Electrophotographic member and electrophotographic image forming apparatus

The laminated structure of a binder resin, perfluoropolyether, and specific ionic liquid in electrophotographic members effectively reduces toner adhesion, enhancing image quality by stabilizing perfluoropolyether distribution and contact angle, addressing the challenge of high-quality image formation.

JP7566553B2Active Publication Date: 2024-10-15CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020162298
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-03
Filing Date
2020-09-28
Publication Date
2024-10-15
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Existing electrophotographic members, such as intermediate transfer belts, face challenges in further reducing toner adhesion to the outer surface, limiting the ability to achieve high-quality images despite efforts to improve transfer characteristics.

Method used

A laminated electrophotographic member structure with a base layer and a surface layer containing a binder resin, perfluoropolyether, and an ionic liquid, where the perfluoropolyether content is 20% to 100% by mass, and the ionic liquid includes a specific anion, achieving a contact angle of 65° or more with hexadecane.

Benefits of technology

This configuration significantly reduces toner adhesion to the outer surface, enabling the formation of high-quality electrophotographic images by stabilizing the perfluoropolyether distribution and enhancing the contact angle, thereby improving image quality and potentially reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566553000018
    Figure 0007566553000018
  • Figure 0007566553000019
    Figure 0007566553000019
  • Figure 0007566553000020
    Figure 0007566553000020
Patent Text Reader

Abstract

To provide a member for electrophotography that has reduced adhesion of toner to an outer surface.SOLUTION: A member for electrophotography has a base layer and a surface layer laminated in this order in a thickness direction. The surface layer contains a binder resin, perfluoropolyether, and an ionic liquid. The content ratio of the perfluoropolyether to the binder is 20 mass% or more and 100 mass% or less. The angle of contact of a surface of the surface layer on the opposite side of a surface facing the base layer to hexadecane is 65° or more.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD This disclosure relates to an electrophotographic member and an electrophotographic image forming apparatus including the electrophotographic member. [Background technology]

[0002] An intermediate transfer belt is one of the members used in an electrophotographic image forming apparatus. In an electrophotographic apparatus that requires high image quality, there is a demand for further improvement in the transfer characteristics of the intermediate transfer belt. As one of such efforts, efforts have been made to improve the transfer characteristics by subjecting the surface of the intermediate transfer belt to various processes. Patent Document 1 discloses an electrophotographic member provided with a surface layer containing a water- and oil-repellent perfluoropolyether in order to reduce the adhesion of toner to the outer surface, which is the toner carrying surface, of the electrophotographic member. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-028613 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been an increasing demand for higher image quality of electrophotographic images. Accordingly, the present inventors have recognized that it is necessary to further reduce the toner adhesion to the outer surface, which is the toner carrying surface, of electrophotographic members such as intermediate transfer belts that have the function of carrying toner in an electrophotographic image forming process. According to the studies of the present inventors, in the electrophotographic member according to Patent Document 1, even if the perfluoropolyether content in the surface layer is simply increased, the effect of reducing the toner adhesion to the outer surface of the electrophotographic member is limited.

[0005] One aspect of the present disclosure is directed to providing an electrophotographic member having an outer surface with reduced toner adhesion, and an electrophotographic image forming apparatus capable of forming high-quality electrophotographic images. [Means for solving the problem]

[0006] According to at least one embodiment of the present disclosure, there is provided an electrophotographic member having a base layer and a surface layer laminated in this order in a thickness direction, the surface layer including a binder resin, a perfluoropolyether, and an ionic liquid, The content ratio of the perfluoropolyether to the binder is 20% by mass or more and 100% by mass or less, The ionic liquid is provided for an electrophotographic member having an anion represented by the following structural formula (1):

[0007] [ka] (In structural formula (1), m and n each independently represent an integer of 1 or more and 4 or less).

[0008] According to at least one aspect of the present disclosure, The electrophotographic member provided has a base layer and a surface layer laminated in this order in the thickness direction, the surface layer containing a binder resin, a perfluoropolyether and an ionic liquid, the content of the perfluoropolyether relative to the binder being 20% ​​by mass or more and 100% by mass or less, and the surface of the surface layer opposite to the side facing the base layer has a contact angle with hexadecane of 65° or more.

[0009] According to at least one aspect of the present disclosure, there is provided an electrophotographic image forming apparatus including the electrophotographic member. Effect of the Invention

[0010] According to one aspect of the present disclosure, it is possible to obtain an electrophotographic member having an outer surface to which toner adhesion is further reduced. Also, according to one aspect of the present disclosure, it is possible to obtain an electrophotographic image forming apparatus capable of forming a high-quality electrophotographic image. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view illustrating an example of an electrophotographic image forming apparatus according to one embodiment of the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view in a thickness direction of an electrophotographic member according to one embodiment of the present disclosure. [Diagram 3] 3 is an explanatory diagram of a supposed mechanism for manifesting the effect of the electrophotographic member according to one embodiment of the present disclosure. FIG. [Figure 4] FIG. 4 is an illustration of an electrophotographic belt according to another embodiment of the present disclosure having grooves on its outer surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] As described above, according to the studies by the present inventors, in the electrophotographic member according to Patent Document 1, even if the content of perfluoropolyether (PFPE) in the surface layer is increased, the effect of reducing the adhesion of toner to the outer surface of the electrophotographic member is limited. The reason is that in a surface layer containing a binder resin and PFPE dispersed in the binder resin, PFPE has a small surface free energy and is therefore easily unevenly distributed at the interface between the surface layer 22 and the air, that is, on the outer surface side of the surface layer. Therefore, toner is less likely to adhere to the outer surface of the electrophotographic member. However, there is an upper limit to the amount of PFPE that can be present near the outer surface of the surface layer, and even if a certain amount or more of PFPE is contained in the surface layer, the excess amount of PFPE is only present inside the surface layer. Therefore, it is difficult to further reduce the toner adhesion to the outer surface of the electrophotographic member by adding an excess amount of PFPE. Therefore, the present inventors have conducted extensive research to further reduce toner adhesion to the outer surface of an electrophotographic member by a method other than increasing the content of PFPE. As a result, they have found that a surface layer containing PFPE and an ionic liquid having an anion represented by the following structural formula (1) can provide an outer surface with extremely low toner adhesion.

