Photocurable resin composition for three-dimensional modeling and method for manufacturing article
The photocurable resin composition addresses the challenge of achieving high toughness and sliding properties by combining specific compounds and particles, enabling the production of durable objects suitable for stereolithography.
Patent Information
- Application Number
- JP2020156653
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-11
- Filing Date
- 2020-09-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-25
AI Technical Summary
Existing photocurable resin compositions struggle to simultaneously achieve high toughness and sliding properties, which are essential for shaping objects used as actual products, and are not suitable for stereolithography due to the use of thermosetting resins.
A photocurable resin composition comprising polyfunctional radically polymerizable compounds, monofunctional radically polymerizable compounds, polyethylene particles, and a curing agent, with specific properties such as average particle diameter and viscosity, to create objects with high toughness and sliding properties.
The composition enables the production of shaped objects with excellent toughness and sliding properties, suitable for stereolithography, ensuring high precision and durability.
Smart Images

Figure 0007566547000013 
Figure 0007566547000001 
Figure 0007566547000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocurable resin composition for three-dimensional modeling and a method for producing a three-dimensional object using the same. [Background technology]
[0002] As an example of the use of a liquid curable resin composition, optical three-dimensional modeling (stereolithography) has been actively researched, in which a curable resin composition is cured layer by layer with light such as ultraviolet light, and the layers are stacked in sequence to produce a desired three-dimensional object. Since stereolithography can produce objects with higher accuracy than other methods, its applications are expanding beyond the production of prototypes for shape confirmation (rapid prototyping) to the production of working models and molds for functionality verification (rapid tooling). It is also expanding to the production of actual products (rapid manufacturing).
[0003] In light of this, the demands for curable resin compositions are becoming more sophisticated. For example, there is a demand for a curable resin composition capable of forming an article having sliding properties showing a low coefficient of friction and high abrasion resistance, and mechanical properties such as high rigidity and toughness, which are comparable to those of general-purpose engineering plastics. Patent Document 1 discloses a technology for imparting excellent sliding properties and abrasion resistance to a thermosetting resin while maintaining the excellent mechanical strength of the thermosetting resin by adding polyolefin powder and potassium titanate fiber to the thermosetting resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 08-231859 Summary of the Invention [Problem to be solved by the invention]
[0005] For objects to be used as practical products, it is desirable for them to have not only high sliding properties but also appropriate toughness, but it is difficult to satisfy both physical properties at the same time.
[0006] Although Patent Document 1 describes mechanical strength, it does not disclose anything about toughness. In addition, the resin composition described in Patent Document 1 is mainly composed of a thermosetting resin, and therefore cannot be used in stereolithography. [Means for solving the problem]
[0007] In order to solve the above problems, an object of the present invention is to provide a photocurable resin composition for three-dimensional modeling, which is capable of producing articles having high toughness and sliding properties.
[0008] The photocurable resin composition for three-dimensional object production according to the present invention is a resin composition comprising a polyfunctional radical polymerizable compound (A), a monofunctional radical polymerizable compound (B), polyethylene particles (C), and a curing agent (D), The polyethylene particles (C) have an average particle size of 50 μm or less and a viscosity average molecular weight of 1.5 million or more, the content of the polyethylene particles (C) is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass in total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B); The resin composition has a viscosity at 25° C. of 50 mPa·s or more and 30,000 mPa·s or less. Effect of the Invention
[0009] By using the photocurable resin composition for three-dimensional modeling according to the present invention, a model having excellent toughness and sliding properties can be provided. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram showing an example of the configuration of a molding apparatus in which the photocurable resin composition of the present invention is used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. Note that the embodiment described below is merely one embodiment of the present invention, and the present invention is not limited to these embodiments.
[0012] <Polyfunctional radically polymerizable compound (A)> The polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition for three-dimensional modeling of the present invention (sometimes simply referred to as a curable resin composition or resin composition) is a compound having two or more radical polymerizable functional groups in the molecule. The radical polymerizable functional group may be an ethylenically unsaturated group. The ethylenically unsaturated group may be a (meth)acryloyl group, a vinyl group, or the like. Examples of the polyfunctional radical polymerizable compound include (meth)acrylate-based compounds, vinyl ether group-containing (meth)acrylate-based compounds, (meth)acryloyl group-containing isocyanurate-based compounds, (meth)acrylamide-based compounds, urethane (meth)acrylate-based compounds, maleimide-based compounds, vinyl ether-based compounds, and aromatic vinyl-based compounds. Among these, from the viewpoints of availability and curability, (meth)acrylate-based compounds and urethane (meth)acrylate-based compounds are preferred.
[0013] Various compounds can be used as the polyfunctional radical polymerizable compound (A) of the present invention, but a polyfunctional radical polymerizable compound having a urethane structure is particularly preferred because it is easy to synthesize, easy to obtain, and the toughness of the resulting molded object is high. A polyfunctional radical polymerizable compound having a polyether structure is preferred because it has low viscosity, has good liquid drainage during molding, and can produce a molded object with high precision. A polyfunctional radical polymerizable compound having a polyester structure or a polycarbonate structure is preferred because it can produce a molded object with high toughness. The polyfunctional radical polymerizable compound (A) may be a single compound or may contain two or more types of these compounds. The polyfunctional radical polymerizable compound (A) in the present invention is a name that collectively refers to one or more types of polyfunctional radical polymerizable compounds contained in the photocurable resin composition.
[0014] In the present invention, the Charpy impact test value measured according to JIS K 7111 is 1.0 kJ / m 2 A value of 3.0 kJ / m or more is considered to be good toughness, and the Charpy impact test value is 3.0 kJ / m 2 A test piece with a toughness of 1.0 kJ / m or more is considered to have excellent toughness. 2 If the support material is less than 100%, or if the test is impossible (for example, the test piece is damaged when a notch is made), there is a high possibility that the model will be damaged when the support material is removed. There is also a risk of the model being damaged when the model is fitted into another component or when the model is subjected to secondary processing. Note that support materials are parts that are created to maintain the desired shape during the modeling process, and are generally removed after modeling is completed.
[0015] The polyfunctional radical polymerizable compound (A) having a urethane structure may be, for example, one obtained by reacting a hydroxyl group-containing (meth)acrylate compound with a polyisocyanate compound. Other examples include one obtained by reacting a hydroxyl group-containing (meth)acrylate compound with a polyisocyanate compound with a polyol compound. Among them, in terms of realizing high toughness, one obtained by reacting a hydroxyl group-containing (meth)acrylate compound with a polyisocyanate compound with a polyol compound is preferred.
[0016] Examples of the hydroxyl group-containing (meth)acrylate compound include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, 2-hydroxyethyl acryloyl phosphate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, dipropylene glycol (meth)acrylate, fatty acid-modified glycidyl (meth)acrylate, and polyethylene glycol mono(meth)acrylate. acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl(meth)acrylate, glycerin di(meth)acrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, pentaerythritol tri(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, ethylene oxide-modified dipentaerythritol penta(meth)acrylate, etc. These hydroxyl group-containing (meth)acrylate compounds may be used alone or in combination of two or more.
