Sputtering Targets
A Cr-based alloy sputtering target with optimized CrB and Cr phases and boron content addresses the issue of fine crystal structure in thin films, providing a durable and homogeneous film for magnetic recording media.
Patent Information
- Application Number
- JP2022194039
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing sputtering targets fail to produce thin films with sufficiently fine crystal structures.
A Cr-based alloy sputtering target containing 10.0 at% to 30.0 at% boron (B) with a metal structure comprising a CrB phase and a Cr single phase, where the ratio of X-ray diffraction peaks is optimized to enhance toughness and prevent cracking during sputtering, manufactured through a process involving mixing CrB and Cr powders and pressurizing and heating.
The target produces a homogeneous thin film with reduced cracking and smaller grain size, suitable for applications like adhesion layers in perpendicular magnetic recording media, ensuring high quality and durability.
Smart Images

Figure 0007566854000001 
Figure 0007566854000002
Abstract
Description
[Technical field]
[0001] This specification discloses a target for use in sputtering to form thin metal films. [Background technology]
[0002] Sputtering is known as a method for forming thin films. In sputtering, a target is used. In sputtering, positive ions in the plasma collide with the target. These collisions cause atoms to fly out of the target. These atoms then adhere to the substrate, forming a thin film.
[0003] An example of a sputtering target is disclosed in JP 2014-164780 A. The target disclosed in this publication is obtained by sintering powder. The material of this powder is a Cr-based alloy. From this target, a thin film (adhesion layer) suitable for perpendicular magnetic recording media can be obtained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP2014-164780A Summary of the Invention [Problem to be solved by the invention]
[0005] There is a demand for a thin film with a finer crystal structure. The target disclosed in JP 2014-164780 A does not allow a thin film with a sufficiently fine crystal structure to be obtained.
[0006] The applicant's intention is to provide a sputtering target which is mainly composed of Cr and which can provide a homogeneous thin film. [Means for solving the problem]
[0007] The material of the sputtering target disclosed in this specification is a Cr-based alloy containing 10.0 at% or more and 30.0 at% or less of B. The metal structure of this target includes a CrB phase and a single Cr phase. The ratio of the X-ray diffraction peak associated with the (111) plane of the CrB phase to the X-ray diffraction peak associated with the (110) plane of the Cr phase is 10% or more and 80% or less.
[0008] Preferably, in this target, the ratio of the X-ray diffraction peak associated with the (213) plane of the Cr5B3 phase to the X-ray diffraction peak associated with the (110) plane of the Cr phase is 20% or less.
[0009] Preferably, the target has a flexural strength of 300 MPa or more in a three-point bending test.
[0010] Preferably, the oxygen content of the Cr-based alloy is 2000 ppm or less.
[0011] The method for producing a sputtering target disclosed in the present specification includes the steps of: (1) providing a first powder, the material of which is CrB; (2) preparing a second powder, the second powder having a material of Cr; (3) mixing the first powder with the second powder to obtain a mixed powder; and (4) Pressurizing and heating the mixed powder Includes.
[0012] Preferably, in step (2), a second powder having an average particle diameter D50 of 20 μm or more is prepared. Effect of the Invention
[0013] This sputtering target can provide a uniform thin film, and is less likely to crack during sputtering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, preferred embodiments will be described in detail with reference to the drawings as appropriate.
[0015] The material of the sputtering target according to this embodiment is a Cr-based alloy containing B. Preferably, in this alloy, the remainder of Cr and B is an inevitable impurity. A thin film can be formed by sputtering using this target. This thin film is suitable for various applications. A typical application of the thin film is as an adhesion layer of a perpendicular magnetic recording medium. This adhesion layer can suppress orientation in the perpendicular magnetic recording medium.
[0016] Cr can contribute to the non-magnetic, adhesive, and corrosion resistance of the adhesive layer. Cr has a BCC structure and has a lattice constant with a small mismatch with the (001) layer (such as an MgO layer) on which the adhesive layer is laminated. Cr can suppress the orientation of the layer on which the adhesive layer is laminated. From these viewpoints, the Cr content in the Cr-based alloy is preferably 60 at% or more.
