Nonaqueous electrolyte and nonaqueous electrolyte secondary battery

The introduction of a silane compound with a heteroaryl group in the non-aqueous electrolyte forms a high-quality SEI film, addressing safety issues in lithium ion secondary batteries with silicon-based electrodes by enhancing decomposability and reactivity, ensuring stability and safety during charging and discharging.

JP7566702B2Active Publication Date: 2024-10-15SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021136372
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-24
Publication Date
2024-10-15
Estimated Expiration
2041-08-24

AI Technical Summary

Technical Problem

Lithium ion secondary batteries using silicon-based negative electrodes face safety issues due to repeated formation and decomposition of the solid electrolyte interphase (SEI) film during charging and discharging, leading to increased surface area and instability, which reduces safety.

Method used

Incorporation of a silane compound with a heteroaryl group into the non-aqueous electrolyte, represented by the general formula Si(R1)l(R2)m(R3)4-l-m, where R1 is a heteroaryl group, R2 is an alkenyl or alkynyl group, and R3 is an alkyl group, forming a high-quality SEI film that suppresses the reactivity of the active material surface with the electrolyte.

Benefits of technology

The silane compound improves the decomposability and reactivity of the SEI film, resulting in a non-aqueous electrolyte secondary battery that is highly safe after charging and discharging, with improved stability and reduced resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566702000001
    Figure 0007566702000001
  • Figure 0007566702000002
    Figure 0007566702000002
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte and a nonaqueous electrolyte secondary battery which are highly safe after charge / discharge.SOLUTION: The nonaqueous electrolyte is used for a nonaqueous electrolyte secondary battery and contains a silane compound represented by the following general formula (1): Si(R1)l(R2)m(R3)4-l-m (1) (where R1 is a C4-20 heteroaryl group; R2 is a C2-20 alkenyl group or alkynyl group; R3 is a C1-20 alkyl group; and l and m each independently represent an integer of 1-3 and are integers satisfying 2≤l+m≤4).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-aqueous electrolyte and a non-aqueous electrolyte secondary battery. [Background technology]

[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are particularly small and lightweight and capable of obtaining high energy density has been promoted. Applications of these secondary batteries are being considered not only for small electronic devices, but also for large electronic devices such as automobiles and power storage systems such as homes.

[0003] Among these, lithium-ion secondary batteries are attracting great attention because they can be easily made small and have a high capacity, and because they offer a higher energy density than lead-acid batteries and nickel-cadmium batteries.

[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and a nonaqueous electrolyte.

[0005] Various additives are used in non-aqueous electrolytes for the purpose of improving the stability and electrical characteristics of non-aqueous electrolyte secondary batteries. As these additives, 1,3-propane sultone (see, for example, Patent Document 1), vinyl ethylene carbonate (see, for example, Patent Document 2), vinylene carbonate (see, for example, Patent Document 3), fluoroethylene carbonate (FEC) (see, for example, Patent Document 4), and the like have been proposed. These additives form a stable solid electrolyte interphase (SEI) film on the negative electrode surface, making it possible to suppress reductive decomposition of the electrolyte.

[0006] It is known that non-aqueous electrolyte secondary batteries using silicon-based negative electrode materials, etc., undergo repeated charging and discharging, resulting in the formation and decomposition of an SEI film containing Li on the silicon surface layer with each cycle. As a result, the surface area of ​​the negative electrode material increases and becomes unstable, and the Li used to form the SEI film is constantly replenished from the positive electrode side, leading to an increase in potential. This results in a significant decrease in safety. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 63-102173 [Patent Document 2] Japanese Patent Application Publication No. 4-87156 [Patent Document 3] Japanese Patent Application Publication No. 5-74486 [Patent Document 4] JP 2006-134719 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in consideration of the above problems, and has an object to provide a nonaqueous electrolyte and a nonaqueous electrolyte secondary battery that are highly safe after charging and discharging. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides a nonaqueous electrolyte for use in a nonaqueous electrolyte secondary battery, the nonaqueous electrolyte comprising a silane compound represented by the following general formula (1): Si(R 1 ) l (R 2 ) m (R 3 ) 4-l-m (1) (In the formula, R 1 is a heteroaryl group having 4 to 20 carbon atoms, R 2is an alkenyl or alkynyl group having 2 to 20 carbon atoms, R 3 is an alkyl group having 1 to 20 carbon atoms. Furthermore, l and m each independently represent an integer of 1 to 3, and are integers that satisfy the relationship 2≦l+m≦4.

[0010] The silane compound contained in the non-aqueous electrolyte of the present invention contains a heteroaryl group, and such a heteroaryl group improves the decomposition property and reactivity of the silane compound after decomposition. The decomposed silane compound forms a good coating (SEI film) on the positive electrode and the negative electrode, so that the reactivity of the active material surface with the electrolyte can be suppressed. As a result, by using such a non-aqueous electrolyte in a secondary battery, a non-aqueous electrolyte secondary battery with high safety after charging and discharging can be obtained.