[0017] Examples of the polyisocyanate-based compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of the polyisocyanate include aliphatic polyisocyanates such as isocyanate and lysine triisocyanate, alicyclic polyisocyanates such as hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, and 1,3-bis(isocyanatomethyl)cyclohexane, as well as trimer compounds or polymer compounds of these polyisocyanates, allophanate-type polyisocyanates, biuret-type polyisocyanates, and water-dispersible polyisocyanates. These polyisocyanate compounds may be used alone or in combination of two or more.
[0018] Examples of the polyol-based compound include polyether-based polyols, polyester-based polyols, polycarbonate-based polyols, polyolefin-based polyols, polybutadiene-based polyols, (meth)acrylic-based polyols, polysiloxane-based polyols, etc. These polyol-based compounds may be used alone or in combination of two or more kinds.
[0019] Examples of polyether polyols include alkylene structure-containing polyether polyols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polybutylene glycol, and polyhexamethylene glycol, and random or block copolymers of these polyalkylene glycols.
[0020] Examples of polyester-based polyols include condensation polymers of polyhydric alcohols and polycarboxylic acids, ring-opening polymers of cyclic esters (lactones), and reaction products of three components: polyhydric alcohols, polycarboxylic acids, and cyclic esters.
[0021] Examples of the polyhydric alcohol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, 1,4-tetramethylene diol, 1,3-tetramethylene diol, 2-methyl-1,3-trimethylene diol, 1,5-pentamethylene diol, neopentyl glycol, 1,6-hexamethylene diol, 3-methyl-1,5-pentamethylene diol, 2,4-diethyl-1,5-pentamethylene diol, glycerin, trimethylolpropane, trimethylolethane, cyclohexanediols (such as 1,4-cyclohexanediol), bisphenols (such as bisphenol A), and sugar alcohols (such as xylitol and sorbitol).
[0022] Examples of the polyvalent carboxylic acid include aliphatic dicarboxylic acids such as malonic acid, maleic acid, fumaric acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, paraphenylenedicarboxylic acid, and trimellitic acid.
[0023] Examples of the cyclic ester include propiolactone, β-methyl-δ-valerolactone, and ε-caprolactone.
[0024] Examples of polycarbonate-based polyols include reaction products of polyhydric alcohols and phosgene, and ring-opening polymers of cyclic carbonates (such as alkylene carbonates).
[0025] Examples of the polyhydric alcohol include the polyhydric alcohols exemplified in the description of the polyester polyol, etc. Examples of the alkylene carbonate include ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, hexamethylene carbonate, etc.
[0026] The polycarbonate polyol may be any compound having a carbonate bond in the molecule and a hydroxyl group at the end, and may have an ester bond in addition to the carbonate bond.
[0027] Examples of the polyfunctional radically polymerizable compound (A) having a polyether structure, a polyester structure, or a polycarbonate structure include those obtained by reacting the above-mentioned polyether polyol, polyester polyol, or polycarbonate polyol with a (meth)acrylic acid chloride or a (meth)acrylic acid bromide.
[0028] In the present invention, the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition is 700 g / eq or more and 8000 g / eq or less. When the polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition is a single compound, a polyfunctional radical polymerizable compound having an ethylenically unsaturated group equivalent of 700 g / eq or more and 8000 g / eq or less is used. The ethylenically unsaturated group equivalent here is a value obtained by ordering the weight average molecular weight of the polyfunctional radical polymerizable compound by the number of ethylenically unsaturated groups in one molecule. The larger the ethylenically unsaturated group equivalent, the smaller the crosslink density in the resin composition after photocuring, and a molded object (article) with good toughness can be obtained. When the photocurable resin composition contains multiple types of polyfunctional radical polymerizable compounds, the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) is the weighted average value of the ethylenically unsaturated group equivalent of each polyfunctional radical polymerizable compound by the weight ratio contained in the photocurable resin composition. A mixture of multiple types of polyfunctional radically polymerizable compounds is used so that the value is 700 g / eq or more and 8000 g / eq or less.
[0029] The larger the ethylenically unsaturated group equivalent of the polyfunctional radically polymerizable compound (A), the more excellent the toughness of the shaped product that can be obtained. However, if the ethylenically unsaturated group equivalent is more than 8000 g / eq, the following problems arise.
[0030] If the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) is too large, the crosslink density in the resin composition after photocuring becomes too small. As a result, the heat resistance and elastic modulus of the molded object decrease, and the shape stability of the molded object decreases. For example, if a heat treatment is performed after molding in order to react unreacted monomers with the molded object, the molded object will deform. In addition, the molded object is prone to deformation when force is applied, which is not preferable in terms of the shape stability of the molded object.
[0031] On the other hand, if the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) is less than 700 g / eq, the crosslink density of the resin composition after photocuring becomes too large. As a result, the toughness of the molded object decreases, and cracks occur when parts are fitted together or during mechanical processing such as screw tightening. Therefore, the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) is preferably 700 g / eq or more and 8000 g / eq or less, and more preferably 700 g / eq or more and 4000 g / eq or less in terms of excellent toughness and shape stability of the obtained molded object.
[0032] The weight average molecular weight (Mw) of the polyfunctional radical polymerizable compound (A) of the present invention is a weight average molecular weight calculated based on the molecular weight of standard polystyrene. The weight average molecular weight was measured using a high performance liquid chromatography (Tosoh Corporation, high-speed GPC device "HLC-8220GPC") with a column: Shodex GPCLF-804 (exclusion limit molecular weight: 2×10 6 , Separation range: 300~2×10 6 ) Two cables can be connected in series and measurements can be made.
[0033] The amount of the polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition according to the present invention is preferably 20 parts by mass or more and 75 parts by mass or less, based on 100 parts by mass of the total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B) described later. If the content of the polyfunctional radical polymerizable compound (A) is less than 20 parts by mass, the curability of the curable resin composition and the toughness of the resulting shaped object tend to decrease. On the other hand, if the content of the polyfunctional radical polymerizable compound (A) is more than 75 parts by mass, the viscosity of the curable resin composition tends to increase, making it difficult to use in a three-dimensional modeling method. Therefore, the content of the polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition for three-dimensional modeling is preferably 20 parts by mass or more and 75 parts by mass or less, more preferably 30 parts by mass or more and 75 parts by mass or less, based on 100 parts by mass of the total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
[0034] <Monofunctional radically polymerizable compound (B)> The monofunctional radical polymerizable compound (B) contained in the photocurable resin composition according to the present invention is a compound having one radical polymerizable functional group in the molecule. By containing the monofunctional radical polymerizable compound (B) in the curable resin composition, it is possible to realize a viscosity suitable for three-dimensional modeling. In addition, by adjusting the amount of the monofunctional radical polymerizable compound (B) added or by appropriately selecting the type, it is possible to adjust the mechanical properties of the model obtained by curing the curable resin composition to a desired range.
[0035] Examples of the monofunctional radical polymerizable compound (B) include, but are not limited to, acrylamide compounds, (meth)acrylate compounds, maleimide compounds, styrene compounds, acrylonitrile compounds, vinyl ester compounds, N-vinyl compounds such as N-vinylpyrrolidone, conjugated diene compounds, vinyl ketone compounds, vinyl halide / vinylidene halide compounds, etc. Among these, acrylamide compounds, (meth)acrylate compounds, maleimide monomers, and N-vinyl compounds are particularly preferred in terms of the excellent curability of the resin composition and the mechanical properties of the resulting shaped object.
