Glass-ceramic articles and methods of making same - Patents.com

A glass-ceramic product with a nanowrinkle layer addresses durability and cleaning challenges by enhancing ease of maintenance and aesthetic appeal, maintaining mechanical and optical properties, suitable for cooking hobs and other applications.

JP7566974B2Active Publication Date: 2024-10-15EUROKERA SOC & NOM COLLECTIF
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023080025
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-10-30
Filing Date
2023-05-15
Publication Date
2024-10-15
Estimated Expiration
2038-10-26

AI Technical Summary

Technical Problem

Existing glass-ceramic products, particularly cooking hobs, face challenges in maintaining durability, ease of cleaning, and aesthetic appeal while ensuring mechanical strength and optical properties, with coatings often complicating maintenance and potentially deteriorating over time.

Method used

A glass-ceramic product with a nanowrinkle layer formed by coating the substrate with materials like silicon, aluminum, titanium, zirconium, tin, and zinc nitrides, oxides, or carbides before ceramization, creating a satin-like surface that enhances cleaning ease and maintains mechanical strength without affecting optical transparency.

Benefits of technology

The nanowrinkle layer provides a durable, easy-to-clean surface with improved scratch resistance and unique aesthetic appearance, maintaining mechanical and optical properties even at high temperatures, suitable for cooking hobs and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566974000001
    Figure 0007566974000001
  • Figure 0007566974000002
    Figure 0007566974000002
  • Figure 0007566974000003
    Figure 0007566974000003
Patent Text Reader

Abstract

To provide a glass-ceramic article which is more functional and practical while taking care of particularly thermal and mechanical limitations.SOLUTION: The present invention relates to a glass-ceramic article, intended in particular to be used with at least one light source and / or at least one heating element, the article comprising at least one substrate, such as a plate, made of glass-ceramic, the substrate being at least partially provided, in particular coated, with at least one nano-wrinkled layer. The present invention also relates to a method for obtaining the article.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of glass ceramics. More specifically, the present invention relates to an article or product made of glass ceramic, in particular intended to cover a heating element or to receive a heating element, for example a cooking hob. A glass ceramic article or an article made of glass ceramic is defined as an article based on a substrate of glass ceramic material, for example a glass ceramic plate, which substrate can, if necessary, be equipped with accessories or additional (decorative or functional) elements required for its final use. The article can refer to the substrate only or to a substrate equipped with additional equipment (for example a cooking hob equipped with a control panel, its heating elements, etc.). The present invention also relates to a method for obtaining the above-mentioned article. [Background technology]

[0002] There are several commonly used glass-ceramic products, particularly glass-ceramic hobs, which are very popular with home appliance dealers, manufacturers, and users, and this success is due in particular to the attractive appearance and ease of cleaning of these hobs.

[0003] Glass-ceramics are originally glasses, also known as precursor or parent or green glasses, whose specific chemical composition allows for a controlled crystallization induced by a suitable heat treatment, called ceramization. This specific, partially crystallized structure gives glass-ceramics their characteristic properties.

[0004] Currently, there are different types of glass-ceramic hobs, each of these variants being the result of extensive research and countless tests; since it is very difficult to modify these hobs and / or their manufacturing methods without the risk of adversely affecting the desired properties, in particular for use as a cooking hob, the glass-ceramic plate must generally have a transmittance at wavelengths of visible light that is low enough to obscure at least some of the heating elements underneath when not in use, and, depending on the case (radiative heating, induction heating, etc.), a transmittance at wavelengths of visible light that is high enough to allow the user to visually detect the heating elements during use, depending on the case (radiative heating, induction heating, etc.); it must also have a high transmittance at wavelengths in the infrared range, in particular in the case of plates with radiative burners. The glass-ceramic hob must also have sufficient mechanical strength required in the field of its use. In particular for use as a cooking hob in the field of domestic appliances, the glass-ceramic hob must have good resistance (for example defined according to EN60335-2-6) to pressure, impacts (supports and drops of cookware, etc.).

[0005] The most common glass-ceramic hobs are dark in colour, in particular black or brown or orange-brown, but there are also hobs with a relatively light appearance (in particular white, for example white with at least 50% haze as described in French Patent No. 2 766 816) or even transparent hobs, usually equipped with an opacifying coating or filter for special colour effects.

[0006] Known (functional and / or decorative) coatings for glass-ceramic hobs conventionally comprise enamels that are based on glass frits and pigments. One advantage of enamels is that they can be deposited on the precursor glass (or on the parent glass or on the green glass) before ceramming and can be fired during ceramming. They can also withstand high temperatures and allow the use of different heating media for the plates. However, they can locally reduce the mechanical resistance of the glass-ceramic plates, can spall, especially in the case of thick deposits or those produced in several passes, and furthermore certain colors are not feasible or difficult to obtain (especially in a single pass). Firing of the enamels can also result in the appearance of undesirable shades (e.g. brown or grey in the case of black enamels).