[0017] B combines with Cr. In the target, B exists as chromium boride. This boride is presumed to pin the growth of crystal grains. A thin film with a small crystal grain size can be formed from this target. Furthermore, B can realize a structure without grain boundaries (amorphous). This structure is homogeneous and isotropic. This structure can contribute to the smoothness of the thin film. From these viewpoints, the B content in the Cr-based alloy is preferably 10 at% or more, more preferably 15 at% or more, and particularly preferably 20 at% or more. From the viewpoint of suppressing cracking of the target during sputtering, this content is preferably 30 at% or less.
[0018] The oxygen content (mass basis) of the Cr-based alloy is preferably 2000 ppm or less. A target made of this Cr-based alloy is less likely to crack during sputtering. Furthermore, a thin film with fewer particles can be obtained from this target. From these viewpoints, the oxygen content is more preferably 1500 ppm or less, and particularly preferably 1000 ppm or less. Ideally, the oxygen content is less than the detection limit.
[0019] The metal structure of the target includes a CrB phase and a single Cr phase. The single Cr phase has extremely excellent toughness. The toughness of the CrB phase is inferior to that of the single Cr phase. However, the CrB phase has a toughness superior to that of other chromium borides. The metal structure including the CrB phase and the single Cr phase can suppress cracking of the target during sputtering.
[0020] Among the multiple peaks of the Cr phase obtained by X-ray diffraction, the peak P1 related to the (110) plane is the largest. Among the multiple peaks of the CrB phase obtained by X-ray diffraction, the peak P2 related to the (111) plane is the largest. The ratio of the X-ray diffraction peak P2 related to the (111) plane of the CrB phase to the X-ray diffraction peak P1 related to the (110) plane of the Cr phase is preferably 10% or more and 80% or less. In a target having this ratio of 10% or more, B is sufficiently dispersed and the amount of compounds with poor toughness is small. From these viewpoints, this ratio is more preferably 20% or more, and particularly preferably 25% or more. In a target having this ratio of 80% or less, the amount of the CrB phase is not excessive. This target is less likely to crack during sputtering. From this viewpoint, this ratio is more preferably 60% or less, and particularly preferably 40% or less.
[0021] Among the multiple peaks of the Cr5B3 phase obtained by X-ray diffraction, the peak P3 relating to the (213) plane is the largest. The ratio of the X-ray diffraction peak P3 relating to the (213) plane of the Cr5B3 phase to the X-ray diffraction peak P1 relating to the (110) plane of the Cr phase is preferably 20% or less. In a target in which this ratio is 20% or less, the amount of the Cr5B3 phase is not excessive. This target is less likely to crack during sputtering. From this viewpoint, this ratio is more preferably 10% or less, and particularly preferably 5% or less. Ideally, this ratio is 0%.
[0022] Peaks P1, P2 and P3 are measured by an X-ray diffraction device. A test piece for X-ray diffraction is cut out from a target by a wire-cut method. The surface of the test piece is smoothed by polishing. The measurement conditions are as follows: Test piece size: 10mm x 20mm x 5mm X-ray source: CuKα ray Scan speed: 4° / min 2θ:20-80° Peaks (peak intensities) are read from the chart obtained by this X-ray diffraction.
[0023] The flexural strength of the target is preferably 300 MPa or more. This target is less likely to crack during sputtering. From this viewpoint, the flexural strength is more preferably 400 MPa or more, and particularly preferably 500 MPa or more.
[0024] The flexural strength is measured by a three-point bending test in accordance with the provisions of "JIS Z 2511." Test pieces for the three-point bending test are cut from the target by the wire cutting method. The measurement conditions are as follows: Test piece size: 2mm x 2mm x 20mm Distance between fulcrums: 10mm The flexural strength BS (MPa) is calculated by the following formula. BS = 3 / 2 × P × L / (t 2 × W) P: Load at break (kN) L: Distance between fulcrums (mm) t: thickness of test piece (mm) W: width of sample (mm)
[0025] The sputtering target may be obtained by a powder metallurgical method, which comprises: (1) providing a first powder, the material of which is CrB; (2) preparing a second powder, the second powder having a material of Cr; (3) mixing the first powder with the second powder to obtain a mixed powder; and (4) Pressurizing and heating the mixed powder By applying pressure and heat, a sputtering target, which is a sintered body, is obtained. This target is processed to a predetermined size and is used for sputtering.
[0026] As described above, the Cr-based alloy of the target contains B. This B originates from the first powder. The material of the first powder is CrB. In other words, the first powder contains 50 at % Cr and 50 at % B. This target does not contain any component originating from a powder whose material is simple B. In this target, B can be uniformly dispersed. A homogeneous thin film can be formed from this target.