[0036] Examples of acrylamide compounds include (meth)acrylamide, N-methyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-tert-butyl(meth)acrylamide, N-phenyl(meth)acrylamide, N-methylol(meth)acrylamide, N,N-diacetone(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-dibutyl(meth)acrylamide, N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, N-[3-(dimethylamino)propyl]acrylamide, and N-tert-octyl(meth)acrylamide.
[0037] Examples of the (meth)acrylate compounds include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, i-octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, 3-hydroxy-1-atamantyl (meth)acrylate, 3,5-Dihydroxy-1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, 2-isopropyl-2-adamantyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycidyl (meth)acrylate, 3-methyl-3-oxetanyl-methyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, (meth)acrylate, phenyl glycidyl (meth)acrylate, dimethylaminomethyl (meth)acrylate, phenyl cellosolve (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, biphenyl (meth)acrylate, 2-hydroxyethyl (meth)acryloyl phosphate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, benzyl (meth)acrylate, butoxytriethylene glycol (meth) ) acrylate, 2-ethylhexyl polyethylene glycol (meth)acrylate, nonylphenyl polypropylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, glycerol (meth)acrylate, trifluoromethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, octafluoropentyl acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, allyl (meth)acrylate acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H,octafluoropentyl (meth)acrylate, epichlorohydrin modified butyl (meth)acrylate, epichlorohydrin modified phenoxy (meth)acrylate, ethylene oxide (EO) modified phthalic acid (meth)acrylate, EO modified succinic acid (meth)acrylate, caprolactone modified 2-hydroxyethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,Examples of such compounds include N-diethylaminoethyl (meth)acrylate, morpholino (meth)acrylate, EO-modified phosphate (meth)acrylate, methyl allyloxyacrylate (product name: AO-MA, manufactured by Nippon Shokubai Co., Ltd.), (meth)acrylates having an imide group (product name: M-140, manufactured by Toagosei Co., Ltd.), and monofunctional (meth)acrylates having a siloxane structure.
[0038] Examples of the maleimide monomer include maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide.
[0039] Other monofunctional radical polymerizable compounds include, for example, styrene derivatives such as styrene, vinyl toluene, α-methyl styrene, chlorostyrene, styrene sulfonic acid and salts thereof, vinyl esters such as vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate, vinyl cyanide compounds such as (meth)acrylonitrile, and N-vinyl compounds such as N-vinyl pyrrolidone, N-vinyl caprolactam, N-vinylimidazole, N-vinyl morpholine, and N-vinyl acetamide.
[0040] These monofunctional radically polymerizable compounds may be used alone or in combination of two or more kinds.
[0041] The amount of the monofunctional radical polymerizable compound (B) contained in the curable resin composition according to the present invention is preferably 25 parts by mass or more and 80 parts by mass or less, based on 100 parts by mass of the total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B). If the ratio of the monofunctional radical polymerizable compound (B) is less than 25 parts by mass, the viscosity of the curable resin composition tends to be significantly high, making it difficult to use for three-dimensional modeling. In addition, if the ratio of the monofunctional radical polymerizable compound (B) is more than 80 parts by mass, both the curability of the curable resin composition and the toughness of the resulting model tend to decrease, which is not preferable. More preferably, it is 25 parts by mass or more and 70 parts by mass or less.
[0042] <Polyethylene particles (C)> The viscosity average molecular weight of the polyethylene particles (C) contained in the curable resin composition according to the present invention is at least 1.5 million. The larger the viscosity average molecular weight of the polyethylene, the more excellent the abrasion resistance.
[0043] Therefore, by including polyethylene particles having a sufficiently high molecular weight in the curable resin composition, the friction coefficient of the article obtained by curing the resin composition can be reduced while improving the wear resistance. If the viscosity average molecular weight of the polyethylene particles is 1.5 million or more, it is more preferable because it can provide high wear resistance that can withstand practical use. In terms of ease of availability, polyethylene particles having a viscosity average molecular weight of 1.8 million or more are more preferable. In the present invention, the viscosity average molecular weight was calculated by determining the intrinsic viscosity using the method described in JP 2013-170231 A.
[0044] The average particle diameter of the polyethylene particles (C) contained in the curable resin composition according to the present invention is preferably 50 μm or less. In the stereolithography method, layers are often laminated in units of 200 μm or less in thickness, so if the average particle diameter is greater than 50 μm, there is a risk of uneven distribution of the polyethylene particles in the layer. On the other hand, if the average particle diameter of the polyethylene particles (C) becomes too small, the viscosity of the curable resin composition increases significantly, so it is preferably 1 μm or more. That is, the average particle diameter of the polyethylene particles (C) is preferably 1 μm or more and 50 μm or less. In view of ease of availability, it is more preferable that it is 10 μm or more and 30 μm or less. In addition, it is preferable that the polyethylene particles (C) are spherical in view of ease of dispersion in the curable resin composition.
[0045] Here, the average particle size of the polyethylene particles (C) refers to the arithmetic mean value of the sphere volume equivalent diameter measured by the Coulter counter method. The specific measurement principle of the Coulter counter method is as follows.
[0046] A container containing an electrolyte with particles dispersed in it is divided into two by a wall with a single pore passing through it. Electrodes are placed on either side of the wall, and a constant current is passed between the electrodes. When the electrolyte is sucked in with a constant suction force on one side of the wall, the particles pass through the pore together with the electrolyte. At this time, the electrolyte in the pore decreases by an amount equivalent to the volume of the particles, and the electrical resistance of the pore increases in proportion to the amount of electrolyte reduced. Since the current flowing through the pore is constant, the voltage between the electrodes changes in proportion to the change in the electrical resistance of the pore. The volume of the particles is measured from the change in this voltage, and the spherical volume equivalent diameter of the particles is calculated from this volume, allowing the particle size distribution to be obtained.
[0047] The specific measurement method is as follows. First, 2 ml of sodium alkylbenzene sulfonate was mixed with 5 mg of polyethylene particles, and the mixture was added to 100 ml of Beckman Coulter's electrolyte ISOTON-II. After that, the sample was prepared by dispersing the particles for about 5 minutes using an ultrasonic disperser. The measurement device for the Coulter counter method was a Beckman Coulter Multisizer 3 with a 200 μm or 400 μm aperture. The device was used to measure the sphere volume equivalent diameter and number of polyethylene particles, and the arithmetic average value of the sphere volume equivalent diameter was calculated from the results.
[0048] The polyethylene particles (C) used in the present invention may be chemically treated on the surface for the purpose of improving dispersibility in the curable resin composition, improving dispersion stability, preventing aggregation, etc. Examples of such chemically treated particles include atmospheric plasma treatment, flame treatment, UV treatment, ozone treatment, and treatment by hydrogen abstraction reaction with peroxide. In addition, the surface after the above treatment may be grafted with a low molecular weight or polymer. Alternatively, the surface of the polyethylene particles may be coated with a low molecular weight or polymer.
[0049] The polyethylene particles (C) contained in the curable resin composition may be a single type of particle, or may contain a plurality of types of particles made of a plurality of different materials.
[0050] The amount of the polyethylene particles (C) contained in the curable resin composition is preferably 5 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B). If the content of the polyethylene particles (C) is within this range, a viscosity applicable to three-dimensional modeling methods is obtained, and the abrasion resistance of the modeled object obtained by curing the resin composition is also increased.
