Synthesis process of semi-aromatic polyethers
A novel synthesis process for semi-aromatic polyethers using aliphatic diols and dihalogenated aromatic compounds at moderate temperatures addresses inefficiencies in existing methods, achieving high molecular weight polymers efficiently and cost-effectively.
Patent Information
- Application Number
- JP2021557213
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-05
- Filing Date
- 2020-04-03
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-04-03
AI Technical Summary
Existing methods for synthesizing polyether sulfones require high temperatures, long reaction times, or the use of expensive and potentially harmful monomers, leading to inefficiencies in productivity and profitability.
A process involving aliphatic diols, dihalogenated aromatic compounds, and hindered strong bases at moderate temperatures (30°C to 120°C) to produce semi-aromatic polyethers with high molecular weights, avoiding the need for high temperatures and expensive monomers.
The process achieves high number average molecular weights of over 5,000 g/mol, reduces reaction time to 12 hours or less, and uses non-toxic solvents, resulting in color-free polymers with improved hydrophilicity and suitability for film production.
Smart Images

Figure 0007566771000001 
Figure 0007566771000002 
Figure 0007566771000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of polymers and to a method for the synthesis of semi-aromatic polyethers based on aliphatic diols, the semi-aromatic polyethers based on aliphatic diols obtainable by the method, and the use of the semi-aromatic polyethers based on aliphatic diols for the production of membranes, manufactured parts and coatings.
[0002] Prior Art Aromatic polyethers, such as polyethersulfones, polyetherketones, and polyetherbenzonitriles, obtained by aromatic nucleophilic substitution, are recognized as high-performance polymers due to their excellent thermal stability and mechanical properties. The main application of these polymers is in liquid and gas phase separation membranes. Commercially available polyethersulfones are synthesized from aromatic diols, such as bisphenol A or 4,4'-dihydroxyphenyl, and dichlorodiphenylsulfone, among others. Therefore, manufacturers have been paying attention to partially or completely replacing aromatic diols, such as bisphenol A, which is known to be an endocrine disruptor, with aliphatic diols.
[0003] Isohexides, or 1,4:3,6-dianhydrohexitols, are rigid bicyclic chiral diols derived from sugars. In particular, isosorbide is obtained from the double dehydration of sorbitol, which is derived from the hydrogenation of glucose. Isohexides are intermediates of choice in the synthesis of many compounds with applications in various fields, such as the plastics industry, and therefore have replaced their petrochemically derived counterparts.
[0004] Thus, Kricheldorf et al. were the first to describe the preparation and characterization of isosorbide-containing polyethersulfones from silylated isosorbide and difluorodiphenyl sulfone (H. Kricheldorf et al., J. Polymer Sci., Part A: Polym. Chem, 1995, 33, 2667-2671).
[0005] Because silylated isosorbide is expensive, Kricheldorf and Chatti modified their polymerization conditions to describe the synthesis of isosorbide-containing polyethersulfone from non-functionalized isosorbide and difluorodiphenyl sulfone in the presence of potassium carbonate (S. Chatti et al., High Perform. Polym., 2009, 21, 105-118).
[0006] International Patent Application No. 2013 / 023997A1 describes a process for the preparation of aromatic polyetherketones based on isosorbide, which involves the reaction between 4,4'-difluorobenzophenone and isosorbide in the presence of potassium carbonate at a temperature of 210°C.
[0007] International Patent Application No. 2014 / 072473A2 describes a process for the preparation of aromatic polyethersulfones based on isosorbide, which comprises the reaction of isosorbide with difluorodiphenylsulfone or dichlorodiphenylsulfone in the presence of potassium carbonate at a temperature of 210° C., and optionally with a fluorinating agent.
[0008] US Patent Application No. 2015 / 0129487A1 describes a method for preparing semi-aromatic polyethersulfones based on non-aromatic cyclic diols such as cyclohexanedimethanol, 1,5-cyclooctanediol, or tetramethylcyclobutanediol, which includes the reaction between 4,4'-difluorodiphenylsulfone and a non-aromatic cyclic diol in the presence of potassium carbonate at a minimum temperature of 160°C, and the reaction between 4,4'-dichlorodiphenylsulfone and a non-aromatic cyclic diol in the presence of potassium carbonate at a minimum temperature of 210-215°C.
[0009] In order to improve the hydrophilicity of polysulfone from the viewpoint of its application in membranes, some researchers have attempted copolymerization of polysulfone with PEG or PEO. The copolymerization is statistical in bisphenol A (HW Kim et al., Journal of Membrane Science, vol. 372, No. 1, p. 116-124, 2011), fluorene-9-bisphenol (KM Diederichsen et al., Macromolecules, vol. 50, No. 10, p. 3831-3840, 2017), hydroxyphenylfluorene (HJ Lee et al., Journal of Membrane Science, vol. 485, p. 10-16, 2015) or bisphenol AF (L. Jujie, X. He et al., J. Polym. Res, vol. 24, no. 1, p. 1, 2017). Generally, when dichlorodiphenyl sulfone is used at high temperatures, only oligomers are obtained (Mn=4,000-13,000 g / mol). When difluorodiphenyl sulfone is used under conventional conditions for polysulfone synthesis, polymers with higher molecular weights are obtained.
[0010] Block copolymerization by nucleophilic aromatic substitution between two blocks (L.H. Hancock et al., Biomaterials, vol.21, no.7, p.725-733, 2000) or transesterification between a polymer and a PEG oligomer in the presence of a strong base, NaH (L.Wang et al., Polymer Chemistry, vol.5, no.8, p.2836-2842, 2014.) has also been investigated. Summary of the Invention [Problem to be solved by the invention]
[0011] Therefore, because the reactivity of diols is low compared to bisphenols (e.g., bisphenol A), the prior art methods for preparing polyethersulfones based on diols and dichlorodiphenylsulfones require heating at high temperatures (210-215°C) in the presence of a weak base such as K2CO3, or the use of a strong base such as NaH, which allows for a more moderate temperature. However, strong bases are known to cause secondary hydrolysis reactions of dihalogenated diphenylsulfones (RN Johnson, AGFarnham, J. Polym. Sci. A-1 Polym. Chem., vol. 5, no. 9, p. 2415-2427, 1967).
[0012] technical issues These known solutions have the drawback of requiring either difluorodiphenylsulfone, a reactive but expensive monomer, or dichlorodiphenylsulfone, which has high reaction temperatures and long reaction times, which are disadvantageous from an industrial point of view in terms of productivity, profitability and energy savings.
[0013] Therefore, there is a need for a method for preparing semi-aromatic polyethers based on aliphatic diols that does not require expensive monomers, high temperatures, or long reaction times, and that results in polymers with high number average molecular weights.
[0014] The present invention improves the situation in that aromatic nucleophilic substitution based on aliphatic diols allows for the access to semi-aromatic polyethers with high number average molecular weights without the need for prolonged heating at high temperatures.
[0015] The present invention relates to a process for the preparation of semi-aromatic polyethers based on aliphatic diols, comprising the following successive steps: a) preparing a mixture comprising an aliphatic diol or a mixture of aliphatic diols, a dihalogenated aromatic or heteroaromatic compound, and a hindered strong base in an organic solvent; and b) heating the mixture at a temperature between 30°C and 120°C for a period of time not exceeding 12 hours.
[0016] The invention also relates to semi-aromatic polyethers based on aliphatic diols of formula I obtainable by the process.
[0017] [ka] During the ceremony, Ar is derived from a dihalogenated aromatic or heteroaromatic compound; R is derived from an aliphatic diol, X is a halogen; n is an integer from 2 to 100, and n is determined by size exclusion chromatography.
[0018] The present invention also relates to the use of the semi-aromatic polyethers of the invention for the production of membranes, manufactured parts, and coatings.
