Insulating resin composition, cured insulating resin body, laminate and circuit board

The insulating resin composition with a specific amine curing agent and high thermal conductivity inorganic filler addresses the heat dissipation and reliability issues of metal-based circuit boards, enhancing performance under severe conditions.

JP7566917B2Active Publication Date: 2024-10-15DENKA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022547000
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-07
Filing Date
2021-09-06
Publication Date
2024-10-15
Estimated Expiration
2041-09-06

AI Technical Summary

Technical Problem

Metal-based circuit boards have lower heat dissipation properties compared to ceramic circuit boards, and they require high insulation reliability under severe conditions of high temperature, high humidity, and high voltage application.

Method used

An insulating resin composition comprising an epoxy resin, a specific amine curing agent with first and second amine compounds, and an inorganic filler with high thermal conductivity, forming an insulating layer with excellent insulation reliability, high heat cycle resistance, and thermal conductivity.

Benefits of technology

The composition forms a circuit board with improved insulation reliability, heat cycle resistance, and heat dissipation under high temperature, high humidity, and high voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566917000014
    Figure 0007566917000014
  • Figure 0007566917000015
    Figure 0007566917000015
  • Figure 0007566917000001
    Figure 0007566917000001
Patent Text Reader

Abstract

This insulating resin composition comprises: an epoxy resin; an amine-based curing agent containing a first amine compound represented by formula (A-1) and a second amine compound represented by formula (A-2); and an inorganic filler having a heat conductivity of 20 W / mK or greater. The content of the inorganic filler is 30-80 vol%. Formula (A-1), formula (A-2) [In the formulae: Y is -NH2 or -NHR1; (R1 is a group represented by (Y-1)); and at least one of the Ys is -NHR1.] Formula (Y-1) [In the formula (Y-1), R2 represents an alkyl group.]
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an insulating resin composition suitable for use in the production of circuit boards (particularly metal-based circuit boards) and a cured product thereof. The present invention also relates to a laminate and a circuit board formed using the insulating resin composition. [Background technology]

[0002] A variety of circuit boards have been put to practical use as circuit boards on which electronic and electrical components such as semiconductor elements are mounted to form hybrid integrated circuits. Circuit boards are classified based on the board material into resin circuit boards, ceramic circuit boards, metal-based circuit boards, etc.

[0003] Resin circuit boards are inexpensive, but because the thermal conductivity of the board is low, their applications are limited to those requiring relatively low power. Ceramic circuit boards, due to the characteristics of ceramics, such as high electrical insulation and heat resistance, are suitable for applications requiring relatively high power, but have the disadvantage of being expensive. On the other hand, metal-based circuit boards have intermediate properties between the two, and are suitable for general-purpose applications requiring relatively high power, such as inverters for refrigerators, inverters for commercial air conditioners, power sources for industrial robots, and power sources for automobiles.

[0004] For example, Patent Document 1 discloses a method for obtaining a circuit board having excellent stress relaxation properties, heat resistance, moisture resistance, and heat dissipation properties by using a composition for circuit boards containing a specific epoxy resin, a curing agent, and an inorganic filler as essential components. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-266533 A Summary of the Invention [Problem to be solved by the invention]

[0006] If ceramic circuit boards could be substituted for metal-based circuit boards, productivity could be improved. However, metal-based circuit boards generally tend to have lower heat dissipation than ceramic circuit boards. Furthermore, in industrial module fields where ceramic circuit boards are used, high voltages may be applied under severe conditions, and high reliability is required under such conditions.

[0007] Therefore, the present invention aims to provide an insulating resin composition capable of forming an insulating layer having excellent insulation reliability, high heat cycle resistance, and high thermal conductivity under conditions of high temperature, high humidity, and high voltage application. Another object of the present invention is to provide a circuit board having an insulating layer made of a cured product of the insulating resin composition, and having excellent insulation reliability, heat cycle resistance, and heat dissipation properties under conditions of high temperature, high humidity, and high voltage application. [Means for solving the problem]

[0008] The present invention includes the following aspects. (1) An insulating resin composition comprising an epoxy resin, an amine-based curing agent containing a first amine compound represented by formula (A-1) and a second amine compound represented by formula (A-2), and an inorganic filler having a thermal conductivity of 20 W / mK or more, wherein the content of the inorganic filler is 30 to 80 volume %. [ka] [In formula (A-1), n 1 represents an integer between 0 and 4, and X 1 represents an alkanediyl group, an oxygen atom, or a sulfur atom. 1 When is 1 or more, there are multiple X 1 may be the same or different.] [ka] [In formula (A-2), n 2 represents an integer between 0 and 4, and X 2represents an alkanediyl group, an oxygen atom, or a sulfur atom, and Y represents -NH2 or -NHR 1 (R 1 represents a group represented by formula (Y-1). A plurality of Y's may be the same or different. However, at least one of the Y's is -NHR 1 n 2 When is 1 or more, there are multiple X 2 may be the same or different.] [ka] [In formula (Y-1), R 2 represents an alkyl group. (2) The insulating resin composition according to (1), wherein the inorganic filler contains an aggregate powder containing aggregates of primary particles. (3) The insulating resin composition according to (2), wherein the aggregate powder has an average particle size of 20 to 100 μm. (4) The insulating resin composition according to (2) or (3), wherein the aggregate powder has a crushing strength of 1 to 30 MPa. (5) The tap density of the agglomerated powder is 0.7 to 2.0 g / cm 3 The insulating resin composition according to any one of (2) to (4), (6) The specific surface area of ​​the agglomerated powder is 3.0 to 10.0 m 2 The insulating resin composition according to any one of (2) to (5), wherein the total weight of the insulating resin composition is 100% or more. (7) The insulating resin composition according to any one of (2) to (6), wherein the agglomerated powder contains boron nitride. (8) The above X 1 and X 2 The insulating resin composition according to any one of (1) to (7), wherein is a methanediyl group. (9) The insulating resin composition according to any one of (1) to (8), wherein the content of the first amine compound in the amine curing agent is 30 to 60 mass % and the content of the second amine compound is 40 to 70 mass %. (10) In the amine-based curing agent, -NHR relative to the total number M1 of -NH2 1The insulating resin composition according to any one of (1) to (9), wherein a ratio (M2 / M1) of a total number M2 of the particles is 0.05 to 0.30. (11) The insulating resin composition according to any one of (1) to (10), wherein a ratio of an active hydrogen equivalent of the amine curing agent to an epoxy equivalent of the epoxy resin is 0.3 to 1.5. (12) An insulating resin cured product, which is a cured product of the insulating resin composition according to any one of (1) to (11). (13) The insulating resin cured body according to (12), which contains crushed pieces of the inorganic filler. (14) Crosslink density is 4.0×10 -2 ~5.0×10 -1 mol / cm 3 The insulating resin cured product according to (12) or (13), (15) The insulating resin cured product according to any one of (12) to (14), which has a storage modulus at −40° C. of 100 GPa or less. (16) A method for producing a cured insulating resin product, comprising: curing the insulating resin composition or a semi-cured product thereof according to any one of (1) to (11) by hot pressing to produce a cured insulating resin product. (17) A laminate comprising a metal plate, the cured insulating resin body according to any one of (12) to (15) disposed on the metal plate, and a metal foil disposed on the cured insulating resin body. (18) A circuit board comprising: a metal plate; the cured insulating resin body according to any one of (12) to (15) disposed on the metal plate; and a circuit portion disposed on the cured insulating resin body. Effect of the Invention