[0007] It is also known to use certain high-temperature resistant paints, in particular silicon-based paints, which are deposited on the substrate after ceramization, but their use remains more limited than that of enamels due to their relatively low resistance, in particular to heat and friction. Summary of the Invention [Problem to be solved by the invention]

[0008] A continuing concern in the field of glass-ceramics is to be able to provide products that are easy to clean and that maintain their appearance and properties over time, whether the glass-ceramic is coated or uncoated. Adding a coating often makes this maintenance even more complicated, because when the glass-ceramic is cleaned, the layer may deteriorate, or the optical or mechanical properties of the glass-ceramic may change.

[0009] The present invention aims to provide a glass-ceramic product, in particular a novel glass-ceramic plate intended for use with one or more heating elements, for example a cooking hob, which is increasingly functional and practical, while respecting the constraints, in particular the thermal and mechanical constraints characteristic of the use of the abovementioned products, and in particular to obtain a glass-ceramic product that is durable and easy to maintain, taking into account the proposal of a simple and preferably flexible solution that allows for the presence of decorations, if necessary, or additional functions as required. [Means for solving the problem]

[0010] This object is achieved by the method developed according to the present invention and the resulting glass-ceramic product thus developed. [Brief description of the drawings]

[0011] [Figure 1] Figure 1a is a schematic, not to scale, cross-section of a portion of a substrate or coated parent glass substrate used to obtain an article according to the invention, and Figure 1b is the substrate or substrate portion obtained after ceramification of the substrate or substrate portion of Figure 1a. [Figure 2a] FIG. 2a shows an optical microscope image of a nanowrinkled surface obtained in accordance with a first exemplary embodiment of the present invention. [Figure 2b] FIG. 2b shows an optical microscope image of a nanowrinkled surface obtained in accordance with a second exemplary embodiment of the present invention. [Figure 2c] FIG. 2c shows an optical microscope image of a nanowrinkled surface obtained in accordance with a third exemplary embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention therefore relates to a novel glass-ceramic article (or product), which has at least one substrate (or support), e.g. a plate, made of a glass-ceramic (material), which is at least partially (on its surface, on at least a part of at least one side) provided with, in particular coated with, at least one nanowrinkle layer (a layer that is nanowrinkled).

[0013] The invention also relates to a method for producing such a glass-ceramic article (having at least one glass-ceramic substrate) from a glass substrate (a parent glass substrate, which forms a glass-ceramic substrate by ceramization), in which at least one layer of a material selected from the group of nitrides and / or oxides and / or carbides and / or alloys of one or more of the elements silicon, aluminum, titanium, zirconium, tin and zinc is applied to at least a portion of the aforementioned glass substrate (parent glass) before ceramization, and the thus coated glass substrate (parent glass substrate) is ceramized, and this ceramization makes it possible to obtain a glass-ceramic substrate at least partially coated with at least one nanowrinkle layer as described above.

[0014] Nanowrinkles (nanofolds) means wrinkles or curved undulations or distortions (or changes of direction that do not form angles or sharp angles) with alternating grooves and ridges on the nanoscale, i.e. wrinkles with an amplitude (or difference in height between the highest point of each wrinkle, the peak of the ridge, and the lowest point, the bottom of the groove) that does not exceed about 1 μm, in particular wrinkles with an amplitude of (strictly) less than 5 μm, more precisely (strictly) less than 2 μm, in particular less than or equal to 1 μm, preferably (strictly) less than 1 μm. The amplitude of the (or each) wrinkle is advantageously a few nanometers to a few hundred nanometers, with the average amplitude (arithmetic mean) generally being around a few hundred nanometers, as specified below.

[0015] The invention is based on the deposition of a layer, in particular of the thin type (whose thickness does not exceed a few tens of μm, in particular does not exceed 20 μm, in particular in this case less than a few μm, in particular less than 2 μm), of a material selected from the above-mentioned group (a so-called "hard" material compared to the glass substrate during ceramization; the glass substrate becomes less viscous and behaves like a soft substrate compared to the layers of the above-mentioned materials, which are relatively hard), on the parent glass before ceramization, which leads to a wrinkled layer (pleating) at the surface on the nanoscale after the heat treatment of ceramization (which is generally carried out at high temperatures of more than 900° C.), and the substrate wrinkles at the surface, which visually undergoes a change in its appearance (the coated surface becomes relatively matte and exhibits a satin metallic appearance in particular in reflection, compared to the uncoated or recoated surface after ceramization. The satin appearance is intermediate between matte and glossy), and which exhibits new and unexpected technical advantages, such as a significant ease of cleaning.

[0016] As will be described below, it is also possible to use a stack of layers or other layers above or below the aforementioned layers, in which case the entire coating is advantageously nanowrinkled. The product according to the invention obtained after ceramming shows good adhesion of the nanowrinkle layer or nanowrinkle coating to the glass-ceramic substrate or to any adjacent layers that may be present on the substrate (without the need for pretreatment of the substrate and / or the use of adhesion promoters, tie layers or primers). This layer or coating is particularly resistant to high temperatures, not showing any peeling even after a thermal shock (for example at about 600° C.). This layer or coating also has good scratch resistance and does not mechanically embrittle the glass-ceramic substrate (unlike, for example, enamel).

