Separator for electrochemical device and method for manufacturing same
The separation membrane with an inorganic coating layer using composite particles and a binder polymer enhances electrode adhesion, addressing binding strength issues and maintaining energy density and stability.
Patent Information
- Application Number
- JP2023505757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-18
- Filing Date
- 2021-09-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-09-15
AI Technical Summary
Existing separation membranes for electrochemical devices face challenges in achieving high binding strength with electrodes, leading to gaps and poor cycle life due to the flexibility of soft pack exteriors, and current solutions compromise energy density or increase resistance.
A separation membrane with an inorganic coating layer containing composite particles coated with a coupling compound and a binder polymer, such as PVAc or EVA, promotes phase separation under humid conditions to enhance binding strength and electrode adhesion.
The membrane achieves improved binding force with electrodes, maintaining energy density and reducing resistance, while being chemically and electrochemically stable, and suitable for mass production.
Smart Images

Figure 0007567026000008 
Figure 0007567026000009 
Figure 0007567026000010
Abstract
Description
[Technical field]
[0001] This application claims priority based on Korean Patent Application No. 10-2020-0120881, filed September 18, 2020.
[0002] The present invention relates to a separator for an electrochemical device and a method for manufacturing the same, and more particularly, to a separator for an electrochemical device including inorganic particles and having improved adhesion to an electrode, and a method for manufacturing the same. [Background technology]
[0003] Recently, lithium ion secondary batteries are widely used as power sources for portable electronic devices such as notebook computers, mobile phones, digital cameras, camcorders, etc. In addition, these lithium ion secondary batteries are also used in transportation such as electric vehicles due to their high energy density.
[0004] As portable electronic devices become smaller and lighter, the exterior of nonaqueous secondary batteries is being simplified. Initially, stainless steel battery cans were used as the exterior, but aluminum can exteriors were developed, and currently soft-pack exteriors made of aluminum laminate packs are also being developed. In the case of soft-pack exteriors made of aluminum laminate, the exterior is flexible, so gaps may form between the electrodes and the separator during charging and discharging, which poses a technical issue of poor cycle life. From the perspective of solving this issue, technology for bonding the electrodes and the separator is important, and many technical proposals have been made.
[0005] Typically, a separator for an electrochemical device has a structure including a porous polymer film (separator substrate) and an inorganic coating layer formed on at least one surface of the separator substrate. The inorganic coating layer includes inorganic particles and a binder polymer, and is introduced to improve the durability (e.g., prevention of membrane breakage) and heat resistance (e.g., prevention of thermal shrinkage) of the separator substrate. PVdF (Polyvinylidene fluoride)-based resins are mainly used as the binder polymer of such separators, and an adhesive surface layer having a high binder resin content is formed near the surface of the inorganic coating layer by migrating the binder resin to the separator surface through a humidified phase separation method. However, the adhesive strength of the PVdF-based resin itself is not high, and it is difficult to ensure a high level of binding strength. To improve the adhesive strength, the content of the binder polymer can be increased or the amount of coating can be increased, but this undesirably increases the thickness of the adhesive layer, lowers the energy density, and increases the resistance. The adhesive layer of the separator must be able to exhibit both high adhesive strength and high ionic conductivity even when it is thin, the separator must be made of a chemically and electrochemically stable material in order to stably use the battery for a long period of time, and the separator manufacturing process must be highly productive and allow for mass production at low cost. As a result, there is a growing demand for the development of a separator for secondary batteries that satisfies the above requirements. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a separator including an inorganic coating layer having improved adhesion to an electrode. Another object of the present invention is to provide a method for manufacturing a separator having the above characteristics. It will be readily understood that the other objects and advantages of the present invention can be achieved by the means or methods described in the claims and combinations thereof. [Means for solving the problem]
[0007] A first aspect of the present invention relates to a separator for an electrochemical device, the separator comprising a porous polymer film substrate and an inorganic coating layer formed on at least one surface of the substrate, the inorganic coating layer comprising inorganic particles and a binder polymer. In the present invention, the inorganic particles comprise composite particles having at least a portion of a surface of the inorganic particles coated with a coupling compound, the coupling compound has introduced therein functional groups capable of binding the inorganic particles to a binder resin, the functional groups comprising at least one selected from an alkyl group, an alkoxy group and an ester group, and the binder polymer comprises an amorphous polymer and / or a partially crystalline polymer having a glass transition temperature (Tg) of 60° C. or less.
[0008] A second aspect of the present invention is the above-mentioned first aspect, wherein the binder polymer contains one or more compounds represented by the following chemical formula 1: [ka] In the above Chemical Formula 1, R is each independently -H, -OR4, -C(=O)-R4, -C(=O)O-R4, -OC(=O)-R4 or -C(=O)NH-R4, and R4 is each independently hydrogen or a substituted or unsubstituted C1 to C5 alkyl group, m is an integer of 1 or more, and n is 0 or an integer of 1 or more.
[0009] In a third aspect of the present invention, in the second aspect, the binder polymer includes at least one selected from polyvinyl acetate (PVAc) and ethylene-vinyl acetate copolymer (polyethylene-co-vinyl acetate).
[0010] A fourth aspect of the present invention is any one of the first to third aspects, wherein the binder polymer has a weight average molecular weight (Mw) of 600,000 or less.
