Polyolefin composite diaphragm

By coating a polyolefin separator with an adhesive layer and covering it with a cellulose base film to form a composite separator, it solves the problems of insufficient thermal stability and liquid absorption performance of traditional polyolefin separators, achieving performance maintenance and improvement at high temperatures. cycle life of energy storage devices while reducing production costs.

CN221861878UActive Publication Date: 2024-10-18NINGBO ROUCHUANG NANO TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202323589921.X
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-10-18
Estimated Expiration
2033-12-27

AI Technical Summary

Technical Problem

Traditional polyolefin separators have poor thermal stability under high temperature conditions and insufficient liquid absorption and liquid retention properties, resulting in a limited operating temperature range and unstable cycle life of energy storage devices. Existing improvement solutions are costly or have great production safety hazards. Nano Fiber separators have low strength and complex preparation processes, making it difficult to achieve industrialization.

Method used

A polyolefin separator is used to coat an adhesive layer on both sides or one side, and the surface of the adhesive layer is coated with a cellulose base film. The cellulose layer limits the thermal shrinkage of the polyolefin layer and improves the thermal stability and stability of the separator. Liquid absorption performance, forming a composite membrane, simplifying the process and reducing costs.

Benefits of technology

It maintains diaphragm performance in high temperature environments, improves the baking efficiency and cycle life of energy storage devices, enhances electrolyte wettability and liquid retention performance, and reduces production costs. It is suitable for lithium batteries, sodium batteries and supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221861878U_ABST
    Figure CN221861878U_ABST
Patent Text Reader

Abstract

The utility model discloses a polyolefin composite diaphragm which comprises a polyolefin diaphragm, an adhesive coating coated on the double surfaces or single surface of the polyolefin diaphragm, and a cellulose base diaphragm coated on the surface of the adhesive coating. The low-thickness polyolefin diaphragm and the nanocellulose diaphragm are compounded, thermal shrinkage of the polyolefin layer can be limited by means of the cellulose layer, the thermal stability of the diaphragm is improved, and the diaphragm can still keep good performance in a high-temperature environment. The baking temperature is higher, the baking time is shortened, and the production efficiency is improved when the method is applied to energy storage devices such as lithium batteries, sodium batteries and supercapacitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of battery diaphragms, in particular to a polyolefin composite diaphragm. Background Art

[0002] Energy storage devices, such as lithium batteries, sodium batteries and supercapacitors, play an important role in modern energy storage and utilization. As an important component of energy storage devices, diaphragms are mainly used to separate positive and negative electrodes, prevent direct electron channels, and allow the formation of ion channels to achieve charge transfer and prevent short circuits. With the rapid development of the new energy industry, the demand for various energy storage devices has increased accordingly, and at the same time, the performance requirements for these energy storage devices have become increasingly higher. As a component that is widely present in energy storage devices such as lithium-ion batteries, sodium-ion batteries, lithium-sulfur batteries, supercapacitors, and activated batteries, diaphragms have a very important impact on the performance of energy storage devices.

[0003] Traditional polyolefin separators have poor thermal stability and are prone to melting or deformation under high temperature conditions, which limits the operating temperature range of energy storage devices. In addition, due to the low surface energy of polyolefin materials, traditional polyolefin separators also have poor liquid absorption and liquid retention properties, which affects the cycle life and performance stability of energy storage devices. Existing technical solutions often use coatings including ceramic particles, organic polymer particles, nano-silicon dioxide, etc. to coat polyolefin separators, using the characteristics of nanoparticles in the coating to improve the thermal stability and electrolyte wettability of the separator. However, these existing technical solutions may be too expensive due to the high cost of coatings, such as CN114976491B, a high heat-resistant battery separator based on titanium dioxide coaxial tubes and its preparation method, CN116435712B, a reinforced modified coating for lithium battery separators, its preparation method and lithium battery separators, etc., or require the use of organic solvents, resulting in production safety hazards and environmental pollution, such as CN110635088, an ion battery separator and its preparation method, CN109148789B, a separator and its preparation method, and a lithium ion battery using the separator, etc. In addition, it is still difficult to make the liquid absorption performance of polyolefin separators comparable to that of cellulose separators by only using coating modification.