[0017] Thus, the invention makes it possible to develop a glass-ceramic product with a nanowrinkled surface in the desired location (for example, over the entire surface of one side or only in a few areas, for example in areas that are relatively frequently exposed to handling or dirt, for example in control or display areas or heating areas, etc.), which can be obtained by the method defined above and has various advantages, such as the advantage of allowing relatively little adhesion of food to the nanowrinkled area or areas or to the surface or surfaces, and the advantage of being significantly easier to clean, as mentioned above, while at the same time the product retains the hardness and mechanical hand strength required for various uses, in particular as a cooking hob. Furthermore, the nanowrinkle layer or nanowrinkle coating does not adversely affect the light transmission of the glass ceramic in the area or areas of interest, while allowing light scattering that prevents glare to the user and has a unique satin-like aesthetic appearance. This nanowrinkling also unexpectedly makes it possible to obtain different types of colors in reflection without the need for additional dyes or pigments or filters (unlike other types of layers), particularly by adjusting the thickness and composition of the nanowrinkle layer as specified below.

[0018] The solution according to the invention therefore makes it possible to obtain functional and aesthetic areas in any desired area of ​​the product in a simple and economical way, without complex operations (the layers can be deposited by low-pressure deposition techniques, for example cathodic sputtering, as shown below), in a durable and highly flexible manner, even if these areas are intended to be exposed to high temperatures. In particular, the article according to the invention has good heat resistance, which is compatible with the use of different types of heaters, and does not cause problems of maintenance, scratches or friction, as mentioned above. In particular, the product according to the invention does not undergo thermal degradation at temperatures of 400° C. or more, which are temperatures that can be reached, in particular in applications such as use as a cooking hob.

[0019] As mentioned above, the article according to the invention has a substrate, which is at least partially (i.e. in or on at least one region of the substrate, on at least one surface or even on multiple surfaces) provided (or equipped) with or coated with at least one layer that is nanowrinkled or a coating in the form of at least one layer that is nanowrinkled. This texture, called nanowrinkles in this case, is located on the surface of the substrate in the desired regions, achieves the above-mentioned advantages, and is observed both in the substrate itself (in its surface layer) and in the coating that would have produced this nanowrinkling. This texture has alternating depressions and protuberances in the form of folds with a certain amplitude and periodicity, and the folds are generally (preferably to obtain the desired effect) multidirectional, the folds that are formed extending in multiple directions parallel to the surface of the substrate, forming an isotropic texture or structure, as explained below in Figures 2a, 2b and 2c. This texture is reflected in the surface layer of the glass-ceramic substrate and replaces any initial micro-roughness in the surface of the parent glass, so that this texture constitutes only roughness with an amplitude of less than 5 μm in the region (or regions) of the substrate where this nanowrinkle layer is provided (if there are other regions that do not have this texture, these other regions can have other textures or superimposed textures if necessary).

[0020] The profile or morphological appearance of this texture or nanowrinkles generally resembles a quasi-periodic curve, which may vary, within certain constraints defined below, depending on the thickness of the coating layer, its nature, and the temperature, process time or applied stress during the manufacturing method used. For example, as mentioned above, the method defined according to the invention provides a shrinkage forming texture that is usually isotropic, but if the substrate is sufficiently soft during the ceramization or cooling stage, it is also possible to control the direction of the wrinkles by applying anisotropic deformations or stresses to the substrate, for example by applying a unidirectional traction simultaneously with cooling. The resulting nanowrinkles may therefore be in a single or main direction (they may be unidirectional nanowrinkles) and / or may be anisotropic, if necessary. The thickness of the coating layer and its nature also influence the morphology of the wrinkles, in particular their period and amplitude, as well as (in particular) the reflective intensity L of the area provided with the coating. * This affects the color of the coating (depending on the

[0021] The nanowrinkles of the present invention are in the form of wrinkles, undulations, ripples or pleats, in particular having peaks that are substantially rounded, (quasi-)periodic, somewhat sinuous and generally multi-directional, with ridges and valleys of substantially constant width and amplitude, as described below in Figures 2a, 2b and 2c.

[0022] The nanowrinkle layer, or the folds of this layer or of the nanowrinkle coating, advantageously have quasi-periodic steps or intervals (the average distance, i.e. the arithmetic mean, between the highest points of two successive peaks or ridges or between the lowest points of two successive depressions) that are between 10 nm and 40,000 nm, preferably between 100 nm and 10,000 nm, in particular between 500 nm and 8,500 nm, in particular more than 500 nm and less than 8,000 nm, or less than 6,000 nm, or less than 5,000 nm, and have an amplitude of less than 5 μm, more precisely less than 2 μm, in particular less than 1 μm, preferably less than 1 μm, in particular between 4 nm and 900 nm, preferably between 50 nm and 850 nm. Measurement and analysis of the period and corrugations is carried out, for example, by atomic force microscopy (AFM) or optical profilometry (for example a stylus profilometer marketed by Bruker under the trade name Dektak), in particular on an analysis surface of 80 μm×80 μm, for example with 1024 measurement points.

