPa), is preferably 50 or more, more preferably 100 or more, and even more preferably 200 or more, from the viewpoint of improving the fixing strength to the base. Furthermore, from the standpoint of increasing the ease with which the decorative material 10 can be removed from the base, the above-mentioned X / E (mT / MPa) is preferably 2000 or less, more preferably 1000 or less, and even more preferably 400 or less.

[0025] Furthermore, from the viewpoint of increasing the ease with which the decorative material 10 can be removed from the base, the flexural modulus E (MPa) of the decorative material 10 is preferably 0.01 MPa or more, more preferably 0.05 MPa or more, and even more preferably 0.10 MPa or more. Furthermore, from the viewpoint of improving the fixing strength to the base, the flexural modulus E (MPa) of the decorative material 10 measured by the method described above is preferably 1.0 MPa or less, more preferably 0.50 MPa or less, and even more preferably 0.30 MPa or less. The method for measuring the flexural modulus E (MPa) of the decorative material 10 will be described later in the Examples section.

[0026] In order to increase the strength of the surface of decorative material 10, the Shore D hardness of the surface (first side 101) of decorative material 10 facing decorative layer 12 is preferably 50 or more, more preferably 60 or more, even more preferably 70 or more, and even more preferably 75 or more, when measured by placing a rubber hardness tester (manufactured by Shimadzu Corporation) vertically on the surface facing decorative layer 12 and applying a load of 500 g from directly above and reading the displayed value. Furthermore, from the standpoint of imparting appropriate flexibility to the cosmetic material 10 and increasing the ease of transporting the cosmetic material 10, the Shore D hardness of the surface of the cosmetic layer 12 side of the cosmetic material 10, as measured by the above-mentioned method, is preferably 120 or less, more preferably 110 or less, even more preferably 95 or less, and even more preferably 85 or less. On the other hand, from the viewpoint of increasing the strength of decorative material 10 at the fixing surface with the base, the Shore D hardness of the surface (second surface 102) of decorative material 10 on the side of magnet layer 14 is preferably 50 or more, more preferably 60 or more, even more preferably 70 or more, and even more preferably 75 or more, as measured by a rubber hardness tester (manufactured by Shimadzu Corporation) placed vertically on the surface on the side of magnet layer 14 and reading the displayed value when a load of 500 g is applied from directly above. In addition, the Shore D hardness of the surface of the magnetic layer 14 side of the decorative material 10 is preferably 120 or less, more preferably 110 or less, even more preferably 95 or less, and even more preferably 85 or less, in the above-mentioned measurement method, from the viewpoint of increasing the ease of removing the decorative material 10 from the base.

[0027] In addition, Figure 1 illustrates a configuration in which decorative material 10 does not have an intervening layer between decorative layer 12 and magnet layer 14, but decorative material 10 may also have a configuration in which an intervening layer is between decorative layer 12 and magnet layer 14. For example, Fig. 2 is a cross-sectional view showing another configuration of the decorative material 10 in this embodiment. In Fig. 2, the basic configuration of the decorative material 10 is the same as that shown in Fig. 1, but in Fig. 2, an adhesive layer 13 is provided between the decorative layer 12 and the magnet layer 14 of the decorative material 10. The configuration of each layer that constitutes the decorative material 10 will now be described in more detail.

[0028] (Magnet layer) The magnet layer 14 is fixed uniformly on one side of the decorative layer 12, and constitutes the second surface 102 of the decorative material 10. By providing the decorative material 10 with the magnet layer 14, the decorative material 10 can be detachably attached to a base containing a ferromagnetic material. Furthermore, the decorative material 10 can be attached to the base at the application site without using a solvent. In order to ensure that the decorative material 10 is fixed sufficiently strongly to the base, it is preferable that the magnetic flux density of the magnet layer 14 is 20 mT or more.

[0029] The magnet layer 14 may be uniformly provided on one side of the decorative layer 12, specifically on the second side of the decorative material 10. For example, the magnet layer 14 may have a patterned planar shape. In addition, in a planar view, the magnet layer may have a plurality of through holes, notches, etc. From the viewpoint of suppressing the in-plane variation in the fixing strength of the decorative material 10 to the base, it is preferable that the magnet layer does not have the above-mentioned through holes or notches. Furthermore, from the standpoint of suppressing in-plane variation in the fixing strength of the decorative material 10 to the base, the magnetic layer 14 is preferably provided over 80% or more of the area viewed from a direction perpendicular to the main surface of the decorative material 10, more preferably over 90% or more of the area viewed from a direction perpendicular to the main surface of the decorative material 10, and even more preferably over the entire side of the second surface 102 of the decorative material 10.

[0030] It is also preferable that the decorative material 10 is a long sheet material, and that the magnet layer 14 is provided over the entire longitudinal direction of the decorative material 10 in a cross-sectional view in the lamination direction of the decorative layer 12 and the magnet layer 14. In this way, the magnet layer 14 is provided without any gaps when the decorative material 10 is viewed from the side, so that the in-plane variation in the fixing strength of the decorative material 10 to the base can be further suitably suppressed.

[0031] From the viewpoint of suppressing in-plane variations in the fixing strength of the decorative material 10 to the base, the magnet layer 14 preferably has a continuous integral structure, and may be, for example, a single layer- or sheet-like member.

[0032] The magnet layer 14 may be an isotropic magnet layer or an anisotropic magnet layer. From the standpoint of increasing the strength with which the decorative material 10 is fixed to the base, it is preferable that the magnet layer 14 be an anisotropic magnet layer. On the other hand, from the standpoint of increasing the ease of removal of the decorative material 10 from the base, it is preferable that the magnet layer 14 be an isotropic magnet layer.

[0033] The magnet layer 14 is preferably multi-pole magnetized on the back surface opposite to the decorative layer 12 . With regard to the magnetization pitch (mm) relative to the total thickness (mm) of the decorative material 10, (magnetization pitch / total thickness) is preferably 1.00 or more, more preferably 1.50 or more, and even more preferably 1.80 or more, from the viewpoint of increasing the fixing strength of the decorative material 10 to the base. In addition, from the viewpoint of increasing the ease of removal of the decorative material 10 from the base, (magnetization pitch / total thickness) may be, for example, 3.5 or less, preferably 3.00 or less, more preferably 2.60 or less, and even more preferably 2.30 or less.