[0051] <Hardening agent (D)> As the curing agent (D), it is more preferable to use a photoradical polymerization initiator. The curable resin composition may contain a thermal radical polymerization initiator in addition to the photoradical polymerization initiator. By containing the thermal radical polymerization initiator in the curable resin composition, the mechanical properties of the shaped object can be further improved by performing a heat treatment after shaping by light irradiation.
[0052] [Photoradical polymerization initiator] Photoradical polymerization initiators are mainly classified into intramolecular cleavage type and hydrogen abstraction type. In the intramolecular cleavage type, a bond at a specific site is cut by absorbing light of a specific wavelength, and a radical is generated at the cut site, which becomes a polymerization initiator and starts the polymerization of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B). In the hydrogen abstraction type, a photoradical polymerization initiator absorbs light of a specific wavelength and becomes excited, and the excited species causes a hydrogen abstraction reaction from the surrounding hydrogen donor, generating a radical. The generated radical then becomes a polymerization initiator and starts the polymerization of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
[0053] Known intramolecular cleavage type photoradical polymerization initiators include alkylphenone-based photoradical polymerization initiators, acylphosphine oxide-based photoradical polymerization initiators, and oxime ester-based photoradical polymerization initiators. These are types in which the bond adjacent to the carbonyl group undergoes α-cleavage to generate radical species. Examples of alkylphenone-based photoradical polymerization initiators include benzyl methyl ketal-based photoradical polymerization initiators, α-hydroxyalkylphenone-based photoradical polymerization initiators, and aminoalkylphenone-based photoradical polymerization initiators. Specific examples of compounds include benzyl methyl ketal-based photoradical polymerization initiators such as 2,2'-dimethoxy-1,2-diphenylethan-1-one (Irgacure® 651, manufactured by BASF), and α-hydroxyalkylphenone-based photoradical polymerization initiators such as 2-hydroxy-2-methyl-1-phenylpropan-1-one (Darocure® 1173, manufactured by BASF), 1-hydroxycyclohexyl phenyl ketone (Irgacure® 184, manufactured by BASF), 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one (Irgacure® 185, manufactured by BASF), and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one (Irgacure® 186, manufactured by BASF). Examples of the aminoalkylphenone-based photoradical polymerization initiator include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (Irgacure(R) 907, BASF) and 2-benzylmethyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone (Irgacure(R) 369, BASF), but are not limited thereto. Examples of acylphosphine oxide-based photoradical polymerization initiators include 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Lucirin(R) TPO, manufactured by BASF) and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure(R) 819, manufactured by BASF), but are not limited thereto.Examples of oxime ester-based photoradical polymerization initiators include, but are not limited to, (2E)-2-(benzoyloxyimino)-1-[4-(phenylthio)phenyl]octan-1-one (Irgacure® OXE-01, manufactured by BASF).
[0054] Examples of the hydrogen abstraction type photoradical polymerization initiator include anthraquinone derivatives such as 2-ethyl-9,10-anthraquinone and 2-t-butyl-9,10-anthraquinone, and thioxanthone derivatives such as isopropylthioxanthone and 2,4-diethylthioxanthone, but are not limited thereto.
[0055] In the present invention, two or more kinds of photoradical polymerization initiators may be used in combination, or one may be used alone. In addition, a thermal radical polymerization initiator may be contained in order to promote a polymerization reaction by heat treatment after shaping.
[0056] The amount of the photoradical polymerization initiator contained in the curable resin composition is preferably 0.1 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B). More preferably, it is 0.1 parts by mass or more and 10 parts by mass or less. If the amount of the photoradical polymerization initiator is small, the polymerization tends to be insufficient. If the amount of the photoradical polymerization initiator is large, the light transmittance decreases and the polymerization tends to be non-uniform.
[0057] [Thermal radical polymerization initiator] The thermal radical polymerization initiator is not particularly limited as long as it generates radicals by heating, and conventionally known compounds can be used. For example, preferred examples include azo compounds, peroxides, and persulfates. Examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(methylisobutyrate), 2,2'-azobis-2,4-dimethylvaleronitrile, and 1,1'-azobis(1-acetoxy-1-phenylethane). Examples of peroxides include benzoyl peroxide, di-t-butylbenzoyl peroxide, t-butyl peroxypivalate, and di(4-t-butylcyclohexyl)peroxydicarbonate. Examples of persulfates include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate.
[0058] The amount of the thermal radical polymerization initiator to be added is preferably 0.1 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass in total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B). If an excessive amount of the thermal radical polymerization initiator is added, the molecular weight does not increase, and physical properties may be deteriorated.
[0059] <Other ingredients> The curable resin composition of the present invention may contain various additives as other optional components within a range that does not impair the object and effect of the present invention. Examples of the additives include resins such as epoxy resins, polyurethanes, polybutadiene, polychloroprene, polyesters, styrene-butadiene block copolymers, polysiloxanes, petroleum resins, xylene resins, ketone resins, and cellulose resins, engineering plastics such as polycarbonates, modified polyphenylene ethers, polyamides, polyacetals, polyethylene terephthalates, polybutylene terephthalates, polyphenylsulfones, polysulfones, polyarylates, polyetherimides, polyetheretherketones, polyphenylene sulfides, polyethersulfones, polyamideimides, liquid crystal polymers, polytetrafluoroethylenes, polychlorotrifluoroethylenes, and polyvinylidene fluorides, fluorine-based oligomers, silicone-based oligomers, and polysulfide-based oligomers. Examples of the additives include reactive monomers such as oligomers, fluorine-containing monomers, and siloxane structure-containing monomers; soft metals such as gold, silver, and lead; layered crystal structure substances such as graphite, molybdenum disulfide, tungsten disulfide, boron nitride, graphite fluoride, calcium fluoride, barium fluoride, lithium fluoride, silicon nitride, and molybdenum selenide; polymerization inhibitors such as phenothiazine and 2,6-di-t-butyl-4-methylphenol; photosensitizers such as benzoin compounds, acetophenone compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds; polymerization initiator assistants, leveling agents, wettability improvers, surfactants, plasticizers, ultraviolet absorbers, silane coupling agents, inorganic fillers, pigments, dyes, antioxidants, flame retardants, thickeners, and defoamers.
[0060] <Curable resin composition> The curable resin composition of the present invention is produced by adding an appropriate amount of other optional components to the essential components of the polyfunctional radical polymerizable compound (A), the monofunctional radical polymerizable compound (B), the polyethylene particles (C), and the curing agent (D) as necessary. Specifically, these components are charged into a stirring vessel and stirred at a temperature of usually 30°C to 120°C, preferably 50°C to 100°C. The stirring time is usually 1 minute to 6 hours, preferably 10 minutes to 2 hours. The total content of the polyfunctional radical polymerizable compound (A), the monofunctional radical polymerizable compound (B), and the polyethylene particles (C) is preferably 25 parts by mass to 100 parts by mass relative to 100 parts by mass of the curable resin composition excluding the curing agent (D). More preferably, it is 75 parts by mass to 100 parts by mass. Of 100 parts by mass of the curable resin composition, the remaining parts by mass excluding the total of the polyfunctional radical polymerizable compound (A), the monofunctional radical polymerizable compound (B), and the polyethylene particles (C) are accounted for by the curing agent (D) and other components described above.