[0023] Advantageously, the ratio of period to amplitude (i.e. the ratio of period to amplitude or period in relation to amplitude, expressed in nanometers) is between 4 and 20, preferably between 5 and 15, in particular between 8 and 14, in particular from about 10 to about 12.

[0024] Advantageously, the nanowrinkle layer is a coating layer, i.e., as opposed to the case where the nanowrinkle layer is a surface layer of the substrate (where the substrate is "comprised" of this layer, rather than "coated" by it) (as described below), the substrate is coated (at its surface in the relevant areas) with the above-mentioned layer, in particular the nanowrinkle layer is a layer or coating applied before ceramization and resulting in wrinkles (pleats) during ceramization, which layer or coating may optionally be subsequently covered by one or more further layers, so that the nanowrinkle profile of the final coating is preserved. This nanowrinkle layer is advantageously made of a material selected from the group of one or more nitrides and / or oxides and / or carbides and / or alloys of silicon, aluminum, titanium, zirconium, tin and zinc, as already seen in the method. Preferably, the material of the layer is selected from the group of nitrides and / or oxides of one or more of the elements silicon, aluminum, titanium, zirconium, tin and zinc, in particular Si 3 N 4 , SiO 2 , TiO 2 , ZnO, SnZnO, or SnO 2 and particularly preferably, this material is silicon nitride (Si 3 N 4 ) or silicon oxide (SiO 2 ), more particularly silicon nitride.

[0025] The nanowrinkle layer coating the substrate is most simply and commonly in the form of a single layer (monolayer) of a material selected from the above-mentioned materials, but it is also possible to have a nanowrinkle layer formed from a stack of (sub-)layers each selected from the above-mentioned materials (all sub-layers forming a layer and being nanowrinkled), or the above-mentioned nanowrinkle layer according to the present invention may itself be part of a stack of layers (a stack which may contain other layers of materials different from the above-mentioned materials), which together form the final coating, which is itself advantageously nanowrinkled.

[0026] The thickness of the nanowrinkle coating, whether formed of the above-mentioned layer (if necessary formed of a stack of quasi-layers) or formed of several layers, is generally between 20 nm and 2000 nm, and may be greater than or equal to 50 nm and less than or equal to 300 nm, in particular less than or equal to 200 nm, with the layers made of materials selected from the above-mentioned materials being thin-film type layers, in particular having a thickness of about 20 nm to about 200 nm, respectively.

[0027] Preferably, the ratio between the thickness of the nanowrinkle layer deposited before ceramming and resulting in wrinkling (pleating) during ceramming and one or more amplitudes of this nanowrinkle layer (i.e. the ratio of thickness to amplitude, expressed in nanometers) is between 0.15 and 0.30, preferably between 0.20 and 0.28, in particular between 0.21 and 0.27.

[0028] The substrate according to the invention may also be coated with other non-nanowrinkle layers according to the invention, which are deposited, for example after ceramization, have a functional and / or decorative effect and are deposited in areas other than the nanowrinkled areas, for example regular enamel-based patterns or paint layers in other parts of the substrate different from the nanowrinkle part or parts.

[0029] The coating layer used for nanowrinkling according to the method of the present invention may later be removed by chemical etching or laser ablation, leaving the surface layer of the glass-ceramic substrate itself as the nanowrinkle layer, which is also advantageous from a cleaning point of view.

[0030] The wrinkles (folds) of the surface layer of the substrate correspond to the nanowrinkles or nanowrinkle layer or nanowrinkle coating. The wrinkles do not destroy the (very good) adhesion between the glass ceramic and the nanowrinkle layer or nanowrinkle coating or nanowrinkle layer, and the resulting nanowrinkles or nanowrinkle coating or nanowrinkle layer does not have air bubbles.

[0031] As mentioned above, nanowrinkles are particularly and advantageously obtained by the procedure indicated in the method according to the invention, namely by applying at least one layer of a material selected from the above-mentioned materials to at least a part of a parent glass substrate which, upon ceramization, results in a glass-ceramic substrate, and then ceramizing the glass substrate thus coated.

[0032] Just to be clear, the manufacture of glass-ceramic hobs is generally carried out as follows: in a melting furnace, a glass of a selected composition is melted to form a glass ceramic, the molten glass is laminated into standard ribbons or sheets by passing the molten glass between laminating rollers, and the glass ribbons are cut to the desired dimensions, and the plates thus cut are then cerammed in a manner known per se; ceramming involves firing the plates according to a selected thermal profile, thereby converting the glass into a polycrystalline material called "glass ceramic", which has a zero or practically zero coefficient of thermal expansion and is particularly resistant to thermal shocks that can reach up to 700°C. Generally, ceramming involves gradually increasing the temperature to the nucleation range, which is generally near the glass transition range, raising it above the nucleation range (e.g., between 650°C and 830°C) for a few minutes (e.g., between 5 and 60 minutes), further increasing the temperature to allow crystal growth (e.g., ceramming in the range of 850°C to 1000°C; the ceramming stage temperature is maintained for a few minutes (e.g., 5 to 30 minutes)), and then rapidly cooling to room temperature.