[0034] The magnetization pitch (mm) of the magnet layer 14 is, for example, 0.2 mm or more, preferably 0.5 mm or more, more preferably 1.0 mm or more, and even more preferably 1.5 mm or more, from the viewpoint of increasing the fixing strength of the decorative material 10 to the base. In order to facilitate the removal of the decorative material 10 from the base, the magnetization pitch (mm) of the magnet layer 14 is preferably 5.0 mm or less, more preferably 4.0 mm or less, and even more preferably 3.5 mm or less.

[0035] The magnet layer 14 can be, for example, a layer made by binding magnet powder with a binder (binding resin), and more specifically, is a magnet sheet. The magnet powder preferably has excellent magnetic properties, for example, an alloy containing R (where R is at least one of the rare earth elements including Y), preferably an alloy containing R (where R is at least one of the rare earth elements including Y), TM (where TM is at least one of the transition metals), and B (boron).

[0036] The binder contained in the magnet layer 14 may be either a thermoplastic resin or a thermosetting resin. Of these, examples of the thermoplastic resin include polyamides (e.g., nylon 6, nylon 46, nylon 66, nylon 610, nylon 612, nylon 11, nylon 12, nylon 6-12, nylon 6-66, nylon 6T, nylon 9T), thermoplastic polyimides, liquid crystal polymers such as aromatic polyesters, polyphenylene oxide, polyphenylene sulfide, polyethylene, polypropylene, polyolefins such as ethylene-vinyl acetate copolymers, modified polyolefins, polyesters such as polycarbonate, polymethyl methacrylate, polyethylene terephthalate (PET), polybutylene terephthalate, polyether, polyether ether ketone, polyetherimide, polyacetal, and the like, as well as copolymers, blends, polymer alloys, and the like mainly made of these, and one or more of these can be mixed and used.

[0037] Examples of the thermosetting resin include various epoxy resins such as bisphenol type, novolac type, and naphthalene type, phenol resin, urea resin, melamine resin, polyester (unsaturated polyester) resin, polyimide resin, silicone resin, and polyurethane resin, and one or more of these can be mixed and used. The thermosetting resin (uncured) used may be liquid or solid (powdered) at room temperature.

[0038] The thickness (average thickness) of the magnet layer 14 may be changed as appropriate from the viewpoint of increasing the adhesive strength of the decorative material 10 to the substrate or from the viewpoint of reducing the overall weight of the decorative material 10, but is preferably 0.10 to 2.92 mm, and more preferably 0.20 to 1.90 mm. The size and shape of the magnet layer 14 may be changed as appropriate depending on the shape of the decorative material 10, etc.

[0039] (adhesive layer) The magnet layer 14 may be fixed to the decorative layer 12 by an adhesive layer 13 as shown in FIG. The material of the adhesive layer 13 is not limited, but may be, for example, mainly made of an adhesive. Examples of the adhesive include an acrylic adhesive, a rubber adhesive, and a silicone adhesive.

[0040] Examples of acrylic pressure sensitive adhesives include polymers or copolymers that are primarily composed of a main monomer component with a low glass transition temperature (Tg) that provides adhesion, a comonomer component with a high Tg that provides adhesiveness and cohesive strength, and a functional group-containing monomer component for crosslinking or improving adhesion.

[0041] Examples of the main monomer component include acrylic esters such as alkyl acrylates, such as ethyl acrylate, butyl acrylate, amyl acrylate, 2-ethylhexyl acrylate, octyl acrylate, cyclohexyl acrylate, and benzyl acrylate, and methacrylic esters such as alkyl methacrylates, such as butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, and benzyl methacrylate.

[0042] Examples of the comonomer component include methyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl acetate, styrene, and acrylonitrile.

[0043] Examples of functional group-containing monomer components include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and N-methylolacrylamide; acrylamide, methacrylamide, and glycidyl methacrylate.

[0044] Examples of rubber-based adhesives include those containing one or more types selected from the group consisting of natural rubber, isoprene rubber, styrene-butadiene, reclaimed rubber, and polyisobutylene, and those mainly containing block copolymers containing rubbers such as styrene-isoprene-styrene and styrene-butadiene-styrene.

[0045] Examples of silicone-based adhesives include those containing one or two types selected from the group consisting of dimethylsiloxane-type silicones and diphenylsiloxane-type silicones.

[0046] The above adhesives may be either non-crosslinked or crosslinked. In the latter case, a crosslinking agent may be added as necessary. Examples of crosslinking agents include epoxy compounds, isocyanate compounds, metal chelate compounds, metal alkoxides, metal salts, amine compounds, hydrazine compounds, and aldehyde compounds. Such adhesives may be either organic solvent type or emulsion type.

[0047] Furthermore, various additives such as plasticizers, tackifiers, thickeners, fillers, antioxidants, preservatives, anti-mold agents, dyes, pigments, etc. may be added to the adhesive layer 13 as necessary.

[0048] (Decorative layer) The configuration of the decorative layer 12 in FIG. 1 and FIG. 2 will be described in more detail below. For example, in this embodiment, the decorative layer 12 may have the configuration shown in Fig. 3. Fig. 3 is a cross-sectional view showing the configuration of a decorative material 10 according to this embodiment.

[0049] 3, decorative layer 12 includes a surface layer 120 and a core layer 129. Decorative layer 12 may be configured to include one or more resins selected from the group consisting of melamine resin, polyvinyl chloride, polyvinyl fluoride, polyvinylidene fluoride, polyester, polytetrafluoroethylene, polyolefin, and (meth)acrylic resin. Decorative layer 12 may also include a solid content of, for example, a thermoplastic emulsion resin.

[0050] 3, the surface layer 120 is in contact with the core layer 129. The surface layer 120 further includes a printing substrate 122, a printed portion 121, a first resin layer 123, and a second resin layer 124. The surface layer 120 is exposed on the first surface 101 of the decorative material 10. However, the surface layer 120 does not have to include the printing base material 122 and the printed portion 121. For example, the surface layer 120 may have a design by including a resin layer or a metal layer that is embossed to provide irregularities. Also, a design may be applied to the surface of the first side 101 of the decorative material 10.

[0051] The decorative layer 12 is a portion that imparts design to a wall surface or the like that is the installation area of ​​the decorative material 10. The decorative layer 12 has a design that creates a beautiful appearance when viewed from the first surface 101 side. In the example shown in Fig. 3, the decorative layer 12 is configured so that the printed portion 121, i.e., the design such as a printed pattern, can be viewed from the first surface 101 side.

[0052] The decorative material 10 may contain a melamine resin or polyvinyl chloride on the surface on the side of the decorative layer 12. The decorative layer 12 may also contain a solid content of a thermoplastic emulsion resin. 3, for example, the surface layer 120 is made of a surface layer material made of a printing base material 122 that carries a resin (first resin layer 123) containing melamine resin on the first surface 101 side that is the design surface, and carries a solid content (second resin layer 124) of thermoplastic emulsion resin on the second surface 102 side that contacts the core layer 129. This will be explained in detail below.