[0013] [ka] (In structural formula (1), m and n each independently represent an integer of 1 or more and 4 or less).

[0014] The inventors speculate as follows why a surface layer containing an ionic liquid containing PFPE and an anion having the structure represented by the above structural formula (1) provides an outer surface with extremely low toner adhesion.

[0015] The ether structure portion of PFPE has an unshared electron pair. Therefore, as shown in FIG. 3, the ether structure portion of PFPE and the cation of the ionic liquid interact with each other, and more cations are present in the vicinity of the ether structure portion. And, an anion, which is a counter ion, is present in the vicinity of the cation. At this time, since the anion is an anion having a structure represented by the above structural formula (1) having a plurality of perfluoroalkyl groups in the molecule, more perfluoroalkyl groups are present in the vicinity of the PFPE. And, since the perfluoroalkyl groups are oriented toward the outer surface side of the surface layer, it is considered that the adhesion of the toner to the outer surface of the surface layer can be further reduced. Note that the PFPE shown in FIG. 3 is an example, and p and q each represent an integer of 0 or 1 or more, and p and q cannot be 0 at the same time. R represents an end group of the PFPE, and is selected from reactive functional groups or non-reactive functional groups described later. In addition, the cation of the ionic liquid also represents a preferred example. By using an ionic liquid containing such a specific anion in combination with PFPE, it becomes possible to obtain an electrophotographic member having a contact angle (hereinafter simply referred to as "contact angle") with hexadecane on the outer surface of 65° or more, which is considered difficult to achieve with PFPE alone. A contact angle of 65° or more results in unprecedented low toner adhesion. The inventors believe that such a high contact angle cannot be achieved, for example, by an ionic liquid that contains an anion having only one perfluoroalkyl group, such as a trifluoromethanesulfonate anion, in the surface layer together with PFPE. Furthermore, by using the ionic liquid containing the specific anion in combination with PFPE, the contact angle that can be achieved by incorporating a specific amount of PFPE in the surface layer can be achieved even if the content of PFPE is reduced from the specific amount, i.e., the amount of PFPE used can be reduced, thereby reducing the manufacturing cost of electrophotographic members.

[0016] Hereinafter, an electrophotographic member according to one aspect of the present disclosure will be described taking an electrophotographic member having an endless shape (hereinafter, also referred to as an electrophotographic belt) as an example. Note that the electrophotographic member according to the present disclosure is not limited to the following embodiment. Specifically, for example, as another form, an electrophotographic member having a roller shape can be mentioned.

[0017] <Electrophotographic materials> 2 has a base layer 21 and a surface layer 22 provided on the outer peripheral surface of the base layer 21. That is, the base layer and the surface layer are laminated in this order in the thickness direction. The surface layer 22 contains a binder resin, a PFPE, and an ionic liquid. The content of the PFPE in the surface layer relative to the binder is 20% by mass or more and 100% by mass or less. Furthermore, the ionic liquid contains an anion having a structure represented by the above structural formula (1).

[0018] As a result of the inventors' investigations, the following has become clear. There is a positive correlation between the contact angle with hexadecane of the surface (outer surface) of the electrophotographic member opposite the side of the surface layer facing the base layer, which is the toner bearing surface of the electrophotographic member, and the toner adhesion to the outer surface. In other words, the larger the value of the contact angle, the smaller the toner adhesion. Therefore, in the present disclosure, the contact angle with hexadecane is used to define the low toner adhesion of the electrophotographic member.

[0019] The electrophotographic member may be composed of only the above two layers, or may have other members on the surface of the base layer opposite the surface layer (the back surface of the electrophotographic member) in addition to the two layers.

[0020] <base layer> A conductive substance can usually be added to the base layer 21 to impart conductivity. Examples of the conductive substance include inorganic conductive particles of carbon such as carbon black, carbon fiber, and carbon nanotubes, and inorganic conductive particles of metal oxides such as zinc antimonate, zinc oxide, tin oxide, and titanium oxide. When used as an intermediate transfer belt, the base layer 21 has a volume resistivity of 1×10 8 Ω cm or more 1×10 12 The surface resistivity of the base layer 21 is preferably adjusted to a range of 1×10 8 Ω / □ or more 1×10 14 It is preferable that the resistance is adjusted to a range of Ω / □ or less. The volume resistivity of the base layer 21 is 1×10 12 By setting the volume resistivity of the base layer 21 to 1×10 Ω·cm or less, it is possible to suppress the deterioration of the primary transferability and secondary transferability due to the application of a certain transfer bias. 8 By setting the surface resistivity at Ω·cm or more, it is possible to suppress the occurrence of resistance unevenness and prevent the occurrence of transfer unevenness and image defects. Furthermore, by setting the surface resistivity of the base layer 21 within the above range, it is possible to reduce image defects caused by peeling discharge when the transfer material leaves the intermediate transfer belt and toner scattering. The thickness of the base layer 21 is preferably 30 μm or more and 150 μm or less in view of mechanical strength and bending resistance.

[0021] <Surface layer> The surface layer 22 contains a binder resin, a PFPE, and an ionic liquid, and may contain additives such as a photopolymerization initiator, a dispersant, and a conductive agent.

[0022] (binder resin) As the binder resin, a styrene resin, an acrylic resin, a methacrylic resin, an epoxy resin, a polyester resin, a polyether resin, a silicone resin, a polyvinyl butyral resin, or a mixture of these resins can be used. The binder resin is used to disperse the PFPE, ensure adhesion to the base layer 21, and ensure mechanical strength properties. Among the above binder resins, methacrylic resin or acrylic resin is preferably used because it is possible to satisfactorily disperse the PFPE constituting the surface layer 22 according to the present disclosure. Hereinafter, acrylic resin and methacrylic resin are collectively referred to as acrylic resin.