[0019] The features disclosed in the following paragraphs may be implemented optionally. They may be implemented independently of one another or in combination with one another.
[0020] In one embodiment, the aliphatic diol used in step a) of the process of the present invention is selected from linear aliphatic diols, branched aliphatic diols, and cyclic aliphatic diols.
[0021] In one embodiment the aliphatic diol used in step a) of the process of the present invention is a branched aliphatic diol.
[0022] In one embodiment the aliphatic diol used in step a) of the process of the present invention is a cycloaliphatic diol.
[0023] In one embodiment the linear diol used in step a) of the process of the present invention is a linear aliphatic diol.
[0024] In one embodiment, the aliphatic diol used in step a) of the process of the present invention is selected from 1,4:3,6-dianhydrohexitols.
[0025] In one embodiment, the 1,4:3,6-dianhydrohexitol used in step a) of the process of the invention is isosorbide.
[0026] In one embodiment, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is selected from dihalogenated aromatic sulfones, dihalogenated aromatic ketones, dihalogenated benzonitriles, dihalogenated diazenes, bis(halophenyl)oxadiazoles, dihalogenated nitrobenzenes, dihalogenated benzoylnaphthalenes, and dihalogenated pyridines.
[0027] In one embodiment, the hindered strong base used in step a) of the process of the present invention is selected from potassium tert-butylate, sodium tert-butylate, lithium tert-butylate, potassium tert-pentylate, sodium tert-pentylate, potassium trimethylsilanolate, sodium trimethylsilanolate, lithium trimethylsilanolate, potassium tetramethylpiperidide, lithium tetramethylpiperidide, potassium bis(trimethylsilyl)amide, and lithium bis(trimethylsilyl)amide.
[0028] In one embodiment, the molar ratio of hindered strong base to aliphatic diol is 1-3.
[0029] In one embodiment, the organic solvent used in step a) of the process of the invention is a polar aprotic solvent or a mixture of polar aprotic solvents.
[0030] In one embodiment, the molar ratio of the aliphatic diol to the dihalogenated aromatic compound is from 0.5 to 1.5.
[0031] In one embodiment, the aliphatic diol-based semi-aromatic polyether of the present invention is characterized in that R is derived from an aliphatic diol selected from linear aliphatic diols and branched aliphatic diols.
[0032] In one embodiment, the aliphatic diol-based semi-aromatic polyethers of the present invention are characterized in that R is derived from 1,4:3,6-dianhydrohexitol.
[0033] In one embodiment, the semi-aromatic polyethers based on aliphatic diols according to the invention are characterized in that they have a polydispersity index of 1.5-5.
[0034] In one embodiment, the aliphatic diol-based semi-aromatic polyethers of the present invention are characterized in that they have a number average molecular weight of 5,000 g / mol or more, as measured by size exclusion chromatography in dimethylformamide at 70° C., a flow rate of 0.7 mL / min, and a polystyrene calibration.
[0035] In one embodiment, the aliphatic diol-based semi-aromatic polyethers of the present invention are characterized by having a glass transition temperature greater than 100°C.
[0036] In one embodiment, the aliphatic diol-based semi-aromatic polyether of formula I is characterized in that X is chlorine.
[0037] In one embodiment, the aliphatic diol-based semi-aromatic polyethers of formula I are characterized by containing a residual fluorine content of less than 100 ppm.
[0038] In one embodiment, the aliphatic diol-based semi-aromatic polyether of formula I is characterized by having a residual silicon content of 10 to 1,000 ppm.
[0039] In one embodiment, the aliphatic diol-based semi-aromatic polyether of formula I is characterized in that it contains a residual chlorine content of 100 to 10,000 ppm.
[0040] technical solution DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention and its variations generally provide a method for preparing semi-aromatic polyethers based on aliphatic diols.
[0041] Surprisingly and unexpectedly, applicants have shown that it is possible to synthesize semi-aromatic polyethers from aliphatic diols, particularly secondary aliphatic diols, and dihalogenated aromatic or heteroaromatic compounds in the presence of a hindered strong base at temperatures of up to 120° C. for periods of up to 12 hours.
[0042] Effect of the Invention Such a solution makes it possible to solve the problems caused by known solutions and to obtain semi-aromatic polyethers based on aliphatic diols without heating to high temperatures, having high number average molecular weights, i.e. more than 5,000 g / mol, preferably more than 6,000 g / mol, more preferably more than 7,000 g / mol, the number average molecular weight being measured by size exclusion chromatography in dimethylformamide at 70° C., a flow rate of 0.7 mL / min, and with polystyrene calibration.
[0043] Furthermore, the process described by the applicant has the advantage that it uses non-toxic solvents, is faster than conventional processes and gives a colorless polymer.
[0044] Other features, details and advantages of the invention will become apparent on reading the following detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] The present invention relates to a process for the preparation of semi-aromatic polyethers based on aliphatic diols, comprising the following successive steps: a) preparing an aliphatic diol or a mixture of aliphatic diols, preferably a mixture comprising an aliphatic diol, a dihalogenated aromatic or heteroaromatic compound, and a hindered strong base in an organic solvent; and b) heating the mixture at a temperature of 30°C to 120°C, preferably at a temperature of 35°C to 110°C, more preferably at a temperature of about 40°C to about 100°C, for a time period of 12 hours or less, preferably 11 hours or less, more preferably 10 hours or less.
[0046] By "semi-aromatic polyether" is meant, for purposes of the present invention, a polyether type polymer formed from two monomers, one of which is aromatic or heteroaromatic and the other of which is non-aromatic.
[0047] Thus, the first step of the process of the present invention consists of preparing an aliphatic diol or a mixture of aliphatic diols, preferably a mixture comprising an aliphatic diol, a dihalogenated aromatic compound and a hindered strong base in an organic solvent.
[0048] By "aliphatic diol" is meant, for the purposes of the present invention, a non-aromatic organic compound having two hydroxyl functional groups. The aliphatic diol may be linear, branched, or cyclic. For the purposes of the present invention, "linear aliphatic diol" and "branched aliphatic diol" do not have a ring structure. For the purposes of the present invention, "cycloaliphatic diol" has one or more ring structures. Preferably, the aliphatic diol is a branched aliphatic diol or a cycloaliphatic diol. Even more preferably, the aliphatic diol is a branched aliphatic diol. The aliphatic diol may contain, in addition to the oxygen atoms of the two hydroxyl groups, one or more heteroatoms, such as oxygen, nitrogen, and sulfur atoms. The aliphatic diol is used in the present invention as a monomer to form the semi-aromatic polyether. Examples of linear aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, and / or 1,10-decanediol. Examples of branched aliphatic diols include 2-methyl-1,3-propanediol, 2,2-dimethylpropane-1,3-diol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-2-butyl-1,3-propanediol, and / or propylene glycol. Examples of cyclic aliphatic diols include cyclohexanedimethanol, tetramethylcyclohexanedimethanol, hydrogenated bisphenol, 1,5-cyclooctanediol, 1,4:3,6-dianhydrohexitol, spiroglycol, adamantanediol, and / or tricyclododecane dimethanol.
[0049] By "1,4:3,6-dianhydrohexitol" is meant for the purposes of the present invention heterocyclic compounds obtained by double dehydration of hexitols such as mannitol, sorbitol and iditol. 1,4:3,6-dianhydrohexitols are mainly in the stereoisomeric form of isomannide, isosorbide and isoidide. 1,4:3,6-dianhydrohexitols are used in the present invention as monomers for forming semi-aromatic polyethers. Preferably, the 1,4:3,6-dianhydrohexitol used in step a) of the process of the present invention is isosorbide.