[0053] The printing substrate 122 may be, for example, pulp, linter, synthetic fiber, or glass fiber. The printing substrate 122 may also be a titanium oxide-containing decorative paper that contains a pigment such as titanium oxide.

[0054] 3, the printed portion 121 imparts design to the cosmetic material 10. The printed portion 121 is ink carried on the printing substrate 122 by printing. The printed portion 121 may be formed in the form of a layer on the surface of the printing substrate 122, or at least a portion of the printed portion 121 may be impregnated into the printing substrate 122. The printing method is not limited, and gravure printing, inkjet printing, offset printing, etc. can be used.

[0055] The first resin layer 123 is a layer containing a resin (A) and is a layer located on the side of the first surface 101 of the printing substrate 122. The first resin layer 123 is preferably a transparent layer. The resin (A) preferably contains a melamine resin. This results in the surface of the decorative material 10 being made of a material containing melamine resin, which can impart suitable hardness to the surface of the decorative layer 12. This in turn can increase the durability of the decorative material 10. In the example shown in FIG. 3, the first resin layer 123 is exposed on the first surface 101 of the decorative material 10.

[0056] The melamine resin is not limited, and for example, a resin obtained by reacting melamine with formaldehyde under neutral or weakly alkaline conditions can be used.

[0057] As the melamine resin, commercially available melamine resins such as those manufactured by Sumitomo Chemical Co., Ltd. may also be used.

[0058] The method for supporting the resin (A) on the first surface 101 of the printing substrate 122 is not limited, and examples thereof include a method in which a resin varnish in which the resin (A) is dissolved in a solvent is applied using an apparatus such as a spray apparatus, a shower apparatus, a kiss coater, or a comma coater, and then the applied resin is dried by heating at approximately 80 to 130°C.

[0059] The solvent for dissolving the resin (A) is not limited, and examples thereof include water, methanol, and the like. Among these, water is preferable. A poor solvent may be used as long as it does not have a negative effect. The solid content of the resin varnish (all components excluding the solvent) is not limited, but is preferably 30 to 70 mass % of the resin varnish, and more preferably 45 to 60 mass %. This can improve the impregnation of the resin varnish into the substrate.

[0060] The second resin layer 124 is a layer containing a resin (B). The resin (B) is, for example, a solid content of a thermoplastic emulsion resin. In this specification, the thermoplastic emulsion resin is a thermoplastic resin dispersed in a solvent to form an emulsion state. The solid content of the thermoplastic emulsion resin refers to the components remaining after removing the solvent from the thermoplastic emulsion resin.

[0061] The solid content of the thermoplastic emulsion resin contains components that exist as emulsion resin particles, has adhesive properties with metals and various materials, and imparts flexibility to the decorative layer 12. Therefore, by carrying the solid content of the thermoplastic emulsion resin on the second surface 102 side of the surface layer 120, the adhesive strength between the surface layer 120 and the core layer 129 can be improved, and the bending processability of the decorative layer 12 can be improved.

[0062] Examples of the solid content of the thermoplastic emulsion resin include emulsion particles of thermoplastic resins such as acrylic resin, urethane resin, vinyl acetate copolymer, urethane acrylic composite particles, styrene butadiene rubber (SBR), and nitrile rubber (NBR). Among these, urethane acrylic composite particles are preferred. In this specification, the term "urethane acrylic composite particles" refers to particles having a heterophase structure of acrylic resin and urethane resin within a single particle.

[0063] Since urethane resin and acrylic resin each have high adhesive strength with core layer 129, the use of urethane acrylic composite particles can provide good adhesive strength with core layer 129. Furthermore, urethane resin has excellent properties, such as toughness, elasticity, and flexibility, while acrylic resin has excellent properties, such as transparency, durability, weather resistance, chemical resistance, and film-forming ability.

[0064] In addition, in this specification, the term "heterogeneous phase structure" refers to a structure in which a single particle contains a plurality of phases made of different types of resins, and examples thereof include a core-shell structure, a localized structure, and a sea-island structure.

[0065] The solid content of the thermoplastic emulsion resin may contain one of these types alone, or may contain a mixture of two or more different types of thermoplastic resins.

[0066] Furthermore, the solid content of the thermoplastic emulsion resin may contain, in addition to the above-mentioned thermoplastic resin emulsion particles, small amounts of a thickener, a penetration promoter, an antifoaming agent, and the like, as necessary.

[0067] The solid content of the thermoplastic emulsion resin preferably contains emulsion resin particles having an average particle size of 30 to 100 nm, and more preferably the average particle size of the emulsion resin particles is 60 to 90 nm, which improves the impregnation between the fibers of the surface layer base material and allows the resin to be impregnated further into the surface layer base material, thereby imparting good flexibility to the surface layer 120.

[0068] The method for supporting the solid content of the thermoplastic emulsion resin on the second surface 102 of the printing substrate 122 is not limited, and can be the same as the above-mentioned method for supporting the resin (A) on the first surface 101 of the printing substrate 122. That is, examples of the method include a method in which a thermoplastic emulsion resin in an emulsion state dissolved in a solvent is applied and dried by heating.

[0069] The solvent used in the thermoplastic emulsion resin is not limited, and may be, for example, water. A poor solvent may be used as long as it does not have a negative effect. The solid content of the thermoplastic emulsion resin (all components excluding the solvent) is not limited, but is preferably 25 to 60 mass % of the thermoplastic emulsion resin, and more preferably 30 to 45 mass %. This can improve the impregnation of the thermoplastic emulsion resin into the substrate.

[0070] The first resin layer 123 and the second resin layer 124 do not have to form a layer by themselves. That is, the resin (A) and the resin (B) only need to be supported on the printing substrate 122. Here, the printing substrate 122 supporting the resin means that the resin is attached to the surface of the printing substrate 122 (support) or is impregnated into the voids inside the printing substrate 122, and is in a state that allows the performance of the supported resin to be expressed after molding of the surface layer material. The first resin layer 123 and the second resin layer 124 have, for example, a layered distribution in the surface layer 120. The resin does not have to be uniformly distributed on the surface of the printing substrate 122 and inside the printing substrate 122.

[0071] The decorative layer 12 may include glass cloth. For example, in the example shown in Fig. 3, the core layer 129 is configured to include, for example, glass cloth or a prepreg having glass cloth as a base material. This can impart heat resistance, non-flammability, rigidity, and the like to the decorative layer 12.