[0009] According to the present invention, there is provided an insulating resin composition capable of forming an insulating layer having excellent insulation reliability, high heat cycle resistance, and high thermal conductivity under conditions of high temperature, high humidity, and high voltage application. Also, according to the present invention, there is provided a circuit board having an insulating layer composed of a cured product of the insulating resin composition, and having excellent insulation reliability, heat cycle resistance, and heat dissipation properties under conditions of high temperature, high humidity, and high voltage application. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing one embodiment of a laminate. [Diagram 2] FIG. 2 is a cross-sectional view illustrating an embodiment of a circuit board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Preferred embodiments of the present invention will now be described in detail.

[0012] (Insulating resin composition) The insulating resin composition of the present embodiment includes an epoxy resin, an amine-based curing agent, and an inorganic filler having a thermal conductivity of 20 W / mK or more. In the present embodiment, the amine-based curing agent contains a first amine compound represented by formula (A-1) and a second amine compound represented by formula (A-2). In the present embodiment, the content of the inorganic filler is 30 to 80 volume %.

[0013] [ka]

[0014] In formula (A-1), n 1 represents an integer between 0 and 4, and X 1 represents an alkanediyl group, an oxygen atom, or a sulfur atom. 1 When is 1 or more, there are multiple X 1 may be the same or different from each other.

[0015] [ka]

[0016] In formula (A-2), n 2 represents an integer between 0 and 4, and X 2 represents an alkanediyl group, an oxygen atom, or a sulfur atom, and Y represents -NH2 or -NHR 1 (R 1represents a group represented by formula (Y-1). A plurality of Y's may be the same or different. However, at least one of the Y's is -NHR 1 n 2 When is 1 or more, there are multiple X 2 may be the same or different from each other.

[0017] [ka]

[0018] In formula (Y-1), R 2 represents an alkyl group.

[0019] The insulating resin composition of the present embodiment can form an insulating resin cured product that can maintain excellent insulating reliability (for example, for 200 hours or more) even under conditions of high temperature and high humidity (for example, 85° C., 85% RH) and high voltage application (for example, DC 1200 V) by combining the above-mentioned amine-based curing agent with an epoxy resin. Therefore, the insulating resin composition of the present embodiment can produce a circuit board that has excellent insulating reliability and heat cycle resistance under conditions of high temperature, high humidity, and high voltage application.

[0020] Although the reason why the above-mentioned effects are obtained is not necessarily clear, it is thought that the use of the second amine compound reduces the crosslink density of the cured body and introduces an alkyl group, which in turn improves the flexibility of the cured body and forms an insulating layer with excellent heat cycle properties.

[0021] In addition, since the insulating resin composition of this embodiment contains the inorganic filler, it is possible to form an insulating resin cured body with high thermal conductivity. Therefore, the insulating resin composition of this embodiment can produce a circuit board with excellent heat dissipation. In this embodiment, by blending a predetermined amount of inorganic filler having a predetermined thermal conductivity, high thermal conductivity is realized while sufficiently obtaining the effects of the above-mentioned insulation reliability and heat cycle resistance.

[0022] The epoxy resin may be any epoxy resin that can be cured by an amine-based curing agent. Examples of the epoxy resin include bisphenol A type epoxy resin, bisphenol S type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, polypropylene glycol type epoxy resin, polytetramethylene glycol type epoxy resin, naphthalene type epoxy resin, phenylmethane type epoxy resin, tetrakisphenolmethane type epoxy resin, biphenyl type epoxy resin, epoxy resin having a triazine ring, bisphenol A alkylene oxide adduct type epoxy resin, dicyclopentadiene type epoxy resin, cresol novolac type epoxy resin, and phenol novolac type epoxy resin. The epoxy resin may be used alone or in combination of two or more types.

[0023] From the viewpoint of heat resistance, the epoxy resin preferably contains at least one ring structure selected from the group consisting of a benzene ring structure, a naphthalene ring structure, and a triazine ring structure.

[0024] The amine-based curing agent is a curing agent that has an amino group and can cure an epoxy resin. In the present embodiment, the amine-based curing agent includes a first amine compound represented by formula (A-1) and a second amine compound represented by formula (A-2).

[0025] In formula (A-1), n 1 is 0 to 4, preferably 0 to 2, and more preferably 0 or 1.

[0026] In formula (A-1), X 1 is an alkanediyl group, an oxygen atom or a sulfur atom, and is preferably an alkanediyl group. The alkanediyl group preferably has 1 to 5 carbon atoms, more preferably 1 to 3 carbon atoms, and further preferably has 1 carbon atom (i.e., a methanediyl group).

[0027] Multiple Xs 1 may be the same or different, but are preferably the same.

[0028] In formula (A-2), n 2 is 0 to 4, preferably 0 to 2, and more preferably 0 or 1.

[0029] In formula (A-2), X 2 is an alkanediyl group, an oxygen atom or a sulfur atom, and is preferably an alkanediyl group. The alkanediyl group preferably has 1 to 5 carbon atoms, more preferably 1 to 3 carbon atoms, and further preferably has 1 carbon atom (i.e., a methanediyl group).

[0030] Multiple Xs 2 may be the same or different, but are preferably the same.

[0031] X 2 X 1 In this embodiment, the amine-based curing agent can be easily produced.

[0032] In formula (A-2), Y is -NH2 or -NHR 1 A plurality of Y's may be the same or different, but at least one of the Y's is -NHR. 1 It is.

[0033] In a preferred embodiment, the amine curing agent has Y in which a portion is -NH2 and the other portion is -NHR 1 and an amine compound (A-2-1) in which all of Y's are -NHR 1 and an amine compound (A-2-2) which is

[0034] In formula (A-2), R 1 is a group represented by formula (Y-1). In formula (Y-1), R 2 R is an alkyl group, preferably an alkyl group having 1 to 8 carbon atoms, and more preferably an alkyl group having 3 to 5 carbon atoms. 2 The alkyl group may be linear, branched or cyclic, and is preferably linear from the viewpoint of further improving the flexibility of the cured body.