[0050] "Dihalogenated aromatic compounds" for the purposes of the present invention means compounds having at least one aromatic ring, preferably two aromatic rings, two halogen atoms and an electron-withdrawing functional group. The halogen atoms are selected from bromine, iodine, chlorine or fluorine, preferably chlorine and fluorine, more preferably the halogen atoms are chlorine atoms. Advantageously, the two halogen atoms are the same. Dihalogenated aromatic compounds are used in the present invention as monomers to form semi-aromatic polyethers.
[0051] The term "dihalogenated heteroaromatic compound" for the purposes of the present invention means a compound having at least one heteroaromatic ring and two halogen atoms. The halogen atoms are selected from bromine, iodine, chlorine or fluorine, preferably chlorine and fluorine, more preferably the halogen atoms are chlorine atoms. Advantageously, the two halogen atoms are the same. The dihalogenated heteroaromatic compound is used in the present invention as a monomer for forming a semi-aromatic polyether.
[0052] The dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is advantageously selected from dihalogenated aromatic sulfones, dihalogenated aromatic ketones, dihalogenated benzonitriles, dihalogenated diazenes, bis(halophenyl)oxadiazoles, dihalogenated nitrobenzenes, dihalogenated benzoylnaphthalenes, and dihalogenated pyridines.Preferably, the dihalogenated aromatic or heteroaromatic compound is selected from dihalogenated diphenyl sulfones, dihalogenated diphenyl ketones, dihalogenated benzonitriles, and dihalogenated pyridines.More preferably, the dihalogenated aromatic or heteroaromatic compound is selected from dichlorodiphenyl sulfones, dichlorodiphenyl ketones, dichlorobenzonitriles, and dichloropyridines.More preferably, the dihalogenated aromatic or heteroaromatic compound is selected from 4,4'-dichlorodiphenyl sulfone, 4,4'-dichlorobenzophenone, 2,6-dichlorobenzonitrile, and 2,6-dichloropyridine. Even more preferably, the dihalogenated aromatic or heteroaromatic compound is selected from 4,4'-dichlorodiphenylsulfone, 2,6-dichlorobenzonitrile, and 2,6-dichloropyridine.
[0053] The term "hindered strong base" for the purposes of the present invention means a base having a large bulky atomic group, such as a branched aliphatic group. Preferably, the hindered strong base is selected from potassium tert-butylate, sodium tert-butylate, lithium tert-butylate, potassium tert-pentylate, sodium tert-pentylate, potassium trimethylsilanolate, sodium trimethylsilanolate, lithium trimethylsilanolate, potassium tetramethylpiperidide, lithium tetramethylpiperidide, potassium bis(trimethylsilyl)amide, and lithium bis(trimethylsilyl)amide. Even more preferably, the hindered strong base used in step a) of the process of the present invention is potassium trimethylsilanolate.
[0054] Indeed, without being bound by any theory, the inventors believe that the use of a hindered strong base at a temperature of 120° C. or less limits side reactions that may occur when using an unhindered strong base, and therefore produces polymers with high number average molecular weights, i.e., greater than 5,000 g / mole, preferably greater than 6,000 g / mole, and even more preferably greater than 7,000 g / mole, as measured by size exclusion chromatography in dimethylformamide at 70° C., at a flow rate of 0.7 mL / min, and using a polystyrene calibration.
[0055] Advantageously, the proportion of the hindered strong base in the mixture is between 1 and 3 molar equivalents relative to the amount of aliphatic diol. The molar ratio of hindered strong base / aliphatic diol is therefore between 1 and 3. Preferably, the molar ratio of hindered strong base / aliphatic diol is about 2.
[0056] The organic solvent used in step a) of the process of the invention is advantageously chosen from polar aprotic solvents.
[0057] The term "polar aprotic solvent" means for the purposes of the present invention a solvent that has a dipole moment that has no acidic hydrogen atoms, ie, no hydrogen atoms bonded to heteroatoms.
[0058] Preferably, the solvent is selected from polar aprotic solvents containing at least one sulfur atom or at least one nitrogen atom.More preferably, the solvent is selected from dimethyl sulfoxide, diethyl sulfoxide, sulfolane, dimethyl sulfone, diethyl sulfone, diisopropyl sulfone, diphenyl sulfone, tetrahydrothiophene-1-monoxide, dimethylacetamide, N,N-dimethylformamide, fluorine methyl-5-(dimethylamino)-2-methyl-5-oxopentanoate, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, either alone or in mixture.More preferably, the solvent is dimethyl sulfoxide.
[0059] The aliphatic diol used in step a) of the process of the present invention is advantageously selected from linear aliphatic diols, branched aliphatic diols and cyclic aliphatic diols.Preferably, the aliphatic diol used in step a) of the process of the present invention is selected from branched aliphatic diols and cyclic aliphatic diols.Even more preferably, the aliphatic diol used in step a) of the process of the present invention is selected from branched aliphatic diols.
[0060] In one embodiment, the aliphatic diol used in step a) of the process of the present invention is a linear aliphatic diol.Preferably, the linear aliphatic diol used in step a) of the process of the present invention is selected from ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol and 1,10-decanediol, alone or in mixture.
[0061] In a preferred embodiment, the aliphatic diol used in step a) of the process of the present invention is a branched aliphatic diol.Preferably, the branched aliphatic diol used in step a) of the process of the present invention is selected from 2-methyl-1,3-propanediol, 2,2-dimethylpropane-1,3-diol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-2-butyl-1,3-propanediol, and propylene glycol, alone or in mixture.Even more preferably, the branched aliphatic diol used in step a) of the process of the present invention is 2,2-dimethylpropane-1,3-diol.
[0062] In a preferred embodiment, the aliphatic diol used in step a) of the process of the present invention is a cycloaliphatic diol.Preferably, the cycloaliphatic diol used in step a) of the process of the present invention is selected from cyclohexanedimethanol, tetramethylcyclohexanedimethanol, hydrogenated bisphenol, 1,5-cyclooctanediol, 1,4:3,6-dianhydrohexitol, spiroglycol, adamantanediol, and tricyclododecane dimethanol, either alone or in mixture.Even more preferably, the cycloaliphatic diol used in step a) of the process of the present invention is selected from 1,4:3,6-dianhydrohexitol.More preferably, the cycloaliphatic diol used in step a) of the process of the present invention is isosorbide.
[0063] The isosorbide used may be in solid form, in particular in the form of powder, granules or flakes, or in liquid form, in particular in molten form. Preferably, the isosorbide is present in solid form.
[0064] In another particularly preferred embodiment, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is a dichlorinated aromatic compound.Preferably, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is selected from dichlorinated aromatic sulfones, dichlorinated aromatic ketones, dichlorinated benzonitriles, and dichlorinated pyridines.Even more preferably, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is selected from dichlorodiphenyl sulfones, dichlorodiphenyl ketones, dichlorobenzonitriles, and dichloropyridines.More preferably, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is selected from 4,4'-dichlorodiphenyl sulfone, 4,4'-dichlorobenzophenone, 2,6-dichlorobenzonitrile, and 2,6-dichloropyridine.Even more preferably, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is selected from 4,4'-dichlorodiphenyl sulfone, 2,6-dichlorobenzonitrile, and 2,6-dichloropyridine.
[0065] Advantageously, the use of dichlorinated aromatic derivatives in the process of the present invention allows the production of semi-aromatic polyethers with number average molecular weights as high as those obtained with semi-aromatic polyethers prepared from difluorinated aromatic derivatives. The use of dichlorinated aromatic derivatives therefore has economic advantages, as they are often cheaper than the corresponding difluorinated aromatic derivatives.
[0066] Moreover, the process of the present invention unexpectedly allows for improved substitution rates when dichlorinated aromatic or heteroaromatic compounds are used in step a), in fact, in the prior art processes, difluorinated monomers are usually used to compensate for the low reactivity of aliphatic diols.
[0067] The nature of the halogenated derivative used can be identified by analysis of the polymer by combustion ion chromatography.