[0004] Nanofiber diaphragm is an emerging diaphragm material with high liquid absorption efficiency and excellent thermal stability, and can withstand high operating temperatures. However, the strength of nanofiber diaphragm is low, and paper breaks are prone to occur during the winding process. And due to its special structure, macropores are prone to occur, which causes the generation of electronic channels, resulting in short circuits and performance degradation of batteries or supercapacitors. CN113471628B A multi-hydrogen bond cross-linked cellulose / carboxylated polyimide nanofiber composite diaphragm and its preparation method and use provide a modified cellulose diaphragm with high mechanical properties, but its cumbersome and complex preparation process and high cost make it difficult to achieve industrialization. CN105304846 A composite non-woven ceramic diaphragm for lithium-ion batteries and its preparation method provide a multi-layer composite non-woven diaphragm with good mechanical and electrochemical properties, but its structure is relatively thick, and the thickness after multi-layer composite far exceeds the thickness that can be accepted by energy storage batteries that generally pursue high energy density. Summary of the invention

[0005] The utility model aims at a novel polyolefin composite diaphragm, which can comprehensively utilize the advantages of traditional polyolefin diaphragms and nanofiber diaphragms, while ensuring that the thickness is within the acceptable range for downstream battery and capacitor production, and at a lower cost, improves the strength and thermal stability of the diaphragm in a simpler and industrialized manner, while meeting the requirements of liquid absorption and liquid retention, so as to improve the performance and cycle life of energy storage devices.

[0006] A polyolefin composite diaphragm comprises a polyolefin diaphragm, an adhesive coating applied on both sides or one side of the polyolefin diaphragm, and a cellulose-based film coated on the surface of the adhesive coating.

[0007] Furthermore, the polyolefin membrane is a polypropylene membrane or a polyethylene membrane.

[0008] Furthermore, the polyolefin separator has a thickness of 4 μm to 10 μm.

[0009] Furthermore, the thickness of the adhesive coating is less than 2 μm.

[0010] Furthermore, the thickness of the nanofiber-based membrane is 4 to 21 μm.

[0011] Preferably, the surface density of the nanofiber-based membrane is 6 to 10 g / ㎡.

[0012] Furthermore, the overall thickness of the composite diaphragm is 8 to 25 μm.

[0013] Furthermore, the nanofiber-based membrane is formed by interweaving nanocellulose fibers and synthetic fibers.

[0014] The diameter of the nanocellulose fiber is no more than 500 nm and the length is 0.3-3 mm;

[0015] Preferably, the surface density of the nanofiber-based membrane is 8 g / ㎡.

[0016] Furthermore, the cellulose-based membrane is interwoven with cotton fibers, bamboo pulp fibers, nano-aramid fibers, and synthetic cellulose fibers.

[0017] The diameters of the cotton fibers, bamboo pulp fibers and nano-aramid fibers are in the range of 500 nm to 0.3 μm and the lengths are in the range of 0.6 to 6 mm.

[0018] Preferably, the surface density of the cellulose-based film is 10 g / ㎡.

[0019] Compared with the prior art, the present invention mainly solves the following technical problems:

[0020] 1. The composite membrane of the utility model is a composite of a low-thickness polyolefin membrane and a nanocellulose membrane by coating an adhesive layer, and the cellulose layer is used to limit the thermal shrinkage of the polyolefin layer, thereby improving the thermal stability of the membrane and maintaining good performance in a high-temperature environment. It can be applied to energy storage devices such as lithium batteries, sodium batteries, and supercapacitors, and the higher baking temperature shortens the baking time and improves production efficiency.