[0011] In this case, the energy level of the lowest unoccupied molecular orbital of the silane compound is preferably −0.40 eV or less.

[0012] At such an energy level, the decomposition property of the silane compound is improved, and a high-quality coating (SEI film) is easily formed.

[0013] The energy level of the highest occupied molecular orbital of the silane compound is preferably −8.8 eV or higher.

[0014] At such an energy level, the decomposition property of the silane compound is improved, and a high-quality coating (SEI film) is easily formed.

[0015] The content of the silane compound in the non-aqueous electrolyte is preferably 0.1% by mass to 5.0% by mass.

[0016] At such a content, a sufficient coating (SEI film) is formed, which makes it easy to suppress the reactivity of the active material surface, and also makes it easy to prevent high resistance due to the formation of an excessive coating (SEI film).

[0017] The present invention also provides a nonaqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and the above nonaqueous electrolyte.

[0018] Since such a nonaqueous electrolyte secondary battery includes the nonaqueous electrolyte of the present invention, it can be a nonaqueous electrolyte secondary battery that is highly safe after charging and discharging.

[0019] In this case, the negative electrode active material particles in the negative electrode are preferably silicon oxide particles coated with a carbon layer.Further, in this case, the silicon oxide particles preferably contain Li2SiO3, and the Li2SiO3 is preferably crystalline.

[0020] In this way, the non-aqueous electrolyte of the present invention can be used in a secondary battery in which the silicon oxide particles covered with a carbon layer are used as the negative electrode active material particles. Moreover, such crystalline Li2SiO3 can be made difficult to dissolve in an aqueous slurry. Effect of the Invention

[0021] The silane compound contained in the non-aqueous electrolyte of the present invention has a heteroaryl group, and such a heteroaryl group improves the decomposition property and reactivity of the silane compound after decomposition. The decomposed silane compound forms a good coating (SEI film) on the positive electrode and the negative electrode, so that the reactivity of the active material surface with the electrolyte can be suppressed. As a result, by using such a non-aqueous electrolyte in a secondary battery, a non-aqueous electrolyte secondary battery with high safety after charging and discharging can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] As described above, there has been a demand for a nonaqueous electrolyte and a nonaqueous electrolyte secondary battery that are highly safe after charging and discharging.

[0023] As a result of intensive research into achieving the above object, the inventors have discovered that the above object can be achieved by introducing a heteroaryl group and further an alkenyl group or an alkynyl group into a silane compound, and have thus completed the present invention.

[0024] That is, the present invention relates to a non-aqueous electrolyte for use in a non-aqueous electrolyte secondary battery, the non-aqueous electrolyte containing a silane compound represented by the following general formula (1). Si(R 1 ) l (R 2 ) m (R 3 ) 4-l-m (1) (In the formula, R 1 is a heteroaryl group having 4 to 20 carbon atoms, R 2 is an alkenyl or alkynyl group having 2 to 20 carbon atoms, R 3 is an alkyl group having 1 to 20 carbon atoms. Furthermore, l and m each independently represent an integer of 1 to 3, and are integers that satisfy the relationship 2≦l+m≦4.

[0025] Hereinafter, the present invention will be described in detail with reference to the preferred embodiments, but the present invention is not limited thereto.

[0026] <Silane compounds> As described above, the nonaqueous electrolyte of the present invention is a nonaqueous electrolyte used in a nonaqueous electrolyte secondary battery, and contains a silane compound represented by the following general formula (1) (hereinafter also referred to as "compound (1)"). Si(R 1 ) l (R 2 ) m (R 3 ) 4-l-m (1)

[0027] In the above general formula (1), R 1 is a heteroaryl group having 4 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and more preferably 4 to 6 carbon atoms.

[0028] R 1Specific examples of the heteroaryl group include a 2-pyridyl group, a 3-pyridyl group, a 4-pyridyl group, a 2-pyrazyl group, a 2-pyrimidyl group, a 4-pyrimidyl group, a 5-pyrimidyl group, a 3-pyridazyl group, a 4-pyridazyl group, a 4-(1,2,3-triazyl group), a 3-(1,2,4-triazyl) group, a 5-(1,2,4-triazyl) group, a 6-(1,2,4-triazyl) group, a 2-(1,3,5-triazyl) group, a 2-quinolyl group, a 2-quinoxalyl group, a 2-quinazolyl group, a 3-cinnolyl group, a 1-isoquinolyl group, a 3-isoquinolyl group, and a 1-phthalazyl group. Examples of such heteroaryl groups include nitrogen-containing heteroaryl groups; oxygen-containing heteroaryl groups such as 2-furyl, 3-furyl, 2-benzofuryl, 3-benzofuryl, and 1-isobenzofuryl groups; sulfur-containing heteroaryl groups such as 2-thienyl, 3-thienyl, 2-benzothienyl, and 3-benzothienyl groups; and heteroaryl groups containing two or more heteroatoms such as 2-oxazolyl, 5-oxazolyl, 3-isoxazolyl, 5-isoxazolyl, 2-benzoxazolyl, 3-benzoisoxazolyl, 2-thiazolyl, and 2-benzothiazolyl groups.