[0011] A fifth aspect of the present invention is any one of the first to fourth aspects, wherein the coupling compound includes a silane-based compound and / or a titanate-based compound.
[0012] A sixth aspect of the present invention is directed to any one of the first to fifth aspects, wherein the inorganic coating layer contains the inorganic particles in a ratio of 50% by weight or more relative to 100% by weight of the total amount of the binder polymer and the inorganic particles, and has a porous structure due to interstitial volumes between the inorganic particles.
[0013] A seventh aspect of the present invention is any one of the first to sixth aspects, wherein the inorganic coating layer includes an electrode adhesive portion in which a binder polymer is distributed at a higher concentration in a surface layer portion than in other portions.
[0014] An eighth aspect of the present invention is any one of the first to seventh aspects, wherein the binder polymer further includes a crystalline binder resin.
[0015] A ninth aspect of the present invention is a method for manufacturing a separator according to any one of the first to eighth aspects, the method including: preparing a polymer solution by adding a solvent and a binder polymer; preparing a slurry for forming an inorganic coating layer by adding inorganic particles to the polymer solution; and coating the slurry on a surface of a porous polymer film substrate and drying the substrate under humidified conditions to perform a humid phase separation process, wherein an electrode adhesive portion having a high binder resin content is formed on a surface of the inorganic coating layer by the humid phase separation process.
[0016] A tenth aspect of the present invention relates to the ninth aspect, wherein the inorganic particles include composite particles coated with a coupling compound. Effect of the Invention
[0017] In the separator according to the present invention, the inorganic coating layer contains a partially crystalline and / or amorphous polymer such as PVAc and EVA as a binder polymer, and the surfaces of the inorganic particles are coated with a coupling agent to prevent the inorganic particles from being detached from the inorganic coating layer. In addition, when the separator is manufactured, phase separation is promoted under humid conditions, and an adhesive part where a large amount of the binder polymer is distributed on the surface of the separator is provided, thereby improving the binding strength with the electrode. [Brief description of the drawings]
[0018] The drawings attached to this specification are illustrative of preferred embodiments of the present invention, and serve to facilitate a better understanding of the technical concept of the present invention together with the above-mentioned contents of the invention, and therefore the present invention should not be interpreted as being limited to only the matters shown in such drawings. Meanwhile, the shape, size, scale, ratio, etc. of elements in the drawings included in this specification are exaggerated in order to emphasize a clearer description.
[0019] [Figure 1] 1 is a schematic diagram illustrating a cross-sectional structure of a separation membrane according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing the results of IR measurement of Composite Particle 1 of an example. [Diagram 3] 1 is an image showing the surface of a separation membrane obtained through Example 1 of the present invention. [Figure 4] 1 is an image showing the surface of a separation membrane obtained through Comparative Example 9 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described in detail below. Prior to this, the terms or words used in the present specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that correspond to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention. Therefore, the configurations shown in the embodiments and drawings described in this specification are merely the most preferable embodiment of the present invention, and do not represent the technical idea of the present invention, so it should be understood that there are various equivalents and modifications that can replace them at the time of this application.
[0021] Throughout the specification of this application, when a part "comprises" a certain element, this does not mean to exclude other elements, but means that it may further include other elements, unless specifically stated to the contrary.
[0022] In addition, the terms "about," "substantially," and the like used throughout the specification of this application are used to mean a numerical value or close to a numerical value when given manufacturing and material tolerances inherent in the stated meaning, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute numerical values are stated to aid in the understanding of this application.
[0023] Throughout the specification of this application, the statement "A and / or B" means "A or B or all of these."
[0024] Certain terminology has been used in the accompanying detailed description of the invention for convenience only and is not intended to be limiting. The words "right", "left", "top" and "bottom" designate directions in the drawings to which reference is made. The words "inwardly" and "outwardly" designate directions toward or away from the geometric center of the designated device, system or component thereof, respectively. "Front", "rear", "upper", "lower" and related words and phrases designate locations and orientations in the drawings to which reference is made and are not intended to be limiting. Such terms include the above-listed words, derivatives thereof and words of similar import.
[0025] Meanwhile, in this specification, unless otherwise specified, the content ratio is based on weight.
[0026] The present invention relates to a separator for an electrochemical device and a method for manufacturing the same. In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy by an electrochemical reaction and is a concept that includes a primary battery and a secondary battery. The secondary battery is capable of being charged and discharged and is a concept that includes a lithium ion battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc.
[0027] 1.Separation membrane 1) Structure of the separation membrane The separator 100 according to the present invention includes a porous polymer substrate 110 and an inorganic coating layer 120 formed on at least one surface of the porous polymer substrate 110. The inorganic coating layer includes inorganic particles and a binder polymer.
[0028] In the present invention, the binder polymer includes an amorphous and / or partially crystalline polymer. In addition, in the present invention, at least a part or the whole of the surface of the inorganic particles is coated with a coupling compound. In addition, the inorganic coating layer may have a porous structure due to the space (interstitial volume) between the inorganic particles. In addition, in one embodiment of the present invention, the inorganic coating layer has an adhesive part having a high content of the binder polymer in a predetermined thickness on the surface layer, thereby providing a strong binding force with the electrode.