[0021] 2. The composite diaphragm of the utility model overcomes the insufficient liquid absorption and liquid retention performance of the traditional polyolefin diaphragm, utilizes the high liquid absorption efficiency of the nanofiber diaphragm, combines the polyolefin diaphragm and the cellulose membrane, enhances the electrolyte wettability of the diaphragm, improves the liquid absorption and liquid retention performance of the diaphragm, and enhances the performance of the energy storage device. It can improve the liquid retention performance of the diaphragm while maintaining a high liquid absorption efficiency, on the one hand, increase the battery production injection rate and improve production efficiency; on the other hand, improve its cycle performance and life during the use of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the structure of the composite membrane in Example 1.

[0023] Figure 2 Schematic diagram of the structure of the membrane in Example 2.

[0024] In the figure, 1-polypropylene membrane; 2-adhesive coating; 3-nanofiber base membrane, 4-polyethylene membrane. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with specific embodiments.

[0026] Explanation of terms

[0027] Homogenizers usually consist of two relatively rotating toothed discs, one of which is fixed and the other is moving. Between the two moving and fixed discs, the material is introduced and subjected to high shear forces. Due to the high-speed rotation of the moving disc, the material is subjected to high friction, causing the fibers or particles to be refined or split into smaller sizes.

[0028] Fiber splitting refers to the phenomenon of fiber breaking and thinning when subjected to mechanical force. In the homogenizing nanomachine, fiber splitting can control the fiber breaking mode and thinning degree by controlling the distance between the blades and the rotation speed.

[0029] Fiber nanofiberization refers to the process of reducing fibers to the nanometer level. In the homogenizing nanomachine, the fibers can be reduced to the nanometer level by controlling the pressure and rotation speed between the toothed discs.

[0030] Example 1

[0031] This embodiment provides a composite diaphragm for lithium batteries and sodium batteries, such as Figure 1 As shown, the diaphragm includes a polypropylene diaphragm 1, an adhesive coating 2 adhered to both sides or one side of the polypropylene diaphragm 1, and a cellulose-based film 3 coated on the surface of the adhesive coating 2.

[0032] Furthermore, a polypropylene diaphragm with a thickness of 10 μm is taken, and an adhesive solution is applied on the upper and lower surfaces of the polypropylene diaphragm to form an adhesive coating 2, the coating thickness is 2 microns, and a cellulose-based film is arranged on the adhesive coating with a thickness of 10 μm. The entire composite diaphragm is then rolled and has a thickness of 20 μm.

[0033] Furthermore, the preparation method of the composite diaphragm is as follows:

[0034] Step 1: Using nanocellulose fibers as raw materials, soften them through alkaline hydrogen peroxide treatment, and use pulping to separate and nanofiberize them, controlling the fiber diameter to be less than 500nm. Add dispersant, and use synthetic fibers in any proportion to make a cellulose-based film with a thickness of about 10μm at a quantitative ratio of 8g / ㎡.

[0035] Step 2: SBR latex, silicone defoamer, sodium dodecyl sulfate wetting agent and deionized water are mixed in a ratio of 100:1:1:1000 and stirred to disperse evenly, and then allowed to stand to obtain an adhesive solution.

[0036] Step 3: Take a 10 μm polypropylene membrane, apply the prepared adhesive solution on the polypropylene membrane by blade coating, with a coating amount of 2 μm, and immediately compound it with a cellulose membrane, and dry it in a hot oven at a temperature of 120°C.

[0037] Step 4: The dried composite diaphragm is hot-pressed by a hot-pressing roller, the roller surface temperature is about 120° C., and the roller thickness is controlled at 20 μm to obtain a prepared composite diaphragm.

[0038] The composite membrane in Example 1 has a strength of 50 MPA and an air permeability of 60 s / 100 CC, and a heat shrinkage rate of no more than 2% at 140° C., while maintaining the liquid absorption efficiency of the nanocellulose membrane, with a liquid absorption height of 16 mm / 10 min. The composite membrane is suitable for various types of high-power batteries and improves production efficiency and operating temperature.

[0039] Example 2

[0040] This embodiment provides a composite diaphragm for supercapacitors, activated batteries, etc. Figure 2 As shown, the separator includes a polyethylene separator 4, an adhesive coating 2 adhered to both sides or one side of the polyethylene separator 4, and a cellulose-based film 3 coated on the surface of the adhesive coating 2.