[0029] Among these, from the viewpoint of ensuring the decomposability of the silane compound and the reactivity after decomposition, a 2-pyridyl group, a 2-furyl group, and a 2-thienyl group are preferred.

[0030] Such heteroaryl groups improve the decomposition property and reactivity of the silane compound after decomposition. The decomposed silane compound forms a high-quality coating (SEI film) on the positive and negative electrodes, which is thought to suppress the reactivity of the active material surface with the electrolyte.

[0031] In the general formula (1), R 2 is an alkenyl or alkynyl group having 2 to 20 carbon atoms, preferably 2 to 10 carbon atoms, and more preferably 2 to 5 carbon atoms.

[0032] R 2Specific examples of the alkenyl group include linear alkenyl groups such as vinyl group, n-propenyl group, n-butenyl group, n-pentenyl group, n-hexenyl group, n-heptenyl group, n-octenyl group, n-nonenyl group, n-decenyl group, n-undecenyl group, and n-dodecenyl group; and branched alkenyl groups such as isopropenyl group, isobutenyl group, isopentenyl group, isohexenyl group, isoheptenyl group, isooctenyl group, isononyl group, isodecenyl group, and isoundecyl group.

[0033] Among these, vinyl and n-propenyl groups are preferred from the viewpoint of ensuring the decomposability and reactivity after decomposition of the silane compound.

[0034] R 2 Specific examples of the alkynyl group include linear alkynyl groups such as ethynyl, 1-propynyl, 1-butynyl, 1-pentynyl, 1-hexynyl, 1-heptynyl, 1-octynyl, 1-nonynyl, 1-decynyl, 1-undecynyl, and 1-dodecynyl groups; and branched alkynyl groups such as 3-methyl-1-butynyl, 3,3-dimethyl-1-butynyl, 3-methyl-1-pentynyl, 4-methyl-1-pentynyl, 3,3-dimethyl-1-pentynyl, 3,4-dimethyl-1-pentynyl, and 4,4-dimethyl-1-pentynyl groups.

[0035] Among these, from the viewpoint of ensuring the decomposability and reactivity after decomposition of the silane compound, an ethynyl group, a 1-propynyl group, and a 1-butynyl group are preferred.

[0036] These alkenyl or alkynyl groups improve the decomposition property and reactivity of the silane compound after decomposition. The decomposed silane compound forms a high-quality coating (SEI film) on the positive and negative electrodes, which is thought to suppress the reactivity of the active material surface with the electrolyte.

[0037] In the general formula (1), R 3 is an alkyl group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 5 carbon atoms.

[0038] R 3 Specific examples of the alkyl group include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, and n-dodecyl groups; and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, isohexyl, isoheptyl, isooctyl, tert-octyl, isononyl, isodecyl, and isoundecyl groups.

[0039] Among these, a methyl group is preferred from the viewpoint of less steric hindrance and facilitating the reaction between silane compounds.

[0040] In general formula (1), l and m each independently represent an integer of 1 to 3, and l and m are integers that satisfy 2≦l+m≦4. From the viewpoint of forming a high-quality coating film (SEI film), it is more preferable that in general formula (1), l and m each independently represent an integer of 1 to 3, and l and m are integers that satisfy l+m=4.