[0035] -NHR to the total number M1 of -NH2 in the amine hardener 1 The ratio (M2 / M1) of the total number M2 of the hydroxyl groups is, for example, 0.05 or more, preferably 0.08 or more, and more preferably 0.10 or more. This allows a cured body to be obtained that has even more excellent insulation reliability under conditions of high temperature, high humidity, and high voltage application. The ratio (M2 / M1) is, for example, 0.30 or less, preferably 0.25 or less, and more preferably 0.20 or less. This tends to further improve the insulation properties of the cured body. That is, the ratio (M2 / M1) may be, for example, 0.05 to 0.30, 0.05 to 0.25, 0.05 to 0.20, 0.08 to 0.30, 0.08 to 0.25, 0.08 to 0.20, 0.10 to 0.30, 0.10 to 0.25, or 0.10 to 0.20.

[0036] The content of the first amine compound in the amine-based curing agent may be, for example, 15% by mass or more, preferably 30% by mass or more, more preferably 40% by mass or more, from the viewpoint of further improving the insulating property of the cured body. Also, the content of the first amine compound in the amine-based curing agent may be, for example, 75% by mass or less, preferably 60% by mass or less, more preferably 55% by mass or less, from the viewpoint of obtaining a cured body having better insulating reliability under conditions of high temperature, high humidity and high voltage application. That is, the content of the first amine compound in the amine-based curing agent may be, for example, 15 to 75% by mass, 15 to 60% by mass, 15 to 55% by mass, 30 to 75% by mass, 30 to 60% by mass, 30 to 55% by mass, 40 to 75% by mass, 40 to 60% by mass, or 40 to 55% by mass.

[0037] The content of the second amine compound in the amine-based curing agent may be, for example, 30% by mass or more, preferably 40% by mass or more, more preferably 45% by mass or more, from the viewpoint of obtaining a cured body having better insulation reliability under conditions of high temperature, high humidity and high voltage application. Also, the content of the second amine compound in the amine-based curing agent may be, for example, 80% by mass or less, preferably 70% by mass or less, more preferably 55% by mass or less, from the viewpoint of further improving the insulation property of the cured body. That is, the content of the second amine compound in the amine-based curing agent may be, for example, 30 to 80% by mass, 30 to 70% by mass, 30 to 55% by mass, 40 to 80% by mass, 40 to 70% by mass, 40 to 55% by mass, 45 to 80% by mass, 45 to 70% by mass, or 45 to 55% by mass.

[0038] The amine-based curing agent may further contain other amine-based curing agents than the first amine compound and the second amine compound, but it is preferable that the first amine compound and the second amine compound are the main components. Specifically, the total content of the first amine compound and the second amine compound in the amine-based curing agent is, for example, 50 mass% or more, preferably 70 mass% or more, more preferably 90 mass% or more, may be 95 mass% or more, may be 99 mass% or more, or may be 100 mass%.

[0039] Examples of the amine-based curing agent other than the first amine compound and the second amine compound include ethylenediamine, diethylenetriamine, hexamethylenediamine, metaphenylenediamine, diaminodiphenylsulfone, pentaethylenediamine, and diethylene glycol bispropylamine.

[0040] The content of the amine-based curing agent is preferably an amount in which the ratio of the active hydrogen equivalent of the amine-based curing agent to the epoxy equivalent of the epoxy resin is in the following range, from the viewpoint of obtaining a cured product having better insulation reliability under conditions of high temperature, high humidity and high voltage application. The ratio of the active hydrogen equivalent of the amine-based curing agent to the epoxy equivalent of the epoxy resin may be, for example, 0.2 or more, preferably 0.3 or more, more preferably 0.5 or more. The ratio of the active hydrogen equivalent of the amine-based curing agent to the epoxy equivalent of the epoxy resin may be, for example, 1.8 or less, preferably 1.5 or less, more preferably 1.2 or less. That is, the ratio of the active hydrogen equivalent of the amine-based curing agent to the epoxy equivalent of the epoxy resin may be, for example, 0.2 to 1.8, 0.2 to 1.5, 0.2 to 1.2, 0.3 to 1.8, 0.3 to 1.5, 0.3 to 1.2, 0.5 to 1.8, 0.5 to 1.5, or 0.5 to 1.2.

[0041] The insulating resin composition of the present embodiment can also be said to be a composition containing a resin component containing an epoxy resin and an amine-based curing agent, and an inorganic filler.

[0042] The total content of the epoxy resin and the amine-based curing agent in the resin component may be, for example, 80 mass% or more, preferably 85 mass% or more, more preferably 90 mass% or more, and even more preferably 95 mass% or more, based on the total amount of the resin component.

[0043] The thermal conductivity of the inorganic filler is 20 W / mK or more, preferably 50 W / mK or more, more preferably 100 W / mK or more. This makes it easier to obtain a cured body with higher thermal conductivity. The upper limit of the thermal conductivity of the inorganic filler is not particularly limited, but may be, for example, 3500 W / mK or less, 2000 W / mK or less, or 600 W / mK or less. This reduces the cost of producing the resin composition. That is, the thermal conductivity of the inorganic filler may be, for example, 20 to 3500 W / mK, 20 to 2000 W / mK, 20 to 600 W / mK, 50 to 3500 W / mK, 50 to 2000 W / mK, 50 to 600 W / mK, 100 to 3500 W / mK, 100 to 2000 W / mK, or 100 to 600 W / mK.

[0044] The inorganic filler can be said to be a filler made of an inorganic material. The inorganic material may be any material that can achieve the above-mentioned thermal conductivity. Examples of the inorganic material include boron nitride, aluminum oxide, magnesium oxide, aluminum nitride, and silicon nitride.

[0045] As the inorganic filler, agglomerated powder containing aggregates of primary particles can be suitably used. When the inorganic filler contains agglomerated powder, at least a part of the agglomerated powder is deformed or crushed by the pressure applied during curing of the insulating resin composition, and the number of contact points between the inorganic fillers (between the agglomerated powders) increases, which tends to further improve the thermal conductivity.

[0046] The average particle size of the aggregated powder may be, for example, 10 μm or more, preferably 20 μm or more, more preferably 25 μm or more, and even more preferably 30 μm or more. This reduces the contact surface between the aggregated powder and the resin component, and tends to further improve the thermal conductivity. The average particle size of the aggregated powder may be, for example, 150 μm or less, preferably 100 μm or less, more preferably 90 μm or less, and even more preferably 80 μm or less. This further improves the filling property with the resin, makes it easier to increase the filling rate, and makes it easier to obtain a cured body with higher thermal conductivity. That is, the average particle size of the agglomerated powder may be, for example, 10 to 150 μm, 10 to 100 μm, 10 to 90 μm, 10 to 80 μm, 20 to 150 μm, 20 to 100 μm, 20 to 90 μm, 20 to 80 μm, 25 to 150 μm, 25 to 100 μm, 25 to 90 μm, 25 to 80 μm, 30 to 150 μm, 30 to 100 μm, 30 to 90 μm, or 30 to 80 μm.