[0061] The viscosity of the curable resin composition of the present invention at 25° C. is preferably 50 mPa·s or more and 30,000 mPa·s or less, and more preferably 50 mPa·s or more and 10,000 mPa·s or less.
[0062] The curable resin composition of the present invention obtained as described above is suitable for use as a modeling material in a stereolithography method. That is, a modeled object having a desired shape can be manufactured by irradiating the curable resin composition of the present invention with a light energy beam in accordance with slice data generated from three-dimensional shape data of an article (modeling model) to be modeled, and supplying energy required for curing.
[0063] <Cured product> The resin cured product of the present invention can be obtained by curing the above-mentioned curable resin composition by irradiation with light energy rays. Examples of light energy rays include ultraviolet rays and infrared rays. Among them, light rays having a wavelength of 300 nm or more and 450 nm or less can be preferably used because they are easily available and the energy is easily absorbed by the photoradical polymerization initiator. As the light source of the light energy rays, ultraviolet or infrared lasers (e.g., Ar lasers, He-Cd lasers, etc.), mercury lamps, xenon lamps, halogen lamps, fluorescent lamps, etc. can be used. Among them, laser light sources are preferably used because they can shorten the modeling time by increasing the energy level, and because they have excellent light collecting properties, they can reduce the irradiation diameter and obtain high modeling accuracy. The light energy rays can be appropriately selected according to the type of radical polymerization initiator contained in the curable resin composition, and multiple combinations can also be used.
[0064] <Functions of the curable resin composition> In the curable resin composition of the present invention, since the ethylenically unsaturated group equivalent of the polyfunctional radically polymerizable compound (A) is 700 g / eq or more and 8000 g / eq or less, it is possible to realize an article having good toughness and shape stability.
[0065] In addition, the article obtained from the curable resin composition of the present invention has a low friction coefficient and high abrasion resistance because it contains polyethylene particles (C) having a viscosity average molecular weight of 1.5 million or more. Furthermore, the polyethylene particles (C) have extremely low water absorption, so that the water absorption rate of the entire cured product can be reduced.
[0066] <Manufacturing method for molded objects> The curable resin composition of the present invention contains a photopolymerization initiator such as a photoradical polymerization initiator as the curing agent (D), and thus can be suitably used for modeling using a stereolithography method. A modeled object made of the curable resin composition can be manufactured using a known stereolithography method. A representative example of a preferred stereolithography method is a method having a step of sequentially curing a photocurable resin composition in layers based on slice data generated from three-dimensional shape data of an article to be modeled, and is roughly divided into two types: a free liquid level method and a regulated liquid level method.
[0067] 1 shows an example of the configuration of a photo-fabrication apparatus 100 using the free liquid surface method. The photo-fabrication apparatus 100 has a tank 11 filled with a liquid photocurable resin composition 10. Inside the tank 11, a modeling stage 12 is provided so as to be drivable in the vertical direction by a drive shaft 13. The irradiation position of a light energy beam 15 for curing the photocurable resin composition 10 emitted from a light source 14 is changed by a galvanometer mirror 16 controlled by a control unit 18 according to slice data, and the surface of the tank 11 is scanned. In the figure, the scanning range is indicated by a thick dashed line.
[0068] The thickness d of the liquid photocurable resin composition 10 cured by the light energy beam 15 is a value determined based on the settings at the time of generating the slice data, and affects the accuracy of the obtained object (reproducibility of the three-dimensional shape data of the object to be molded). The thickness d is achieved by the control unit 18 controlling the drive amount of the drive shaft 13.
[0069] First, the control unit 18 controls the drive shaft 13 based on the settings, and the photocurable resin composition is supplied to the stage 12 at a thickness d. The liquid curable resin composition on the stage 12 is selectively irradiated with light energy rays based on slice data so as to obtain a cured resin layer having a desired pattern, and a cured resin layer is formed. Next, the stage 12 is moved in the direction of the white arrow, and an uncured curable resin composition is supplied to the surface of the cured resin layer at a thickness d. Then, light energy rays 15 are irradiated based on the slice data, and a cured product integrated with the previously formed cured resin layer is formed. By repeating this layer-by-layer curing process, a desired three-dimensional object can be obtained.
[0070] The three-dimensional object thus obtained is taken out of the tank 11, and the unreacted curable resin composition remaining on the surface is removed, and then washed as necessary. As the washing agent, an alcohol-based organic solvent, such as alcohols such as isopropyl alcohol and ethyl alcohol, can be used. In addition, a ketone-based organic solvent, such as acetone, ethyl acetate, methyl ethyl ketone, or an aliphatic organic solvent, such as terpenes, can be used. After washing with the washing agent, post-curing by light irradiation or heat irradiation can be performed as necessary. Post-curing can cure the unreacted curable resin composition that may remain on the surface and inside of the three-dimensional object, and can suppress the stickiness of the surface of the three-dimensional object, as well as improve the initial strength of the three-dimensional object.
[0071] Examples of light energy rays used in the production include ultraviolet rays, electron beams, X-rays, and radiation. Among them, ultraviolet rays having a wavelength of 300 nm or more and 450 nm or less are preferably used from an economical point of view. As a light source that generates ultraviolet rays, ultraviolet lasers (e.g., Ar lasers, He-Cd lasers, etc.), mercury lamps, xenon lamps, halogen lamps, fluorescent lamps, etc. can be used. Among them, laser light sources are preferably used because they have excellent light-collecting properties, can increase the energy level to shorten the modeling time, and can obtain high modeling accuracy.
[0072] When forming a cured resin layer having a predetermined pattern by irradiating a surface made of a curable resin composition with active energy rays, the resin can be cured by a pointillist method or a line drawing method using light energy rays focused in a dotted or line shape. Alternatively, the resin can be cured by irradiating the active energy rays in a planar manner through a planar drawing mask formed by arranging a plurality of microscopic light shutters such as liquid crystal shutters or digital micromirror shutters.
[0073] Similarly, modeling by the regulated liquid level method is also preferable. In the optical modeling apparatus using the regulated liquid level method, the stage 12 of the optical modeling apparatus 100 in FIG. 1 is provided so as to raise the model above the liquid level, and the light irradiation means is provided below the tank 11. A typical modeling example by the regulated liquid level method is as follows. First, the support surface (modeling surface) of the support stage, which is provided so as to be freely raised and lowered, and the bottom surface of the tank containing the curable resin composition are set at a predetermined distance, and the curable resin composition is supplied between the support surface of the support stage and the bottom surface of the tank, i.e., onto the modeling surface. Next, light is selectively irradiated from the bottom surface side of the tank containing the curable resin composition to a predetermined thickness d between the stage support surface and the bottom surface of the tank by a laser light source or a projector according to slice data. The curable resin composition between the stage support surface and the bottom surface of the tank is cured by the irradiation of light, and a solid cured resin layer is formed. After that, the support stage is raised, and the cured resin layer is peeled off from the bottom surface of the tank.
[0074] Next, the height of the support stage is adjusted so that the surface (modeling surface) of the cured resin layer formed on the support stage is a predetermined distance from the bottom surface of the tank. Then, by selectively irradiating light in the same manner as above, a new cured resin layer is formed between the cured resin layer and the bottom surface of the tank, i.e., on the modeling surface, which is integrated with the previously formed cured resin layer. This process is then repeated a predetermined number of times with or without changing the light irradiation pattern, thereby forming a three-dimensional object in which multiple cured resin layers are stacked together.