[0033] The application or deposition of the layer (or each layer, if necessary) of a material selected from the abovementioned materials on the parent glass before ceramming can be carried out by any suitable and rapid technique capable of forming a layer of this type, particularly flat or uniform, in particular by deposition methods under low pressure, in particular magnetron-assisted, such as cathode sputtering, or by chemical vapor deposition (CVD), if necessary plasma-enhanced chemical vapor deposition (PECVD). The application is preferably carried out by cathode sputtering, in particular magnetron-assisted cathode sputtering.

[0034] The coated substrate is then subjected to a ceramming heat treatment (at temperatures up to 850-1000°C) as described above, usually for a period of several tens of minutes. During the high-temperature ceramming step, the glass substrate loses its viscosity, the glass densifies (crystallization of the glass matrix) and undergoes a volumetric reduction or shrinkage (usually isotropic if no stress is applied), in particular a volumetric reduction or shrinkage of about 1.5%. The shrinkage of the substrate results from the temperature increase above the glass transition temperature of the substrate glass and the subsequent cooling of the substrate, as well as the difference between the thermal shrinkage of the substrate glass and the thermal shrinkage of the coating layer, causing the layer and the glass surface to wrinkle or wrinkle. The wrinkles do not destroy the adhesion between the glass ceramic and the thin layer, and the method does not produce bubbles.

[0035] By this method nanoscale wrinkling of the coated areas is easily achieved, potentially over a large area. The surface of the coated areas becomes satin-like and diffuse and pleasant to the touch. The nanowrinkles can replace any microscopic roughness of the original glass surface, if desired.

[0036] If necessary, the method may include a cutting operation (generally prior to ceramming), e.g. by water jet, mechanical wheel tracing, etc., followed by a shaping operation (grinding, chamfering, etc.).

[0037] The nanowrinkle layer or coating can cover only a portion of the substrate, or it can cover all of one surface, for example, an upper surface at a position of use that is particularly susceptible to cleaning, or it can cover all or a portion of a lower surface of the substrate.

[0038] Preferably, the substrate (or the article according to the invention, when it is formed only from the substrate) is a plate, in particular a plate intended to be used with, in particular to cover or receive, at least one light source and / or heating element. This substrate (or this plate) is generally geometrically shaped, in particular rectangular, or even square, or even circular or elliptical, etc., and generally has an "upper" or "outer" face in the position of use (the visible face or the face facing the user), another "lower" or "inner" face in the position of use (generally hidden, for example in a frame or box of a fixture), and a slice (or edge or thickness). The upper face is generally flat and smooth, but may also have at least one raised area and / or at least one recessed area and / or at least one opening and / or at least one chamfered edge (these features are added during the manufacture of the substrate, for example by rolling or folding or pressing, etc., or by reworking). Such variations in features advantageously constitute a continuous variation of the plate (without changes in material or accessories). The lower face may also be flat and smooth, or may be provided with pins.

[0039] The thickness of the glass-ceramic substrate is generally at least 2 mm, in particular at least 2.5 mm, advantageously less than 15 mm, in particular between about 3 mm and 15 mm, in particular about 3 mm to 8 mm or about 3 mm to 6 mm. The substrate is preferably a flat or quasi-flat plate (in particular a plate having a deflection of less than 0.1% in the diagonal direction of the plate, preferably about 0).

[0040] The substrate may be based on any glass ceramic, which advantageously has a zero or substantially zero CTE, in particular a thermal expansion coefficient of 30×10 between 20° C. and 700° C. (in absolute value). -7 K -1 Less than 15×10 between 20°C and 700°C -7 K -1 Less than or even 5×10 -7 K -1 have a CTE of less than

[0041] Preferably, a substrate is used with a dark appearance, with low transparency and low diffusion, in particular based on any glass ceramic having an intrinsic light transmission in the range of 0.8% to 40%, in particular 0.8% to 5%, in particular 0.8% to 2%, and an optical transmission (determined in a known manner by taking the ratio between the transmitted and incident intensities at a given wavelength) of at least 2.5% for a wavelength of 625 nm included in the visible range. "Intrinsic" means that the plate has such a transmission as such, without the presence of any coating. In particular, a substrate is used with a black or brown appearance, which in combination with a light source arranged below allows to display illuminated areas or decorations while hiding any elements below. It may in particular be based on a black glass ceramic having crystals of β-quartz structure in the residual glass phase, the absolute value of whose expansion coefficient is advantageously less than 15×10 -7 K -1 Less than or even 5×10 -7 K -1It may be a glass ceramic of the type described below, for example of the plate sold by Eurokera under the name Kerablack+, in particular an arsenic-refined glass ceramic of the composition described in EP 0 437 228 A or US 5 070 045 A or FR 2 657 079 A, ​​or a tin-refined glass ceramic containing less than 0.2% arsenic oxide, for example of the composition described in WO 2012 / 156444, or a glass ceramic refined with one or more sulfides, as described in WO 2008053110.