[0047] In this specification, the average particle size of the agglomerated powder refers to the particle size at 50% of the cumulative value of the cumulative particle size distribution measured by particle size distribution measurement using a laser diffraction light scattering method in accordance with JIS Z8825.

[0048] The crushing strength of the agglomerated powder may be, for example, 0.5 MPa or more, preferably 1 MPa or more, more preferably 1.5 MPa or more. This suppresses the destruction of the agglomerated powder before curing (for example, during the production of the insulating resin composition, during the production of a semi-cured body of the insulating resin composition, etc.), and the above-mentioned effect is more significantly exhibited. The crushing strength of the agglomerated powder may be, for example, 40 MPa or less, preferably 30 MPa or less, more preferably 20 MPa or less. This makes it easier to deform or crush the agglomerated powder when the insulating resin composition is cured, and the above-mentioned curing is more significantly exhibited. That is, the crushing strength of the agglomerated powder may be, for example, 0.5 to 40 MPa, 0.5 to 30 MPa, 0.5 to 20 MPa, 1 to 40 MPa, 1 to 30 MPa, 1 to 20 MPa, 1.5 to 40 MPa, 1.5 to 30 MPa, or 1.5 to 20 MPa.

[0049] In this specification, the crushing strength of the agglomerated powder means a value obtained from the test force when the particles are deformed, measured in accordance with JIS R 1639-5. More specifically, for example, the test force is measured using a micro compression tester "MCT-510" (manufactured by Shimadzu Corporation, product name), and the crushing strength can be calculated based on the following formula. S t =AP / πd 2 In the formula, S t is the crushing strength (MPa), A is the coefficient, P is the breaking test force (N), and d is the particle diameter (mm). The coefficient A in the formula is determined according to the components that make up the agglomerated powder. For example, in the case of boron nitride agglomerated powder, it is determined to be "2.8" based on the Journal of the Mining Industry of Japan, Vol. 81, p. 1024, 1965. The test is a compression test using a flat indenter with a diameter of 200 μm, and the test conditions are a set test force of 49 (mN) and a load speed of 0.25 (mN / sec). The measurement is performed 10 times, and the average value of the crushing strength calculated for each measurement is regarded as the crushing strength of the agglomerated powder.

[0050] The tap density of the agglomerated powder is, for example, 0.4 g / cm 3 or more, preferably 0.6 g / cm 3 More preferably, 0.7 g / cm 3 This leads to improved coating properties of the resin composition and improved insulating properties of the cured product. The tap density of the aggregated powder is, for example, 3.0 g / cm. 3 or less, preferably 2.0 g / cm 3 Less than 1.0 g / cm, more preferably 1.0 g / cm 3 This makes it easier to obtain the above-mentioned suitable crushing strength, and the thermal conductivity of the hardened body tends to be improved. That is, the tap density of the agglomerated powder is, for example, 0.4 to 3.0 g / cm 3 , 0.4~2.0g / cm 3 , 0.4~1.0g / cm 3 , 0.6~3.0g / cm 3 , 0.6~2.0g / cm 3 , 0.6~1.0g / cm 3 , 0.7~3.0g / cm 3, 0.7~2.0g / cm 3 or 0.7 to 1.0 g / cm 3 It may be.

[0051] In this specification, the tap density of the agglomerated powder can be measured using a commercially available device in accordance with JIS R1628. 3 The mixture is filled into a special container and tapped under the conditions of a tapping time of 180 seconds, 180 tappings, and a tap lift of 18 mm, after which the bulk density is measured and this is taken as the tapped density.

[0052] The specific surface area of ​​the agglomerated powder is, for example, 1.5 m 2 / g or more, preferably 2.0m 2 / g or more, more preferably 2.5m 2 / g or more, more preferably 3.0m 2 / g or more, more preferably 3.5m 2 / g or more. This increases the contact area between the agglomerated powders in the insulating resin composition, making it easier to improve the thermal conductivity. In addition, the specific surface area of ​​the agglomerated powder is, for example, 12.0 m 2 / g or less, preferably 10.0m 2 / g or less, more preferably 8.0m 2 / g or less, more preferably 6.0m 2 / g or less. This tends to improve the coatability of the insulating resin composition and the insulating properties of the cured product. That is, the specific surface area of ​​the aggregated powder is, for example, 1.5 to 12.0 m 2 / g, 1.5-10.0m 2 / g, 1.5-8.0m 2 / g, 1.5-6.0m 2 / g, 2.0-12.0m 2 / g, 2.0-10.0m 2 / g, 2.0-8.0m 2 / g, 2.0-6.0m 2 / g, 2.5-12.0m 2 / g, 2.5-10.0m 2 / g, 2.5-8.0m 2 / g, 2.5-6.0m 2 / g, 3.0-12.0m 2 / g, 3.0-10.0m 2 / g, 3.0-8.0m 2 / g, 3.0-6.0m 2 / g, 3.5-12.0m 2 / g, 3.5-10.0m 2 / g, 3.5-8.0m 2 / g or 3.5~6.0m 2 / g.

[0053] In this specification, the specific surface area of ​​the agglomerated powder refers to a value calculated by using a commercially available measuring device that utilizes the gas adsorption phenomenon and applying the BET single point method as a method for calculating the specific surface area.

[0054] The agglomerated powder is preferably an agglomerated powder containing boron nitride, and more preferably an agglomerated powder composed of boron nitride (boron nitride agglomerated powder). The boron nitride agglomerated powder may be, for example, an agglomerate in which scaly primary particles of boron nitride are aggregated into a spherical shape.

[0055] In this embodiment, the inorganic filler may be a combination of agglomerated powder and a filler other than the agglomerated powder. The ratio of the agglomerated powder to the inorganic filler may be, for example, 30% by volume or more, preferably 50% by volume or more, more preferably 70% by volume or more, and even more preferably 90% by volume or more, and may be 95% by volume or more, or may be 100% by volume (i.e., no filler other than the agglomerated powder is included).