[0029] In one embodiment of the present invention, the separation membrane has a thickness of 5 to 30 μm, and is appropriately adjusted within the above range, for example, 10 μm or more or 25 μm or less, and has an air permeability of about 50 to 3000 sec / 100 cc.
[0030] The term "permeability" as used herein means the time it takes for 100cc of air to pass through a measurement target such as a separator or a porous polymer substrate, and may be expressed in units of seconds / 100cc, interchangeably with permeability, and is usually expressed as a Gurley value, etc. In a specific embodiment of the present invention, the permeability is measured in accordance with JIS P8117.
[0031] Meanwhile, in the present invention, the porosity and pore size are measured using an adsorption gas such as nitrogen using BELSORP (BET equipment) manufactured by BEL JAPAN, or by a method such as mercury intrusion porosimetry or capillary flow porosimetry. Alternatively, in one embodiment of the present invention, the thickness and weight of the obtained inorganic coating layer are measured, and the porosity can be calculated from the measured thickness and weight and the theoretical density of the inorganic coating layer.
[0032] 2) Porous polymer base material The porous polymer substrate refers to a substrate having a plurality of pores formed therein, the pores being interconnected with each other and allowing gas or liquid to pass from one side of the substrate to the other side, while blocking electrical contact between the negative electrode and the positive electrode and providing a porous ion-conducting barrier through which ions pass.
[0033] The material constituting such a porous polymer substrate can be any organic or inorganic material having electrical insulation. In particular, from the viewpoint of imparting a shutdown function to the substrate, it is desirable to use a thermoplastic resin as the constituent material of the substrate. Here, the shutdown function refers to a function in which, when the battery temperature becomes high, the thermoplastic resin dissolves and closes the holes in the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery. As the thermoplastic resin, a thermoplastic resin having a melting point of less than 200°C is suitable, and polyolefin is particularly desirable.
[0034] In addition, the porous polymer substrate may further include at least one of polymer resins such as polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene. The porous polymer substrate may be, but is not limited to, a nonwoven fabric, a porous polymer film, or a laminate of two or more of these.
[0035] Specifically, the porous polymer substrate is any one of the following a) to e).
[0036] a) A porous film formed by melting / extruding a polymer resin; b) a multilayer film having two or more layers of the porous film of a) laminated thereon; c) a nonwoven web produced by accumulating filaments obtained by melting / spinning a polymer resin; d) a multilayer film having two or more layers of the nonwoven fabric web of b) laminated thereon; e) A porous composite membrane having a multi-layer structure comprising two or more of the above a) to d).
[0037] In the present invention, the porous polymer substrate preferably has a thickness of 3 to 12 μm or 5 to 12 μm. If the thickness is less than this range, the conductive barrier function is insufficient, while if the thickness is excessively beyond this range (i.e., if it is too thick), the resistance of the separator increases excessively.
[0038] In one embodiment of the present invention, the weight-average molecular weight of the polyolefin is preferably 100,000 (g / mol) to 5,000,000. If the weight-average molecular weight is less than 100,000, it may be difficult to ensure sufficient mechanical properties. If it is more than 5,000,000, the shutdown characteristics may be deteriorated or molding may be difficult.
[0039] In the present specification, the term molecular weight refers to weight average molecular weight (Mw). The unit may be g / mol. Such molecular weight may be measured, for example, by gel permeation chromatography (GPC, PL GPC220, Agilent Technologies).
[0040] The puncture strength of the porous polymer substrate is 300 gf or more from the viewpoint of improving the production yield. The puncture strength of the porous substrate refers to the maximum puncture load (gf) measured by a puncture test using a Kato tech KES-G5 handy compression tester under the conditions of a needle tip curvature radius of 0.5 mm and a puncture speed of 2 mm / sec.
[0041] In a specific embodiment of the present invention, the porous polymer substrate may be any planar porous polymer substrate used in electrochemical devices. For example, an insulating thin film having high ion permeability and mechanical strength, a pore diameter of typically 10 to 100 nm, and a thickness of typically 5 to 12 μm may be used.
[0042] 3) Inorganic coating layer In the present invention, the separator includes an inorganic coating layer formed on at least one surface of the porous polymer substrate. The inorganic coating layer includes a mixture including a binder polymer and inorganic particles. The inorganic coating layer is attached to each other by a binder (i.e., the binder polymer connects and fixes the inorganic particles) so that the inorganic particles can be kept bound to each other within the layer. In one embodiment, the inorganic particles are densely packed together and may have a number of micropores due to interstitial volumes formed between the inorganic particles. These micropores are connected to each other to form a porous structure that allows gas or liquid to pass from one side to the other side. In one embodiment of the present invention, the inorganic particles are coated on all or at least a part of the surface with a binder polymer, and the particles are bound to each other by the binder polymer through surface and / or point bonding. In one embodiment of the present invention, the inorganic particles are included in the inorganic coating layer at a ratio of 50% by weight or more, preferably 60% by weight or more, 70% by weight or more, or 80% by weight or more, based on 100% by weight of the total amount of the binder polymer and the inorganic particles, and more preferably 95% by weight or less, or 90% by weight or less, within the above range.
[0043] The inorganic coating layer preferably has a thickness of 1 to 5 μm on one side of the porous polymer substrate. The thickness is preferably 3 μm or more, and within this range, the adhesive strength with the electrode is excellent, resulting in increased cell strength of the battery. On the other hand, if the thickness is 4 μm or less, it is advantageous in terms of cycle characteristics and resistance characteristics of the battery.