[0041] Specific examples of compound (1) include 2-pyridyltrivinylsilane, di(2-pyridyl)divinylsilane, tri(2-pyridyl)vinylsilane, methyldivinyl-2-pyridylsilane, di(2-pyridyl)methylvinylsilane, 2-furyltrivinylsilane, di(2-furyl)divinylsilane, tri(2-furyl)vinylsilane, divinyl-2-furylmethylsilane, di(2-furyl)methylvinylsilane, 2-thienyltrivinylsilane, di(2-thienyl)divinylsilane, tri(2-thienyl)vinylsilane, divinylmethyl-2-thienylsilane, di (2-thienyl)methylvinylsilane, 3-pyridyltrivinylsilane, di(3-pyridyl)divinylsilane, tri(3-pyridyl)vinylsilane, divinylmethyl-3-pyridylsilane, di(3-pyridyl)methylvinylsilane, 3-furyltrivinylsilane, di(3-furyl)divinylsilane, tri(3-furyl)vinylsilane, divinyl-3-furylmethylsilane, di(3-furyl)methylvinylsilane, 3-thienyltrivinylsilane, di(3-thienyl)divinylsilane, tri(3-thienyl)vinylsilane, divinylmethyl-3-thienylsilane , di(3-thienyl)methylvinylsilane, 2-pyridyltriethynylsilane, diethynyldi(2-pyridyl)silane, ethynyltri(2-pyridyl)silane, diethynylmethyl-2-pyridylsilane, di(2-pyridyl)ethynylmethylsilane, 2-furyltriethynylsilane, diethynyldi(2-furyl)silane, ethynyltri(2-furyl)silane, diethynyl-2-furylmethylsilane, ethynyldi(2-furyl)methylsilane, 2-thienyltriethynylsilane, diethynyldi(2-thienyl)silane, ethynyltri(2-thienyl)silane, diethinylmethyl-2-thienylsilane, ethynylmethyldi(2-thienyl)silane, 3-pyridyltriethynylsilane, diethinyldi(3-pyridyl)silane, ethynyltri(3-pyridyl)silane, diethinylmethyl-3-pyridylsilane, di(3-pyridyl)ethynylmethylsilane, 3-furyltriethynylsilane, diethinyldi(3-furyl)silane, ethynyltri(3-furyl)silane, diethinylmethyl-3-furylsilane, ethhinyldi(3-furyl)methylsilane, 3-thienyltriethynylsilane, diethinyldi(3-thienyl)silane,Examples include ethynyltri(3-thienyl)silane, diethynylmethyl-3-thienylsilane, and di(3-thienyl)ethynylmethylsilane.

[0042] The silane compound represented by the above general formula (1) can be obtained, for example, by reacting an organometallic reagent prepared from furan and n-butyllithium with vinylhalosilane.

[0043] [Content in non-aqueous electrolyte] The content of the compound (1) in the non-aqueous electrolyte is preferably 0.1% by mass to 5.0% by mass, more preferably 0.1% by mass to 4.0% by mass, and even more preferably 0.1% by mass to 2.0% by mass. With such a content, a sufficient coating (SEI film) is formed, and the reactivity of the active material surface is easily suppressed. In addition, it is easy to prevent high resistance due to excessive coating (SEI film) formation.

[0044] [Lowest Unoccupied Molecular Orbital (LUMO) energy level] The lowest unoccupied molecular orbital (LUMO) energy level of the silane compound (compound (1)) is preferably -0.40 eV or less, more preferably -0.60 eV or less, even more preferably -0.70 eV or less, and particularly preferably -0.85 eV or less. The LUMO energy level is related to the reductive decomposition property of the silane compound. With such an energy level, the decomposition property of the silane compound is improved, and a high-quality coating (SEI film) is easily formed.

[0045] [Highest Occupied Molecular Orbital (HOMO) energy level] The highest occupied molecular orbital (HOMO) energy level of the silane compound is preferably -8.8 eV or more, more preferably -8.0 eV or more, even more preferably -7.5 eV or more, and particularly preferably -7.0 eV or more. The HOMO energy level is related to the oxidative decomposition property of the silane compound. With such an energy level, the decomposition property of the silane compound is improved, and a high-quality coating film (SEI film) is easily formed.

[0046] [How to calculate energy levels] The energy levels of the lowest unoccupied molecular orbital (LUMO) and the highest occupied molecular orbital (HOMO) can be obtained by quantum chemical calculation. Gaussian, GAMESS, etc. can be used as quantum chemical calculation software. From the viewpoint of calculation accuracy and calculation cost, the density functional method is preferably used as the calculation method. B3LYP is preferably used as the exchange correlation functional, and 6-311+G(d,p) is preferably used as the basis function.

[0047] <Nonaqueous electrolyte secondary battery> [Non-aqueous electrolyte] The non-aqueous electrolyte of the present invention is a non-aqueous solvent having an electrolyte salt dissolved therein, and contains the compound (1), and may contain other materials as additives. At least a part of the active material layer or the separator is impregnated with the non-aqueous electrolyte.

[0048] Examples of non-aqueous solvents include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, and tetrahydrofuran. Among these, from the viewpoint of obtaining better characteristics, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. In this case, by combining a high-viscosity solvent such as ethylene carbonate or propylene carbonate with a low-viscosity solvent such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate, the dissociation property and ion mobility of the electrolyte salt are improved, and more advantageous characteristics can be obtained.

[0049] When an alloy-based negative electrode containing a silicon-based negative electrode material is used, it is particularly desirable to include at least one of halogenated chain carbonates or halogenated cyclic carbonates as a solvent. This allows a stable coating to be formed on the surface of the negative electrode active material during charging and discharging, particularly during charging. Here, the halogenated chain carbonate is a chain carbonate having a halogen as a constituent element (at least one hydrogen is substituted with a halogen). Also, the halogenated cyclic carbonate is a cyclic carbonate having a halogen as a constituent element (i.e., at least one hydrogen is substituted with a halogen).