[0056] The content of the inorganic filler in the insulating resin composition is 30% by volume or more, preferably 35% by volume or more, more preferably 40% by volume or more, based on the total amount of the insulating resin composition. This tends to further improve the thermal conductivity of the cured product. In addition, the content of the inorganic filler in the insulating resin composition is 80% by volume or less, preferably 75% by volume or less, more preferably 70% by volume or less, based on the total amount of the insulating resin composition. This further improves the coatability of the insulating resin composition, making it easier to obtain a cured product with excellent insulation properties. That is, the content of the inorganic filler in the insulating resin composition may be, for example, 30 to 80% by volume, 30 to 75% by volume, 30 to 70% by volume, 35 to 80% by volume, 35 to 75% by volume, 35 to 70% by volume, 40 to 80% by volume, 40 to 75% by volume, or 40 to 70% by volume, based on the total amount of the insulating resin composition.

[0057] The inorganic filler may be blended in the insulating resin composition so that the content in the insulating resin cured body is within a predetermined range. From the viewpoint of further improving the thermal conductivity, the content of the inorganic filler in the insulating resin cured body is preferably 30% by volume or more, more preferably 35% by volume or more, and even more preferably 40% by volume or more. The content of the inorganic filler in the insulating resin cured body is preferably 80% by volume or less, more preferably 75% by volume or less, and may be 70% by volume or less. That is, the content of the inorganic filler in the insulating resin cured body may be, for example, 30 to 80% by volume, 30 to 75% by volume, 30 to 70% by volume, 35 to 80% by volume, 35 to 75% by volume, 35 to 70% by volume, 40 to 80% by volume, 40 to 75% by volume, or 40 to 70% by volume.

[0058] The volume of the inorganic filler can be determined by dividing the mass of the inorganic filler by the true specific gravity of the inorganic filler.

[0059] The insulating resin composition may further contain other components than those described above. For example, the insulating resin composition may further contain a curing accelerator, a discoloration inhibitor, a surfactant, a coupling agent, a colorant, a viscosity modifier, an antioxidant, an ion scavenger, etc., as necessary.

[0060] The content of other components is preferably 5 mass % or less, more preferably 2 mass % or less, based on the total amount of the insulating resin composition, and may be 0 mass %.

[0061] (Insulating resin hardened body) The insulating resin cured body of the present embodiment is a cured body of the insulating resin composition described above. The insulating resin cured body can form an insulating layer that has excellent insulation reliability, high heat cycle resistance, and high thermal conductivity under conditions of high temperature, high humidity, and high voltage application.

[0062] The insulating resin cured body of the present embodiment may contain, for example, a cured body of the above-mentioned resin component and an inorganic filler or a crushed product thereof, and preferably contains a cured body of the above-mentioned resin component and a crushed product of the inorganic filler.

[0063] The crosslink density of the insulating resin cured body is 1.0×10 -2 mol / cm 3 More preferably, it is 4.0×10 -2 mol / cm 3 It is more preferable that the crosslink density of the cured insulating resin is 8.0×10 or more. This improves the strength of the cured product and further suppresses the occurrence of cracks in a heat cycle test, thereby forming an insulating layer with excellent heat cycle resistance. In addition, the crosslink density of the cured insulating resin is 8.0×10 or more. -1 mol / cm 3 It is preferable that the value is less than 5.0×10 -1 mol / cm 3 This further improves the flexibility of the cured body, and an insulating layer having even better stress relaxation properties can be formed. That is, the crosslink density of the cured insulating resin body is, for example, 1.0×10 -2 ~8.0×10 -1 mol / cm 3 , 1.0×10 -2 ~5.0×10 -1 mol / cm 3 , 4.0×10 -2 ~8.0×10 -1 mol / cm 3 , or 4.0×10 -2 ~5.0×10-1 mol / cm 3 The crosslink density can be expressed as the ratio of -NH2 to the total number M1 of -NH2 in the amine-based curing agent. 1 The amount of the functional group can be appropriately adjusted by adjusting the ratio (M2 / M1) of the total number M2 of the epoxy resins or by adjusting the molecular weight and the number of functional groups of the epoxy resin.

[0064] In this specification, the crosslink density of the insulating resin cured body refers to a value calculated by the following method. <Method for measuring crosslink density> (1) Preparation of measurement samples The insulating resin cured body is cut with a diamond cutter into a plate measuring 1 mm x 3 mm x 40 mm to prepare a measurement sample. (2) Measurement of storage modulus The storage modulus of the measurement sample at temperature T1 (K) is measured by the DMA method (JIS K 0129 (2005)) using a dynamic viscoelasticity measuring device (manufactured by T&A Instruments, "RSA 3"). The temperature T1 is defined as the glass transition point of the resin component constituting the insulating resin cured body + 30 (K). The measurement is performed in the temperature range of -50°C to +250°C under conditions of a frequency of 10 Hz and a heating rate of 10°C / min. (3) Calculation of cross-link density From the above measurement results, the crosslink density (mol / cm 3 ) where the gas constant is 8.31429 J / (mol K). Crosslink density = storage modulus / (3 x gas constant x T1)

[0065] The storage modulus of the insulating resin cured body at −40° C. is preferably 100 GPa or less, more preferably 50 GPa or less. This tends to further improve the heat cycle property. There is no particular lower limit for the storage modulus of the insulating resin cured body at −40° C.

[0066] In this specification, the storage modulus of the insulating resin cured body refers to a value measured by the following method. <Method for measuring storage modulus> (1) Preparation of measurement samples The insulating resin cured body is cut into a plate of 1 mm x 3 mm x 40 mm size to prepare a measurement sample. (2) Measurement of storage modulus Using a dynamic viscoelasticity measuring device ("RSA 3" manufactured by T&A Instruments), the storage modulus is measured in the temperature range of -50°C to +250°C under conditions of a frequency of 10 Hz and a heating rate of 10°C / min.

[0067] The method for producing the insulating resin cured body is not particularly limited. For example, the insulating resin cured body can be produced by heat treating the insulating resin composition to cure it. The heat treatment may be carried out in one step or two steps. By carrying out the heat treatment in two steps, the insulating resin cured body can be formed via a semi-cured body of the insulating resin composition.

[0068] When the heat treatment is carried out in one step, the heat treatment temperature may be, for example, 40 to 220° C., and preferably 70 to 180° C., and the heat treatment time may be, for example, 0.5 to 48 hours, and preferably 1 to 6 hours.

[0069] When the heat treatment is carried out in two stages, the temperature of the first stage heat treatment may be, for example, 40 to 150° C., and preferably 50 to 100° C., and the heat treatment time may be, for example, 0.2 to 8 hours, and preferably 0.5 to 5 hours. The temperature of the second stage heat treatment may be, for example, 70 to 220° C., and preferably 120 to 180° C., and the heat treatment time may be, for example, 0.5 to 9 hours, and preferably 1 to 6 hours.