[0023] Examples of the polymerizable monomer for forming the acrylic resin include the following (i) and (ii). As the polymerizable monomer, those commercially available as paints can also be used. (i) At least one acrylate selected from the group consisting of pentaerythritol triacrylate, pentaerythritol tetraacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, alkyl acrylate, benzyl acrylate, phenyl acrylate, ethylene glycol diacrylate, and bisphenol A diacrylate. (ii) At least one methacrylate selected from the group consisting of pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, ditrimethylolpropane tetramethacrylate, dipentaerythritol hexamethacrylate, alkyl methacrylates, benzyl methacrylate, phenyl methacrylate, ethylene glycol dimethacrylate, and bisphenol A dimethacrylate. Among these, high hardness is preferable in consideration of rubbing against other members such as a photoreceptor, a cleaning blade, etc. For this reason, it is preferable to use a large amount of difunctional or higher crosslinkable monomers in the acrylic resin to achieve a higher hardness.

[0024] To form an acrylic resin from such a polymerizable monomer, a photopolymerization initiator may be added and polymerization may be carried out by electron beam or ultraviolet light. Examples of the photopolymerization initiator include radical-generating photopolymerization initiators such as benzophenone, thioxanthone, benzyl dimethyl ketal, α-hydroxyketone, α-hydroxyalkylphenone, α-aminoketone, α-aminoalkylphenone, monoacylphosphine oxide, bisacylphosphine oxide, hydroxybenzophenone, aminobenzophenone, titanocene, oxime ester, and oxyphenylacetic acid ester.

[0025] The content of the binder resin is preferably 20% by mass or more from the viewpoint of surface layer strength, based on the mass of the total solid content of the surface layer 22. Also, from the viewpoint of preventing insufficient toner adhesion caused by a relative decrease in the PFPE and ionic liquid components with an increase in the content, the content is preferably 70% by mass or less.

[0026] The thickness of the surface layer 22 is preferably 1 μm or more and 20 μm or less. By making the thickness of the surface layer 22 1 μm or more, it is possible to maintain low toner adhesion and suppress peeling, thereby ensuring durability. By making the thickness of the surface layer 22 20 μm or less, the necessary bending resistance performance can be obtained.

[0027] (PFPE) Perfluoropolyethers (PFPEs) are oligomers or polymers that contain perfluoroalkyleneoxy as a repeating unit. Examples of perfluoroalkyleneoxy repeating units include difluoromethyleneoxy (-CF2O-), tetrafluoroethyleneoxy (-CF2CF2O-), and hexafluoropropyleneoxy (-CF2CF2CF2-O- or -C(CF3)FCF2O-). As the PFPE, either a PFPE having a reactive functional group capable of forming a bond or a state close to a bond with the binder resin, or a PFPE having a non-reactive functional group that does not form a bond or a state close to a bond with the binder resin can be used. The PFPE having the above-mentioned reactive functional group can improve the compatibility between the binder resin and the PFPE by interaction with the binder resin, and can stably disperse the PFPE in the binder resin. When the binder resin is formed by addition reaction, examples of the reactive functional group that causes an addition reaction with the monomer for forming the binder resin include an acrylic group, a methacrylic group, and an oxysilanyl group. Examples of PFPE having an acrylic or methacrylic group include "Fluorolink MD500", "Fluorolink MD700", "Fluorolink 5101X", "Fluorolink 5113X", and "Fluorolink AD1700" (all trade names, manufactured by Solvay Specialty Polymers), and "Optool DAC" (trade name, manufactured by Daikin Industries, Ltd.).

[0028] In the case where the binder resin is formed by an addition reaction, examples of the non-reactive functional group that does not undergo an addition reaction with the monomer for forming the binder resin include a hydroxyl group, a trifluoromethyl group, and a methyl group. Examples of such PFPEs include "Fomblin D2", "Fomblin M60", and "Fluorolink S10" (all trade names, manufactured by Solvay Specialty Polymers), "Demnum S-20", "Demnum S-65", and "Demnum S200" (all trade names, manufactured by Daikin Industries, Ltd.). Among these, from the viewpoint of low toner adhesion to the surface of electrophotographic members, PFPEs having a non-reactive functional group are preferred.

[0029] The content of PFPE in the surface layer must be 20% by mass or more relative to the binder resin (100% by mass) so that a sufficient amount of PFPE is present in the vicinity of the surface of surface layer 22 on the side opposite to the side facing base layer 21. If there is too much oil-like PFPE, the PFPE will seep out from the surface of the electrophotographic member and adhere to the toner, decreasing the toner adhesion, and therefore the content of PFPE in the surface layer must be 100% by mass or less relative to the binder resin.

[0030] (Ionic Liquid) An ionic liquid is a liquid composed of cations and anions, and is a salt that exists as a liquid over a wide temperature range. In particular, it refers to a salt that has a melting point of 100°C or lower by using relatively large organic ions as the ionic species that make up the salt. In the present disclosure, the ionic liquid preferably has an anion containing a plurality of perfluoroalkyl groups from the viewpoint of low toner adhesion, that is, improving the contact angle with hexadecane, when used in electrophotographic members.

[0031] Anion (negative ion) As the anion species constituting the ionic liquid, a sulfonylimide ion having two perfluoroalkyl groups, as shown in the following structural formula (1), can be used.

[0032] [ka]

[0033] In structural formula (1), m and n each independently represent an integer of 1 or more and 4 or less. Specific examples of anions satisfying structural formula (1) include bis(trifluoromethanesulfonyl)imide ion, bis(perfluoroethanesulfonyl)imide ion, bis(perfluoropropanesulfonyl)imide ion, bis(nonafluorobutanesulfonyl)imide ion (also referred to as bis(perfluorobutanesulfonyl)imide ion), trifluoromethanesulfonylperfluoropropanesulfonylimide ion, trifluoromethanesulfonylperfluorobutanesulfonylimide ion, and the like.

[0034] Cations (positive ions) The cationic species constituting the ionic liquid is not particularly limited, and any cation that forms a pair with the sulfonylimide ion represented by the structural formula (1) to form the ionic liquid can be used. Preferable specific examples of this cation include cations selected from the group of structures represented by the following structural formulas (2) to (7), or cations having a reactive functional group represented by the following structural formula (8).