[0050] The type of halogen is not particularly limited, but fluorine is preferred from the viewpoint of forming a better quality coating than other halogens. The number of halogens is preferably as large as possible, since the resulting coating is more stable and the decomposition reaction of the electrolyte is reduced.

[0051] Examples of halogenated chain carbonates include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. Examples of halogenated cyclic carbonates include 4-fluoro-1,3-dioxolan-2-one, 4,5-difluoro-1,3-dioxolan-2-one, etc.

[0052] The electrolyte salt may include at least one of light metal salts such as lithium salts, for example. Examples of the lithium salt include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).

[0053] From the viewpoint of obtaining high ionic conductivity, the content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less, more preferably 0.8 mol / kg or more and 2.0 mol / kg or less, and even more preferably 0.8 mol / kg or more and 1.5 mol / kg or less, relative to the nonaqueous solvent.

[0054] The non-aqueous electrolyte of the present invention may contain unsaturated carbon-bonded cyclic carbonates, sultones (cyclic sulfonic acid esters) and acid anhydrides as further separate additives in addition to compound (1). The unsaturated carbon-bonded cyclic carbonates may be contained from the viewpoint of a stable coating form on the negative electrode surface during charging and discharging and suppression of decomposition reaction of the non-aqueous electrolyte, and examples thereof include vinylene carbonate and vinylethylene carbonate. Furthermore, the sultones may be contained from the viewpoint of improving the chemical stability of the battery, and examples thereof include propane sultone and propene sultone. Furthermore, the acid anhydrides may be contained from the viewpoint of improving the chemical stability of the electrolyte, and examples thereof include propane disulfonic acid anhydride.

[0055] The nonaqueous electrolyte secondary battery of the present invention comprises a positive electrode and a negative electrode in addition to the nonaqueous electrolyte.

[0056] [Positive electrode] The positive electrode has a configuration in which, for example, a positive electrode active material layer is provided on one or both sides of a positive electrode current collector.

[0057] Here, the positive electrode current collector is formed of a conductive material such as aluminum.

[0058] On the other hand, the positive electrode active material layer contains one or more positive electrode materials capable of absorbing and releasing lithium ions, and may contain other materials such as a binder, a conductive assistant, a dispersant, etc., depending on the design. In this case, the binder and conductive assistant may be the same as the negative electrode binder and negative electrode conductive assistant described below.

[0059] As the positive electrode material, from the viewpoint of obtaining a high battery capacity and excellent cycle characteristics, for example, lithium-containing compounds such as composite oxides containing lithium and transition metal elements or phosphate compounds containing lithium and transition metal elements can be mentioned. As the transition metal elements, nickel, iron, manganese, and cobalt are preferable, and the lithium-containing compound is a compound having at least one or more of these transition metal elements. As the chemical formula of the thium-containing compound, for example, it is represented by LixM1O2 or LiyM2PO4. In the formula, M1 and M2 represent at least one or more transition metal elements. The values of x and y represent different values depending on the battery charge and discharge state, but generally satisfy 0.05 ≦ x ≦ 1.10 and 0.05 ≦ y ≦ 1.10.

[0060] Specific examples of the composite oxide containing lithium and transition metal elements include, for example, lithium cobalt composite oxide (Li x CoO2), lithium nickel composite oxide (Li x NiO2), lithium nickel cobalt composite oxide, lithium nickel cobalt composite oxide (lithium nickel cobalt aluminum composite oxide; NCA, lithium nickel cobalt manganese composite oxide + NCM), and the like.

[0061] Specific examples of the phosphate compound containing lithium and transition metal elements include, for example, lithium iron phosphate compound (LiFePO4), lithium iron manganese phosphate compound (LiFe 1-u Mn u PO4, provided that 0 < u < 1), and the like. By using these positive electrode materials, a high battery capacity can be obtained and excellent cycle characteristics can also be obtained.

[0062] [Negative electrode] The negative electrode has, for example, a configuration having a negative electrode active material layer on a negative electrode current collector. This negative electrode active material layer may be provided on both sides or only one side of the negative electrode current collector.

[0063] [Negative electrode current collector] The negative electrode current collector is made of a material having excellent electrical conductivity and excellent mechanical strength. Examples of the electrical conductive material that can be used for the negative electrode current collector include copper (Cu) and nickel (Ni). It is preferable that the electrical conductive material is a material that does not form an intermetallic compound with lithium (Li).

[0064] From the viewpoint of improving the physical strength of the negative electrode current collector, it is preferable that the negative electrode current collector contains carbon (C) or sulfur (S) in addition to the copper (Cu) or nickel (Ni). In particular, when the current collector has an active material layer that expands during charging, the current collector contains the above elements, which has the effect of suppressing deformation of the electrode including the current collector. The contents of the above contained elements are not particularly limited, but are preferably 100 mass ppm or less each from the viewpoint of obtaining a higher deformation suppression effect. Such a deformation suppression effect can further improve the cycle characteristics.