[0070] By carrying out a heat treatment while maintaining the insulating resin composition or a semi-cured product thereof in a predetermined shape, an insulating resin cured product having a predetermined shape can be obtained. For example, by applying the insulating resin composition onto a metal plate, laminating a metal foil as necessary, and curing the composition, a layered insulating resin cured product can be formed on the metal plate.

[0071] The insulating resin cured body may be produced by a production method including a step of curing the insulating resin composition or a semi-cured body thereof by hot pressing. In particular, when the inorganic filler contains aggregated powder, such a production method is preferable because it is possible to easily produce an insulating resin cured body containing a cured body of the resin component and crushed material of the inorganic filler.

[0072] The conditions of the hot press are not particularly limited. The pressing pressure may be, for example, 1 MPa or more, preferably 5 MPa or more, more preferably 8 MPa or more. This tends to suppress the generation of voids inside the hardened body and improve the insulation. The pressing pressure may be, for example, 30 MPa or less, preferably 25 MPa or less, more preferably 20 MPa or less. This tends to suppress excessive crushing of the aggregated powder and improve the thermal conductivity. The heating temperature may be the same as the temperature of the second heat treatment described above. That is, the pressing pressure may be, for example, 1 to 30 MPa, 1 to 25 MPa, 1 to 20 MPa, 5 to 30 MPa, 5 to 25 MPa, 5 to 20 MPa, 8 to 30 MPa, 8 to 25 MPa, or 8 to 20 MPa.

[0073] (Laminate) The laminate of the present embodiment includes a metal plate, a cured insulating resin body disposed on the metal plate, and a metal foil disposed on the cured insulating resin body. In the laminate of the present embodiment, the metal plate and the metal foil may be separated by the cured insulating resin body, and the cured insulating resin body may function as an insulating layer.

[0074] The metal material constituting the metal plate is not particularly limited, and examples thereof include aluminum, aluminum alloys, copper, copper alloys, iron, and iron alloys such as stainless steel. The metal plate may be made of one type of metal material, or may be made of two or more types of metal materials. In addition, the metal plate may have a single-layer structure or a multi-layer structure.

[0075] The thickness of the metal plate is not particularly limited, and may be, for example, 0.5 to 3.0 mm from the viewpoint of suitability for producing a circuit board.

[0076] The metal material constituting the metal foil is not particularly limited, and examples thereof include copper, aluminum, nickel, etc. The metal foil may be composed of one type of metal material, or may be composed of two or more types of metal materials. In addition, the metal foil may have a single-layer structure or a multi-layer structure.

[0077] The thickness of the metal foil is not particularly limited, and may be, for example, 0.009 to 1.0 mm from the viewpoint of suitability for producing a circuit board.

[0078] The thickness of the insulating resin cured body is not particularly limited, and may be, for example, 0.05 to 0.30 mm from the viewpoint of suitability for producing a circuit board.

[0079] The laminate preferably has a 90 degree peel strength of the metal foil of 2 N / cm or more, more preferably 4 N / cm or more at 85°C. Since such a laminate is likely to maintain sufficient adhesion between the metal foil and the cured insulating resin even under conditions of high temperature, high humidity and DC voltage application, the laminate can provide a circuit board with even better heat cycle resistance. The peel strength is measured by the method described above.

[0080] The method for producing the laminate is not particularly limited. For example, the laminate can be produced by a method including a step of applying an insulating resin composition onto a metal plate, curing or semi-curing the composition, and a step of bonding a metal foil onto the cured or semi-cured insulating resin composition (i.e., an insulating resin cured body or semi-cured body). The method may further include a step of curing the semi-cured body of the insulating resin composition (preferably a step of curing the semi-cured body of the insulating resin composition by hot pressing). The bonding of the metal foil may be performed by, for example, a roll lamination method, a lamination press method, or the like.

[0081] The laminate can also be produced by a method including a step of applying an insulating resin composition onto a metal foil and curing or semi-curing the composition, and a step of bonding a metal plate onto the cured or semi-cured insulating resin composition (i.e., an insulating resin cured body or semi-cured body). The method may further include a step of curing the semi-cured body of the insulating resin composition (preferably a step of curing the semi-cured body of the insulating resin composition by hot pressing).

[0082] Fig. 1 is a cross-sectional view showing a preferred embodiment of a laminate. The laminate 10 shown in Fig. 1 includes a metal plate 1, a metal foil 3, and an insulating layer 2 made of a cured insulating resin interposed between the metal plate 1 and the metal foil 3. By processing the metal foil 3 of the laminate 10 into a predetermined pattern, a circuit board can be easily formed.

[0083] (Circuit board) The circuit board of the present embodiment includes a metal plate, a cured insulating resin body disposed on the metal plate, and a circuit portion disposed on the cured insulating resin body. In the circuit board of the present embodiment, the metal plate and the circuit portion may be separated by the cured insulating resin body, and the cured insulating resin body may function as an insulating layer.

[0084] The metal plate may be, for example, the same as the metal plate in the laminate described above.

[0085] The circuit part may be made of a metal material. Examples of the metal material constituting the circuit part include the same metal material as the metal foil described above. The circuit part may be the metal foil described above processed into a predetermined pattern.

[0086] The thickness of the circuit portion is not particularly limited, and may be, for example, 0.035 to 0.5 mm from the viewpoint of the amount of current and heat dissipation.

[0087] The thickness of the insulating resin cured body is not particularly limited, and may be, for example, 0.07 to 0.2 mm from the viewpoints of insulation and heat dissipation.

[0088] The method for producing the circuit board is not particularly limited. For example, the circuit board can be produced by a method including a step of processing the metal foil of the above-mentioned laminate into a predetermined pattern. The method for processing (etching) the metal foil is not particularly limited, and a conventionally known method may be applied.

[0089] Fig. 2 is a cross-sectional view showing a preferred embodiment of a circuit board. The circuit board 20 shown in Fig. 2 includes a metal plate 1, a circuit portion 4, and an insulating layer 2 made of a cured insulating resin interposed between the metal plate 1 and the circuit portion 4. The circuit board 20 may be, for example, a circuit portion 4 formed by processing the metal foil 3 of the laminate 10.