[0072] The thickness of the core layer 129 is preferably 50 μm or more, and more preferably 80 μm or more, which can provide sufficient heat resistance and non-combustibility to the decorative layer 12. There is no upper limit to the thickness, but since a larger thickness increases the thickness and weight of the decorative layer 12 and also increases the cost, it is preferable to set the thickness within the range allowed in the design of the final product, and for example, it is preferably 350 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.

[0073] Moreover, from the viewpoint of reducing weight or improving ease of transport, the overall thickness of the decorative layer 12 is preferably 80 μm or more, more preferably 100 μm or more, and even more preferably 150 μm or more. From the viewpoint of improving the fixing strength to the base, the overall thickness of the decorative layer 12 is preferably 700 μm or less, more preferably 600 μm or less, and even more preferably 400 μm or less.

[0074] In addition, when the core layer 129 is impregnated with an adhesive, the core layer 129 may also function as the adhesive layer 13. The decorative layer 12 may further have a protective layer. The protective layer can be provided so as to be exposed on the first surface 101.

[0075] In addition, while FIG. 3 shows an example in which the printed portion 121 is located inside the decorative layer 12, the printed portion 121 may be located on the surface of the decorative layer 12 on the first surface 101 side.

[0076] The structure of the decorative material 10 is not limited to the above examples. The decorative material 10 can be composed of one or more of the following materials: cloth, hemp, cotton, silk, etc.; plastic resins such as polyvinyl chloride, PET, polyolefin, etc.; metals (foils) such as SUS, aluminum, etc.; paper such as cardboard, wood, bamboo, and rattan.

[0077] In addition, from the viewpoint of reducing the weight of the decorative material 10 and making the decorative material 10 easier to transport, if an intervening layer such as an adhesive layer 13 is provided between the decorative layer 12, or between the decorative layer 12 and the magnet layer 14, it is preferable that the decorative layer 12 and the intervening layer do not have a ferromagnetic layer.

[0078] On the other hand, the decorative layer 12 or the intermediate layer may have a layer containing a metal other than a ferromagnetic material. For example, in the decorative material 10 shown in FIG. 3, the surface layer 120 may contain a metal layer. More specifically, the metal layer may be provided between the core layer 129 and the second resin layer 124. By providing a metal layer, it is possible to impart a metallic luster to the decorative layer 12. The metal layer is, for example, a layer containing one or more selected from the group consisting of aluminum, gold, and silver. The thickness of the metal layer is not limited, but is preferably 1 nm to 300 μm in thickness from the viewpoint of imparting a metallic luster without impairing the flexibility of the cosmetic material 10.

[0079] (Method of manufacturing decorative materials) Next, a method for producing the decorative material 10 will be described below. The decorative material 10 is formed, for example, by fixing the magnet layer 14 to the decorative layer 12 via the adhesive layer 13. Specifically, an adhesive or the like that constitutes the adhesive layer 13 is applied to the decorative layer 12, and the magnet layer 14 is laminated thereon. However, the magnet layer 14 to which the adhesive has been applied may also be laminated on the decorative layer 12. In this embodiment, predetermined materials are selected and combined for the decorative layer 12, the magnet layer 14, and, if present, the adhesive layer 13. This makes it possible to stably obtain the decorative material 10 having an X / W ratio within the above-mentioned range.

[0080] The decorative layer 12 is produced, for example, as follows. The decorative layer 12 is obtained by overlapping the surface layer 120 and the core layer 129, and laminating them by heating and pressurizing them. In addition, by overlapping a predetermined plate material when forming the decorative layer 12, the surface roughness and light reflectance of the first surface 101 of the decorative material 10 can be adjusted, thereby improving the design.

[0081] The surface layer 120 is obtained as follows. First, a printed portion 121 is formed by printing a design such as a pattern on a printing substrate 122. Next, a first resin layer 123 is formed on one surface of the printing substrate 122 on which the printed portion 121 is provided, and a second resin layer 124 is formed on the other surface.

[0082] The manufacturing method of the decorative material 10 is not limited to the above-mentioned method. For example, a carrier film may be used as necessary. The carrier film is used to protect one of the layers during manufacturing or to facilitate manufacturing. The carrier film is subsequently removed and is therefore no longer included in the decorative material 10.

[0083] The decorative material 10 obtained as described above can be used, for example, in an interior or exterior construction method in which a decorative material comprising a magnetic material is attached to a base containing a ferromagnetic material.

[0084] Next, the effects of this embodiment will be described. According to this embodiment, the magnet layer 14 is uniformly provided on one side of the decorative layer 12, and X / W is within the above-mentioned specific range, so that the decorative material 10 can be easily removed from the base while the fixing strength of the decorative material 10 to the base is sufficiently ensured. Furthermore, since the magnet layer 14 is uniformly provided on one surface of the decorative layer 12, variation in the adsorption strength of the decorative material 10 within the surface on which the decorative material 10 is placed can be suppressed.

[0085] Second embodiment 4 is a cross-sectional view illustrating the structure of the decorative material 10 in this embodiment. The decorative material 10 shown in FIG. 4 is the same as the decorative material 10 described in the first embodiment (FIG. 3) except for the structure of the decorative layer 12.

[0086] 4, the decorative layer 12 includes a first resin layer 123, a second resin layer 124, and a printed portion 121. The second resin layer 124 functions as a printing base material 122.

[0087] The first resin layer 123 is, for example, a transparent resin film. The first resin layer 123 contains a synthetic resin, for example, polyvinyl chloride, polyvinyl fluoride, polyvinylidene fluoride, polyester, polytetrafluoroethylene, polyolefin resin, or (meth)acrylic resin. The first resin layer 123 is laminated on the second resin layer 124 on which the printed portion 121 is formed, for example, by lamination using an embossing rolling process. The thickness of the first resin layer 123 is, for example, 10 μm or more and 80 μm or less.

[0088] The second resin layer 124 includes a synthetic resin, for example, polyvinyl chloride, polyvinyl fluoride, polyvinylidene fluoride polyester, polyolefin resin, or (meth)acrylic resin. The second resin layer 124 may further include a non-flammable inorganic filler. Examples of the inorganic filler include CaCO3, Mg(OH)2, Al(OH)3, SiO2, and clay (for example, montmorillonite or kaolin). The thickness of the second resin layer 124 is, for example, 60 μm or more and 150 μm or less. The second resin layer 124 can be formed, for example, by casting or calendaring.