[0035] [ka]

[0036] In structural formulas (2) to (7), R1 to R 15 each independently represents a hydrocarbon group having 1 to 8 carbon atoms. Examples of the hydrocarbon group include the following: i) a linear or branched saturated hydrocarbon group having 1 to 8 carbon atoms; ii) a linear or branched unsaturated hydrocarbon group having 2 to 8 carbon atoms; iii) a substituted or unsubstituted saturated alicyclic hydrocarbon group having 3 to 8 carbon atoms; iv) a substituted or unsubstituted unsaturated alicyclic hydrocarbon group having 4 to 8 carbon atoms; and v) a substituted or unsubstituted aromatic hydrocarbon group (phenyl group) having 6 carbon atoms. Here, examples of the substituents of the saturated alicyclic hydrocarbon group, the unsaturated alicyclic hydrocarbon group and the aromatic hydrocarbon group include alkyl groups having 1 to 3 carbon atoms. The number of carbon atoms in the "hydrocarbon group having 1 to 8 carbon atoms" includes the number of carbon atoms of the substituent.

[0037] [ka]

[0038] In structural formula (8), R 16 ~R 18 Each of R1 to R2 in the structural formulae (2) to (7) independently represents a hydrocarbon group having 1 to 8 carbon atoms. 15 The same groups as those shown in the above can also be mentioned. 19 represents a hydrogen atom or a methyl group, and l represents an integer of 1 or more and 8 or less.

[0039] Each cation will be explained in detail below. Here, we will explain in order a) imidazolium-based ions (structural formula (2)), b) ammonium-based ions (structural formula (3)), c) pyridinium-based ions (structural formula (4)), d) piperidinium-based ions (structural formula (5)), e) pyrrolidinium-based ions (structural formula (6)), f) phosphonium-based ions (structural formula (7)), and g) acryloyl or methacryloyl-based ions (structural formula (8)).

[0040] a) Imidazolium ions Specific examples of the imidazolium ion represented by the above structural formula (2) are given below. 1-ethyl-3-methylimidazolium ion, 1-butyl-3-methylimidazolium ion, 1-hexyl-3-methylimidazolium ion, 1-methyl-3-octylimidazolium ion, 1-(tert-butyl)-3-methylimidazolium ion, 1-phenyl-3-methylimidazolium ion, 1-(2,4-dimethylphenyl)-3-methylimidazolium ion.

[0041] b) Ammonium ions Specific examples of the ammonium ion represented by the above structural formula (3) are given below. N,N,N-trimethyl-N-propylammonium ion (TMPA), N,N,N-tributyl-N-methylammonium ion, N,N,N-trioctyl-N-methylammonium ion, N-butyl-N,N,N-trimethylammonium ion, N-(tert-butyl)-N,N,N-trimethylammonium ion, N-phenyl-N,N,N-trimethylammonium ion, N-(2,4-dimethylphenyl)-N,N,N-trimethylammonium ion.

[0042] c) Pyridinium ions Specific examples of the pyridinium ion represented by the above structural formula (4) are given below. 1-ethylpyridinium ion, 1-butylpyridinium ion, 1-hexylpyridinium ion, 1-(tert-butyl)pyridinium ion, 1-phenylpyridinium ion, and 1-(2,4-dimethylphenyl)pyridinium ion.

[0043] d) Piperidinium ions Specific examples of the piperidinium ion represented by the above structural formula (5) are given below. N-methyl-N-ethylpiperidinium ion, N-methyl-N-propylpiperidinium ion, N-(tert-butyl)-N-methylpiperidinium ion, N-phenyl-N-methylpiperidinium ion, N-(2,4-dimethylphenyl)-N-methylpiperidinium ion.

[0044] e) Pyrrolidinium ions Specific examples of the pyrrolidinium ion represented by the above structural formula (6) are given below. N-methyl-N-propylpyrrolidinium ion, N-methyl-N-butylpyrrolidinium ion, N-(tert-butyl)-N-methylpyrrolidinium ion, N-phenyl-N-methylpyrrolidinium ion, N-(2,4-dimethylphenyl)-N-methylpyrrolidinium ion.

[0045] f) Phosphonium ions Specific examples of the phosphonium ion shown in the above structural formula (7) are given below. Trimethylpropylphosphonium ion, tributylmethylphosphonium ion, triethylpentylphosphonium ion, (tert-butyl)-trimethylphosphonium ion, phenyl-trimethylphosphonium ion, (2,4-dimethylphenyl)-trimethylphosphonium ion.

[0046] g) Methacryloyl or acryloyl ions Specific examples of the methacryloyl or acryloyl ion shown in the above structural formula (8) are given below. (2-acryloyloxyethyl)trimethylammonium ion, (2-methacryloyloxyethyl)trimethylammonium ion, (2-acryloyloxyethyl)tributylammonium ion, (2-methacryloyloxyethyl)tributylammonium ion.

[0047] Among the cations represented by the above structural formulas (2) to (8), cations having a planar cyclic structure (structural formula (2), structural formula (4), structural formula (5), structural formula (6)) have small steric hindrance when reacting with PFPE. For this reason, they are preferred in that they react with the ether group of PFPE without covering the perfluoroalkyl group portion, and thus facilitate improvement of the low toner adhesion of electrophotographic members. Among these, the imidazolium ion represented by structural formula (2) is more preferred in that it has the smallest steric hindrance. In addition, the methacryloyl or acryloyl ion shown in the structural formula (8) has a reactive functional group that can form a bond or a state close to a bond with the binder resin when an acrylic resin is used as the binder resin. Therefore, the compatibility between the binder resin and the ionic liquid is improved due to the interaction with the binder resin, and the ionic liquid is stably dispersed, which is preferable in terms of surface layer strength compared to when an equivalent amount of other ionic liquid is used.

[0048] The content of the ionic liquid in the surface layer is preferably 25% by mass or more, particularly 50% by mass or more, based on the content of PFPE (100% by mass), in order to ensure that the cations of the ionic liquid interact with the ether structure portion of PFPE.The content of the ionic liquid is preferably 150% by mass or less, in order to effectively utilize the perfluoroalkyl group portion of PFPE to improve the contact angle of the surface. The content of the ionic liquid can be determined by extracting the ionic liquid from the surface layer and quantifying it. A solvent capable of dissolving the ionic liquid is selected as the solvent used for extraction. A specific example is methyl ethyl ketone (MEK). The solvent in the extract after extraction is removed using a rotary evaporator or the like, and the ionic liquid is isolated by various types of chromatography, whereby the content of the ionic liquid in the surface layer can be quantified.