[0090] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0092] <Example 1> (Amine-based hardener) As the amine-based curing agent, an amine-based curing agent (1) containing 37 mass% of an amine compound represented by the following formula (A-1-1), 17 mass% of an amine compound represented by the following formula (A-1-2), 32 mass% of an amine compound represented by the following formula (A-2-1), and 12 mass% of an amine compound represented by the following formula (A-2-2) was prepared. These amine compounds can be synthesized by known methods. [ka]

[0093] (Preparation of insulating resin composition) 35.9 parts by volume of bisphenol A type epoxy resin (EXA850CRP, manufactured by Mitsubishi Chemical Corporation, referred to as "epoxy resin (1)" in the table) and 14.07 parts by volume of the amine-based curing agent (1) were mixed by stirring at 25°C. Next, boron nitride agglomerated powder (manufactured by Denka Company, average particle size 60 μm, crushing strength 11 MPa, tap density 0.72 g / cm) was added. 3 , specific surface area 4.5m 2 / g, thermal conductivity 110 W / mK, referred to as "inorganic filler (1)" in the table.) 50.0 volume parts, hardening accelerator (2E4MZ, Shikoku Chemical Industry Co., Ltd., specific gravity 0.975 g / cm 3 0.2 parts by volume of the above was added and mixed with stirring for 15 minutes using a planetary mixer to obtain an insulating resin composition.

[0094] (Creating circuit boards) The insulating resin composition was applied onto a 0.05 mm thick polyethylene terephthalate (PET) film so that the thickness after curing would be 0.20 mm, and then heated at 100°C for 15 minutes to produce a sheet in a B-stage (semi-cured) state.

[0095] Next, the prepared sheet was peeled off from the PET film and placed on a copper plate with a thickness of 2.0 mm, and a copper foil with a thickness of 0.035 mm (GTS-MP, manufactured by Furukawa Circuit Foil Co., Ltd.) was placed on top of the copper plate. A surface pressure of 100 kgf / cm was applied using a press machine. 2 The mixture was then heated and cured at 180° C. for 180 minutes while applying pressure to obtain a laminate.

[0096] Next, after masking predetermined positions with an etching resist, the copper foil was etched using a sulfuric acid-hydrogen peroxide mixed solution as an etching solution. The etching resist was removed, and the copper foil was washed and dried to obtain a circuit board with a circular electrode of 20 mm in diameter made of copper foil.

[0097] <Example 2> A circuit board was obtained in the same manner as in Example 1, except that a naphthalene-type epoxy resin (HP4032D, manufactured by DIC Corporation, referred to as “epoxy resin (2)” in the table) was used instead of the bisphenol A-type epoxy resin, and the amounts of each component were changed as shown in Table 1.

[0098] <Example 3> As an amine-based curing agent, an amine-based curing agent (2) containing 50 mass% of an amine compound represented by formula (A-1-1), 18 mass% of an amine compound represented by formula (A-1-2), and 30 mass% of an amine compound represented by formula (A-2-2) was prepared. A circuit board was obtained in the same manner as in Example 1, except that the amine-based curing agent (2) was used instead of the amine-based curing agent (1) and the blending amounts of each component were changed as shown in Table 1.

[0099] <Examples 4 to 6> A circuit board was obtained in the same manner as in Example 1, except that the blending amounts of each component were changed as shown in Table 1 or Table 2.

[0100] <Example 7> Instead of inorganic filler (1), boron nitride agglomerated powder (manufactured by Denka Co., Ltd., average particle size 40 μm, crushing strength 11 MPa, tap density 0.77 g / cm 3 , specific surface area 4.5m 2 A circuit board was obtained in the same manner as in Example 1, except that an inorganic filler (2) having a molecular weight of 1.0 kg / g and a thermal conductivity of 110 W / mK was used, and the blending amounts of each component were changed as shown in Table 2.

[0101] <Example 8> Instead of the inorganic filler (1), boron nitride agglomerated powder (manufactured by Denka Co., Ltd., average particle size 70 μm, crushing strength 2 MPa, tap density 0.52 g / cm 3 , specific surface area 2.5m 2 A circuit board was obtained in the same manner as in Example 1, except that an inorganic filler (1) having a molecular weight of 1.5g / g and a thermal conductivity of 110 W / mK, which is represented in the table as “inorganic filler (3)”.

[0102] <Example 9> Instead of inorganic filler (1), boron nitride agglomerated powder (manufactured by Denka Co., Ltd., average particle size 40 μm, crushing strength 7.9 MPa, tap density 0.77 g / cm 3 , specific surface area 2.0m 2A circuit board was obtained in the same manner as in Example 1, except that an inorganic filler (4) having a molecular weight of 1.0 kg / g and a thermal conductivity of 110 W / mK was used, and the blending amounts of each component were changed as shown in Table 2.

[0103] <Example 10> A circuit board was obtained in the same manner as in Example 1, except that aluminum nitride filler (manufactured by Denka, average particle size 32 μm, thermal conductivity 180 W / mK, referred to in the table as "inorganic filler (5)") and alumina filler AA2 (manufactured by Sumitomo Chemical, average particle size 2 μm, thermal conductivity 30 W / mK, referred to in the table as "inorganic filler (6)") were used instead of inorganic filler (1) and the amounts of each component were changed as shown in Table 2.

[0104] <Comparative Example 1> A circuit board was obtained in the same manner as in Example 1, except that diaminodiphenylsulfone (DDS) was used as a curing agent instead of the amine-based curing agent (1) and the amounts of each component were changed as shown in Table 3.

[0105] <Comparative Example 2> A circuit board was obtained in the same manner as in Example 1, except that methylenedianiline (diaminodiphenylmethane, DDM) was used as a curing agent instead of the amine-based curing agent (1) and the amounts of each component were changed as shown in Table 3.

[0106] <Comparative Example 3> A circuit board was obtained in the same manner as in Example 1, except that a novolac-type phenolic resin (VH-4150, manufactured by DIC Corporation) was used as a curing agent instead of the amine-based curing agent (1) and the amounts of each component were changed as shown in Table 3.

[0107] <Comparative Example 4> A circuit board was obtained in the same manner as in Example 1, except that silica filler A-1 (manufactured by Tatsumori Co., Ltd., average particle size 12 μm, thermal conductivity 2 W / mK, referred to as "inorganic filler (7)" in the table) was used instead of inorganic filler (1) and the amount of each component was changed as shown in Table 3.

[0108] <Comparative Example 5> A circuit board was obtained in the same manner as in Example 1, except that the blending amounts of each component were changed as shown in Table 3.

[0109] The examples and comparative examples were evaluated by the following methods. The results are shown in Tables 1 to 3.

[0110] [Evaluation of thermal conductivity] The sheets in the B-stage (semi-cured) state obtained by the above method were stacked and press-molded to produce a thermally conductive sheet with a length of 10 mm, width of 10 mm and thickness of 0.5 mm. The thermal diffusivity α was measured by the laser flash method, and the thermal conductivity λ was calculated from the following formula. Note that the thermal conductivity should preferably be 8 W / mK or more. λ=α×Cp×ρ The specific heat Cp was calculated from DSC measurements. The specific gravity ρ of the thermally conductive sheet was calculated using the following formula, by measuring the weight of the sheet in air and in distilled water at a temperature of 25°C and an atmospheric pressure of 1013 hPa using a specific gravity measurement kit AD-1653 (product name) made by A&D Co., Ltd. ρ=A / (AB)×(ρ0-d)+d (In the formula, A represents the mass of the thermally conductive sheet in air, B represents the mass of the thermally conductive sheet in distilled water, ρ0 represents the density of distilled water, and d represents the density of air.)