[0044] Meanwhile, in the present invention, the inorganic coating layer has an electrode adhesive part 121 having a high content of binder polymer in the surface part due to the characteristics of the manufacturing method described below. FIG. 1 is a schematic diagram of a cross-sectional structure of a separator 100 according to an embodiment of the present invention. Referring to FIG. 1, the separator of the present invention has an inorganic coating layer 120 formed on the surface of a porous polymer substrate 110, and the binder polymer is distributed in a higher concentration in the surface part of the inorganic coating layer than in other parts. In this specification, for convenience of explanation, the surface part where the binder polymer is distributed in a higher concentration is referred to as the "electrode adhesive part 121". In one embodiment of the present invention, the electrode adhesive part is a result of the binder polymer migrating to the surface part by a manufacturing method such as humid phase separation. Therefore, the electrode adhesive part is not a structure physically separated from the inorganic coating layer, but is inseparably bonded to the surface of the inorganic coating layer as a part of the inorganic coating layer, and the thickness of the electrode adhesive part is non-uniform.
[0045] B. Inorganic coating layer material B1. Binder polymer In one embodiment of the present invention, the binder polymer includes a semi-crystalline polymer, an amorphous-crystalline polymer, or a mixture thereof. In one embodiment of the present invention, in consideration of improving the adhesive strength between the electrode and the separator, the semi-crystalline polymer has a crystallinity of 60% or less. Specifically, the binder polymer may include one or more compounds represented by the following Chemical Formula 1:
[0046] [ka]
[0047] In the above formula 1, R is each independently -H, -OR4, -C(=O)-R4, -C(=O)O-R4, -OC(=O)-R4, or -C(=O)NH-R4. In addition, R4 is each independently hydrogen or a substituted or unsubstituted C1-C5 alkyl group. The m is an integer of 1 or more, and the n is 0 or an integer of 1 or more. In one embodiment of the present invention, the compound of the above formula 1 may include at least one selected from polyvinyl acetate (PVAc) and ethylene-vinyl acetate copolymer.
[0048] In one embodiment of the present invention, the crystallinity is expressed as a percentage by dividing the melting enthalpy (ΔH) value actually measured by DSC by the melting enthalpy (ΔH) value of a theoretical perfect crystal (crystallinity 100%). Here, the melting enthalpy value of a theoretical perfect crystal can be found in the Polymer Handbook for known polymers, and can be calculated by extrapolation of the crystallinity of unknown or newly synthesized materials by extending the crystallinity of two or more points.
[0049] In one embodiment of the present invention, the binder polymer has a glass transition temperature of 60° C. or less, preferably 30 to 50° C. When the binder polymer satisfies this range, the adhesive strength between the separator and the electrode is improved, for example, an electrode-separator adhesive strength of 300 gf / 25 mm (60° C., 6.5 MPa) or more can be secured. In the present invention, the adhesive strength is based on the result of dissolving the binder polymer in acetone at a concentration of 5 wt%, coating it on a polymer film substrate at 23° C. and a relative humidity of 45%, adhering the obtained resultant to an electrode at 60° C. and 6.5 MPa, and measuring the peel strength.
[0050] Meanwhile, in one embodiment of the present invention, the binder polymer preferably has a weight average molecular weight (Mw) of 600,000 or less. If the molecular weight (Mw) exceeds this range, it is difficult to ensure sufficient electrode adhesive strength.
[0051] In the present specification, the term molecular weight refers to weight average molecular weight (Mw), the unit of which can be g / mol, and such molecular weight can be measured, for example, by gel permeation chromatography (GPC, PL GPC220, Agilent Technologies).
[0052] Meanwhile, in one embodiment of the present invention, the binder polymer may further include a fluorine-based binder polymer such as polyvinylidene fluoride, polyvinylidene hexafluoroethylene, polyvinylidene trifluoride (TrFE), polyvinylidene chlorofluoroethylene (CTFE), polyvinylidene 1,2-difluoroethylene, or polyvinylidene tetrafluoroethylene (TFE). In addition, the binder may further include polymethylmethacrylate, polybutylacrylate, polybutylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, acetylpropionylcellulose, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose, etc. As the additional binder polymer, one or more of the above examples may be added. The content of the additional binder polymer is appropriately adjusted in consideration of adhesive strength, for example, in the range of 30 wt % or less with respect to 100 wt % of the binder polymer.
[0053] In one embodiment of the present invention, the inorganic coating layer may further include an additive such as a dispersant and / or a thickener in an amount of 1 to 3 wt % based on 100 wt % of the inorganic coating layer. In one embodiment of the present invention, the additive may be one or more selected from the group consisting of polyvinylpyrolidone (PVP), polyvinylalcohol (PVA), hydroxyethyl cellulose (HEC), hydroxypropyl cellulose (HPC), ethylhydroxy ethyl cellulose (EHEC), methyl cellulose (MC), carboxymethyl cellulose (CMC), hydroxyalkyl methyl cellulose, and cyanoethyl polyvinyl alcohol.