[0089] 4 is manufactured in the same manner as the decorative material 10 according to the first embodiment, except for the method of forming the decorative layer 12. In this embodiment, the decorative layer 12 is obtained by forming a printed portion 121 by printing on the surface of the second resin layer 124 that faces the first surface 101, and then forming a first resin layer 123 so as to cover the printed portion 121.

[0090] According to this embodiment, it is possible to obtain the same effects as those of the first embodiment. Furthermore, according to this embodiment, for example, it is possible to simplify the manufacturing process of the decorative layer 12 and the decorative material 10 including the same.

[0091] Next, a modification of this embodiment will be described. For example, in the decorative material 10 shown in Fig. 4, a metal layer may be provided at a predetermined position, for example, between the second resin layer 124 and the adhesive layer 13. The configuration of the metal layer may be the configuration described above in the first embodiment. By providing a metal layer, it is possible to impart a metallic luster to the decorative layer 12.

[0092] 4, a protective layer may be further provided on the side of the first surface 101 of the decorative layer 12. By providing a protective layer, the durability of the decorative material 10 is further improved. Specifically, the protective layer is a transparent layer having scratch resistance. The protective layer is exposed on the first surface 101 of the decorative material 10. The protective layer is composed of, for example, a resin (C) and a filler. The thickness of the protective layer is not limited, but is, for example, 5 μm or more and 100 μm or less.

[0093] Resin (C) includes, for example, one or more selected from the group consisting of reactive polyurethane resins, polyester resins, polyolefin resins, acrylic resins, acrylic-urethane resins, silicones, and fluoropolymers.

[0094] Examples of the filler include beads or particles made of alumina, silica, chromium oxide, iron oxide, zirconium, titanium, or a mixture thereof, but are not limited thereto. The particle shape of the filler includes, but is not limited to, spherical, tufted, spheroidal, acicular, polyhedral, cylindrical, or amorphous. The hardness of the filler is, for example, 8 to 15 Mohs hardness. The average particle size of the filler may be equal to or greater than the thickness of the protective layer after drying, for example, 10 μm or more and 110 μm or less. It is preferable that the filler is uniformly dispersed in the protective layer.

[0095] The protective layer may further include a crosslinking agent. Examples of the crosslinking agent include a bisamide crosslinking agent, an aziridine crosslinking agent, a carbodiimide crosslinking agent, an epoxy crosslinking agent, and an isocyanate crosslinking agent. The content of the crosslinking agent is, for example, 5 parts by mass or more and 30 parts by mass or less in terms of solid content relative to 100 parts by mass of the resin (C).

[0096] The protective layer can be formed by applying a material containing the above-mentioned components to the surface of the first resin layer 123 that will become the first surface 101, for example, by a bar coating method, and pressing it between a heated roll and an unheated nip roll.

[0097] (Third embodiment) In this embodiment, a specific example of an application method using the decorative material 10 described in the above embodiment will be described. Figures 5 and 6 are diagrams for explaining the construction method in this embodiment. Figure 5 shows a cross section of a wall constructed by the method of this embodiment. Figure 6 is a perspective view of a wall constructed by the method of this embodiment, with a part of the base 20 and the decorative material 10 omitted.

[0098] The application method of this embodiment is an interior or exterior application method that includes a step of attaching a decorative material having a magnetic material (magnetic layer 14), specifically the decorative material 10 described in the above embodiment, to a base 20 containing a ferromagnetic material. Moreover, according to the construction method of this embodiment, a wall structure including a laminate of the base 20 containing a ferromagnetic material and the decorative material 10 described in the above embodiment can be obtained. This will be explained in detail below.

[0099] The construction method of the present embodiment is, for example, a method for constructing an interior wall or an exterior wall of a room, a passageway, etc. There is no limitation on the building to which the interior or exterior is constructed, and examples thereof include buildings and houses.

[0100] The decorative material 10 is a member that is integrated with the wall to give the wall an aesthetic look. In Fig. 5 and Fig. 6, the decorative material 10 includes, for example, a decorative layer 12, a magnet layer 14, and an adhesive layer 13 that bonds the decorative layer 12 and the magnet layer 14. The decorative material 10 may be any of those described in any of the above-mentioned embodiments.

[0101] The decorative material 10 is fixed so as to cover almost the entirety of the base 20. For example, 95% or more of the surface of the base 20 opposite the building structure 30 is covered with the decorative material 10. In the example of Fig. 5 and Fig. 6, the base 20 has multiple base layers. The base layer is a layer located between the wall framework and the decorative material 10. Alternatively, the base layer is a layer embedded in the wall framework so as to be located inside the wall relative to the decorative material 10. The base layers, either alone or in combination, perform functions such as structural reinforcement, heat insulation, moisture resistance, waterproofing, and fire resistance. In the example of Fig. 5 and Fig. 6, the base 20 includes a first base layer 22 and a second base layer 24. However, the base 20 may further include other base layers. The base 20 is fixed to the building structure 30.

[0102] The framework 30 is, for example, the framework of a building, and is a framework that supports the structure of the building. The framework 30 is made of wood, metal, reinforced concrete, etc. The base 20 does not necessarily have to be fixed to the framework 30 of the building. For example, a laminate of the base 20 and the decorative material 10 may be part of a partition that divides an interior space. The decorative material 10 may also function as a corner material with a protruding corner, a trim material, a joiner, a notice panel, etc.

[0103] The base 20 includes a ferromagnetic material, and a magnet is attracted to the base 20. The ferromagnetic material is, for example, iron. In this embodiment, the base 20 includes a ferromagnetic layer including a ferromagnetic material. For example, at least one of the second base layer 24 and the first base layer 22 is a ferromagnetic layer. Here, it is preferable that the base layer of the base 20 that is closest to the decorative material 10 is a ferromagnetic material layer. In this way, the fixing strength of the decorative material 10 to the base 20 can be improved. Examples of base layers other than the ferromagnetic layer include inorganic boards such as calcium silicate boards, gypsum boards, and volcanic glass laminates, and wooden plywood.

[0104] In this embodiment, the ferromagnetic layer is, for example, a plate material containing a ferromagnetic material. The plate material containing a ferromagnetic material is, for example, a plate of a ferromagnetic material such as an iron plate. The plate material containing a ferromagnetic material may be a composite member of a material other than a ferromagnetic material and a ferromagnetic material such as iron powder or iron foil. By using the composite member, it is possible to improve the degree of freedom of shape and reduce the weight. Examples of materials other than a ferromagnetic material include resin, wood, gypsum, calcium silicate, cement, and glassy materials. In the composite member, the material other than a ferromagnetic material and the ferromagnetic material may be mixed or laminated. The composite member is obtained, for example, by mixing resin particles or wood chips with iron powder and forming it into a plate shape. Alternatively, the composite member is obtained by laminating and bonding a plate-shaped member of a material other than a ferromagnetic material and iron foil. In addition, when the base layer is formed of an earth wall, the composite member may be formed by forming a layer using earth mixed with a ferromagnetic material. The thickness of the ferromagnetic layer is not limited, but is, for example, 1 mm or more and 20 mm or less.