[0068] Advantageously, the molar ratio of dihalogenated aromatic or heteroaromatic compound / aliphatic diol in the mixture is between 0.5 and 1.5, preferably between 0.7 and 1.3, more preferably between 0.9 and 1.1. More preferably, the molar ratio of dihalogenated aromatic or heteroaromatic compound / aliphatic diol in the mixture is about 1.
[0069] Thus, the semi-aromatic polyether is formed by the reaction between an aliphatic diol as monomer and a dihalogenated aromatic or heteroaromatic compound. Advantageously, the total proportion of monomer, i.e. the sum of the amount of aliphatic diol and the amount of dihalogenated aromatic or heteroaromatic compound, is between 10% and 50% by weight, preferably between 20% and 40% by weight, based on the sum of the weight of the solvent and the weight of the monomer. Even more preferably, the proportion of monomer is about 30% by weight, based on the weight of the solvent and the weight of the monomer.
[0070] The second step of the process of the present invention comprises heating the mixture prepared in step a) to a temperature between 30° C. and 120° C. for a period of time not exceeding 12 hours. This heating step allows the reaction of the aliphatic diol with the dihalogenated aromatic or heteroaromatic compound to be initiated to form the semi-aromatic polyether.
[0071] The heating step is preferably carried out at a temperature of 35° C. to 110° C., more preferably 40° C. to 100° C., for a period of 11 hours or less, more preferably 10 hours or less.
[0072] Thus, the method of the present invention is particularly advantageous not only in terms of productivity since it is possible to obtain semi-aromatic polyethers in 12 hours or less, but also in terms of energy saving since it is not necessary to heat to temperatures exceeding 120°C.
[0073] In a particular embodiment, the heating step is initiated at a temperature of 30°C to 50°C, preferably 35°C to 45°C, and even more preferably about 40°C, and then the temperature is gradually increased to a temperature of 80°C to 120°C, preferably 90°C to 110°C, and even more preferably about 100°C.
[0074] It is to the merit of the present inventors that it has been shown that starting the heating step at a temperature between 30°C and 50°C and gradually increasing the temperature to a temperature between 80°C and 120°C can prevent decomposition of the dihalogenated aromatic or heteroaromatic compound, particularly when the dihalogenated aromatic or heteroaromatic compound is selected from dihalogenated aromatic sulfones, preferably dihalodiphenyl sulfones, even more preferably dichlorodiphenyl sulfones, and more preferably when the dihalogenated aromatic or heteroaromatic compound is 4,4'-dichlorodiphenyl sulfone.
[0075] At the end of the heating step, the semi-aromatic polyether obtained can be recovered by techniques known to those skilled in the art, for example by precipitation of the semi-aromatic polyether. A preferred technique for precipitation of the semi-aromatic polyether consists of adding the reaction medium to a large amount of water, about 10 times the volume of the reaction medium. The semi-aromatic polyether can then be dried according to techniques known to those skilled in the art, for example in an oven under reduced pressure.
[0076] Thus, the process of the invention makes it possible to obtain semi-aromatic polyethers based on aliphatic diols having physical properties that are particularly suitable for the production of films.
[0077] Another subject of the invention therefore relates to semi-aromatic polyethers based on aliphatic diols obtainable by the process of the invention, characterized in that they correspond to formula I:
[0078] [ka] During the ceremony, Ar is derived from a dihalogenated aromatic or heteroaromatic compound; R is derived from an aliphatic diol, X is a halogen; n is an integer from 2 to 100, and n is determined by size exclusion chromatography.
[0079] The polydispersity index of the semi-aromatic polyethers based on aliphatic diols of the present invention can be determined by techniques known to those skilled in the art, in particular by size exclusion chromatography using polystyrene calibration, for example at a flow rate of 0.7 mL / min in dimethylformamide at 70° C. The semi-aromatic polyethers based on aliphatic diols of the present invention have a polydispersity index of 1.5 to 5, preferably 2 to 4.5.
[0080] The number average molecular weight of the semi-aromatic polyethers based on aliphatic diols of the present invention can be determined by techniques known to the skilled person, specifically, for example, by size exclusion chromatography in dimethylformamide at 70° C., at a flow rate of 0.7 mL / min, with polystyrene calibration. Advantageously, the semi-aromatic polyethers based on aliphatic diols of the present invention have a number average molecular weight of 5,000 g / mol or more, preferably 6,000 g / mol or more, more preferably 7,000 g / mol or more. In one embodiment, the semi-aromatic polyethers based on aliphatic diols of the present invention have a number average molecular weight of 6,000 to 9,000 g / mol, preferably 6,500 to 9,000 g / mol, even more preferably 7,000 to 9,000 g / mol, where the number average molecular weight is measured by size exclusion chromatography in dimethylformamide at 70° C., at a flow rate of 0.7 mL / min, with polystyrene calibration.
[0081] The glass transition temperature of the semi-aromatic polyethers based on aliphatic diols according to the invention can be determined by techniques known to those skilled in the art, in particular by differential scanning calorimetry (DSC) in a perforated aluminum crucible at a flow rate of 80 mL / min in nitrogen at 10° C. / min or 20° C. / min, preferably at 10° C. / min from 20° C. to 300° C. The semi-aromatic polyethers according to the invention have a glass transition temperature above 100° C., preferably above 120° C., even more preferably above 140° C.
[0082] When the aliphatic diol is isosorbide, the glass transition temperature of the aliphatic diol-based semi-aromatic polyether of the present invention is above 140°C, preferably 140°C to 260°C, and even more preferably 150°C to 250°C.
[0083] In one embodiment, the aliphatic diol-based semi-aromatic polyethers of the present invention are semi-crystalline. By "semi-crystalline polymer" is meant a polymer having crystalline and amorphous regions.
[0084] The contact angle of the semi-aromatic polyethers of the present invention can be determined by techniques known to those skilled in the art, in particular by goniometric measurements using a goniometer. The semi-aromatic polyethers obtained by the process of the present invention have a contact angle with water of 50° to 70°, preferably about 63°.
[0085] In the preferred semi-aromatic polyethers based on aliphatic diols of formula I, Ar, R, X and n are defined as follows: Ar is derived from a dihalogenated aromatic sulfone, a dihalogenated aromatic ketone, a dihalogenated benzonitrile, or a dihalogenated pyridine, preferably Ar is derived from a dihalogenated diphenyl sulfone, a dihalogenated diphenyl ketone, a dihalogenated benzonitrile, or a dihalogenated pyridine, more preferably Ar is derived from a dichlorodiphenyl sulfone, a dichlorodiphenyl ketone, a dichlorobenzonitrile, or a dichloropyridine, more preferably Ar is selected from the following:
[0086] [ka]
[0087] [ka]
[0088] [ka]
[0089] [ka] Even more preferably, Ar is selected from:
[0090] [ka]
[0091] [ka]
[0092] [ka] R is derived from an aliphatic diol, preferably R is derived from an aliphatic diol selected from linear aliphatic diols, branched aliphatic diols, and cyclic aliphatic diols, and even more preferably R is derived from an aliphatic diol selected from linear aliphatic diols and branched aliphatic diols; X is a halogen, preferably X is selected from F and Cl, more preferably X is Cl; n is an integer from 2 to 100, preferably n is an integer from 10 to 100, where n is determined by size exclusion chromatography, preferably in dimethylformamide at 70° C., at a flow rate of 0.7 mL / min, using polystyrene calibration.
[0093] In one embodiment, the aliphatic diol-based semi-aromatic polyether is defined by formula I, except that when Ar is derived from a 4,4'-halodiphenylsulfone, R is not derived from isosorbide, cyclohexanedimethanol, tetramethylcyclobutanediol, or cis-1,5-cyclooctanediol, and when Ar is derived from a 4,4'-dihalobenzophenone, R is not derived from isosorbide.