[0054] B2.Inorganic particles In a specific embodiment of the present invention, the inorganic particles are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present invention are not particularly limited as long as they do not undergo oxidation and / or reduction reactions within the operating voltage range of the applied electrochemical device (e.g., 0 to 5 V based on Li / Li+). In particular, when inorganic particles having a high dielectric constant are used as the inorganic particles, they can contribute to an increase in the dissociation degree of the electrolyte salt, for example, the lithium salt, in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte solution.
[0055] For the reasons described above, it is preferable that the inorganic particles include high dielectric constant inorganic particles having a dielectric constant of 5 or more, preferably 10 or more. Non-limiting examples of inorganic particles having a dielectric constant of 5 or more include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti yO3 (PLZT, 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O3 - PbTiO3 (PMN - PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, AlOOH, SiC, and TiO2, or mixtures thereof, etc.
[0056] Also, as the inorganic particles, inorganic particles having lithium ion transport ability, that is, inorganic particles containing lithium element but not storing lithium and having the function of moving lithium ions can be used. Non - limiting examples of inorganic particles having lithium ion transport ability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y - based glass such as 14Li2O - 9Al2O3 - 38TiO2 - 39P2O5 (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), Li 3.25 Ge 0.25 P 0.75 S4 such as lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride such as Li3N (Li x N y , 0 < x < 4, 0 < y < 2), SiS2 - based glass such as Li3PO4 - Li2S - SiS2 (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), P2S5 - based glass such as LiI - Li2S - P2S5 (Li xP y S z There are, for example, cases where 0 < x < 3, 0 < y < 3, 0 < z < 7, or a mixture thereof, etc.
[0057] On the other hand, in one embodiment of the present invention, the inorganic particles may include composite particles whose surfaces are coated with a coupling compound. At least a part or all of the surface of the composite particles is coated with the coupling compound. In this specification, the coating means that the coupling agent is bonded or adhered to the surface of the inorganic particles by chemical, physical, electrochemical, or other methods.
[0058] In a specific embodiment of the present invention, the coupling agent has at least one or more functional groups selected from an alkyl group, an alkoxy group, or an ester group. For example, there are silane - based coupling agents, fatty acids, titanate - based coupling agents, etc., and one or two or more of them are used.
[0059] On the other hand, when the coupling agent contains an alkyl group, it is desirable that the number of carbon atoms is 8 or less. When the number of carbon atoms exceeds 8, the dispersibility in a highly polar ketone - based solvent such as acetone is low, which is disadvantageous for the production of the slurry for forming the inorganic coating layer.
[0060] The silane coupling agent may include two or more functional groups selected from the group consisting of a phenyl group, a vinyl group, an epoxy group, an amino group, an acryloxy group, a methacryloxy group, a methoxy group, an ethoxy group, an alkyl group, an isocyanurate group, and an isocyanate group. Examples of such silane coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, ... Examples of the silane include trimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, decyltrimethoxysilane, and trifluoropropyltrimethoxysilane. Of these, one or a mixture of two or more types may be used.
[0061] Examples of the fatty acid include stearic acid, palmitic acid, lauric acid, oleic acid, and linoleic acid, and one or a mixture of two or more of these may be used.
[0062] Examples of the titanate coupling agent include monoalkoxy titanate, neoalkoxy titanate, isopropyl tridioctyl phosphate titanate, isopropyl tridioctyl pyrophosphate titanate, oleyl titanate, isopropyl trioleyl titanate, isopropyl tristearyl titanate, and isopropyl triisostearyl titanate. Examples of such titanium acylates include tributoxytitanium stearate, isopropoxytitanium triisostearate, and mono-i-propoxytitanium tri-i-stearate; titanium alkoxides include titanium tetraethoxide, titanium tetrapropoxide, titanium tetrabutoxide, tetracyclohexyl titanate, and tetrabenzyl titanate; and titanium chelates include di-n-butoxy bis(triethanolaminate)titanium, titanium diisopropoxy bis(acetylacetonate), titanium tetraacetylacetonate, titanium di-2-ethylhexoxy bis(2-ethyl-3-hydroxyhexoxide), and titanium diisopropoxy bis(ethyl acetoacetate). These may be used alone or in mixtures of two or more kinds.
[0063] Meanwhile, the average particle size of the inorganic particles is not particularly limited, but is preferably in the range of 0.1 to 1.5 μm in order to form an inorganic coating layer of uniform thickness and to have a suitable porosity. If it is less than 0.1 μm, the dispersibility decreases, and if it exceeds 1.5 μm, the thickness of the inorganic coating layer formed increases.
[0064] 2. Manufacturing method of inorganic coating layer A method for manufacturing a separator according to one aspect of the present invention includes the steps of preparing a slurry for an inorganic coating layer, the slurry including inorganic particles, a binder polymer, and a solvent; and coating or drying the slurry on at least one surface of a separator substrate. The drying step is performed under humid conditions. Alternatively, the drying step is performed by drying the porous substrate coated with the slurry in a non-solvent for the binder polymer, for example, under humid conditions, so that the binder resin is solidified and migrates to the separator surface.
[0065] First, a polymer binder solution is prepared by dissolving the prepared binder polymer in a solvent. Then, the polymer binder solution is added to a mixture containing inorganic particles and a solvent, and mixed to prepare a slurry for forming an inorganic coating layer. The inorganic particles are added in a state of being crushed to have a predetermined average particle size. Alternatively, the inorganic particles can be added and then crushed and dispersed while controlling the average particle size to have a predetermined size using a ball mill method or the like. An auxiliary agent such as a dispersant can be further added to the mixture and / or slurry as necessary.