[0105] The base 20 only needs to contain a ferromagnetic material in at least a portion of the base 20 when viewed from a direction perpendicular to the main surface, and does not need to contain a ferromagnetic material throughout. The area of ​​the area containing the ferromagnetic material relative to the entire area of ​​the base 20 is not limited, but is preferably 20% or more, and more preferably 50% or more. For example, the base 20 may include a ferromagnetic material layer patterned in a lattice shape. In addition, it is preferable that the area of ​​the base 20 facing the outer periphery of each decorative material 10 contains a ferromagnetic material.

[0106] Since the base 20 contains a ferromagnetic material, the magnet layer 14 is attracted to the base 20, and the decorative material 10 can be fixed to the base 20. According to the application method of this embodiment, the decorative material 10 is detachable from the base 20, so that when the decorative material 10 becomes dirty or damaged, or when the interior or exterior design is to be changed, the decorative material 10 can be easily replaced in a short time without damaging the base 20. In addition, when fixing the decorative material 10 to the base 20 at the application site, there is no need to use an adhesive. Therefore, no odor due to organic solvents or the like is generated during drying. Furthermore, since the base 20 can be quickly and easily fixed to the decorative material 10, the application period can be shortened.

[0107] As shown in Fig. 6, the first base layer 22 and the second base layer 24 may each be formed of a plurality of plate materials. Here, it is preferable that the boundaries between the plurality of plate materials in the first base layer 22 and the boundaries between the plurality of plate materials in the second base layer 24 do not overlap each other except at intersections. This prevents fire from leaking and spreading from the boundaries in the event of a fire, improving fire resistance.

[0108] In the second base layer 24, which is the base layer closest to the decorative material 10, the boundaries between the multiple plate materials are filled with putty 201. Furthermore, the putty 201 smooths out any steps that occur at the boundaries between the plate materials.

[0109] The decorative material 10 is fixed to the base 20 by magnetic force. A plurality of decorative materials 10 may be laid out on one wall surface. This makes it easier to transport the decorative materials 10 to the application site. When a plurality of decorative materials 10 are arranged and fixed to a wall surface, gaps may be provided between the decorative materials 10. This makes it difficult for the decorative materials 10 to warp even if they expand or contract due to moisture or the like. However, if the entire decorative material 10 is made of a material that does not expand or contract easily, such as resin, there is no need to provide gaps between the decorative materials 10.

[0110] The plate material containing a ferromagnetic material may have one or more openings. By having an opening in the plate material, the weight of the base 20 can be reduced, and the earthquake resistance of the building can be improved. However, from the viewpoint of improving fire resistance, it is preferable that the opening does not overlap the boundary between the plates constituting the other base layers.

[0111] Moreover, the construction method according to this embodiment may further include a step of fixing the base 20 to a structural member (framework) of the wall, such as the main body 30, and a step of fixing the decorative material 10 to the base 20 by magnetic force. In the process of fixing the base 20, a plurality of plate materials are attached to the structural member with a stapler, screws, etc. so as to cover almost the entire wall surface, forming a first base layer 22. Next, a plurality of plate materials are attached to the first base layer 22 with a stapler, screws, etc. so as to cover almost the entire first base layer 22, forming a second base layer 24. For example, the second base layer 24 is a ferromagnetic layer. Then, putty 201 is applied to the boundaries between the plurality of plate materials constituting the second base layer 24 to fill the gaps and smooth out the steps. Next, in the process of fixing the decorative material 10 to the base 20 by magnetic force, the magnet layer 14 of the decorative material 10 is oriented toward the base 20, and the decorative material 10 is attached to the base 20.

[0112] If it is desired to replace the decorative material 10, the decorative material 10 is peeled off from the base 20 and a new decorative material 10 is affixed to the base 20.

[0113] It should be noted that another sheet material may be sandwiched between the ferromagnetic layer of the base 20 and the decorative material 10. In this way, the design is not lost even when the decorative material 10 is unavoidably removed. Examples of the sheet material include a resin sheet such as a polyvinyl chloride sheet, and paper. The sheet material may be attached as part of the base 20 so as to form, for example, the outermost surface of the base 20 (the surface closest to the decorative material 10), or may be sandwiched between the base 20 and the decorative material 10. Also, instead of providing a sheet material, a coating film made of paint may be formed on the outermost surface of the base 20. In this case, the same effect can be obtained.

[0114] The application method according to this embodiment can be realized by using an interior or exterior application set including a base material containing a ferromagnetic material and a decorative material 10 having a magnet layer 14. In this embodiment, the base material containing a ferromagnetic material is a member that constitutes the ferromagnetic layer, and is a plate material containing the above-mentioned ferromagnetic material. When it is desired to replace the decorative material 10, it is sufficient to prepare only a new decorative material 10 separately.

[0115] Next, the effects of this embodiment will be described. According to this embodiment, the decorative material 10 having the above-described configuration is attached to a base 20 containing a ferromagnetic material, thereby improving the balance between the fixing strength of the decorative material 10 to the base 20 and the ease of removing the decorative material 10 from the base 20. For example, by attaching a decorative material 10 having a magnet layer 14 to a base 20 containing a ferromagnetic material, a wall structure can be realized that allows the decorative material 10 to be easily replaced in a short time when it is desired to replace it.

[0116] Furthermore, since there is no need to use adhesives at the construction site, the decorative material can be attached in a short time, and odors caused by organic solvents, etc. can be avoided.

[0117] Next, a modification of this embodiment will be described. For example, in the application methods shown in Figures 5 and 6, the ferromagnetic layer may be a solidified paint containing a ferromagnetic material. By attaching the decorative material 10 having the magnet layer 14 to the base 20 containing a ferromagnetic material, a wall structure can be realized that allows the decorative material 10 to be easily replaced in a short time when it is desired to replace it. In addition, the base containing the ferromagnetic material can be easily prepared by applying paint, and application can be easily made to curved wall surfaces, etc.