[0049] (Additives) The surface layer may contain additives as necessary within the scope that does not impede the manifestation of the effects of the present disclosure. A dispersant may be used to more stably form PFPE as a domain in the surface layer of the electrophotographic member. The dispersant is a compound having a site with affinity to perfluoroalkyl chains and hydrocarbon chains, that is, a compound having amphiphilicity with both fluorine affinity and fluorine aversion, and a surfactant, an amphiphilic block copolymer, or an amphiphilic graft copolymer is preferably used as the dispersant. Among these, the dispersant is preferably the following (i) or (ii): (i) a block copolymer obtained by copolymerizing a vinyl monomer having a fluoroalkyl group with an acrylate or methacrylate, (ii) a comb-type graft copolymer obtained by copolymerizing an acrylate or methacrylate having a fluoroalkyl group with a methacrylate macromonomer having polymethyl methacrylate in the side chain. Examples of the block copolymer (i) above include "Modiper" (registered trademark) F200, F210, F2020, F600, and FT-600 manufactured by NOF Corporation. As the comb-type graft copolymer of (ii) above, fluorine-based graft polymers include "Aron" (registered trademark) GF-150, GF-300, GF-400, and GF-420 manufactured by Toagosei Co., Ltd.

[0050] Furthermore, in order to impart electrical conductivity, a conductive agent may be contained in the surface layer 22. Examples of the conductive agent include carbon-based conductive particles such as carbon black, carbon fiber, and carbon nanotubes, and metal oxides such as zinc antimonate, zinc oxide, tin oxide, and titanium oxide. Examples of other additives include filler particles, lubricants, conductive aids, curing agents, antioxidants, UV absorbers, pH adjusters, crosslinking agents, pigments, thickeners, and the like that are known in the art.

[0051] <Method of Manufacturing Electrophotographic Members> Using FIG. 1, an electrophotographic image forming apparatus (electrophotographic apparatus) of the present disclosure having an intermediate transfer belt as one embodiment of an electrophotographic member according to the present disclosure will be described in detail below, but the present disclosure is not limited to this embodiment. The base layer 21 of the intermediate transfer belt can be prepared by the following method. For example, when a thermosetting resin such as polyimide is used, the conductive agent and, if necessary, the additive are dispersed in a varnish together with a precursor of the thermosetting resin or a soluble thermosetting resin and a solvent, and the varnish is coated on the mold of a centrifugal molding device.The coated film is then baked to form a semiconductive film.

[0052] When a thermoplastic resin is used, the conductive agent and the thermoplastic resin are mixed, and additives may be added if necessary, and the mixture is melt-kneaded in a twin-screw kneader or the like to produce a semiconductive resin composition. Next, this resin composition is extruded by melt extrusion into a sheet, film or cylinder to obtain the base layer. The endless base layer can be formed, for example, from a resin tube obtained by melt extruding a resin composition from a cylindrical die. Alternatively, it can be formed by joining the ends of a resin sheet or film obtained by extrusion molding into a sheet or film shape to form a cylindrical shape. In addition to the extrusion molding method, it can also be molded using a known molding method such as a heat press method, an injection molding method, a stretch blow molding method, or an inflation molding method. In addition, the molded base layer may be subjected to a surface treatment such as coating with a treatment agent or polishing.

[0053] The surface layer 22 of the intermediate transfer belt can be formed, for example, by the following method. First, a polymerizable monomer, a polymerization initiator, a PFPE, an ionic liquid, and other additives, such as a dispersant, a conductive agent, and other additives, are dissolved and dispersed in an appropriate organic solvent to form the binder resin, which is the above-described constituent material of the surface layer 22, to obtain a surface layer coating liquid. Next, the surface layer coating liquid is applied onto the outer periphery of the base layer 21 by a method such as ring coating, dip coating, or spray coating, and dried at 60 to 90° C. to remove the organic solvent. After that, the intermediate transfer belt of this embodiment is obtained by UV curing using an ultraviolet irradiator.

[0054] Furthermore, the surface layer preferably has an uneven shape such as grooves on its outer surface, which reduces the contact area with other contact members such as a cleaning blade, and further reduces toner adhesion to the outer surface. The method of imparting the uneven shape is not particularly limited. For example, the intermediate transfer belt having the above-mentioned surface layer supported by a core or the like is rotated in the circumferential direction while being in contact with a wrapping film containing abrasive grains, and the surface of the surface layer is polished to impart the uneven shape. In addition, a method such as imprint processing in which a mold previously processed into a desired shape is brought into contact can also be used.

[0055] FIG. 4 is an explanatory diagram of an electrophotographic belt according to another embodiment of the present disclosure having grooves on the outer surface. A plurality of grooves 401 are provided on the outer peripheral surface of an electrophotographic belt 405 (hereinafter also referred to as the "outer surface"). Each of the grooves 401 crosses a straight line in a direction perpendicular to the circumferential direction of the electrophotographic belt 405 and extends non-parallel to the circumferential direction. Specifically, each of the grooves 401 preferably has a narrow angle θ with respect to the circumferential direction that is greater than 0° and less than ±3°. More preferably, the narrow angle θ is less than ±1°. When the narrow angle that the groove 401 makes with respect to the circumferential direction is within the above range, the portion of the cleaning blade that contacts the region of the electrophotographic belt sandwiched between two adjacent grooves 401 is not fixed, so that it is possible to suppress wear only in that portion.

[0056] A plurality of grooves 401 are provided on the outer surface of the electrophotographic belt. The outer surface of the electrophotographic belt is composed of only a first region 402 having n grooves intersecting a virtual line in a direction perpendicular to the circumferential direction, and a second region 403 having more than n grooves intersecting the virtual line. The first region and the second region are arranged alternately in the circumferential direction. The number n of the grooves 401 is an integer of 1 or more, and is not particularly limited as long as toner cleaning can be stably performed, but is preferably 2,000 to 120,000. If the number is 2,000 or more, the area of ​​the cleaning member (cleaning blade) that comes into contact with the portion not provided with the grooves 401 is reduced, thereby making it possible to reduce the frictional force generated between the cleaning blade and the electrophotographic belt 405. If the number is 120,000 or less, the toner on the grooves 401 can be transferred better.