[0042] Alternatively, a transparent substrate can be used, which is coated, if necessary, with an opacifying coating, typically on its lower surface, for example with sheets sold under the name Keralite™ by Eurokera.

[0043] The above-mentioned substrate (which may preferably be dark in appearance or opaque and transparent) provided with a nanowrinkle layer or nanowrinkle coating has in particular a light transmittance LT between 0% and 10%, a light reflectance between 8% and 20% and a diffusion coefficient of more than 90%.

[0044] The optical measurements are carried out in accordance with EN410. In particular, the light transmittance LT is measured in accordance with EN410 using luminant D65 and is the total transmittance (in particular integrated in the visible range and weighted by the sensitivity curve of the human eye), taking into account the direct and possibly diffuse transmittance. The measurements are carried out, for example, using a spectrophotometer with an integrating sphere (in particular by a spectrophotometer marketed by Perkin Elmer under the name Lambda 950). The light reflection is also measured in total reflection mode by a spectrophotometer (for example a spectrophotometer marketed by Perkin Elmer under the name Lambda 950). The degree of light scattering is defined as the ratio of the diffuse transmittance to the total transmittance using luminant D65 and is also evaluated, for example, by a spectrophotometer with an integrating sphere used for the measurement of light transmittance and light reflection.

[0045] As mentioned above, the presence on the substrate of other types of coatings than the above-mentioned layers is not excluded, in particular other functional layers (scratch-resistant layers, anti-overflow layers, opacifying layers, etc.) or additional, in particular local, decoration (e.g. enamel on the upper side to form simple patterns or logos).

[0046] The article according to the invention may further comprise, in association with or in combination with the substrate, one or more light sources and / or one or more heating elements (or, for example, one or more radiant or halogen elements and / or one or more ambient atmosphere gas burners and / or one or more induction heating elements), typically located below the substrate.

[0047] The source or sources may be integrated into and / or coupled to one or more display type structures (e.g. 7-segment LEDs), electronic control panels with touch-sensitive buttons and digital displays, etc. The light sources may advantageously be formed by light-emitting diodes arranged at a certain distance apart, which may be associated with one or more optical guides.

[0048] The article may optionally have at least one waveguide in combination with the light source for propagating light from one part of the article to another (particularly by total internal reflection or by metallic reflection), one or more light sources working in concert with the guide(s) and for example coupled to and / or irradiating through an end of the associated guide(s), and / or one or more filters below the substrate, typically between the light source(s) and the substrate.

[0049] The article according to the invention may in particular be a cooking hob or any glass-ceramic article, for example a glass-ceramic worktop or a central island, or even a console-type piece of furniture (for example with the substrate forming the upper part), etc., with a display or at least one lighting area with functional or decorative features, and / or a heating element. In its most common application, the article according to the invention is intended to be used as a cooking hob, which is generally intended to be integrated into a stove top or range, which also has a heating element, for example a radiant or halogen burner or an induction heating element. In another advantageous application, the article according to the invention is a worktop with a different display, and not necessarily a cooking area.

[0050] The article may also include (or be associated with) one or more additional functional elements (a frame, one or more connectors, one or more cables, one or more control elements, etc.).

[0051] The accompanying non-limiting drawings serve to illustrate the invention.

[0052] FIG. 1b shows an article, or part of an article, according to the invention, having a glass-ceramic substrate 1 and coated with a nanowrinkle layer 2 of a material selected from nitrides and / or oxides and / or carbides and / or alloys of one or more elements selected from silicon, aluminum, titanium, zirconium, tin and zinc; the nanowrinkle layer formed by alternating depressions 3 and protuberances 4 has an amplitude a of less than 5 μm, more precisely less than 2 μm, in particular less than or equal to 1 μm, preferably less than 1 μm, in particular between 4 nm and 900 nm, preferably between 50 nm and 850 nm, a period p of between 10 nm and 40000 nm, preferably between 100 nm and 10000 nm, in particular between 500 nm and 8500 nm, and a thickness e (uniform over the entire surface of the layer) of about 20 nm to about 200 nm. The nanowrinkles are reproduced in the thickness of the coating layer and over a certain depth of the glass-ceramic substrate that corresponds to the amplitude of the wrinkles; the substrate surface 1a carrying the coating and the coating layer 2 are intimately integrated with each other, thus forming a single assembly with an identical profile.

[0053] This substrate is obtained by ceramming a parent glass substrate 1' (Fig. 1a) coated in selected areas with a layer 2'. The layer 2' is a flat-shaped layer of material selected from the group of nitrides and / or oxides and / or carbides and / or alloys of one or more of the elements silicon, aluminum, titanium, zirconium, tin and zinc, deposited for example by cathode sputtering, in particular magnetron-assisted sputtering. This layer has the same thickness as the nanowrinkle layer obtained after ceramming.

[0054] The nanowrinkle layer (shown in simplified cross section in FIG. 1b) is generally isotropic and quasi-periodic. Optical microscope images of nanowrinkle surfaces 2a, 2b, 2c obtained in three different exemplary products formed according to the invention by varying the thickness of the coating layer are shown; the thickness is 50 nm in FIG. 2a, 100 nm in FIG. 2b, and 200 nm in FIG. 2c. The deposited layer is a silicon nitride layer, the glass-ceramic substrate is a translucent black glass-ceramic marketed by Eurokera under the name KeraBlack+ or KeraVision, the plate having a smooth upper surface and a smooth lower surface and a thickness of 4 mm.