[0094] In one embodiment, the aliphatic diol used in step a) of the process of the present invention is a linear aliphatic diol, in which case R is derived from a linear aliphatic diol and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula Ia.
[0095] [ka] During the ceremony, X, Ar and n are as defined in formula I; L is derived from a linear aliphatic diol, preferably L is derived from a linear aliphatic diol selected from ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8 octanediol, and 1,10-decanediol.
[0096] In one embodiment, the aliphatic diol used in step a) of the process of the present invention is a branched aliphatic diol, in which case R is derived from the branched aliphatic diol and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula Ib.
[0097] [ka] During the ceremony, X, Ar and n are as defined in formula I; B is derived from a branched aliphatic diol, preferably B is derived from a branched aliphatic diol selected from 2-methyl-1,3-propanediol, 2,2-dimethylpropane-1,3-diol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-2-butyl-1,3-propanediol and propylene glycol, more preferably B is derived from 2,2-dimethylpropane-1,3-diol.
[0098] In a preferred variant of this embodiment, the aliphatic diol used in step a) of the process of the invention is 2,2-dimethylpropane-1,3-diol, in which case B is derived from 2,2-dimethylpropane-1,3-diol and the aliphatic diol-based semi-aromatic polyether of the invention is of formula Ib-i.
[0099] [ka] wherein X and Ar are as defined in formula Ib.
[0100] In a preferred embodiment, the aliphatic diol used in step a) of the process of the present invention is a cycloaliphatic diol, in which case R is derived from a cycloaliphatic diol and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula Ic:
[0101] [ka] During the ceremony, X, Ar and n are as defined in formula I; Cy is derived from a cycloaliphatic diol, preferably Cy is derived from a cycloaliphatic diol selected from cyclohexanedimethanol, tetramethylcyclohexanedimethanol, hydrogenated bisphenol, 1,5-cyclooctanediol, 1,4:3,6-dianhydrohexitol, spiroglycol, adamantanediol, and tricyclododecane dimethanol, still more preferably Cy is derived from a cycloaliphatic diol selected from 1,4:3,6-dianhydrohexitol, and even more preferably Cy is derived from isosorbide.
[0102] In a preferred embodiment variant, the cycloaliphatic diol used in step a) of the process of the invention is 1,4:3,6-dianhydrohexitol, in which case Cy is derived from 1,4:3,6-dianhydrohexitol and the semi-aromatic polyether based on an aliphatic diol of the invention is of formula Ic-i.
[0103] [ka] wherein Ar, X, and n are as defined in formula I.
[0104] In an even more preferred variant of this embodiment, the cycloaliphatic diol used in step a) of the process of the invention is isosorbide, in which case Cy is derived from isosorbide and the aliphatic diol-based semi-aromatic polyether of the invention is of formula Ic-ii.
[0105] [ka] wherein Ar, X, and n are as defined in formula I.
[0106] In another preferred embodiment, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is 4,4'-dichlorodiphenylsulfone, in which case Ar is derived from 4,4'-dichlorodiphenylsulfone and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula II:
[0107] [ka] where n and R are as defined in formula I.
[0108] In a variant of this embodiment, the aliphatic diol used in step a) of the process of the invention is a linear aliphatic diol, in which case R is derived from a linear aliphatic diol and the aliphatic diol-based semi-aromatic polyether of the invention is of formula IIa.
[0109] [ka] wherein n and L are as defined in formula Ia.
[0110] In another variation of this embodiment, the aliphatic diol used in step a) of the process of the invention is a branched aliphatic diol, in which case R is derived from the branched aliphatic diol and the aliphatic diol-based semi-aromatic polyether of the invention is of formula IIb:
[0111] [ka] wherein n and B are as defined in formula Ib.
[0112] Preferably, the branched aliphatic diol used in step a) of the process of the invention is 2,2-dimethylpropane-1,3-diol, in which case B is derived from 2,2-dimethylpropane-1,3-diol and the semi-aromatic polyether based on an aliphatic diol of the invention is of formula IIb-i.
[0113] [ka] wherein n is as defined in formula Ib.
[0114] In another variation of this embodiment, the aliphatic diol used in step a) of the process of the invention is a cycloaliphatic diol, in which case R is derived from a cycloaliphatic diol and the aliphatic diol-based semi-aromatic polyether of the invention is of formula IIc:
[0115] [ka] wherein n and Cy are as defined in formula Ic.
[0116] Preferably, the cycloaliphatic diol used in step a) of the process of the invention is 1,4:3,6-dianhydrohexitol, in which case Cy is derived from 1,4:3,6-dianhydrohexitol and the semi-aromatic polyether based on an aliphatic diol of the invention is of formula IIc-i.
[0117] [ka] wherein n is as defined in formula Ic.
[0118] Even more preferably, the cycloaliphatic diol used in step a) of the process of the present invention is isosorbide, in which case Cy is derived from isosorbide and the semi-aromatic polyether based on an aliphatic diol of the present invention is of formula IIc-ii.
[0119] [ka] wherein n is as defined in formula Ic.
[0120] In another preferred embodiment, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is 2,6-dichlorobenzonitrile, in which case Ar is derived from 2,6-dichlorobenzonitrile and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula III.
[0121] [ka] where n and R are as defined in formula I.
[0122] In another variation of this embodiment, the aliphatic diol used in step a) of the process of the invention is a cycloaliphatic diol, in which case R is derived from a cycloaliphatic diol and the aliphatic diol-based semi-aromatic polyether of the invention is of formula IIIa:
[0123] [ka] wherein n and Cy are as defined in formula Ic.
[0124] Preferably, the cycloaliphatic diol used in step a) of the process of the invention is 1,4:3,6-dianhydrohexitol, in which case Cy is derived from 1,4:3,6-dianhydrohexitol and the aliphatic diol-based semi-aromatic polyether of the invention is of formula IIIa-i:
[0125] [ka] wherein n is as defined in formula Ic.
[0126] Even more preferably, the cycloaliphatic diol used in step a) of the process of the present invention is isosorbide, in which case Cy is derived from isosorbide and the semi-aromatic polyether based on an aliphatic diol of the present invention is of formula IIIa-ii.
[0127] [ka] wherein n is as defined in formula Ic.
[0128] In another preferred embodiment, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is 2,6-dichloropyridine, in which case Ar is derived from 2,6-dichloropyridine and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula IV.
[0129] [ka] where n and R are as defined in formula I.
[0130] In another variation of this embodiment, the aliphatic diol used in step a) of the process of the present invention is a cycloaliphatic diol, in which case R is derived from a cycloaliphatic diol and the aliphatic diol-based semi-aromatic polyether of the present invention is of formula IVa.
[0131] [ka] wherein n and Cy are as defined in formula Ic.
[0132] Preferably, the cycloaliphatic diol used in step a) of the process of the invention is 1,4:3,6-dianhydrohexitol, in which case Cy is derived from 1,4:3,6-dianhydrohexitol and the semi-aromatic polyether based on an aliphatic diol of the invention is of formula IVa-i.
[0133] [ka] wherein n is as defined in formula Ic.
[0134] Even more preferably, the cycloaliphatic diol used in step a) of the process of the present invention is isosorbide, in which case Cy is derived from isosorbide and the semi-aromatic polyether based on an aliphatic diol of the present invention is of formula IVa-ii.
[0135] [ka] wherein n is as defined in formula Ic.
[0136] In another embodiment, the dihalogenated aromatic or heteroaromatic compound used in step a) of the process of the present invention is a dichlorinated aromatic compound, in which case the aliphatic diol-based semi-aromatic polyether of the present invention is of formula I, where X is chlorine.
[0137] According to this embodiment, the aliphatic diol-based semi-aromatic polyethers of the present invention have a residual fluorine content of less than 100 ppm, as determined by combustion-ion chromatography.