[0118] Specifically, the base 20 includes a third base layer in addition to the first base layer 22 and the second base layer 24. The third base layer is provided between the second base layer 24 and the magnet layer 14. The third base layer is a ferromagnetic layer made of a solidified paint containing a ferromagnetic material. The solidified paint is a solid obtained by solidifying or hardening the paint. In this configuration, the first base layer 22 and the second base layer 24 do not need to contain a ferromagnetic material. That is, the first base layer 22 and the second base layer 24 may be inorganic boards such as calcium silicate boards, gypsum boards, and volcanic vitreous laminates, or wooden plywood. The third base layer is formed by applying paint containing a ferromagnetic material to another base layer and solidifying or hardening it.

[0119] In a configuration in which a third base layer made of a solidified paint containing a ferromagnetic material is provided, in the process of fixing the base 20 to the structural member (framework) of the wall, the first base layer 22 and the second base layer 24 are formed, putty 201 is applied, and then paint containing a ferromagnetic material (hereinafter also simply referred to as "paint") is applied to the surface of the second base layer 24, as in the construction method described above. The third base layer is formed when the paint dries. Next, a process of fixing the decorative material 10 to the base 20 by magnetic force is performed, as in the construction method described above.

[0120] At least one of the first base layer 22 and the second base layer 24 may be formed using a base board material in which paint containing a ferromagnetic material is applied to a board material such as a calcium silicate board, a gypsum board, or a wooden plywood, and the paint is dried to form a solidified product. In this way, there is no need to dry the paint at the construction site, and it is possible to prevent the generation of odor. In addition, there is no need to set aside a drying time, and construction can be performed in a short time.

[0121] The paint is preferably applied so as to cover the entire second base layer 24, but may be applied so as to cover only a portion of the second base layer 24. When viewed from a direction perpendicular to the main surface of the base 20, the area of ​​the region to which the paint is applied relative to the entire area of ​​the base 20 is not limited, but is preferably 20% or more, and more preferably 50% or more. For example, the base 20 may be painted in a lattice pattern. In addition, it is preferable to paint the regions of the base 20 that face the outer periphery of each decorative material 10.

[0122] The paint contains a ferromagnetic material and a binder. The ferromagnetic material is, for example, a ferromagnetic powder such as iron powder. The particle size is not limited, but the median diameter D of the ferromagnetic powder is preferably 100 nm or more. 50 The thickness is preferably 0.02 mm or more and 0.2 mm or less, and more preferably 0.05 mm or more and 0.1 mm or less. This makes it easier to apply the paint uniformly. The content of the ferromagnetic powder in the solid matter of the paint is preferably 50 mass % or more and 90 mass % or less, and more preferably 60 mass % or more and 80 mass % or less. This allows the decorative material 10 to be fixed to the base 20 with sufficient magnetic force.

[0123] Examples of the binder contained in the paint include the same resins as those exemplified as the binder contained in the magnet layer 14 .

[0124] In addition to the ferromagnetic material and the binder, the paint may contain a solvent, a plasticizer, a dispersant, a thickener, and other additives. The total content of these additives is, for example, 5% by mass or less based on the solidified paint. The paint can be obtained by mixing the above-mentioned components.

[0125] Such an application method can be realized by using an interior or exterior application set including a base material containing a ferromagnetic material and a decorative material 10 having a magnet layer 14. The base material containing a ferromagnetic material is a base plate material on which a paint containing a ferromagnetic material or a solidified paint containing a ferromagnetic material is formed.

[0126] Although the embodiments of the present invention have been described above with reference to the drawings, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES

[0127] (Examples 1 to 5 and Comparative Example 1) A decorative material having a magnet layer and a decorative layer having the configurations shown in Table 1 was produced by the following method and evaluated. The evaluation results are also shown in Table 1.

[0128] Example 1 A decorative material having the configuration shown in FIG. 3 was produced. Specifically, a pattern (printed portion 121) was printed on a titanium oxide-containing decorative paper as a printing substrate 122, and a melamine resin (first resin layer 123) was supported on the printed surface. In addition, a solid content (second resin layer 124) of a thermoplastic emulsion resin was supported on the surface opposite to the printed surface of the printing substrate 122. The laminate thus obtained to become the surface layer 120 and a glass cloth 1 having a thickness of 100 μm that constitutes the core layer 129 were overlapped, and the laminate was integrated by heating and pressurizing to obtain a laminate 1 (thickness 0.3 mm) to become the decorative layer 12. A magnet sheet 1 (thickness of adhesive layer 13: 0.1 mm) coated with adhesive was attached to the glass cloth 1 side of the laminate 1 to obtain a decorative material 1. An acrylic adhesive was used as the adhesive, and a one-sided magnetized isotropic multi-pole magnetized sheet (manufactured by Nichirei Magnet Corporation, 004404, thickness 1.2 mm, magnetization pitch 3.0 mm) was used as the magnet sheet 1 used in the magnet layer 14.

[0129] Example 2 Cosmetic material 2 was obtained in the same manner as in Example 1, except that magnet sheet 2 was used instead of magnet sheet 1. As magnet sheet 2, a one-sided magnetized isotropic magnetized sheet (manufactured by Mag-X Corporation, NT-7S 0.8 plain, thickness 0.8 mm, magnetization pitch 2.0 mm) was used.

[0130] Example 3 A decorative material 3 was obtained in the same manner as in Example 1, except that laminate 2 (thickness: 0.5 mm) was used instead of laminate 1 serving as decorative layer 12, and magnet sheet 3 was used instead of magnet sheet 1. Laminate 2 was obtained in the same manner as laminate 1, except that glass cloth 2 having a thickness of 250 μm was used instead of glass cloth 1. In addition, as magnet sheet 3, a one-sided magnetized anisotropic multipolar magnetized sheet (manufactured by Nichirei Magnet Corporation, 007863, thickness 0.4 mm, magnetization pitch 2.0 mm) was used.

[0131] Example 4 A decorative material was produced with the configuration shown in Fig. 2. Specifically, the liner was peeled off from a film laminated with a 0.1 mm thick polyvinyl chloride film that would become the decorative layer 12 and an adhesive layer 13 (0.1 mm thick) made of an acrylic adhesive, and the film was attached to a magnet sheet 2 that would become the magnet layer 14 at 55°C, to obtain the decorative material 4.

[0132] Example 5 A decorative material 6 was obtained in the same manner as in Example 4, except that magnet sheet 3 was used instead of magnet sheet 2.

[0133] Comparative Example 1 A decorative material 5 was obtained in the same manner as in Example 1, except that magnet sheet 4 was used instead of magnet sheet 1. As magnet sheet 4, a one-sided magnetized isotropic magnetized sheet (manufactured by Nichirei Magnet Corporation, 004014, thickness 3.0 mm, magnetization pitch 5.0 mm) was used.