[0055] The resulting nanowrinkle surface is mostly in the form of elongated, more or less sinuous folds (wrinkles), each of which has a substantially constant width, is multidirectional (in several directions) and is practically isotropic. The period (quasi-period) between two folds is 2000 nm for a 50 nm thick layer, 5000 nm for a 100 nm thick layer and 8000 nm for a 200 nm thick layer, respectively. The amplitude is 185 nm for a 50 nm thick layer, 450 nm for a 100 nm thick layer and 800 nm for a 200 nm thick layer, respectively. The ratio between the period and the amplitude (period to amplitude) is 10.81 for a 50 nm thick layer, 11.11 for a 100 nm thick layer and 10 for a 200 nm thick layer, respectively. The ratio between thickness and amplitude (thickness to amplitude) is 0.27 for the 50 nm thick layer, 0.22 for the 100 nm thick layer, and 0.25 for the 200 nm thick layer, respectively.

[0056] The substrate and the resulting nanowrinkle layer showed no peeling after a thermal shock at 620° C., and no deterioration in appearance after 100 hours at 580° C.

[0057] The substrate and resulting nanowrinkle layer also showed improved ease in cleaning with tomato paste carbonized for 20 minutes at 200° C. Fewer than five double wipes with a conventional yellow sponge (without a scrubbing surface) soaked in water were required to completely clean the surface of the nanowrinkle-bearing substrate.

[0058] The coatings were also found to reduce the formation of scratches during cleaning. The light transmittance obtained for the various substrates coated with the coatings of the thicknesses tested (50, 100, and 200 nm in this example) was about 1%, the light reflectance was between 8% and 20%, and the light scattering degree was greater than 90%, respectively.

[0059] For comparison, the same test was performed on the same glass ceramic plate without nanowrinkle coating. In the test of cleaning tomato paste carbonized at 200°C for 20 minutes, more than 30 double wipes were required with the same water-soaked sponge described above to completely clean the surface. In addition, the surface had relatively many visible scratches. In addition, about 1% light transmittance, less than 5% light reflectance, and less than 5% light scattering were obtained for this plate.

[0060] For comparison, the same test was carried out on the same glass-ceramic plate, but in this case coated with a 200 nm thick silicon nitride layer and deposited after ceramization (thus without nanowrinkling). In a test to clean a tomato concentrate carbonized at 200°C for 20 minutes, more than 30 double wipes with the same water-soaked sponge described above were required to completely clean the surface. Also, a light transmittance of about 1%, a light reflectance of about 20%, and a light scattering degree of less than 5% were obtained for this plate.

[0061] The articles according to the invention, in particular the plates, can be advantageously used in particular to create novel cooking hobs for stove tops or ranges, or novel work tables, consoles, sideboards, central islands, etc. The invention according to the present disclosure includes the following aspects: <Aspect 1> A glass-ceramic article, in particular intended to be used with at least one light source and / or at least one heating element, the article comprises at least one substrate, e.g. a plate, made of glass ceramic, The substrate is at least partially provided with at least one nanowrinkle layer, in particular coated with at least one nanowrinkle layer; Glass-ceramic articles. <Aspect 2> 2. The glass-ceramic article of embodiment 1, wherein the nanowrinkle layer has a period and an amplitude such that the ratio between the period and the amplitude is between 4 and 20, preferably between 5 and 15, in particular between 8 and 14. <Aspect 3> 3. The glass-ceramic article according to claim 1 or 2, characterized in that the nanowrinkle layer has a period between 10 nm and 40000 nm, preferably between 100 nm and 10000 nm, in particular between 500 nm and 8500 nm. <Aspect 4> 4. The glass-ceramic article according to any one of the preceding claims, characterized in that the nanowrinkle layer has an amplitude of less than 5 μm, more precisely less than 2 μm, in particular equal to or less than 1 μm, preferably less than 1 μm, in particular between 4 nm and 900 nm, preferably between 50 nm and 850 nm. <Aspect 5> 5. The glass-ceramic article of any one of claims 1 to 4, wherein the nanowrinkle layer is isotropic. <Aspect 6> 6. The glass-ceramic article of any one of the preceding claims, wherein the nanowrinkle layer is a coating layer of a material selected from the group of nitrides and / or oxides and / or carbides and / or alloys of one or more of the following elements: silicon, aluminum, titanium, zirconium, tin, and zinc. <Aspect 7> 7. The glass-ceramic article according to any one of the preceding claims, characterized in that the nanowrinkle coating has a thickness between 20 and 2000 nm, preferably 50 nm or more and 300 nm or less, in particular 200 nm or less. <Aspect 8> 8. The glass-ceramic article of any one of the preceding claims, wherein the nanowrinkle layer is a layer deposited prior to ceramming of a glass substrate to form the glass-ceramic substrate, and wherein the layer provides wrinkling during ceramming of the glass substrate to the glass-ceramic substrate. <Aspect 9> 9. The glass-ceramic article according to embodiment 8, wherein the ratio between the thickness of the nanowrinkle layer and the amplitude of the layer is between 0.15 and 0.30, preferably between 0.20 and 0.28, in particular between 0.21 and 0.27. <Aspect 10> 10. The glass-ceramic article of any one of the preceding claims, wherein the nanowrinkle layer is a surface layer of the glass-ceramic substrate itself. <Aspect 11> 11. The glass-ceramic article of any one of the preceding claims, wherein the article or substrate is a cooking hob or worktop. <Aspect 12> applying at least one layer of a material selected from the group of nitrides and / or oxides and / or carbides and / or alloys of one or more of the elements silicon, aluminum, titanium, zirconium, tin, and zinc to at least a portion of the glass substrate; and ceramizing the thus coated glass substrate; A method of making the glass-ceramic article of any one of embodiments 1-11. <Aspect 13> 13. The method according to embodiment 12, wherein the layer is subsequently removed, for example by chemical etching or laser ablation.