[0138] According to this embodiment, the aliphatic diol-based semi-aromatic polyether of the present invention also has a residual silicon content of 10-1000 ppm, which is determined by combustion-ion chromatography.
[0139] According to this embodiment, the aliphatic diol-based semi-aromatic polyether of the present invention has a residual chlorine content of 100-10,000 ppm, which is determined by combustion-ion chromatography.
[0140] Advantageously, the aliphatic diol-based semi-aromatic polyethers of the present invention have a solubility parameter that allows them to be soluble in solvents suitable for the production of films. Thus, the semi-aromatic polyether based on an aliphatic diol of the present invention, preferably the semi-aromatic polyether based on an aliphatic diol of formula IIc-ii, has a good solubility at room temperature (20-25° C.) at a concentration of 10 mg / mL in a solvent selected from formic acid, acetonitrile, acetic acid, dimethyl sulfoxide, acrylonitrile, epichlorohydrin, acetone, methyl acetate, N,N-dimethylformamide, 2-methoxyethanol, propylene carbonate, butan-2-one, 2-ethoxyethanol, dimethylethanolamine, pyridine, furfuryl alcohol, N-methyl-2-pyrrolidine, benzaldehyde, benzyl alcohol, isophorone, hydrazine, dimethylisosorbide, methyl 4-(dimethylcarbamoyl)-2-methylbutanoate, preferably dimethylsulfoxide, acrylonitrile, N,N-dimethylformamide, N-methyl-2-pyrrolidine, and methyl 4-(dimethylcarbamoyl)-2-methylbutanoate.
[0141] Another subject of the invention therefore relates to the use of the semi-aromatic polyethers based on aliphatic diols according to the invention for the production of membranes, manufactured parts and coatings.
[0142] Membranes can be prepared from the aliphatic diol-based semi-aromatic polyethers of the present invention according to techniques known to those skilled in the art.
[0143] In particular, the membranes obtained using the semi-aromatic polyethers based on aliphatic diols of the present invention have advantageous properties in terms of hydrophilicity and gas permeability. The membranes may be in the form of porous or non-porous films. The membranes may be produced in the form of monofilaments or hollow fibers.
[0144] The semi-aromatic polyethers based on aliphatic diols of the present invention can be used in aqueous media, including body fluids.The semi-aromatic polyethers based on aliphatic diols of the present invention are biocompatible and therefore can be used in the form of membranes, for example in the medical field, such as hemodialysis, or in the consumer field (food and beverage), wastewater treatment field.
[0145] The porous membranes in the form of tubes or hollow fibers can have various pore sizes known to those skilled in the art, depending on their application (microfiltration, ultrafiltration, nanofiltration, reverse osmosis). The performance of the membranes for water obtained with the semi-aromatic polyethers of the invention can be improved by techniques known to those skilled in the art, in particular by the use of sulfonated monomers or by post-treatment of the membranes by sulfonation or surface treatment to avoid fouling.
[0146] The membranes in the gas phase can be used to produce nitrogen by separating nitrogen mixtures, to produce oxygen from air, and to produce methane by separating methane and CO2. The performance of the gas membranes obtained with the semi-aromatic polyethers of the invention can be improved by techniques known to those skilled in the art, in particular by using hindered monomers or by adding additives such as substituted bisphenols, naphthalenes or fluorenes, or by forming pores using thermally unstable compounds.
[0147] The membrane in the form of a film or sheet can be used for optical or packaging purposes.
[0148] Molded parts can be produced from the semi-aromatic polyethers based on aliphatic diols of the invention according to techniques known to those skilled in the art. By injection molding the semi-aromatic polyethers based on aliphatic diols of the invention, parts can be produced that are used in the medical sector, in dental applications replacing metal, glass and other disposable or reusable instruments, and in the aviation, electronics and automotive sectors.
[0149] Another subject of the invention relates to the use of the semi-aromatic polyethers based on aliphatic diols according to the invention as coating resins for metals to prevent corrosion.
[0150] Coatings obtained from the semi-aromatic polyethers based on aliphatic diols of the present invention can be applied to metals used in the consumer sector (food and beverages), marine sector in ship hulls, aerospace, automotive, electrical sector in electrical equipment sector with cables and electronic equipment with circuits. The resins of the semi-aromatic polyethers based on aliphatic diols of the present invention can be applied to other substrates such as glass or carbon fiber to form composites by evaporating the solvent from the resin. Composites formed from the semi-aromatic polyether resins based on aliphatic diols of the present invention can be used in the aerospace and automotive fields to replace metal parts.
[0151] The invention will be understood more clearly on reading the following examples, which are intended to be purely illustrative and do not in any way limit the scope of protection. EXAMPLES
[0152] Abbreviation: DCBN: 2,6-dichlorobenzonitrile; DCDPS: 4,4'-dichlorodiphenyl sulfone; DCP: 2,6-dichloropyridine; DFBN: 2,6-difluorobenzonitrile; DFDPS: 4,4'-difluorodiphenyl sulfone; DFP: 2,6-difluoropyridine; DMAc: dimethylacetamide; DMF: N,N-dimethylformamide, DMSO: dimethyl sulfoxide; DSC: differential scanning calorimetry; PDI: polydispersity index, Mn: number average molecular weight, NMP: N-methyl-2-pyrrolidone, PS: polystyrene, SEC: size exclusion chromatography; Tm: melting point Tg: glass transition temperature, THF: tetrahydrofuran.
[0153] For the illustrative examples presented below, the following reagents were used: Isosorbide (purity >99.5%): Polysorb(R) LP (Roquette Freres) DCDPS (purity>99%): Alfa Aesar, SiOMe3K / THF(2M): Acros Organics, 2,2-Dimethylpropane-1,3-diol (>99%): Acros Organics, Bisphenol A (>99%): Sigma Aldrich; K2CO3 (>99%): Sigma Aldrich; DFDPS (>99%): Sigma Aldrich; DFP (>99%): Acros Organics, DCP (>98%): Acros Organics, DFBN (>99%): Acros Organics, DCBN (>90%): Fluka, purified by sublimation.
[0154] Example 1: Preparation of semi-aromatic polyethersulfone of the present invention based on isosorbide 1.46 g (0.01 mol, 1 eq.) of isosorbide (stored in a desiccator) and 2.87 g (0.01 mol, 1 eq.) of DCDPS are dissolved in 10.11 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The reaction medium is immersed in an oil bath and heated to 40 ° C to dissolve both monomers. 9.05 g (0.0199 mol, 1.99 eq.) of SiOMe3K dissolved in THF (2 M) are added. After the addition of the base, the temperature is gradually increased to 100 ° C for several hours and then the medium is left under stirring at 100 ° C for 2 hours. At that time, the medium becomes more viscous. The medium is then precipitated in 300 mL of distilled water and the product obtained is rinsed once with water and then once with a water / methanol mixture of 80:20 (v / v). The product is collected by Buchner filtration and dried in an oven under vacuum.
[0155] Example 2: Preparation of semi-aromatic polyethersulfone of the present invention based on dimethylpropane-1,3-diol 1.04 g (0.01 mol, 1 eq.) of 2,2-dimethylpropane-1,3-diol and 2.87 g (0.01 mol, 1 eq.) of DCDPS are dissolved in 9.13 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The reaction medium is immersed in an oil bath and heated to 40 ° C to dissolve both monomers. 9.05 g (0.0199 mol, 1.99 eq.) of SiOMe3K dissolved in THF (2 M) are added. After the addition of the base, the temperature is gradually increased to 100 ° C and this temperature is maintained for 1 h. At this time, the medium becomes more viscous. The medium is then precipitated in 300 mL of distilled water and the product obtained in the form of a white powder is recovered by Büchner filtration and dried in an oven under reduced pressure. The polymer has a melting point Tm of 290 ° C.