[0057] The number of grooves in the second region is preferably 2n-10 or more and 2n+10 or less. When the number of grooves in the second region is 2n-10 or more, the position of the contact portion of the cleaning blade at the boundary between the first region and the second region can be stably changed. When the number of grooves in the second region is 2n+10 or less, the toner on the grooves can be transferred more efficiently.

[0058] There is no particular restriction on the spacing between adjacent grooves, but it is preferable that the spacing be approximately equal from the viewpoint of toner cleaning. By making the spacing uniform, localized wear of the blade can be suppressed.

[0059] The circumferential length of the second region is preferably 0.01 to 50 mm. Each of the grooves may be discontinuous in the circumferential direction, and the second region may include the end of each groove. When the circumferential length of the second region is 50 mm or less, the toner on the grooves can be transferred more efficiently.

[0060] At least one second region is present on the outer surface of the electrophotographic belt 405. In particular, it is preferable that one to three regions are present, and it is more preferable that two to three regions are present in the circumferential direction of the electrophotographic belt. By having two to three second regions present in the circumferential direction of the electrophotographic belt, the toner on the grooves can be transferred more efficiently. The depth of the groove 401 is preferably 0.10 μm or more and less than 5.0 μm, and more preferably 0.20 μm or more and 2.0 μm or less. By setting the groove depth within the above range, the contact state of the cleaning blade against the electrophotographic belt can be stabilized for a long period of time.

[0061] The width of the groove is preferably 0.10 μm or more and less than 3.0 μm, more preferably 0.20 μm or more and 2.0 μm or less. By making the width of the groove within the above range, it is possible to maintain the transferability of the toner and maintain the image quality of the electrophotographic belt. The processing method for forming the groove can be, for example, a known processing method such as cutting, etching, or imprinting. From the viewpoint of the processing reproducibility of the groove and the processing cost, imprinting is preferred.

[0062] The thickness of the electrophotographic belt 405 is preferably 10 μm or more and 500 μm or less, particularly preferably 30 μm or more and 150 μm or less. The electrophotographic belt 5 of the present embodiment may be used as a belt, or may be wound around or covered on a drum or roll used as an electrophotographic member.

[0063] <Electrophotographic image forming apparatus> FIG. 1 is a schematic cross-sectional view of an electrophotographic image forming apparatus (hereinafter, also referred to as an "electrophotographic apparatus") according to one embodiment of the present disclosure, which is provided with an electrophotographic member according to one embodiment of the present disclosure as an intermediate transfer belt. As shown in FIG. 1, the electrophotographic device has a total of four process units for each color, which are image forming means including a charging means, an exposure means, a developing means, a cleaner, etc., arranged around a drum-shaped electrophotographic photosensitive member (hereinafter referred to as a photosensitive drum) as an image carrier. The images on the photosensitive drums formed in the process units are sequentially transferred in multiple layers to an intermediate transfer belt that moves and passes adjacent to the drum at multiple primary transfer sections, forming a full-color toner image. Thereafter, the toner images formed on the intermediate transfer belt are transferred collectively onto a recording material at a secondary transfer section. The toner image on the recording material is then fused and fixed to the recording material by heat and pressure at a fixing section.

[0064] The electrophotographic apparatus will now be described in detail. This image forming apparatus has four image forming units Y·M·C·K, numbered first through fourth, arranged in parallel from left to right in the drawing. Each image forming unit Y·M·C·K is an electrophotographic process mechanism of a laser scanning exposure type having the same configuration, and has a photosensitive drum 1 as an image carrier. Electrophotographic process means acting on this photosensitive drum 1 include a charging roller 2 as charging means, an exposure device 3 as exposure means, a developing device 4 as developing means, a primary transfer roller 5 as primary transfer means, a drum cleaner 6, etc. The intermediate transfer belt 7 is stretched over three parallel rollers: a secondary transfer opposed roller 8 which also serves as a drive roller, a deviation correction roller 9 which also serves as a tension roller, and a driven roller 10. The deviation correction roller 9 is located on the first image forming unit Y side, the secondary transfer opposed roller 8 on the fourth image forming unit K side, and the driven roller 10 below the secondary transfer roller 8. The lower surface of the intermediate transfer belt between the deviation correction roller 9 and the driven roller 10 is in contact with the upper surfaces of the photosensitive drums 1 of the image forming units Y, M, C, and K. The deviation correction roller 9 can be adjusted for alignment to control the deviation of the intermediate transfer belt. The primary transfer roller 5 of each image forming unit Y, M, C, K is disposed inside the intermediate transfer belt between the deviation correction roller 9 and the driven roller 10, and is pressed against the upper surface of the photosensitive drum 1 with the intermediate transfer belt 7 sandwiched therebetween. The contact portion between the photosensitive drum 1 of each image forming unit Y, M, C, K and the intermediate transfer belt 7 is the primary transfer nip portion T1. The contact portion between the intermediate transfer belt 7 and the secondary transfer roller 12 is the secondary transfer nip portion T2. ​​A registration roller pair 13 is disposed upstream of the secondary transfer nip portion T2 in the recording material conveying direction. In addition, a recording material conveying belt device and a fixing device (not shown) are disposed in this order downstream of the secondary transfer nip portion T2 in the recording material conveying direction.

[0065] The operation for forming a full-color image is as follows. The first to fourth image forming units Y, M, C, and K are driven at a predetermined control timing of the image formation sequence. As a result of this driving, each photosensitive drum 1 is rotated in the clockwise direction of the arrow at the same predetermined speed. The intermediate transfer belt 7 is also rotated by the secondary transfer opposing roller 8 in the counterclockwise direction of the arrow at the same speed as the photosensitive drum 1. The surface of the rotating photosensitive drum 1 is uniformly charged to a predetermined polarity and potential by a charging roller 2. The charged surface of the drum 1 is image-exposed by an exposure device 3. In this embodiment, the exposure device 3 is a laser scanner that outputs laser light modulated according to an image information signal to scan and expose the charged surface of the photosensitive drum 1. As a result, an electrostatic image (electrostatic latent image) corresponding to the scanning and exposure pattern is formed on the drum surface. The formed electrostatic image is developed into a toner image by a developing device 4.

