Method for manufacturing a preform for an anti-resonant hollow-core fiber with nested capillaries, preform, and intermediate product
By prefabricating capillary blanks with controlled ellipticity and adjusting geometric parameters, the method addresses the alignment challenges in anti-resonant hollow core fiber manufacturing, ensuring precise and reproducible fiber production.
Patent Information
- Application Number
- JP2023529035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-17
- Filing Date
- 2021-11-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-11
AI Technical Summary
Existing methods for manufacturing anti-resonant hollow core fibers face challenges in maintaining precise geometric alignment and positioning of nested capillaries due to elliptical deformations during the stretching process, leading to inconsistent and non-reproducible fiber quality.
The method involves prefabricating capillary blanks with nested capillaries having controlled ellipticity, adjusting geometric parameters such as equilibrium pressures and taper ratios to minimize elliptical deformation, and using precise machining techniques to ensure accurate positioning and alignment during the assembly of capillary blanks within the sleeve tube.
This approach enables the production of anti-resonant hollow core fibers with high precision and reproducibility, maintaining the advantages of prefabricated capillary blanks while reducing elliptical deformations, thereby improving the accuracy and consistency of the fiber drawing process.
Smart Images

Figure 0007567054000005 
Figure 0007567054000006 
Figure 0007567054000007
Abstract
Description
[Technical field]
[0001] The invention belongs to the field of optical fiber technology, and in particular to the field of anti-resonant hollow core fibers. Such fibers make it possible to guide light in a "hollow" core, which is either evacuated or filled with gas. This fiber technology promises low optical attenuation, a very wide transmission spectrum (especially in the UV or even IR wavelength range), and low latency in data transmission. Furthermore, these fibers are suitable for spectroscopy and for the transmission of short laser pulses.
[0002] In particular, the present invention relates to a method of manufacturing an anti-resonant hollow-core fiber comprising a hollow core extending along a longitudinal axis of the fiber and a sheath region surrounding the hollow core, the sheath region comprising a plurality of anti-resonant elements, the method comprising: (a) providing a sleeve tube, the sleeve tube having a sleeve tube inner bore and a sleeve tube longitudinal axis along which a sleeve tube wall defined by an inner side and an outer side extends; (b) providing a tubular anti-resonant element preform, at least a portion of which exists as a capillary blank comprising at least one ARE outer capillary and at least one nested NE inner capillary connected to an inner surface of the ARE outer capillary, the production of the capillary blank comprising: (b1)Outer diameter OD ARE and inner diameter ID ARE On the inside surface of the ARE outer tube having an outer diameter OD NE and inner diameter ID NE and fixing the NE inner tube having the capillary blank assembly to form a capillary blank assembly. (b2) The capillary blank assembly is thermally stretched to a maximum outer diameter OD ARE_cap and maximum wall thickness WT ARE_cap forming a capillary blank having and (c) mounting a capillary blank at a target location inside the sleeve wall to form a primary preform having a hollow core region and a sheath region; (d) stretching the primary preform to form a hollow-core fiber or further processing the primary preform to form a secondary preform from which a hollow-core fiber is drawn; and Includes.
[0003] The invention also relates to a method of manufacturing a preform for an anti-resonant hollow-core fiber, the anti-resonant hollow-core fiber comprising a hollow core extending along a longitudinal axis of the fiber and an inner sheath region surrounding the hollow core, the sheath region comprising a plurality of anti-resonant elements, the method comprising: (a) providing a sleeve tube, the sleeve tube having a sleeve tube inner bore and a sleeve tube longitudinal axis along which a sleeve tube wall defined by an inner side and an outer side extends; (b) providing a tubular anti-resonant element preform, at least a portion of which exists as a capillary blank comprising at least one ARE outer capillary and at least one nested NE inner capillary connected to an inner surface of the ARE outer capillary, the production of the capillary blank comprising: (b1)Outer diameter OD ARE and inner diameter ID ARE On the inside surface of the ARE outer tube having an outer diameter OD NE and inner diameter ID NE and fixing the NE inner tube having the capillary blank assembly to form a capillary blank assembly. (b2) The capillary blank assembly is thermally stretched to a maximum outer diameter OD ARE_cap and maximum wall thickness WT ARE_cap forming a capillary blank having and (c) mounting a capillary blank at a target location inside the sleeve wall to form a primary preform having a hollow core region and a sheath region; (d) Optionally, further processing the primary preform to form a secondary preform for a hollow-core fiber, the further processing being performed by a hot forming process, namely: (i) elongation, (ii) Collapse, (iii) collapse and simultaneous extension; (iv) Collapse of additional sheath material; (v) collapse and subsequent expansion of additional sheath material; (vi) Collapse and simultaneous expansion of additional sheath material. and Includes.