[0156] Example 3: Preparation of semi-aromatic polyether nitriles of the present invention from isosorbide and dichlorobenzonitrile 1.46 g (0.01 mol, 1 eq.) of isosorbide (stored in a desiccator) and 1.72 g (0.01 mol, 1 eq.) of DCBN are dissolved in 7.42 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The reaction medium is immersed in an oil bath and heated to 30 ° C to dissolve the isosorbide. 9.05 g (0.0199 mol, 1.99 eq.) of SiOMe3K dissolved in THF (2 M) are added. After the addition of the base, the temperature is fixed at 30 ° C for 1 h 30. The temperature is then fixed at 100 ° C and the medium is left at 100 ° C for 2 h with stirring. At this time the medium becomes more viscous. The medium is then precipitated in 300 mL of distilled water. The product is recovered by Büchner filtration and dried in an oven under reduced pressure.
[0157] Example 4: Preparation of semi-aromatic polyether nitriles of the present invention from isosorbide and dichloropyridine 1.46 g (0.01 mol, 1 eq.) of isosorbide (stored in a desiccator) and 1.48 g (0.01 mol, 1 eq.) of DCP are dissolved in 6.86 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The reaction medium is immersed in an oil bath and heated to 40 ° C to dissolve the isosorbide. 9.05 g (0.0199 mol, 1.99 eq.) of SiOMe3K dissolved in THF (2 M) are added. After the addition of the base, the temperature is fixed at 100 ° C for 2 hours. At this time, the medium becomes more viscous. The medium is then precipitated in 300 mL of distilled water. The product is recovered by Büchner filtration and dried in an oven under reduced pressure.
[0158] Counterexample 1: Preparation of aromatic polyethersulfones based on bisphenol A 11.53 g (0.050 mol, 1 eq.) of bisphenol A, 14.51 g (0.050 mol, 1 eq.) of DCDPS and 15.35 g (0.10 mol, 2 eq.) of K2CO3 are dissolved in a 67:33 DMAc / toluene mixture (69 g DMAc and 34 g toluene, or 20% m) in a three-neck flask equipped with a Dean-Stark apparatus, a stirring blade and a nitrogen inlet, filled with toluene with a condenser thereon. The flask is heated at 160° C. for 14 hours. The reaction medium is diluted with NMP and then precipitated in water in the form of white threads. The polymer is recovered by Büchner filtration and dried in an oven under reduced pressure.
[0159] Counterexample 2: Preparation of isosorbide-based semi-aromatic polyethersulfone according to the method described in WO 2014 / 072473 A2 (Example 8) 2.0 g (0.014 mol, 1 eq.) of isosorbide (placed in a desiccator), 4.1 g (0.014 mol, 1 eq.) of DCDPS and 3.78 g (0.028 mol, 2 eq.) of K2CO3 are dissolved in 9 g of sulfolane in a three-necked flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The flask is heated to 210 ° C in an oil bath for 6 hours. The reaction medium is diluted with NMP and then precipitated in the form of a beige powder in 300 mL of a 50:50 (v / v) water / methanol mixture, Büchner filtered and then dried in an oven under reduced pressure.
[0160] Counterexample 3: Preparation of semi-aromatic polyethersulfone based on isosorbide and DFDPS at 140℃ 2.92 g (0.020 mol, 1 eq.) of isosorbide (placed in a desiccator), 5.08 g (0.020 mol, 1 eq.) of DFDPS and 5.58 g (0.040 mol, 2 eq.) of K2CO3 are dissolved in 18.7 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The round-bottom flask is heated to 140 ° C for 24 hours using an oil bath. At the end of the reaction, 15 mL of DMSO is added to dilute the medium. The reaction medium is then precipitated in the form of filaments in 1,000 mL of water, Büchner filtered and then dried in an oven under reduced pressure.
[0161] Counterexample 4: Commercially available polyethersulfone Commercially available granular resin purchased from Acros Organics was used for elemental analysis comparison (Acros code: 17891, CAS: 25135-51-7).
[0162] Counterexample 5: Preparation of semi-aromatic polyether nitriles from isosorbide and difluorobenzonitrile 1.37 g (9.4 mmol, 1 eq.) of isosorbide (placed in a desiccator), 1.30 g (9.4 mmol, 1 eq.) of DFBN, 2.59 g (18.7 mmol, 2 eq.) of K2CO3 and 1.03 g (10.3 mmol, 1.1 eq.) of CaCO3 are dissolved in 6.61 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade and a nitrogen inlet. The round-bottom flask is heated with an oil bath at 140 ° C for 24 h and then at 160 ° C for 24 h. At the end of the reaction, 10 mL of DMSO is added to dilute the medium. The reaction medium is then precipitated in the form of filaments in 300 mL of water, Büchner filtered and then dried in an oven under reduced pressure.
[0163] Counterexample 6: Preparation of semi-aromatic polyether nitriles from isosorbide and dichlorobenzonitrile 2.92 g (20 mmol, 1 eq.) of isosorbide (placed in a desiccator), 3.44 g (20 mmol, 1 eq.) of DCBN and 5.58 g (40 mmol, 2 eq.) of K2CO3 are dissolved in 25.45 g of sulfolane in a three-necked flask equipped with a gooseneck and a nitrogen inlet. The round-bottom flask is heated to 210° C. for 4 hours using an oil bath. At the end of the reaction, the reaction medium is precipitated in 300 mL of water in the form of threads, Büchner filtered and then dried in an oven under reduced pressure.
[0164] Counterexample 7: Preparation of semi-aromatic polyetherpyridines from isosorbide and difluoropyridine 1.46 g (10 mmol, 1 eq.) of isosorbide (placed in a desiccator), 1.15 g (10 mmol, 1 eq.) of DFP, 1.1 g (11 mmol, 1 eq.) of CaCO3, and 2.76 g (20 mmol, 2 eq.) of K2CO3 are dissolved in 6.61 g of DMSO in a three-neck flask equipped with a gooseneck, a stirring blade, and a nitrogen inlet. The flask is heated with an oil bath at 120 ° C for 15 h and then at 140 ° C for 48 h. At the end of the reaction, 2 mL of DMSO are added to dilute the medium. The reaction medium is then precipitated in the form of filaments in 300 mL of water, Büchner filtered, and then dried in an oven under reduced pressure.
[0165] The number average molecular weight (Mn) and polydispersity index (PDI) of the obtained polyethers are determined by size exclusion chromatography (SEC). The glass transition temperature (Tg) and melting point (Tm) of the obtained polyethers are determined by differential scanning calorimetry (DSC).
[0166] The characterizations that apply to the examples are described below. - Differential Scanning Calorimetry (DSC): Differential scanning calorimetry analyses were performed on a DSC, Mettler Toledo, in nitrogen at a flow rate of 80 mL / min, 10°C / min or 20°C / min from 20°C to 300°C. in perforated aluminum crucibles. - Size Exclusion Chromatography (SEC): Estimation of number average molecular weights was performed by SEC on a PS calibrated Agilent PLgel 5 μm column in DMF at 70° C. with a flow rate of 0.7 mL / min. - Elemental analysis: Estimation of the amount of atoms in mg / kg (ppm) in a 20 g sample by combustion-ion chromatography.
[0167] Characterization of the inventive polymers (Examples 1-4) is shown in Tables 1 and 2 in comparison with counterexamples 1-3 and 5-7.
[0168] [Table 1]
[0169] a A semi-crystalline polymer that is insoluble in DMF. b Measured with polystyrene calibration. c Glass transition temperature (Tg). d Melting point (Tm).
[0170] [Table 2]
[0171] Table 2 shows that short, low temperature reactions using SiOMe3K base result in higher glass transition temperatures for samples derived from halogenated monomers compared to reactions using K2CO3.