[0111] [Insulation evaluation] The insulation strength of the circuit board obtained by the above method was measured using TOS 8650 (product name) manufactured by Kikusui Electronics Co., Ltd. in accordance with JIS C 6481. When the thermally conductive sheet is 0.20 mm thick, the insulation strength is preferably 8 kV or more (40 kV / mm or more).

[0112] [Storage modulus and crosslink density of cured insulating resin] The insulating resin composition was degassed in a vacuum, and then cured under the following curing conditions: 50°C for 3 hours and 160°C for 6 hours to obtain an insulating resin cured body. The obtained insulating resin cured body was cut out with a diamond cutter to obtain a plate-shaped measurement sample of 1 mm x 3 mm x 40 mm. The storage modulus of this measurement sample was measured at a temperature T1 (K) by the DMA method (JIS K 0129 (2005)) using a dynamic viscoelasticity measuring device (manufactured by T&A Instruments, "RSA 3"). The temperature T1 was set to the glass transition point of the resin component constituting the insulating resin cured body + 30 (K), and the storage modulus was measured in the temperature range of -50°C to +250°C under the conditions of a frequency of 10 Hz and a heating rate of 10°C / min. From the above measurement results, the crosslink density (mol / cm 3 ) was calculated. Crosslink density = storage modulus / (3 x gas constant x T1)

[0113] [Reliability evaluation by high temperature and high pressure bias test (THB)] A high temperature and high voltage bias test (THB) was conducted under test conditions of applying a DC voltage of 1200 V between the metal foil and metal plate in an environment of 85°C and 85% humidity. A rating of A was given for durability of 350 hours or more, and a rating of C for durability of less than 200 hours.

[0114] [Evaluation of heat cycle resistance] Six chip resistors measuring 2.0mm x 1.25mm were mounted on a circuit board using lead-tin eutectic solder, and a heat cycle test was carried out 500 times, with one cycle being -40℃ for 7 minutes and +125℃ for 7 minutes. After the test, the cross-sections of the connections between the solder and the components were observed using a 50x microscope to check for crack occurrence. The same test was carried out three times, and the number of connections that had cracks out of 18 connections (6 x 3 times) was calculated and evaluated.

[0115] [Table 1]

[0116] [Table 2]

[0117] [Table 3] [Explanation of symbols]

[0118] 1...metal plate, 2...insulating layer, 3...metal foil, 4...circuit portion, 10...laminate, 20...circuit board.

Claims

1. Epoxy resin, an amine-based curing agent containing a first amine compound represented by formula (A-1) and a second amine compound represented by formula (A-2); An inorganic filler having a thermal conductivity of 20 W / mK or more; Including, The content of the inorganic filler is 30 to 80% by volume, In the amine-based curing agent, the ratio of the total number M 2 of --NHR 1 to the total number M 1 of --NH 2 (M 2 / M 1 ) is 0.05 to 0.

30. [Formula 1] [In formula (A-1), n 1 represents an integer of 0 to 4; X 1 represents an alkanediyl group, an oxygen atom, or a sulfur atom. 1 When is 1 or more, there are multiple X 1 may be the same or different. [Case 2] [In formula (A-2), n 2 represents an integer of 0 to 4; X 2 represents an alkanediyl group, an oxygen atom or a sulfur atom, and Y represents -NH 2 Or -NHR 1 (R 1 represents a group represented by formula (Y-1). A plurality of Y's may be the same or different. However, at least one of the Y's is -NHR. 1 It is. 2 When is 1 or more, there are multiple X 2 may be the same or different. [C3] [In formula (Y-1), R 2 represents an alkyl group.

2. The insulating resin composition according to claim 1 , wherein the inorganic filler comprises an aggregate powder containing aggregates of primary particles.

3. 3. The insulating resin composition according to claim 2, wherein the aggregate powder has an average particle size of 20 to 100 μm.

4. 4. The insulating resin composition according to claim 2, wherein the crushing strength of the agglomerated powder is 1 to 30 MPa.

5. The tap density of the agglomerated powder is 0.7 to 2.0 g / cm 3 The insulating resin composition according to any one of claims 2 to 4.

6. The specific surface area of ​​the agglomerated powder is 3.0 to 10.0 m 2 The insulating resin composition according to any one of claims 2 to 5, wherein the molecular weight of the insulating resin composition is 100% or more.

7. The insulating resin composition according to any one of claims 2 to 6, wherein the agglomerated powder contains boron nitride.

8. The X 1 and the X 2 The insulating resin composition according to any one of claims 1 to 7, wherein is a methanediyl group.

9. The insulating resin composition according to any one of claims 1 to 8, wherein the content of the first amine compound in the amine-based curing agent is 30 to 60 mass% and the content of the second amine compound is 40 to 70 mass%.

10. 10. The insulating resin composition according to claim 1, wherein a ratio of an active hydrogen equivalent of the amine-based curing agent to an epoxy equivalent of the epoxy resin is 0.3 to 1.

5.

11. An insulating resin cured product, which is a cured product of the insulating resin composition according to any one of claims 1 to 10.

12. The insulating resin cured product according to claim 11 , comprising crushed pieces of the inorganic filler.

13. Crosslink density is 4.0 x 10 -2 ~5.0 x 10 -1 mol / cm 3The insulating resin cured product according to claim 11 or 12,

14. The insulating resin cured product according to any one of claims 11 to 13, having a storage modulus at -40°C of 100 GPa or less.

15. A method for producing a cured insulating resin product, comprising: curing the insulating resin composition or a semi-cured product thereof according to any one of claims 1 to 10 by hot pressing to produce a cured insulating resin product.

16. A laminate comprising a metal plate, the insulating resin cured body according to any one of claims 11 to 14 arranged on the metal plate, and a metal foil arranged on the insulating resin cured body.

17. A circuit board comprising: a metal plate; the insulating resin cured body according to any one of claims 11 to 14 disposed on the metal plate; and a circuit portion disposed on the insulating resin cured body.

Citation Information

Patent Citations

  • Liquid aromatic amine epoxy resin curing agent and preparation method thereof

    CN102532486A

  • Epoxy resin composition

    JP1983103526A

  • Method for constructing coke oven and temporary shed for constructing the coke oven

    JP2008266533A

  • Boron nitride powder and use thereof

    JP2014040341A

  • Epoxy resin composition, epoxy resin sheet and metal base circuit board using the same

    JP2017082091A