[0075] <Application> The use of the curable resin composition according to the present invention and the article which is the cured product thereof is not particularly limited. For example, it can be used for various purposes such as resin for 3D printers using stereolithography, sports goods, medical and nursing care products, custom-made products such as artificial limbs, dentures and bones, industrial machinery and equipment, precision equipment, electric and electronic equipment, electric and electronic parts, building materials and supplies. EXAMPLES
[0076] EXAMPLES In order to explain the present invention in detail, examples are given below, but the present invention is not limited to these examples.
[0077] <Example 1> The components were mixed according to the following recipe, heated to 75°C, and stirred for 2 hours with a stirrer to prepare a curable resin composition. Table 1 shows the resin composition and content of the prepared curable resin composition together with other examples.
[0078] [Polyfunctional radically polymerizable compound (A)] Nippon Kayaku "KAYARAD UX6101" 55 parts by weight KAYARAD UX6101 is a urethane acrylate with a weight average molecular weight of 6,500 and two acryloyl groups per molecule as radical polymerizable substituents, and an ethylenically unsaturated group equivalent of 3,250 g / eq.
[0079] [Monofunctional radical polymerizable compound (B)] Isobornyl methacrylate 45 parts by weight Isobornyl methacrylate is a methacrylic acid ester having the structure shown below.
[0080] [ka]
[0081] [Polyethylene particles (C)] 25 parts by weight of "Mipelon XM-221U" manufactured by Mitsui Chemicals Mipelon XM-221U has a viscosity average molecular weight of 2 million and is a spherical particle, with the arithmetic mean value of the sphere volume equivalent diameter measured by the Coulter counter method being 25 μm.
[0082] [Hardening agent (D)] Omnirad184 (photoradical polymerization initiator manufactured by IGM Resins, 1-hydroxycyclohexyl phenyl ketone) 2 parts by mass
[0083] [Creating test piece X] A test piece was prepared from the prepared photocurable resin composition by the following method. First, a metal mold having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm, or a silicon mold having a length of 30 mm, a width of 30 mm, and a thickness of 4 mm was sandwiched between two pieces of quartz glass, and the curable resin composition was poured into the mold. The poured curable resin composition was irradiated with an ultraviolet ray irradiator (manufactured by HOYA CANDEO OPTRONICS, product name "LIGHT SOURCE EXECURE3000") at 5 mW / cm. 2 The mold was irradiated with ultraviolet light from both sides for 360 seconds each to obtain a cured product. The total energy irradiated to cure the photocurable resin composition was 3600 mJ / cm 2 The obtained cured product was placed in a heating oven at 50°C for 1 hour and then in a heating oven at 100°C for 2 hours to perform heat treatment, thereby obtaining a test piece X having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The test piece X was used in the Charpy impact test described later. The results are shown in Table 2.
[0084] [Creating test piece Y] The prepared curable resin composition was used to model a three-dimensional rectangular parallelepiped shape of 30 mm x 30 mm x 4 mm using a 3D printer (DWS-020X, a photolithography device using the regulated liquid surface method). The model was created by stacking 30 mm x 4 mm x 50 μm thick cured resin layers to a height of 30 mm. The resulting model was irradiated with ultraviolet light for 30 minutes using a UVCuring Unit M (DWS), then placed in a heating oven at 50 ° C for 1 hour, and then placed in a heating oven at 100 ° C for 2 hours to perform heat treatment, thereby creating a test piece Y. The test piece Y was used to evaluate the moldability, friction coefficient, and wear resistance described later. The results are shown in Table 2.
[0085] [evaluation] (Moldability) The moldability was evaluated based on the dimensional error of the test piece Y, which was 30 mm x 30 mm x 4 mm in size. The evaluation criteria were as follows. If the test piece satisfied evaluation criterion B, it was determined that good moldability had been obtained, and if the test piece satisfied evaluation criterion A, it was determined that excellent moldability had been obtained. A: Dimensional error is within ±3% B: Dimensional error is greater than ±3% C: Unable to model The dimensions of each side were measured after molding with a 3D printer and before heat treatment at 100°C.
[0086] (Charpy impact test) In accordance with JIS K 7111, a 2 mm deep, 45° notch was made in the center of test piece A using a notch-making machine (manufactured by Toyo Seiki Seisakusho, product name "Notching Tool A-4"). An impact tester (manufactured by Toyo Seiki Seisakusho, product name "IMPACT TESTER IT") was used to break the test piece from the back of the notch with an energy of 2 J. The energy required for breakage was calculated from the angle at which the hammer, which had been swung up to 150°, swung back after the test piece broke, and this was taken as the Charpy impact strength and used as an index of toughness. If test piece X broke when making the notch, the Charpy impact strength was set to 0.0 KJ / m 2The toughness evaluation criteria are as follows. If evaluation criterion B is satisfied, it is judged that good toughness has been obtained, and if evaluation criterion A is satisfied, it is judged that excellent toughness has been obtained. A: 3.0 kJ / m 2 End B: 1.0 kJ / m 2 More than 3.0kJ / m 2 less than C: 1.0 kJ / m 2 less than
[0087] (Specific wear rate and friction coefficient) The specific wear rate and the friction coefficient were measured in accordance with JIS K 7218 Method A under the conditions shown below. Measuring device: A&D friction and wear tester MODEL EMF-III-F Test environment: 23℃±2℃, humidity 50%±5%RH Test piece: Test piece Y (size 30mm x 30mm, thickness 4mm) Mating material: S45C, ring shape, surface roughness approx. 0.8μmRa, contact area 2cm 2 Load: 50N Sliding speed: 50cm / s Test duration: 100 minutes Sliding distance: 3km The counter material was pressed against the test piece Y with the above load and slid at the above speed. The sliding was stopped after 100 minutes, and the wear weight was measured from the weight of the test piece Y before and after the sliding. The wear volume was calculated from the measured wear weight and the specific gravity of the test piece Y. The calculated wear volume was divided by the sliding distance and the load to obtain the specific wear amount (unit: mm 3 N -1 km -1 ) was used as an index of abrasion resistance. The evaluation criteria for abrasion resistance are shown below. If evaluation criterion B is met, it is judged that good abrasion resistance has been obtained, and if evaluation criterion A is met, it is judged that excellent abrasion resistance has been obtained. A: 0.1 mm 3 N -1 km -1 less than B: 0.1 mm 3 N -1 km -1More than 0.5mm 3 N -1 km -1 Less than C: 0.5mm 3 N -1 km -1 End
[0088] The coefficient of friction was calculated by dividing the average value of the friction force for 10 seconds before and after 60 minutes from the start of sliding by the load. The evaluation criteria for the coefficient of friction are as follows. If evaluation criterion B is met, it is judged that a good coefficient of friction has been obtained, and if evaluation criterion A is met, it is judged that an excellent coefficient of friction has been obtained. A: Less than 0.3 B: 0.3 or more and less than 0.7 C:0.7 or more
[0089] <Examples 2 to 6 and Comparative Examples 1 to 4> Except for changing the contents of each of the components (A), (B), and (D) contained in the curable resin composition and the type or content of the polyethylene particles as shown in Table 1, the curable resin composition was prepared in the same manner as in Example 1 and evaluated in the same manner as in Example 1. The results are summarized in Table 2. The contents of the polyfunctional radical polymerizable compound and the monofunctional radical polymerizable compound shown in the table are the contents of the polyfunctional radical polymerizable compound in parts by mass relative to a total of 100 parts by mass of the polyfunctional radical polymerizable compound and the monofunctional radical polymerizable compound. The amount of polyethylene particles (C) added is the content of the polyethylene particles (C) in parts by mass relative to a total of 100 parts by mass of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
[0090] The types of polyethylene particles (C) used are as follows:
[0091] [Polyethylene particles (C)] "Mipelon PM-200" manufactured by Mitsui Chemicals Mipelon PM-200 has a viscosity average molecular weight of 1.8 million and is a spherical particle, with an arithmetic mean value of the sphere volume equivalent diameter measured by the Coulter counter method of 10 μm.