[0172] Residual chlorine, fluorine, and silicon content were measured by combustion-ion chromatography for Example 1 and Counterexamples 3 and 4. The results are shown in Table 3. These results show that Example 1 contains less than 100 ppm residual fluorine content and 80 ppm silicon content due to the use of SiOMe3K base.
[0173] [Table 3]
[0174] Preparation of membranes Films can be prepared from a 20 wt% solution of polymer in DMSO cast onto a glass plate. The solvent is then evaporated using the following thermal cycle: 80°C for 1 hour, 100°C for 1 hour, 120°C for 1 hour, 150°C for 1 hour, and 180°C for 2 hours. Example 1 yields a clear and relatively colorless film after curing. Also, the membranes of counter examples 1 and 3 are obtained using NMP as a solvent. In contrast, in counter example 2, no film is formed. The results are shown in Table 4.
[0175] [Table 4]
[0176] These results show that the method of the invention makes it possible to obtain isosorbide-based semi-aromatic polyethers from 4,4'-dichlorodiphenyl sulfone at low temperatures, i.e. temperatures between 40°C and 100°C, having sufficient mechanical properties to enable the production of films.
[0177] By way of comparison, the preparation of an aromatic polyethersulfone based on bisphenol A having sufficient mechanical properties to allow the production of a film requires heating at 160°C for 14 hours (Rebuttal Example 1), and the preparation of an aromatic polyethersulfone based on isosorbide and 4,4'-difluorodiphenylsulfone as K2CO3 base having sufficient mechanical properties to allow the production of a film requires heating at 140°C for 24 hours (Rebuttal Example 3).
[0178] Finally, reproduction of the operating conditions described in WO 2014 / 072473 A2 does not allow the production of semi-aromatic polyethers based on isosorbide having sufficient mechanical properties to allow the production of films (counterexample 2).
[0179] The characterization applied to the membranes is described below. Contact angle: The contact angle was measured with water according to Young's law.
[0180] [Number 1] σ s =γ sl +σ1 cosθ During the ceremony, σs is the surface tension of the solid / gas interface, γsl is the surface tension of the solid / liquid interface, σ1 is the surface tension of the liquid / gas interface, θ is the contact angle.
[0181] [Table 5]
[0182] The contact angles of the films obtained from the semi-aromatic polyether of Example 1 obtained by the method of the present invention show that the polymer is more hydrophilic than the reference polysulfone based on bisphenol (Table 5). The hydrophilicity of the semi-aromatic polyether is an advantage in the separation properties of the aqueous phase.
[0183] List of cited references Patent Literature For all useful purposes, the following patent documents are cited: - patcit1: International Publication No. 2013 / 023997A1 (publication number), - patcit2: International Publication No. 2014 / 072473A2 (publication number), and - patcit3: U.S. Patent No. 2015 / 0129487A1 (Publication No.).
[0184] Non-patent literature For all useful purposes, reference is made to the following non-patent material: - nplcit1: H. Kricheldorf et al., J. Polymer Sci., Part A: Polym. Chem., 1995, 33, 2667~2671; - nplcit2:S.Chattiら,High perform.Polym.,2009,21,105~118; - nplcit3:HWKimら,Journal of Membrane Science,vol.372,no.1,p.116~124,2011; - nplcit4:KMDiederichsenら,Macromolecules,vol.50,no.10,p.3831~3840,2017; - nplcit5:HJLeeら,Journal of Membrane science,vol.485,p.10~16,2015; - nplcit6:L.Jujie,X.Heら,J.Polym.Res,vol.24,no.1,p.1,2017; - nplcit7:LFHancockら,Biomaterials,vol.21,no.7,p.725~733,2000; - nplcit8: L. Wang, Polymer Chemsitry, vol.5, no.8, pp. 2836~2842, 2014; - nplcit9:RNJohnson,AGFarham,J.Polym.Sci.A-1 Polym.Chem.,vol.5,no.9,p.2415~2427,1967.
Claims
1. A process for the preparation of semi-aromatic polyethers based on 1,4:3,6-dianhydrohexitol, comprising the following successive steps: a) preparing a mixture comprising an aliphatic diol or a mixture of aliphatic diols, a dihalogenated aromatic or heteroaromatic compound, and a hindered strong base in an organic solvent; and b) heating the mixture at a temperature between 30° C. and 120° C. for a period of time up to 12 hours; The method of claim 1, wherein the hindered strong base is selected from potassium tert-butylate, sodium tert-butylate, lithium tert-butylate, potassium tert-pentylate, sodium tert-pentylate, potassium trimethylsilanolate, sodium trimethylsilanolate, lithium trimethylsilanolate, potassium tetramethylpiperidide, lithium tetramethylpiperidide, potassium bis(trimethylsilyl)amide, and lithium bis(trimethylsilyl)amide.
2. 2. The method of claim 1, wherein the aliphatic diol is selected from linear aliphatic diols, branched aliphatic diols, and cyclic aliphatic diols.
3. The method of claim 2, wherein the cycloaliphatic diol is selected from the 1,4:3,6-dianhydrohexitols.
4. 4. The method according to claim 1, wherein the dihalogenated aromatic or heteroaromatic compound is selected from dihalogenated aromatic sulfones, dihalogenated aromatic ketones, dihalogenated benzonitriles, dihalogenated diazenes, bis(halophenyl)oxadiazoles, dihalogenated nitrobenzenes, dihalogenated benzoylnaphthalenes, and dihalogenated pyridines.
5. 5. The process according to claim 1, wherein the molar ratio of hindered strong base to aliphatic diol is between 1 and 3.
6. 6. The process according to claim 1, wherein the organic solvent is a polar aprotic solvent or a mixture of polar aprotic solvents.
7. 7. The process according to claim 1, wherein the molar ratio of aliphatic diol / dihalogenated aromatic compound is between 0.5 and 1.
5.
8. Formula I: [Formula 1] wherein Ar is derived from a dihalogenated aromatic or heteroaromatic compound; R is derived from an aliphatic diol, X is a halogen; 8. The method according to claim 1, wherein n is an integer between 2 and 100, and n is determined by size exclusion chromatography.
9. The method of claim 8, wherein R is derived from an aliphatic diol selected from a linear aliphatic diol and a branched aliphatic diol.
10. The method of claim 8, wherein R is derived from 1,4:3,6-dianhydrohexitol.
11. The method according to claim 8, wherein the semi-aromatic polyether based on an aliphatic diol of formula I has a polydispersity index of 1.5 to 5.
12. The method according to any one of claims 8 to 11, wherein the number average molecular weight of the semi-aromatic polyether based on an aliphatic diol of formula I is 5,000 g / mol or more, wherein the number average molecular weight is measured by size exclusion chromatography in dimethylformamide at 70°C, at a flow rate of 0.7 mL / min, using polystyrene calibration.
13. The method according to claim 8, wherein the semi-aromatic polyether based on an aliphatic diol of formula I has a glass transition temperature of greater than 100°C.
14. The method according to claim 8, wherein X is chlorine.
15. The method according to claim 14, wherein the aliphatic diol-based semi-aromatic polyether of formula I contains a residual fluorine content of less than 100 ppm.
16. The method of claim 14, wherein the aliphatic diol-based semi-aromatic polyether of formula I contains a residual silicon content of 10 to 1,000 ppm.
17. The method of claim 14, wherein the aliphatic diol-based semi-aromatic polyether of formula I contains a residual chlorine content of 100 to 10,000 ppm.
18. 18. The method according to claim 8, wherein the semi-aromatic polyethers based on aliphatic diols of formula I are used for the production of membranes, components and coatings.
Citation Information
Patent Citations
JP1967007799B1
Method for manufacturing polyether-ether-ketone
JP2010070658A
Polyarylene ether sulfone
JP2015533916A
Polysulfone copolymer excellent in heat resistance and chemical resistance, and method for producing the same
JP2017525818A
Method for producing aromatic polyethersulfone containing isohexide
JP2021535247A