[0066] Next, the binder polymer is applied onto a porous polymer substrate and allowed to stand for a predetermined period of time under humid conditions to solidify (dry).
[0067] Under such humidification conditions, the binder polymer is solidified, and phase separation of the binder polymer in the slurry is induced. In one embodiment of the present invention, the humidification conditions are a relative humidity of about 30 to 70%. During the phase separation, the solvent migrates to the surface of the inorganic coating layer, and the binder polymer migrates to the surface of the inorganic coating layer as the solvent migrates, forming an electrode adhesive part with a high binder polymer content in the surface layer, thereby providing high adhesive strength between the electrode and the separator.
[0068] The solvent may be a component capable of dissolving the binder polymer used. As such a solvent, it is preferable to use a ketone-based solvent. In an embodiment of the present invention, specific examples of the solvent may be appropriately selected and used from polar amide solvents such as acetone, methyl ethyl ketone, N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and dimethylformamide, but are not limited thereto.
[0069] Meanwhile, as described above, the inorganic particles may include composite particles whose surfaces are coated with a coupling agent. The composite particles may be prepared by a spray coating method in which a solution in which a coupling agent is dispersed is sprayed onto the surfaces of the inorganic particles to coat the surfaces of the inorganic particles with the coupling agent. Alternatively, the inorganic particles may be dispersed in a suitable solvent such as water, and then the coupling agent may be added and stirred to coat the surfaces of the inorganic particles with the coupling agent. The method of coating or covering the inorganic particles with the coupling agent is not particularly limited to any one method, and known coating methods such as a spray coating method may be used.
[0070] Meanwhile, the application of the slurry is not particularly limited, and may be performed by a conventional coating method such as a Mayer bar, a die coater, a reverse roll coater, a gravure coater, etc. When the inorganic coating layer is formed on both sides of the separation membrane, it is possible to apply the coating liquid to each side, and then perform humid phase separation and drying, but it is more preferable from the viewpoint of productivity to apply the coating liquid to both sides of the porous substrate at the same time, and then perform humid phase separation and drying.
[0071] 3. An electrode assembly including the separator Meanwhile, the present invention provides a secondary battery including the separator. The battery includes an anode, a cathode, and a separator interposed between the anode and the cathode, and the separator has the above-mentioned characteristics.
[0072] In the present invention, the positive electrode includes a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material, a conductive material, and a binder polymer on at least one surface of the current collector. The positive electrode active material includes a layered compound such as lithium manganese composite oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li x Mn y Ni z Co (1-y-z) O2 (where x is 0.5 to 2, x + y + z = 1), chemical formula Li 1+x Mn 2-x O4 (where x is 0 to 0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x O2 (where M is one or more selected from Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and x = 0.01 to 0.3), lithium nickel oxide represented by; chemical formula Li a Ni x Co y Mn z O2 (0 < a < 1.5, 0 < [x, y, z] < 1, x + y + z = 1), chemical formula LiMn 2-x M x O2 (where M is Co, Ni, Fe, Cr, Zn, or Ta, and x = 0.01 to 0.1) or a lithium manganese composite oxide represented by Li2Mn3MO8 (where M is Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of Li in the chemical formula is substituted with an alkaline earth metal ion; a disulfide compound; Fe2(MoO4)3, and may include a mixture of one or more of them.
[0073] In the present invention, the negative electrode includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material, a conductive material, and a binder polymer on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, graphitizable carbon, and graphite-based carbon as the negative electrode active material; Lix Fe2O3 (0 < x ≤ 1), Li x WO2 (0 < x ≤ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, 2, 3 elements of the periodic table, halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8) and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; one or more mixtures selected from titanium oxides may be included.
[0074] In a specific embodiment of the present invention, the conductive material is, for example, any one selected from the group consisting of graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, activated carbon, and polyphenylene derivative, or a mixture of two or more of these conductive materials. More specifically, it is one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, ketjen black, channel black, furnace black, lamp black, summer black, denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more of these conductive materials.
[0075] The current collector is not particularly limited as long as it does not induce a chemical change in the battery and has high conductivity. For example, stainless steel, copper, aluminum, nickel, titanium, fired carbon, or those surface-treated with carbon, nickel, titanium, silver, etc. on the surface of aluminum or stainless steel are used.
[0076] The binder polymer may be a polymer commonly used for electrodes by those skilled in the art. Non-limiting examples of the binder polymer include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, acetylpropionyl cellulose, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxymethyl cellulose, but are not limited thereto.
[0077] The electrode assembly prepared as above can be placed in a suitable case and an electrolyte can be injected to manufacture a battery.
[0078] In the present invention, the electrolyte is + B - A salt having the structure: + Li + , Na + , K + or a combination thereof, such as B - PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 -or a salt containing an anion such as the above or a combination thereof is dissolved or dissociated in an organic solvent including, but not limited to, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma-butyrolactone (g-butyrolactone), an ester compound, and a mixture of one or more selected from the above.