[0065] The surface of the negative electrode current collector may be roughened or may not be roughened. Examples of the roughened negative electrode current collector include metal foils that have been electrolytically treated, embossed, or chemically etched. Examples of the non-roughened negative electrode current collector include rolled metal foils.

[0066] [Negative electrode active material layer] The negative electrode active material layer includes a negative electrode active material capable of absorbing (inserting) and releasing lithium ions, and may further include other materials such as a negative electrode binder (binder) and a conductive assistant from the viewpoint of battery design. The negative electrode active material includes negative electrode active material particles, and examples of the negative electrode active material particles include carbon compound particles (carbon-based negative electrode active material), silicon compound particles (silicon-based negative electrode active material), germanium compound particles (germanium-based negative electrode active material), and tin compound particles (tin-based negative electrode active material). Among these, it is preferable to include carbon compound particles (carbon-based negative electrode active material) and silicon compound particles (silicon-based negative electrode active material), more preferably to include silicon compound particles (silicon-based negative electrode active material), and particularly preferable to include silicon compound particles containing a silicon compound containing oxygen.

[0067] The negative electrode active material includes carbon compound particles (carbon-based negative electrode active material), silicon compound particles (silicon-based negative electrode active material), germanium compound particles (germanium-based negative electrode active material), tin compound particles (tin-based negative electrode active material), etc., preferably includes carbon compound particles (carbon-based negative electrode active material) or silicon compound particles (silicon-based negative electrode active material), more preferably includes silicon compound particles (silicon-based negative electrode active material), and particularly preferably includes a silicon oxide material containing a silicon compound containing oxygen. This silicon compound, SiO x From the viewpoint of cycle characteristics and resistance of silicon oxide, it is preferable that x, which is the composition ratio of silicon and oxygen constituting SiO, is a number that satisfies 0.8≦x≦1.2. x In the composition, it is preferable that x is close to 1 because high cycle characteristics can be obtained. Note that the composition of the silicon compound in the present invention does not necessarily mean 100% purity, and may contain trace amounts of impurity elements.

[0068] It is preferable that the silicon compound contains as little crystalline Si as possible. By containing as little crystalline Si as possible, it is possible to prevent the reactivity with the electrolyte from becoming too high, and as a result, it is possible to prevent the battery characteristics from deteriorating.

[0069] The silicon compound contains Li, and it is desirable that a part of it is in the form of Li2SiO3 as silicate. This Li2SiO3 is crystalline, but active during charging and discharging. In the slurry state, it remains Li2SiO3, but changes to Li4SiO4 by repeated charging and discharging.

[0070] The higher the crystallinity of Li2SiO3, the more difficult it is to convert to Li4SiO4. On the other hand, when the crystallinity is low, it becomes easier to dissolve in the slurry, so there is an optimal range.

[0071] Specifically, the negative electrode active material particles have a peak due to a Si(111) crystal plane obtained by X-ray diffraction using Cu-Kα radiation before charging and discharging the negative electrode active material particles, the crystallite size corresponding to the crystal plane is 5.0 nm or less, and the ratio A / B of the intensity A of the peak due to the Si(111) crystal plane to the intensity B of the peak due to the Li2SiO3(111) crystal plane satisfies the following formula (2): 0.4≦A / B≦1.0 (2) It is preferable that the following is satisfied.

[0072] The degree of Li silicate enlargement and the degree of Si crystallization (for example, the crystallite size corresponding to the Si(111) crystal plane) can be confirmed by X-ray diffraction (hereinafter also referred to as "XRD").

[0073] The X-ray diffraction device used may be a D8 ADVANCE manufactured by Bruker. The X-ray source is a Cu Kα ray source and a Ni filter, and measurements are performed from 10 to 40° with an output of 40 kV / 40 mA, a slit width of 0.3°, a step width of 0.008°, and a counting time of 0.15 seconds per step.

[0074] The peak due to the Si(111) crystal plane appears near 2θ=28.4° in the X-ray diffraction chart.

[0075] The crystallite size corresponding to the Si(111) crystal plane is preferably 5.0 nm or less, more preferably 4.0 nm or less, and even more preferably 2.5 nm or less, and is desirably substantially amorphous.

[0076] The ratio A / B of the intensity A of the peak resulting from the Si(111) crystal plane to the intensity B of the peak resulting from the Li2SiO3(111) crystal plane is preferably 0.40≦A / B≦1.00, more preferably 0.45≦A / B≦0.75, and further preferably 0.50≦A / B≦0.70. Here, the peak resulting from the Li2SiO3(111) crystal plane appears in the range of 2θ=17° to 21° in the X-ray diffraction chart.