[0004] Furthermore, the present invention relates to a capillary blank as an intermediate product for manufacturing an antiresonant hollow-core fiber, comprising at least one ARE outer capillary and at least one nested inner capillary connected to the inner surface of the ARE outer capillary.
[0005] Additionally, the present invention relates to a preform for an anti-resonant hollow-core fiber, the preform having a hollow core region and a sheath region, the sheath region comprising a sleeve tube having a sleeve tube wall and a plurality of tubular anti-resonant element preforms arranged inside the sleeve tube wall.
[0006] Conventional single-mode optical fibers made of solid materials have a glass core region surrounded by a glass sheath region with a lower refractive index. Light guiding is based on total internal reflection between the core and sheath regions. However, the interaction of the guided light with the solid material is associated with increased latency in data transmission and a relatively low damage threshold for high-energy radiation.
[0007] These drawbacks are avoided or reduced by "hollow-core fibers", in which the core comprises a vacuum cavity filled with gas or liquid. In hollow-core fibers, the interaction of light with the glass is smaller than in solid-core fibers. The refractive index of the core is smaller than that of the sheath, so that light guiding by total internal reflection is not possible and the light usually escapes from the core into the sheath. Depending on the physical mechanism of light guiding, hollow-core fibers are divided into "photonic band-gap fibers" and "anti-resonant reflecting fibers".
[0008] In the case of a "photonic bandgap fiber", the hollow core region is surrounded by a sheath in which small hollow channels are periodically arranged. The periodic structure of the hollow channels in the sheath leads to an effect called "photonic bandgap" based on semiconductor technology, according to which light of a certain wavelength range scattered in the sheath structure can constructively interfere due to Bragg reflection in the central cavity and cannot propagate laterally in the sheath.
[0009] In an embodiment of a hollow-core fiber called an "anti-resonant hollow-core fiber" (ARHCF), the hollow core region is surrounded by an inner sheath region in which so-called "anti-resonant elements" (or "anti-resonance elements", "AREs" for short) are located. The walls of the anti-resonant elements, evenly distributed around the hollow core, can act as a Fabry-Perot cavity operating at anti-resonance, reflecting the incident light and guiding it through the fiber core.
[0010] This fiber technology promises low optical attenuation, a very wide transmission spectrum (even within the UV or IR wavelength range), and low latency in data transmission.
[0011] Hollow-core fibers are used in the fields of data transmission, high-power beam guidance, e.g. for material processing, modal filtering, and nonlinear optics, especially for supercontinuum generation from the ultraviolet to the infrared wavelength range. Furthermore, they are suitable for spectroscopic applications and for the transmission of short laser pulses. [Background technology]
[0012] A disadvantage of anti-resonant hollow-core fibers is that higher order modes are not necessarily suppressed, so that anti-resonant hollow-core fibers are often not pure single mode over long transmission distances, resulting in degraded output beam quality.
[0013] In the paper "Nested anti-resonant nodeless hollow core fiber" by Francesco Poletti (Optics Express, Vol. 22, No. 20 (2014); DOI: 10.1364 / OE 22.023807), a fiber design is proposed in which the anti-resonant element is not designed as a simple single structural element, but instead consists of multiple nested structural elements. The nested anti-resonant element is designed in such a way that the higher-order core modes, but not the fundamental core mode, are phase-matched to the sheath modes and suppressed. As a result, the propagation of the fundamental core mode is always ensured, and the hollow-core fiber can be efficiently single-mode over a limited wavelength range.