[0041] Furthermore, a polyethylene diaphragm with a thickness of 5 μm is taken, and an adhesive solution is applied on the upper and lower surfaces of the polyethylene diaphragm to form an adhesive coating 2, the coating thickness is 1 micron, and a cellulose-based film is arranged on the adhesive coating with a thickness of 15 μm. The entire composite diaphragm is then rolled and has a thickness of 20 μm.

[0042] Furthermore, the preparation method of the composite diaphragm is as follows:

[0043] Step 1: Use cotton fiber, bamboo pulp fiber and nano-aramid as raw materials, prepare pulp according to the mass ratio of 7:2:1, and use a double-disc refiner to perform fiber separation and fiber nano-refining.

[0044] Dispersants and defoamers were added, and the fiber mixture was used to make a fiber-based membrane with a thickness of 15 μm at a quantitative weight of 10 g / ㎡.

[0045] The cellulose-based membrane is formed by interweaving cotton fiber, bamboo pulp fiber, and nano-aramid

[0046] Step 2: Mix the aqueous polyurethane emulsion, modified polysiloxane leveling agent, and deionized water in a mass ratio of 50:1:1000, stir and disperse them evenly, and let them stand to obtain an adhesive solution.

[0047] Step 3: Take a 5 μm polyethylene membrane, apply the prepared adhesive solution on the polyethylene membrane by spraying, with a coating amount of 1 μm, and immediately compound it with a cellulose membrane, and dry it by infrared at a temperature of 105°C.

[0048] Step 4: The dried composite diaphragm is hot-pressed by a hot-pressing roller, the roller surface temperature is about 105° C., and the roller thickness is controlled at 20 μm to obtain a prepared composite diaphragm.

[0049] The composite membrane in Example 2 has a strength of 40 MPA and an air permeability of 40s / 100CC, a heat shrinkage rate of no more than 2% at 140°C, and maintains a high liquid absorption efficiency of the fiber layer, with a liquid absorption height of 20 mm / 10min. The composite membrane is suitable for various energy storage devices and can effectively improve their performance and service life.

Claims

1. A polyolefin composite diaphragm, characterized in that: The invention comprises a polyolefin separator, an adhesive coating applied on both sides or one side of the polyolefin separator, and a cellulose-based film coated on the surface of the adhesive coating.

2. The polyolefin composite diaphragm according to claim 1, characterized in that: The polyolefin diaphragm is a polypropylene diaphragm or a polyethylene diaphragm.

3. The polyolefin composite diaphragm according to claim 1, characterized in that: The polyolefin separator has a thickness of 4 μm to 10 μm.

4. The polyolefin composite diaphragm according to claim 1, characterized in that: The thickness of the adhesive coating is less than 2 μm.

5. The polyolefin composite diaphragm according to claim 1, characterized in that: The cellulose-based film has a thickness of 4-21 μm.

6. The polyolefin composite diaphragm according to claim 1, characterized in that: The overall thickness of the composite diaphragm is 8-25 μm.

7. The polyolefin composite diaphragm according to claim 1, characterized in that: The cellulose-based film is formed by interweaving nanocellulose fibers and synthetic fibers.

8. The polyolefin composite diaphragm according to claim 7, characterized in that: The diameter of the nanocellulose fiber is no more than 500 nm and the length is 0.3-3 mm.

9. The polyolefin composite diaphragm according to claim 1, characterized in that: The cellulose-based film is formed by interweaving cotton fibers, bamboo pulp fibers, nano-aramid fibers and synthetic cellulose fibers.

10. The polyolefin composite diaphragm according to claim 9, characterized in that: The diameters of the cotton fiber, bamboo pulp fiber and nano-aramid fiber are in the range of 500nm-0.6μm, and the lengths are in the range of 0.6-6mm.

Citation Information

Cited By

  • Composite separator, preparation method therefor and use thereof

    WO2025139822A1