[0066] By the electrophotographic process as described above, the first image forming unit Y forms a yellow toner image corresponding to the yellow component image among the color separation component images of the full-color original image on the surface of the photosensitive drum 1. The second image forming unit M forms a magenta toner image corresponding to the magenta component image, and the third image forming unit C forms a cyan toner image corresponding to the cyan component image, each at a predetermined control timing. Also, the fourth image forming unit K forms a black toner image corresponding to the black component image at a predetermined control timing. Then, at the primary transfer nip T1 of the first image forming unit Y, the yellow toner image formed on the photosensitive drum 1 is primarily transferred onto the intermediate transfer belt 7 which is being rotated. Next, at the primary transfer nip T1 of the second image forming unit M, the magenta toner image formed on the photosensitive drum 1 is primarily transferred and superimposed on the yellow toner image on the intermediate transfer belt 7. Similarly, at the primary transfer nip T1 of the third image forming unit C and the fourth image forming unit K, the cyan toner image and the black toner image are sequentially primarily transferred onto the intermediate transfer belt 7.

[0067] That is, toner images of four colors in total, yellow, magenta, cyan, and black, are sequentially superimposed and superimposed (multiple) transferred at predetermined positions onto the intermediate transfer belt 7, thereby forming a composite full-color unfixed toner image. At each primary transfer nip T1, the primary transfer of the toner image from the photosensitive drum 1 to the intermediate transfer belt 7 is as follows. That is, a predetermined primary transfer bias is applied to the primary transfer roller 5 from a primary transfer power supply unit (not shown), and the toner image is electrostatically transferred from the photosensitive drum 1 to the intermediate transfer belt 7. The primary transfer bias is a DC voltage of a predetermined potential, with a polarity opposite to the charge polarity of the toner. In each image forming unit Y·M·C·K, the surface of the photosensitive drum 1 after passing through the primary transfer nip is cleaned by the drum cleaner 6 to remove any residual toner from the primary transfer, and is repeatedly used for image formation.

[0068] The full-color unfixed toner image compositely formed on the intermediate transfer belt 7 as described above is conveyed by the continued rotation of the intermediate transfer belt 7 to reach the secondary transfer nip portion T2, which is the contact portion between the secondary transfer roller 12 and the intermediate transfer belt 7. Then, at the timing when the leading edge of the full-color unfixed toner image formed on the intermediate transfer belt 7 reaches the secondary transfer nip portion T2, the start of rotation of the registration roller pair 13 is controlled so that the print start position of the recording material P coincides with the secondary transfer nip portion T2. ​​In the process in which the recording material P is nipped and conveyed through the secondary transfer nip portion T2, a secondary transfer bias of a predetermined potential and of a polarity opposite to the charge polarity of the toner is applied from the secondary transfer power supply portion to the secondary transfer roller 12. The secondary transfer bias is a DC voltage of a predetermined potential and of a polarity opposite to the charge polarity of the toner.

[0069] As a result, the full-color unfixed toner images on the intermediate transfer belt 7 are secondarily transferred all at once onto the recording material P. The recording material P leaving the secondary transfer nip portion T2 is separated from the intermediate transfer belt 7 and introduced into the fixing device by the recording material conveying belt device. There, the toners of the respective color toner images are melted and mixed, and fixed (fixed into a fixed image) onto the surface of the recording material as a full-color print image, and the full-color print is discharged outside the machine.

[0070] After the recording material is separated, the surface of the intermediate transfer belt 7 is cleaned by the intermediate transfer belt cleaner 11 to remove the secondary transfer residual toner during the subsequent rotation of the intermediate transfer belt 7, in preparation for the next image forming process. The intermediate transfer belt cleaner 11 brings a cleaning member (blade) into contact with the surface of the intermediate transfer belt 7 to scrape off the secondary transfer residual toner adhering to the belt surface. The residual toner is then collected as recovered toner in a recovered toner box in the intermediate transfer belt cleaner 11. A patch detection sensor 20 (toner image detection means) having a function of detecting image density is provided at a position facing the intermediate transfer belt portion stretched by the tension roller 10. This sensor optically detects reflected light and scattered light of light irradiated onto an adjustment toner image (patch image) formed on the intermediate transfer belt. A toner image for adjustment (patch image) is formed on the intermediate transfer belt during a period other than the period during which the toner image to be secondarily transferred to the recording material is primarily transferred onto the intermediate transfer belt. Depending on the result, the image forming conditions are adjusted. EXAMPLES

[0071] The present disclosure will be specifically described below with reference to examples and comparative examples, but the present disclosure is not limited thereto. In each example, an intermediate transfer belt was produced as the electrophotographic member of the present disclosure.

[0072] The measurement and evaluation methods used in each example are described below. <Evaluation of low toner adhesion (contact angle)> The adhesion was evaluated based on the contact angle of normal hexadecane (n-HD), which was measured using a contact angle meter (product name: PCA-11, manufactured by Kyowa Interface Science Co., Ltd.).

[0073] <Image evaluation> The intermediate transfer belt of the example or comparative example was installed in place of the intermediate transfer belt installed in a full-color electrophotographic image forming apparatus (product name: iRC2620; manufactured by Canon Inc.). Then, a blue solid image was printed on the entire surface of a recording material (plain paper 4024 of Xerox Corporation) to perform image evaluation. The printed image was visually observed and evaluated according to the following criteria. A: There is absolutely no unevenness in the image. B: There is almost no unevenness in the image. C: There are some unevenness in the image.