Claims

1. A glass-ceramic article intended for use with at least one light source and / or at least one heating element, the article comprises at least one substrate, e.g. a plate, made of glass ceramic, The substrate is at least partially provided with at least one nanowrinkle layer; the nanowrinkle layer has a period and an amplitude such that the ratio between the period and the amplitude is between 8 and 14; The nanowrinkle layer has a period between 10 nm and 40,000 nm; The nanowrinkle layer has an amplitude between 4 nm and 900 nm; the ratio between the thickness of the nanowrinkle layer and the amplitude of the layer is between 0.15 and 0.30; The nanowrinkle layer is a coating layer of a material selected from the group consisting of nitrides and / or oxides and / or carbides and / or alloys of one or more elements of silicon, aluminum, titanium, zirconium, tin, and zinc; The article or substrate is a cooking hob or worktop; Glass-ceramic articles.

2. A glass-ceramic article intended for use with at least one light source and / or at least one heating element, comprising: the article comprises at least one substrate, e.g. a plate, made of glass ceramic, The substrate is at least partially provided with at least one nanowrinkle layer; the nanowrinkle layer has a period and an amplitude such that the ratio between the period and the amplitude is between 8 and 14; The nanowrinkle layer has a period between 10 nm and 40,000 nm; The nanowrinkle layer has an amplitude between 4 nm and 900 nm; the ratio between the thickness of the nanowrinkle layer and the amplitude of the layer is between 0.15 and 0.30; The nanowrinkle layer is a coating layer, and the thickness of the nanowrinkle coating is between 20 nm and 2000 nm, preferably 50 nm or more and 300 nm or less, in particular 200 nm or less; The article or substrate is a cooking hob or worktop; Glass-ceramic articles.

3. 3. The glass-ceramic article according to claim 1 or 2, characterized in that the nanowrinkle layer has a period between 500 nm and 8500 nm.

4. 4. The glass-ceramic article according to claim 1, wherein the nanowrinkle layer has an amplitude between 50 nm and 850 nm.

5. The glass-ceramic article according to any one of claims 1 to 4, characterized in that the nanowrinkle layer is isotropic.

6. applying at least one layer of a material selected from the group of nitrides and / or oxides and / or carbides and / or alloys of one or more of the elements silicon, aluminum, titanium, zirconium, tin, and zinc to at least a portion of the glass substrate; and ceramizing the thus coated glass substrate; A method for producing the glass-ceramic article of any one of claims 1 to 5.

7. A method for producing a glass-ceramic article intended to be used with at least one light source and / or at least one heating element, comprising: the article comprises at least one substrate, e.g. a plate, made of glass ceramic, The substrate is at least partially provided with at least one nanowrinkle layer; the nanowrinkle layer has a period and an amplitude such that the ratio between the period and the amplitude is between 8 and 14; The nanowrinkle layer has a period between 10 nm and 40,000 nm; The nanowrinkle layer has an amplitude between 4 nm and 900 nm; The ratio between the thickness of the nanowrinkle layer and the amplitude of the layer is between 0.15 and 0.

30. The nanowrinkle layer is a coating layer, depositing a layer prior to ceramming of a glass substrate to form the glass-ceramic substrate, the layer providing wrinkling during ceramming of the glass substrate to the glass-ceramic substrate. method.

8. 8. The method according to claim 7, characterized in that the ratio between the thickness of the nanowrinkle layer and the amplitude of the layer is between 0.15 and 0.30, preferably between 0.20 and 0.28, in particular between 0.21 and 0.27.

Citation Information

Patent Citations

  • Stain-proof glass

    JP2002326841A

  • Sheet-like glass-ceramic body having at least one matted portion, and method for manufacturing glass-ceramic body of the same kind

    JP2005220011A

  • Top plate for cooking device

    JP2015176753A

  • Method of decorating a substrate surface and articles thereby

    US20160368308A1

  • Display cover member and method for manufacturing same

    WO2015137196A1