[0079] Meanwhile, in a specific embodiment of the present invention, the organic solvent contains an ester-based compound, and preferably, the ester-based compound is present in an amount of 30 wt % or more, 50 wt % or more, 60 wt % or more, or 65 wt % or more relative to 100 wt % of the organic solvent.
[0080] In a specific embodiment of the present invention, the ester compound includes one or more selected from the group consisting of isobutyl propionate, isoamyl propionate, isobutyl butyrate, isopropyl propionate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl butyrate, ethyl butyrate, propyl butyrate, and butyl butyrate.
[0081] The present invention also provides a battery module including a battery having the electrode assembly as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool powered by a battery-type motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc., electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, and power storage systems.
[0082] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those skilled in the art.
[0083] [Separation membrane production] Examples 1 to 6 The composite particles and binder resin were put into acetone to obtain slurries for forming inorganic coating layers. The solid content of each slurry, excluding acetone, was about 13 to 15 wt%. The slurries were applied to both sides of a separator (polyethylene, porosity 45 vol%, thickness 9 μm), and then dried under a relative humidity of 23°C and 45% humidity. After drying, the thickness of the coating layer on both sides was 6 μm (3 μm on each side), and the loading of the coating layer was 7.2 g / m2 relative to the separator area. 2Then, the membrane was cut into 60 mm (length) x 25 mm (width) to obtain a separator. FIG. 3 shows the surface of the separator obtained through Example 1 of the present invention, and it can be seen that the binder resin covers the surface of the coating layer due to phase separation of the binder resin. The composition of the inorganic particles / composite particles and binder polymer used in each Example is the same as in Table 1 below. In Table 1 below, Examples 1, 3, 5, and 6 use Al(OH)3 (D50: 900 nm) surface-treated with trimethoxypropylsilane as the composite particle (composite particle 1), and Examples 2 and 4 use Al(OH)3 (D50: 900 nm) surface-treated with isopropyltrioleyltitanate as the composite particle (composite particle 2). The composite particles were obtained by spraying solutions containing each coupling agent while stirring Al(OH)3 particles to coat the inorganic particle surface, and drying at 90°C for 2 hours after spraying.
[0084] The presence or absence of a surface coating was confirmed by IR analysis of Composite Particle 1. Figure 2 shows the IR analysis results of an uncoated composite particle and Composite Particle 1, from which a CH peak and a Si-O peak, which are the results of the coating, were confirmed.
[0085] Meanwhile, the presence or absence of coating for Composite Particle 2 was confirmed through a dispersibility evaluation. Uncoated particles (Al(OH)3) and PVAc were mixed in a weight ratio of 75:25 and then added to acetone. The solid content excluding the solvent was 15wt%. This was placed in a Dispersion Analyzer (Lumisizer, LUM Co.) and rotated at a speed of 1,000 rpm to apply centrifugal force, and the sedimentation rate over time was measured. Meanwhile, a similar experiment was conducted for Composite Particle 2. The results are summarized in Table 2 below. As can be seen from Table 2 below, it was confirmed that the sedimentation rate of coated Composite Particle 2 was significantly lower than that of uncoated particles due to the coating with a titanate-based compound.
[0086] [Table 1]
[0087] [Table 2]
[0088] Comparative Examples 1 to 8 The inorganic particles, binder resin, and dispersant were added to acetone to obtain slurries for forming inorganic coating layers. The solid content of each slurry, excluding acetone, was about 13 to 15 wt%. The slurries were applied to both sides of a separator (polyethylene, porosity 45 vol%, thickness 9 μm), and then dried under a relative humidity of 23°C and 45% humidity. After drying, the thickness of the coating layer on both sides was 6 μm (3 μm on each side), and the loading of the coating layer was 7.2 g / m2 relative to the separator area. 2 Then, it was cut into a size of 60 mm (length) x 25 mm (width) to obtain a separator. The compositions of inorganic particles / composite particles and binder polymers used in each comparative example are the same as those in Tables 3 and 4 below.
[0089] Comparative Example 9 A slurry for forming an inorganic coating layer was obtained in the same manner as in Example 1. The slurry was applied to both sides of a separator (polyethylene, porosity 45 vol%, thickness 9 μm) and then naturally dried at room temperature to remove the solvent. After drying, the thickness of the coating layer was 6 μm on both sides (3 μm on each side), and the loading of the coating layer was 7.2 g / m2 relative to the separator area. 2 4 shows the surface of the separator obtained in Comparative Example 9, in which no phase separation of the binder resin occurs and no binder resin is observed on the surface of the inorganic coating layer. As a result, it was difficult to ensure electrode adhesion compared to the Examples.
[0090] [Table 3]
[0091] [Table 4]
[0092] (2) Evaluation Experiment 1) Evaluation of peel strength The separators obtained from Example 1 and Comparative Example 5 were cut to a size of 15 mm x 100 mm. A double-sided adhesive tape was attached to a glass plate, and the prepared separator was attached so that the surface of the inorganic coating layer was attached to the adhesive tape. Then, the end of the attached separator was mounted on a UTM device (LLOYD Instrument, LF plus), and a force was applied at a measurement speed of 300 mm / min at an angle of 180° to measure the force required to peel the inorganic coating layer from the porous polymer substrate. In the case of Example 1, the peeling force was measured to be 127 gf / 15 mm, and in the case of Comparative Example 5, it was measured to be 36 gf / 15 mm. Thus, it was confirmed that the separator according to the present invention has excellent peeling force when PVDF-HFP, a crystalline polymer, is used.