[0077] The median diameter of the negative electrode active material, as measured by a laser diffraction method, is preferably 5.0 μm or more and 15.0 μm or less, more preferably 5.5 μm or more and 10.0 μm or less, and even more preferably 6.0 μm or more and 8.0 μm or less, from the viewpoint of controlling the reaction with the electrolyte or suppressing the expansion of the negative electrode active material due to charging and discharging.

[0078] The negative electrode active material layer may contain a mixed negative electrode active material containing the silicon-based negative electrode active material and a carbon-based active material. This reduces the electrical resistance of the negative electrode active material layer and can alleviate the expansion stress caused by charging. Examples of the carbon-based active material include natural graphite, artificial graphite, hard carbon, and soft carbon.

[0079] The negative electrode active material layer of the present invention contains the negative electrode active material of the present invention capable of absorbing and releasing lithium ions, and may further contain other materials such as a negative electrode binder and a conductive assistant from the viewpoint of battery design.

[0080] As the negative electrode binder, for example, one or more of polymer materials, synthetic rubber, etc. can be used. As the polymer materials, for example, polyvinylidene fluoride, polyimide, polyamideimide, aramid, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, carboxymethyl cellulose, etc. can be mentioned. As the synthetic rubber, for example, styrene butadiene rubber, fluorine rubber, ethylene propylene diene, etc. can be mentioned.

[0081] Examples of the negative electrode conductive assistant include fine carbon particles, carbon black, acetylene black, graphite, Ketjen black, carbon nanotubes, and carbon nanofibers, and any one or more of these can be used.

[0082] The negative electrode active material layer is formed, for example, by a coating method in which a silicon-based negative electrode active material, a binder, and the like are mixed with a negative electrode conductive assistant and a carbon-based active material as necessary, and then the mixture is dispersed in an organic solvent, water, or the like and coated.

[0083] [Separator] The separator separates the lithium metal or the positive electrode from the negative electrode, prevents current short circuit caused by contact between the two electrodes, and allows lithium ions to pass through. The separator is formed of a porous film made of, for example, synthetic resin or ceramic, and may have a laminated structure in which two or more types of porous films are laminated. Examples of synthetic resins include polytetrafluoroethylene, polypropylene, and polyethylene. EXAMPLES

[0084] The present invention will be described in more detail below by showing examples and comparative examples of the present invention, but the present invention is not limited to these examples.

[0085] <Common features between the Examples and Comparative Examples> [HOMO and LUMO energy levels] After structural optimization of the silane compound, the HOMO and LUMO energy levels were calculated. Gaussian 16 was used as the quantum chemical calculation software. The calculation was performed using density functional theory with B3LYP as the exchange-correlation functional and 6-311+G(d,p) as the basis set.

[0086] [Example 1] [Preparation of negative electrode] An electrolytic copper foil having a thickness of 15 μm was used as a negative electrode current collector. This electrolytic copper foil contained carbon and sulfur at concentrations of 70 ppm by mass each.

[0087] As the silicon-based negative electrode active material, KSC-7130 (silicon oxide particles containing Li2SiO3 and coated with a carbon layer, median diameter 6.5 μm, manufactured by Shin-Etsu Chemical Co., Ltd., see Journal of Power Sources 450 (2020) 227699) and artificial graphite (median diameter 15 μm) were used. As the negative electrode conductive assistant, carbon nanotubes and carbon microparticles with a median diameter of approximately 50 nm were used. As the negative electrode binder, sodium polyacrylate and carboxymethyl cellulose were mixed in a dry mass ratio of 9.3:83.7:1:1:4:1, respectively, and then diluted with pure water to prepare a negative electrode mixture slurry.

[0088] The negative electrode mixture slurry was applied to the negative electrode current collector and dried in a vacuum atmosphere at 100° C. for 1 hour. After drying, the deposition amount (area density) of the negative electrode active material layer per unit area on one surface of the negative electrode was 7.0 mg / cm 2 It was.

[0089] [Preparation of positive electrode] Next, the positive electrode was created. The positive electrode active material was a lithium nickel cobalt composite oxide (LiNi 0.7 Co 0.25 Al 0.05 A positive electrode mixture was prepared by mixing 95 parts by mass of O, 2.5 parts by mass of a positive electrode conductive assistant, and 2.5 parts by mass of a positive electrode binder (polyvinylidene fluoride: PVDF). The positive electrode mixture was then dispersed in an organic solvent (N-methyl-2-pyrrolidone: NMP) to form a paste-like slurry. The slurry was then applied to both sides of a positive electrode current collector using a coating device with a die head, and dried using a hot air drying device. At this time, a positive electrode current collector with a thickness of 15 μm was used. Finally, compression molding was performed using a roll press. The positive electrode density at this time was 20 mg / cm on one side. 2 It was decided.