[0092] "Mipelon XM-220" manufactured by Mitsui Chemicals Mipelon XM-220 has a viscosity average molecular weight of 2 million and is a spherical particle, with an arithmetic mean value of the sphere volume equivalent diameter measured by the Coulter counter method of 30 μm.
[0093] Sumitomo Seika's "Flo-Thane UF20S" FLOTHEN UF20S has a viscosity average molecular weight of 150,000 and an arithmetic mean value of the sphere volume equivalent diameter measured by the Coulter counter method of 30 μm.
[0094] Mitsui Chemicals "Hixx Million 240M" Hi-Zex Million 240M has a viscosity average molecular weight of 2.4 million and an arithmetic mean value of the volume-equivalent sphere diameter measured by the Coulter counter method of 160 μm.
[0095] <Examples 7 to 15 and Comparative Examples 5 to 6> Curable resin compositions were prepared in the same manner as in Example 1, except that the types or contents of each of the components (A), (B), and (D) contained in the curable resin composition and the content of the polyethylene particles were changed as shown in Table 3, and were evaluated in the same manner as in Example 1. Examples 11 to 15 and Comparative Examples 5 to 6 are examples in which a plurality of types of polyfunctional radical polymerizable compounds are contained as the polyfunctional radical polymerizable compound (A). Examples 11 to 15 are mixtures of a polyfunctional radical polymerizable compound having an ethylenically unsaturated group equivalent of 700 g / eq or more and 8000 g / eq or less and a polyfunctional radical polymerizable compound having an ethylenically unsaturated group equivalent of less than 700 g / eq. The mixture ratio is prepared so that the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) is 700 g / eq or more and 8000 g / eq or less. On the other hand, Comparative Examples 5 to 6 are prepared so that the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) is less than 700 g. The results are summarized in Table 4.
[0096] The types of each component used are as follows:
[0097] [Polyfunctional radically polymerizable compound (A)] “Shikou UV-7550B” manufactured by Nippon Gosei Chemical Industry Co., Ltd. Shiko UV-7550B is a urethane acrylate with a weight average molecular weight of 2,400 and three acryloyl groups per molecule as radical polymerizable substituents, and an ethylenically unsaturated group equivalent of 700 g / eq.
[0098] “Shikou UV-3550AC” manufactured by Nippon Gosei Chemical Industry Co., Ltd. Shikoh UV-3550AC is a mixture of 70 parts by mass of urethane acrylate and 30 parts of ACMO, which is a monofunctional radical polymerizable compound (B). The weight average molecular weight of the urethane acrylate is 14,000, and each molecule contains two acryloyl groups as radical polymerizable substituents, and the ethylenically unsaturated group equivalent is 7,000 g / eq.
[0099] In addition, the resin compositions in Table 3 are shown as parts by mass of the urethane acrylate component and parts by mass of the monofunctional radical polymerizable compound (A), and ACMO, respectively.
[0100] “Shikou UV-6630B” manufactured by Nippon Gosei Chemical Industry Co., Ltd. Shiko UV-6630B is a urethane acrylate with a weight average molecular weight of 3,000 and two acryloyl groups per molecule as radical polymerizable substituents, and an ethylenically unsaturated group equivalent of 1,500 g / eq.
[0101] Daicel Allnex "EBECRYL8210" EBECRYL8210 is a urethane acrylate having a weight average molecular weight of 600 and four acryloyl groups per molecule as radically polymerizable substituents, and an ethylenically unsaturated group equivalent of 150 g / eq.
[0102] "NK Ester A-BPE-4" manufactured by Shin-Nakamura Chemical Industry Co., Ltd. NK Ester A-BPE-4 is an ethoxylated bisphenol A diacrylate with a molecular weight of 512 and two acryloyl groups per molecule as radical polymerizable substituents, and has an ethylenically unsaturated group equivalent of 256 g / eq.
[0103] "NK Ester A-9300" manufactured by Shin-Nakamura Chemical Industry Co., Ltd. NK Ester A-9300 is an ethoxylated isocyanuric acid triacrylate with a molecular weight of 423 and three acryloyl groups per molecule as radical polymerizable substituents, and an ethylenically unsaturated group equivalent of 141 g / eq.
[0104] "NK Ester A-DCP" manufactured by Shin-Nakamura Chemical Industry Co., Ltd. NK Ester A-DCP has a molecular weight of 304 and is a diacrylate with an alicyclic structure in which two acryloyl groups per molecule serve as radical polymerizable substituents, and the ethylenically unsaturated group equivalent is 152 g / eq.
[0105] Shin-Nakamura Chemical Industry Co., Ltd. "NK Ester ABE-300" NK Ester ABE-300 is an ethoxylated bisphenol A diacrylate with a molecular weight of 466 and two acryloyl groups per molecule as radical polymerizable substituents, and has an ethylenically unsaturated group equivalent of 233 g / eq.
[0106] [Monofunctional radical polymerizable compound (B)] Isobornyl acrylate (alicyclic ester acrylate monomer), structure shown below.
[0107] [ka]
[0108] "ACMO" (acrylamide monomer) manufactured by KJ Chemicals, the structure of which is shown below.
[0109] [ka]
[0110] "Imilex P" (maleimide monomer) manufactured by Nippon Shokubai, the structure of which is shown below.
[0111] [ka]
[0112] "Imilex C" (maleimide monomer) manufactured by Nippon Shokubai, the structure of which is shown below.
[0113] [ka]
[0114] "DMAA" (acrylamide monomer) manufactured by KJ Chemical; the structure is shown below.
[0115] [ka]
[0116] "DAAM" (acrylamide monomer) manufactured by KJ Chemical; the structure is shown below.
[0117] [ka]
[0118] "N-vinyl-ε-caprolactam" (N-vinyl monomer) manufactured by Tokyo Chemical Industry Co., Ltd., the structure of which is shown below.
[0119] [ka]
[0120] [Hardening agent (D)] Omnirad819 (IGM Resins photoradical polymerization initiator bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide)
[0121] [Table 1]
[0122] [Table 2]
[0123] [Table 3]
[0124] [Table 4]
[0125] As can be seen from Tables 2 and 4, Examples 1 to 15 according to the present invention all had good moldability. In addition, the Charpy impact strength of test piece X, which was prepared by curing the curable resin composition of the present invention, was 1.0 KJ / m 2 The coefficient of friction of test piece Y is less than 0.7, and the specific wear amount is 0.5 mm 3 N -1 km -1 In other words, it was confirmed that by using the photocurable resin composition according to the present invention, an article having both good toughness and high sliding properties can be obtained.