[0027] Since B originates from the first powder, even if the second powder has a relatively large particle size, uniform dispersion of B can be achieved. Since the second powder with a large particle size is mixed with the first powder, a target with a low oxygen content can be obtained. Specifically, a target with an oxygen content of 2000 ppm or less can be obtained by this manufacturing method. This target is less likely to crack during sputtering.
[0028] From the viewpoint of a low oxygen content, the average particle diameter D50 of the second powder is preferably 20 μm or more, more preferably 40 μm or more, and particularly preferably 50 μm or more. The average particle diameter D50 is preferably 250 μm or less. The average particle diameter D50 is the particle diameter when the cumulative volume is 50% in the cumulative volume curve of the powder. The average particle diameter D50 is measured by a laser diffraction / scattering type particle size distribution measuring device.
[0029] The CrB of the first powder is a compound that is stable against heat. CrB is unlikely to become the origin of new compounds during sintering. This manufacturing method can provide a target that is substantially free of layers other than the CrB phase and the Cr single phase. This manufacturing method can provide a target with a small amount of compounds such as Cr5B3. This manufacturing method can provide a target in which the ratio of peak P2 to peak P1 is 10% or more and 80% or less. This manufacturing method can provide a target in which the ratio of peak P3 to peak P1 is 20% or less. This manufacturing method can provide a target with a flexural strength of 300 MPa or more. This target is unlikely to crack during sputtering. A homogeneous thin film can be formed from this target.
[0030] From this target, an adhesion layer for a perpendicular magnetic recording medium can be obtained by sputtering. From this target, other thin films can be obtained by sputtering.
[0031] The present specification is also directed to a method for producing a thin film, the method comprising the steps of: (1) preparing a target whose material is a Cr-based alloy containing 10.0 at% or more and 30.0 at% or less of B, whose metal structure contains a CrB phase and a single Cr phase, and whose ratio of an X-ray diffraction peak relating to a (111) plane of the CrB phase to an X-ray diffraction peak relating to a (110) plane of the Cr phase is 10% or more and 80% or less; and (2) A step of sputtering the target. This manufacturing method can produce high quality thin films, such as adhesion layers for perpendicular magnetic recording media. EXAMPLES
[0032] The effects of the sputtering targets according to the examples will be explained below, but the scope of the present specification should not be construed as being limited based on the description of these examples.
[0033] [Example 1] A first powder was prepared. The material of this first powder was CrB. This CrB contained 50 at% B. The average particle diameter D50 of this first powder was 10 μm. Furthermore, a second powder was prepared. The material of this second powder was pure Cr. The average particle diameter D50 of this second powder was 60 μm. The first powder and the second powder were put into a V-type mixer to obtain a mixed powder. The mixed powder was filled into a can made of carbon steel, having a diameter of 200 mm and a length of 10 mm. After the powder was degassed in vacuum, a billet was made by HIP. The HIP conditions were as follows. Sintering temperature: 1000℃ Pressure: 120MPa Hold time: 2 hours This billet was sliced to obtain the sputtering target of Example 1.
[0034] [Examples 2-6 and Comparative Examples 1 and 7] Sputtering targets of Examples 2-6 and Comparative Examples 1 and 7 were obtained in the same manner as in Example 1, except that the mixing ratio of the first powder and the second powder was adjusted and the sintering temperature was set as shown in Table 2 below.
[0035] [Comparative Example 2-6] A sputtering target of Comparative Example 2-6 was obtained in the same manner as in Example 1, except that a predetermined amount of pure B powder was used instead of the first powder, a predetermined amount of powder made of pure Cr and having an average particle diameter D50 of 60 μm was used instead of the second powder, and the sintering temperature was as shown in Table 2 below.
[0036] [Comparative Example 8] A sputtering target of Comparative Example 8 was obtained in the same manner as in Example 1, except that the starting material was pure Cr powder alone.
[0037] [Comparative Examples 9-11] Sputtering targets of Comparative Examples 9-11 were obtained in the same manner as in Example 1, except that a predetermined amount of pure B powder was used instead of the first powder, and a predetermined amount of fine powder made of pure Cr and having an average particle diameter D50 of 10 μm was used instead of the second powder.