[0093] 2) Evaluation of electrode adhesion The adhesive strength between the electrode and the separator was measured. First, artificial graphite (average particle size 16μm), Super C65, styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were mixed in a weight ratio of 95.9:1:1.9:1.2, respectively, and water was added to prepare a negative electrode slurry. The negative electrode slurry was applied to a copper foil in a thickness of 65μm, vacuum dried at about 130℃ for 8 hours, and rolled to obtain a thickness of 1.4875cm. 2 The negative electrode loading was 3.60 mAh / cm 2 It was manufactured to be.
[0094] The obtained negative electrode was cut to a size of 25 mm x 100 mm. Separators manufactured in Examples (1 to 6) and Comparative Examples (1 to 8) were also cut to a size of 25 mm x 100 mm. The prepared separator and negative electrode were stacked on top of each other, inserted between 100 μm PET films, and bonded using a flat press. The flat press was heated and pressed at 60°C and 6.5 MPa for 1 second. The bonded separator and negative electrode were attached to a slide glass using double-sided tape. The end of the separator adhesive surface (10 mm or less from the end of the adhesive surface) was removed and attached to a 25 mm x 100 mm PET film and single-sided adhesive tape so that the lengthwise direction was connected. Then, the slide glass was attached to the lower holder of a UTM device (LLOYD Instrument, LF plus), and the separator and attached PET film were attached to the upper holder of the UTM device, and a force was applied at 180° at a measurement speed of 300 mm / min to measure the force required to peel off the inorganic coating layer facing the anode from the cathode. In the cases of Examples 1 to 6, the measured adhesive strength exceeded 100 gf / 25 mm, but Comparative Examples 1 to 8 showed adhesive strength values that were much lower than this.
Claims
1. A separator for electrochemical devices, The separator includes a porous polymer film substrate and an inorganic coating layer formed on at least one surface of the substrate. The inorganic coating layer includes inorganic particles and a binder polymer, The inorganic particles include composite particles in which at least a portion of the surface of the inorganic particles is coated with a coupling compound, The coupling compound has a functional group capable of binding the inorganic particles and the binder polymer, and the functional group includes at least one selected from an alkyl group, an alkoxy group, and an ester group; The binder polymer includes an amorphous polymer and / or a partially crystalline polymer having a glass transition temperature (Tg) of 60° C. or less, The binder polymer is at least one compound represented by the following formula 1: The binder polymer includes at least one compound represented by the following Chemical Formula 1 and a crystalline binder polymer, and the crystalline binder polymer is included in an amount of 30% by weight or less based on 100% by weight of the binder polymer, 【Chemistry 1】 wherein each R is independently -H, -OR 4 , -C(=O)-R 4 , -C(=O)O-R 4 , -OC(=O)-R 4 , or -C(=O)NH-R 4 , each R 4 is independently hydrogen or a substituted or unsubstituted C1 to C5 alkyl group, said m is an integer of 1 or more, and said n is 0 or an integer of 1 or more; Separation membrane for electrochemical elements.
2. 2. The separator for an electrochemical device according to claim 1, wherein the binder polymer comprises at least one selected from the group consisting of polyvinyl acetate (PVAc) and ethylene-vinyl acetate copolymer.
3. 3. The separator for an electrochemical device according to claim 1, wherein the binder polymer has a weight average molecular weight (Mw) of 600,000 or less.
4. The separator for an electrochemical device according to claim 1 , wherein the coupling compound comprises a silane-based compound and / or a titanate-based compound.
5. 5. The separator for electrochemical devices according to claim 1 , wherein the inorganic coating layer contains the inorganic particles in a ratio of 50% by weight or more with respect to 100% by weight of a total amount of the binder polymer and the inorganic particles, and has a porous structure due to interstitial volumes between the inorganic particles.
6. The separator for an electrochemical device according to claim 1 , wherein the inorganic coating layer includes an electrode adhesive portion in which the binder polymer is distributed at a higher concentration in a surface layer portion than in other portions.
7. A method for producing the separation membrane according to any one of claims 1 to 6, The method comprises: preparing a polymer solution by adding a solvent and a binder polymer; preparing a slurry for forming an inorganic coating layer by adding inorganic particles to the polymer solution; and applying the slurry to a surface of a porous polymer film substrate and drying the slurry under humid conditions to perform a humid phase separation process. The method for manufacturing a separator for an electrochemical device, wherein an electrode adhesive part having a high content of a binder polymer is formed on a surface of the inorganic coating layer by the humidification phase separation process.
8. The method for manufacturing a separator for an electrochemical device according to claim 7 , wherein the inorganic particles include composite particles coated with a coupling compound.
Citation Information
Patent Citations
Diaphragm of organic / inorganic composite porous coating, and preparation method of diaphragm
CN103390741A
Separator for electrochemical element, electrochemical element and manufacturing method thereof
JP2011054503A
Method for manufacturing separator, separator formed by the same method, and method for manufacturing electrochemical element including the same
JP2014160665A
Separator with a porous coating layer and electrochemical element equipped therewith
JP2014510388A
Composite porous separator and electrochemical device
JP2015191886A