[0126] In addition, in the results of Table 2, Comparative Example 1, in which no polyethylene particles (C) were added, did not satisfy the evaluation criterion B in terms of the specific wear rate and friction coefficient. In Comparative Example 2, in which 66.7 parts by mass of polyethylene particles (C) were added, the viscosity increased, and therefore a three-dimensional object could not be produced. From these results and the results of Examples 1 to 6, it was confirmed that the amount of polyethylene particles (C) added is preferably 5 to 50 parts by mass relative to 100 parts by mass in total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
[0127] Furthermore, in Comparative Example 3, in which the viscosity average molecular weight of the added polyethylene particles (C) was 150,000, the specific wear rate did not satisfy evaluation criterion B. From this result and the results of Examples 1 to 6, it was found that the viscosity average molecular weight of the polyethylene particles (C) is preferably 1.5 million or more.
[0128] In addition, in the case of Comparative Example 4 in which the average particle diameter of the added polyethylene particles (C) exceeded 50 μm in modeling using a 3D printer, the particle diameter was larger than the thickness of one layer, so a three-dimensional model could not be created. Although it depends on the device used for modeling and the modeling conditions, considering the results of Examples 1 to 6, it is considered that the average particle diameter of the polyethylene particles (C) is preferably 50 μm or less.
[0129] From the results in Table 4, Examples 7 to 15, in which the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition was 700 g / eq or more, were good in all items. However, Comparative Examples 5 and 6, in which the ethylenically unsaturated group equivalent of the polyfunctional radical polymerizable compound (A) contained in the photocurable resin composition was less than 700 g / eq, did not satisfy evaluation criterion B in the Charpy impact test, and good toughness was not obtained. From these results, it was found that the ethylenically unsaturated group equivalent of the radical polymerizable compound (A) is preferably 700 g / eq or more. [Explanation of symbols]
[0130] 10 Photocurable resin composition 11 tanks 12 Modeling Stage 13 Drive 14 Light source 15 Light Energy Rays 17 Sculptures 18 Control Unit 100 Stereolithography equipment
Claims
1. A resin composition comprising a polyfunctional radical polymerizable compound (A), a monofunctional radical polymerizable compound (B), polyethylene particles (C), and a curing agent (D), The polyethylene particles (C) have an average particle size of 50 μm or less and a viscosity average molecular weight of 1.5 million or more, the content of the polyethylene particles (C) is 5 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass in total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B), A resin composition, characterized in that the viscosity of the resin composition at 25°C is 50 mPa·s or more and 30,000 mPa·s or less.
2. 2. The resin composition according to claim 1, wherein the polyfunctional radically polymerizable compound (A) has an ethylenically unsaturated group equivalent of 700 g / eq or more and 8,000 g / eq or less.
3. The resin composition according to claim 1 or 2, characterized in that the polyfunctional radical polymerizable compound (A) is a single polyfunctional radical polymerizable compound having an ethylenically unsaturated group equivalent of 700 g / eq or more and 8000 g / eq or less.
4. The resin composition according to claim 1 or 2, characterized in that the polyfunctional radical polymerizable compound (A) is a mixture of a plurality of types of polyfunctional radical polymerizable compounds, and the ethylenically unsaturated group equivalent weighted-average of the ethylenically unsaturated group equivalents of the respective compounds is 700 g / eq or more and 8000 g / eq or less.
5. 3. The resin composition according to claim 1, wherein the polyfunctional radical polymerizable compound (A) is a mixture of a polyfunctional radical polymerizable compound having an ethylenically unsaturated group equivalent of 700 g / eq or more and 8000 g / eq or less and a polyfunctional radical polymerizable compound having an ethylenically unsaturated group equivalent of less than 700 g / eq.
6. 6. The resin composition according to claim 1, wherein the content of the polyfunctional radical polymerizable compound (A) is 20 parts by mass or more and 75 parts by mass or less relative to 100 parts by mass in total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
7. 7. The resin composition according to claim 1, wherein the content of the monofunctional radical polymerizable compound (B) is 20 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass in total of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
8. 8. The resin composition according to claim 1, wherein a content of the curing agent (D) is 0.1 parts by mass or more and 15 parts by mass or less relative to a total of 100 parts by mass of the polyfunctional radical polymerizable compound (A) and the monofunctional radical polymerizable compound (B).
9. 9. The resin composition according to claim 1, wherein the polyethylene particles (C) have an average particle size of 1 μm or more.
10. 10. The resin composition according to claim 1, wherein the polyethylene particles (C) have an average particle size of 10 μm or more and 30 μm or less.
11. 11. The resin composition according to claim 1, wherein the polyethylene particles (C) have a viscosity average molecular weight of 1,800,000 or more.
12. 12. The resin composition according to claim 1, wherein the polyethylene particles (C) have a viscosity average molecular weight of 2,000,000 or less.
13. The resin composition according to any one of claims 1 to 12, characterized in that the monofunctional radically polymerizable compound (B) is selected from the group consisting of an acrylamide-based compound, a (meth)acrylate-based compound, a maleimide-based compound, and an N-vinyl compound.
14. The resin composition according to any one of claims 1 to 13, characterized in that the polyfunctional radically polymerizable compound (A) is a (meth)acrylate-based compound having any one of a polyether structure, a polyester structure, and a polycarbonate structure, or a urethane (meth)acrylate-based compound.
15. The resin composition according to any one of claims 1 to 14, wherein the polyfunctional radically polymerizable compound (A) has a urethane structure.
16. The resin composition according to any one of claims 1 to 15, wherein the curing agent (D) contains a photoradical polymerization initiator.
17. A cured resin product obtained by copolymerizing the resin composition according to claim 1 .
18. The Charpy impact strength of the cured resin is 1.0 kJ / m 2 The cured resin material according to claim 17,
19. The specific wear amount of the cured resin is 0.5 mm 3 ・N -1 ・Km -1 The cured resin material according to claim 17 or 18, wherein the cured resin material has a viscosity of less than 1000 MPa.
20. 20. The cured resin according to claim 17, wherein the cured resin has a friction coefficient of less than 0.
7.
21. A method for manufacturing an article using a stereolithography method, comprising the steps of: disposing a photocurable resin composition on a modeling surface; A step of irradiating the photocurable resin composition with light energy based on slice data of a model to cure the composition; Including, A method for producing a three-dimensional object, comprising the step of: forming a photocurable resin composition comprising the photocurable resin composition according to claim 1 ;
22. The method for manufacturing a three-dimensional object according to claim 21, further comprising a step of subjecting the object obtained by the irradiation of the light energy to a heat treatment.
23. 23. The method for manufacturing a three-dimensional object according to claim 21 or 22, wherein the light energy is light emitted from a laser light source or a projector.
Citation Information
Patent Citations
Resin composition for optical three-dimensional shaping
JP1995026060A
Thermosetting resin composition for sliding member
JP1996231859A
Photoresist composition for three-dimensional photo- forming
JP2001342204A
Radiation-curable composition
JP2004352781A
Polymerizable composition
JP2005250438A