[0090] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed as a non-aqueous solvent, and lithium hexafluorophosphate (LiPF6) was dissolved as an electrolyte salt to prepare an electrolyte solution. In this case, the solvent composition was EC:DMC=30:70 in volume ratio, and the content of the electrolyte salt was 1 mol / kg relative to the solvent. As an additive, 2.0 mass% of di(2-pyridyl)divinylsilane (PDVS) was added to prepare a non-aqueous electrolyte. The structural formula of PDVS is shown in Table 1.

[0091] [Preparation of non-aqueous electrolyte secondary battery] Next, a battery was assembled as follows. The battery was designed so that the negative electrode utilization rate was 95%. The utilization rate can be calculated using the following formula. Utilization rate = (positive electrode capacity - negative electrode loss) / (negative electrode capacity - negative electrode loss) x 100

[0092] [Nail penetration safety test] First, to stabilize the battery, two cycles of charging and discharging were performed at 0.2 C in an atmosphere of 25 °C, and then the 1st, 100th, 300th, and 500th cycles were charged and discharged at 0.7 C and 0.5 C. At this time, the charging voltage was 4.3 V, the discharge cut-off voltage was 2.5 V, and the charge cut-off rate was 0.07 C.

[0093] After 1, 100, 300, and 500 cycles, the batteries were fully charged and a nail with a diameter of 2 mm was pierced at a speed of 0.1 mm / sec to check the heat generation and ignition behavior. Safety was evaluated according to the following criteria: ◎: No ignition or heat generation ○: No ignition △: Ignition ×: Violent ignition

[0094] [Examples 2 to 5] The same procedure as in Example 1 was carried out except that the type of additive (silane compound) was changed as shown in Tables 1 and 2. In addition, FDVS is di(2-furyl)divinylsilane, TDVS is di(2-thienyl)divinylsilane, PTVS is 2-pyridyl-trivinylsilane, and PDES is diethynyldi(2-pyridyl)silane. All of these correspond to the general formula (1).

[0095] [Comparative Example 1] The same procedure as in Example 1 was carried out, except that no additive (silane compound) was added.

[0096] [Table 1]

[0097] [Table 2]

[0098] As is clear from the above results, it was confirmed that the safety is maintained even if the cycle is repeated by adding the silane compound containing the heteroaryl group represented by the above general formula (1) to the non-aqueous electrolyte of the present invention. The decomposition products (coatings) of these silane compounds can suppress the reactivity of the active material surface with the electrolyte.

[0099] The silane compound contained in the nonaqueous electrolyte of the present invention tends to have a higher HOMO and a lower LUMO than vinylene carbonate (HOMO: -7.3881 eV, LUMO: -0.6123 eV), which is known as a typical additive, and it has been suggested that the silane compound has high decomposition property and high reactivity after decomposition and is likely to form a high-quality coating (SEI film). [Industrial Applicability]

[0100] According to the present invention, a non-aqueous electrolyte that is highly safe after charging and discharging can be provided.

[0101] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A non-aqueous electrolyte for use in a non-aqueous electrolyte secondary battery, The non-aqueous electrolyte is characterized in that it contains a silane compound represented by the following general formula (1): Si(R 1 ) l (R 2 ) m (R 3 ) 4-l-m (1) (In the formula, R 1 is a heteroaryl group having 4 to 20 carbon atoms, R 2 is an alkenyl or alkynyl group having 2 to 20 carbon atoms, R 3 is an alkyl group having 1 to 20 carbon atoms. In addition, l and m each independently represent an integer of 1 to 3, and are integers satisfying 2≦l+m≦4.

2. 2. The non-aqueous electrolyte according to claim 1, wherein the energy level of the lowest unoccupied molecular orbital of the silane compound is −0.40 eV or less.

3. 3. The non-aqueous electrolyte according to claim 1, wherein the energy level of the highest occupied molecular orbital of the silane compound is −8.8 eV or higher.

4. 4. The non-aqueous electrolyte according to claim 1, wherein the content of the silane compound in the non-aqueous electrolyte is 0.1% by mass to 5.0% by mass.

5. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and the non-aqueous electrolyte according to any one of claims 1 to 4.

6. 6. The non-aqueous electrolyte secondary battery according to claim 5, wherein the negative electrode active material particles in the negative electrode are silicon oxide particles covered with a carbon layer.

7. The silicon oxide particles are Li 2 SiO 3 The Li 2 SiO 37. The nonaqueous electrolyte secondary battery according to claim 6, wherein the electrolyte is crystalline.

Citation Information

Patent Citations

  • Non-aqueous electrolyte and battery containing non-aqueous electrolyte

    CN110400969A

  • Lithium secondary battery

    JP1988102173A

  • Nonaqueous electrolyte battery

    JP1992087156A

  • Nonaqueous electrolyte battery

    JP1993074486A

  • Electrolyte and battery

    JP2006134719A