[0038] [Oxygen content] A test piece was cut out from the target by wire cutting. The mass of this test piece was about 1 g. The surface of this test piece was polished, and the oxygen content was measured using an oxygen / nitrogen analyzer (manufactured by Horiba, Ltd., product name "EMGA-920"). The results are shown in Table 2 below.
[0039] [X-ray diffraction] The target was subjected to X-ray diffraction by the above-mentioned method. The ratio (P2 / P1) of the X-ray diffraction peak P2 related to the (111) plane of the CrB phase to the X-ray diffraction peak P1 related to the (110) plane of the Cr phase was calculated. Furthermore, the ratio (P3 / P1) of the X-ray diffraction peak P3 related to the (213) plane of the Cr5B3 phase to this peak P1 was calculated. The results are shown in Table 3 below. When the peak P2 could not be distinguished from noise and the ratio (P2 / P1) was 1% or less, it was indicated as "<1%". When the peak P3 could not be distinguished from noise and the ratio (P3 / P1) was 1% or less, it was indicated as "<1%". In the targets of Examples 1-6 and Comparative Examples 1-3, 7, and 9-11, no peaks other than the peak P2 whose ratio to the diffraction peak P1 was 1% or more were observed. In the target of Comparative Example 4-6, no peaks other than peaks P2 and P3 having a ratio of 1% or more to diffraction peak P1 were observed.
[0040] [Area ratio measurement] A test piece was cut from the target by wire cutting. The size of this test piece was 10 mm x 20 mm x 5 mm. The distribution of Cr and B in this test piece was observed using an EPMA (electron probe microanalyzer), and the area ratio Ps of the part where B was not present was calculated. The results are shown in Table 3 below. In the EPMA, counts of 70 or more were counted. Each count was divided by the total count (62,500) to calculate the area ratio. The measurement conditions for the EPMA were as follows: Range: 2mm x 2mm Beam size: 8μm Number of data points: 250 x 250 The results are shown in Table 2 below.
[0041] [Deflection test] The flexural strength of the target was measured by the above-mentioned method, and the results are shown in Table 3 below.
[0042] [Number of particles in thin film] A thin film was formed by sputtering a target (diameter: 95 mm, thickness: 2 mm) under the following sputtering conditions: Substrate material: cleaned glass Chamber atmosphere: atmospheric pressure 1×10 -4 The pressure was evacuated to below 0.6 Pa, and 99.99% pure Ar gas was introduced at 0.6 Pa. Thin film thickness: 20nm The thin film was observed with an optical surface analyzer, and the number of particles having a size of 0.1 μm or more was counted. The results are shown in Table 2 below.
[0043] [Crystal grain size] The thin film was observed by TEM to measure the average crystal grain size. The ratio of this average crystal grain size to the crystal grain size of Cr in Comparative Example 1 was calculated. The results are shown in Table 2 below.
[0044] [Table 1]
[0045] In addition to the components listed in Table 1, each sputtering target contains unavoidable impurities.
[0046] [Table 2]
[0047] As is clear from Table 2, the sputtering targets of each example have excellent bending strength. Furthermore, the thin films obtained from these targets have few particles and small crystal grain sizes. From these evaluation results, the superiority of this sputtering target is clear. [Industrial Applicability]
[0048] Thin films for various applications can be produced from the sputtering targets described above.
Claims
1. The material is a Cr-based alloy containing 10.0 at% or more and 30.0 at% or less of B, The metal structure includes a CrB phase and a Cr single phase, a ratio of an X-ray diffraction peak relating to a (111) plane of the CrB phase to an X-ray diffraction peak relating to a (110) plane of the Cr phase is 10% or more and 80% or less; Cr for the X-ray diffraction peak for the (110) plane of the Cr phase 5 B 3 A sputtering target having an X-ray diffraction peak ratio relating to the (213) plane of the phase of 20% or less.
2. 2. The sputtering target according to claim 1, having a flexural strength of 300 MPa or more in a three-point bending test.
3. 3. The sputtering target according to claim 1, wherein the Cr-based alloy has an oxygen content of 2000 ppm or less.
Citation Information
Patent Citations
Target member for sputtering and its production
JP1994041735A
Cr target material and its production
JP2000199055A
Cr ALLOY FOR MAGNETIC RECORDING AND SPUTTERING TARGET MATERIAL, AND PERPENDICULAR MAGNETIC RECORDING MEDIUM USING THE SAME
JP2014164780A