[0134] (Methods for measuring and evaluating the physical properties of cosmetic materials) The decorative materials obtained in the above examples were subjected to the following measurements and evaluations. (surface magnetic flux density, basis weight) The surface magnetic flux density X (mT) of the surface where the magnet layer of the decorative material is exposed, i.e., the second surface, was measured using a Tesla Meter TM-701 manufactured by KANETEC. The basis weight W (kg / m 2 ) and measure X / W(mT m 2 The value was calculated using the formula (1 / kg).

[0135] (Shore D hardness) A rubber hardness tester (Shimadzu) was placed perpendicular to the surface to be measured, and the displayed value was read when a load of 500 g was applied from directly above.

[0136] (Flexural modulus) The measurement sample was 20 mm wide and 80 mm long, and the sample was bent into a loop and attached so that it overlapped by 10 mm. The repulsive force when the loop was crushed in the diametric direction at a speed of 3 mm / min was measured using a Tensilon (manufactured by A&D Co., Ltd.), and the elastic modulus (MPa) was calculated from the obtained repulsive force, which was defined as the flexural elastic modulus E.

[0137] (immobilization strength) The fixing strength of the cosmetic material obtained in each example was evaluated by the following method. Specifically, a galvanized steel plate with a vinyl chloride sheet (thickness 0.2 mm) attached to its surface was prepared as a base. The prepared base was set up so that its surface was parallel to the vertical direction, and a 10 cm square decorative material was attached to the base. At this time, the second surface 102 of the decorative material was made to face the base. A weight was then attached to the first surface 101 of the decorative material, and it was confirmed whether the decorative material would shift relative to the base. If there was no shift with a 300 g weight, it was marked as "◎", if there was no shift with a 200 g weight but there was shift with a 300 g weight, it was marked as "◯", and if there was shift with a 200 g weight, it was marked as "X".

[0138] (Ease of removal) The ease of removal of the cosmetic material obtained in each example was evaluated by the following method. Specifically, a galvanized steel plate with a vinyl chloride sheet (thickness 0.2 mm) attached to its surface was prepared as a base. The surface of the prepared base was set up so that it was parallel to the vertical direction, and a 30 cm square decorative material was attached to the base. At this time, the second surface 102 of the decorative material was made to face the base. The load required to peel off the decorative material by gripping a corner with a double clip and lifting it up was measured with a digital force gauge (manufactured by SHINPO Corporation). If it could be peeled off with a force of 2 N or less, it was marked as "○", and if more force was required, it was marked as "×".

[0139] [Table 1]

[0140] As can be seen from Table 1, the decorative materials obtained in each Example had excellent fixing strength to the base material. Furthermore, the decorative materials obtained in each Example exhibited a suitably high fixing strength, and could be easily removed from the base material. [Explanation of symbols]

[0141] 10 Cosmetic materials 12 Makeup layer 13 Adhesive layer 14 Magnet layer 20. Base 22 1st base layer 24 Second base layer 30 skeleton 101 Page 1 102 Side 2 120 Surface layer 121 Printing Department 122 Printing base material 123 1st resin layer 124 2nd resin layer 129 Core layer 201 Pate

Claims

1. A decorative material having a decorative layer and a magnet layer uniformly provided on one surface of the decorative layer, The basis weight W (kg / m 2 ) for the magnetic flux density X (mT) of the decorative material, X / W (mT・m 2 / kg) is 5.0 or more and 18.0 or less, The decorative material in which the magnet layer is magnetized with multiple poles on the back surface of the surface facing the decorative layer, and the magnetization pitch (mm) relative to the total thickness (mm) of the decorative material is 2.00 or more and 3.00 or less (excluding 2.0).

2. the Shore D hardness of the surface of the decorative material on the side of the decorative layer is 50 or more and 110 or less, as measured by a method in which a rubber hardness tester (manufactured by Shimadzu Corporation) is placed perpendicularly to the surface on the side of the decorative layer and a load of 500 g is applied from directly above to read the displayed value; The decorative material according to claim 1, wherein the Shore D hardness of the surface of the decorative material on the side of the magnet layer is 50 or more and 110 or less, as measured by a rubber hardness tester (manufactured by Shimadzu Corporation) placed perpendicular to the surface on the side of the magnet layer and a load of 500 g applied from directly above to read the displayed value.

3. 3. The decorative material according to claim 1 or 2, wherein the thickness of the decorative material is 0.5 mm or more and 3.0 mm or less.

4. 4. The decorative material according to claim 1, wherein the magnet layer is a continuous integral structure.

5. The decorative material is a long sheet material, The decorative material according to claim 1 , wherein the magnet layer is provided over the entire length of the decorative material in a cross-sectional view in a lamination direction of the decorative layer and the magnet layer.

6. The decorative material according to any one of claims 1 to 5, wherein the decorative layer, or, if an intervening layer is provided between the decorative layer and the magnet layer, the decorative layer and the intervening layer do not have a ferromagnetic layer.

7. The decorative material according to claim 1 , wherein the decorative layer comprises glass cloth.

8. The decorative material according to any one of claims 1 to 7, wherein the decorative layer contains one or more resins selected from the group consisting of melamine resins, polyvinyl chloride, polyvinyl fluoride, polyvinylidene fluoride, polyester, polytetrafluoroethylene, polyolefins, and (meth)acrylic resins.

9. The decorative material according to claim 1 , wherein the decorative layer contains a solid content of a thermoplastic emulsion resin.

10. The decorative material according to claim 1 , wherein the decorative material contains a melamine resin or polyvinyl chloride on a surface on the decorative layer side.

11. The decorative material according to claim 1 , which is used in an interior or exterior construction method in which a decorative material comprising a magnetic material is attached to a base containing a ferromagnetic substance.

12. A wall structure comprising a laminate of a substrate containing a ferromagnetic material and the decorative material according to any one of claims 1 to 11.

13. 12. An interior or exterior application set comprising a base material containing a ferromagnetic material and the decorative material according to claim 1.

14. A method for applying interior or exterior coating, comprising the step of attaching the decorative material according to any one of claims 1 to 11 to a substrate containing a ferromagnetic material.

Citation Information

Patent Citations

  • Elevator interior material

    JP2002128429A

  • Decorative plate with magnetic layer and method for fitting the plate

    JP2004098296A

  • Decorative plate and storage using it

    JP2005254544A

  • Decorative material sheet, sheet wound body, construction method, wall structure and construction set

    JP2018083328A

  • Decorative material

    JP2018122480A