[0074] <Surface strength evaluation> The surface layer strength was evaluated based on the measured hardness. The hardness of the surface layer 22 was measured using a Berkovich type indenter with a microindentation hardness tester (product name: Nanoindenter G200 type, manufactured by Agilent Technologies, Inc.). The measurement area was a region of 100 to 200 nm from the outermost surface of the surface layer 22 in the thickness direction, and the average hardness in this region was calculated. The measured values ​​were evaluated based on the following criteria. Rank A: Hardness = 0.15 GPa or more Rank B: Hardness = 0.10 GPa or more, less than 0.15 Pa Rank C: Hardness = less than 0.1 GPa

[0075] (Materials used in preparing the coating material for forming the surface layer according to the examples and comparative examples) The materials used in the preparation of the coating materials for forming the surface layer according to the examples and comparative examples are shown in Tables 1 to 4 below.

[0076] [Table 1]

[0077] [Table 2]

[0078] [Table 3]

[0079] [Table 4]

[0080] (Preparation of Surface Coatings 1 to 21) The materials were mixed in the amounts shown in Tables 5-1 to 5-2 below using a stirring homogenizer (manufactured by AS ONE Corporation) to prepare coating materials 1 to 21 for forming surface layers.

[0081] (Preparation of Surface Layer Forming Paints C-1 to C-3) The materials were mixed in the amounts shown in Table 5-3 below using a stirring homogenizer (manufactured by AS ONE Corporation) to prepare coating materials C-1 to C-3 for forming the surface layer.

[0082] [Table 5-1]

[0083] [Table 5-2]

[0084] [Table 5-3]

[0085] Example 1 The electrophotographic belt 1 according to this embodiment was produced using, as the base layer 21, an intermediate transfer belt made of polyimide that was installed in a full-color copier (product name: iRC2620, manufactured by Canon Inc.). That is, a coating film of the surface layer forming paint 1 was formed on the outer peripheral surface of the base layer 21, and the coating film was dried at a temperature of 70° C. for 3 minutes. Then, ultraviolet rays were irradiated with an integrated light amount of 500 mJ / cm 2 The coating was cured by irradiating the coating so as to obtain a coating having a thickness of 4 μm. Thus, an electrophotographic belt 1 having a surface layer with a thickness of 4 μm was produced. The intermediate transfer belt 1 thus obtained was subjected to the above-mentioned various evaluations.

[0086] [Examples 2 to 21] Electrophotographic belts 2 to 21 according to Examples 2 to 21 were produced and evaluated in the same manner as in Example 1, except that the coating materials 2 to 21 for forming the surface layer were used to form the surface layer. Table 6 shows the evaluation results of the electrophotographic belts 1 to 21.

[0087] [Table 6]

[0088] [Comparative Examples 1 to 3] Electrophotographic belts C-1 to C-3 according to Comparative Examples 1 to 3 were produced and evaluated in the same manner as in Example 1, except that the surface layer forming coating materials C-1 to C-3 were used to form the surface layer. Table 7 shows the evaluation results of the electrophotographic belts C-1 to C-3.

[0089] [Table 7] [Explanation of symbols]

[0090] 7 Intermediate transfer belt 21 Base layer 22 Surface layer

Claims

1. An electrophotographic member having a base layer and a surface layer laminated in this order in a thickness direction, the surface layer comprises a binder resin, a perfluoropolyether, and an ionic liquid; The content ratio of the perfluoropolyether to the binder is 20% by mass or more and 100% by mass or less, The ionic liquid is an electrophotographic member having an anion represented by the following formula (1): 【Chemistry 1】 (In structural formula (1), m and n each independently represent an integer of 1 or more and 4 or less).

2. The electrophotographic member according to claim 1, wherein the surface of said surface layer opposite the side facing said base layer has a contact angle with hexadecane of 65° or more.

3. The electrophotographic member according to claim 1 or 2, wherein the ionic liquid has a cation selected from the group of structures represented by the following structural formulas (2) to (7): 【Chemistry 2】 (In structural formulas (2) to (7), R 1 ~R 15 each independently represents a hydrocarbon group having 1 to 8 carbon atoms.

4. The electrophotographic member according to claim 1 or 2, wherein the ionic liquid has a cation represented by the following structural formula (8): 【Chemistry 3】 (In structural formula (8), R 16 ~R 18 Each independently represents a hydrocarbon group having 1 to 8 carbon atoms. 19 represents a hydrogen or a methyl group, and l represents an integer of 1 or more and 8 or less.

5. 5. The electrophotographic member according to claim 1, wherein the content of the ionic liquid relative to the perfluoropolyether is 25% by mass or more and 150% by mass or less.

6. 6. The electrophotographic member according to claim 1, wherein the binder resin is an acrylic resin.

7. 7. The electrophotographic member according to claim 1, wherein the electrophotographic member is an electrophotographic belt having an endless shape.

8. 8. The electrophotographic member according to claim 7, wherein the electrophotographic belt has a plurality of grooves on a surface of the surface layer opposite to a side facing the base layer.

9. 9. The electrophotographic member according to claim 8, wherein, assuming that a straight line is laid on the surface in a direction perpendicular to a circumferential direction of the electrophotographic belt, the plurality of grooves intersect the straight line and extend in a direction non-parallel to the circumferential direction.

10. The surface of the surface layer opposite to the side facing the base layer is a first region in which the number of the grooves intersecting the straight line is n; a second region in which the number of the grooves intersecting the straight line is greater than n; 10. The electrophotographic member according to claim 9, wherein the first regions and the second regions are alternately disposed in the circumferential direction of the electrophotographic belt (wherein n is an integer of 1 or more).

11. The electrophotographic member according to any one of claims 7 to 10, wherein the electrophotographic belt is an intermediate transfer belt.

12. An electrophotographic image forming apparatus comprising the electrophotographic member according to any one of claims 1 to 11.

13. 13. The electrophotographic image forming apparatus according to claim 12, further comprising a cleaning member disposed in contact with a surface of said surface layer of said electrophotographic member opposite to a surface facing said base layer.

Citation Information

Patent Citations

  • Rotor, transfer unit, and image forming apparatus

    JP2013044878A

  • Conductive belt and electrophotographic device

    JP2014132329A

  • Member for electrophotography, process cartridge, and electrophotographic apparatus

    JP2015028613A

  • Conductive belt and electrophotographic device

    JP2015230456A

  • Electrophotographic member and electrophotographic image forming apparatus

    JP2019012124A