[0014] Preforms for such "nested anti-resonant nodeless hollow core fiber (NANF)" consist of multiple anti-resonant elements (AREs). They are often manufactured by the so-called "stack and draw" method. For example, to manufacture a preform for a hollow core fiber with a "NANF" design, multiple anti-resonant element preforms, each of which consists of an anti-resonant element outer tube (hereinafter abbreviated as ARE outer tube) and an anti-resonant element inner tube (hereinafter abbreviated as NE inner tube) located on one side of the inner surface of the ARE outer tube, are attached inside a sleeve tube.
[0015] Each of the anti-resonant preforms has a certain deviation from its set-point shape, and each positioning and shaping step inevitably results in a geometric deviation that can be added to the absolute geometric error in the preform. This demands high precision when positioning and fixing the output elements in their respective target positions, especially when the arrangement is compact and the distance of the output elements from each other is short. In order to achieve low attenuation values and a wide transmission range, in addition to the uniform wall thickness of the anti-resonant elements, their azimuthal position, especially on the inner wall of the sleeve tube, is also important. The attachment point of the NE inner tube on the ARE outer tube must have the same azimuthal position as the attachment point of the ARE outer tube on the inner wall of the sheath tube. In addition, both the distance between the individual attachment points and the circumferential distance between the ARE outer tubes must be as uniform as possible. This cannot be easily achieved even with the "stack and draw" technique.
[0016] A simplification in this regard results from the technique in which a prefabricated capillary blank is produced, which comprises an ARE outer capillary and at least one NE inner capillary fixed to the inner wall of the ARE outer capillary. This technique is described, for example, in the document "Hollow-core revolver fibre with a double-capillary reflective cladding" by AF Kosolapov, GKAlagashev, AN Kolyadin, ADPryamikov, ASBiriukov, IA Bufetov, EMDianov (Kvantovaya Elektronika, 2016, Vol. 46, no. 3, pp. 267-270). The prefabrication of the capillary blank consists in this case of stretching together an ARE outer tube made of quartz glass and an NE inner tube made of quartz glass welded to its inner wall to form a capillary blank. The stretched capillary blank thus consists of an ARE outer capillary and an NE inner capillary fixedly connected thereto. Five of the stretched capillary blanks are attached to the inner wall of a fused silica sleeve using a template with five-fold symmetry, the capillary blanks are fused to the inner wall, and the assembly is stretched to form a primary preform from which a hollow-core fiber is subsequently drawn. Summary of the Invention [Problem to be solved by the invention]
[0017] Although prefabricated capillary blanks have advantages in terms of ease and precision of assembly, it has been found that they are prone to elliptical (oval) deformation of the initially circular tube cross section when the component assembly is stretched. During softening and stretching, the inner NE tube is melted onto the inner surface of the outer ARE tube. As a result of this contact, forces act against the inner surface of the outer ARE tube that can result in deformation of the cross section and an elliptical cross-sectional shape.
[0018] Thus, in the known method, the elongated capillary blank has an elliptical cross section with a long cross-sectional axis of 6.28 mm and a short cross-sectional axis of 6.12 mm. L Axial length ratio A L / A K and the shortest cross-sectional axis A K Axial length ratio A L / A K is 1.026. This axial ratio is also referred to herein as "ellipticity" or "ovality."
[0019] The ellipticity of the capillary blank makes it more difficult to mount it accurately on the inner wall of the sleeve tube, for example, the templates used for mounting are typically designed with a circular cross section, which also makes it difficult to determine its outer diameter for the subsequent drawing process, thus preventing accurate and reproducible prediction of the drawing result in the form of a hollow-core fiber.
[0020] However, to maintain a resonant or anti-resonant condition, even small dimensional variations on the order of magnitude of the operating wavelength of the guided light cannot be tolerated.
[0021] It is therefore an object of the present invention to provide a method for manufacturing an anti-resonant hollow-core fiber and a preform for an anti-resonant hollow-core fiber, which can maintain the advantages of pre-fabricated capillary blanks in terms of ease and precision of assembly, but the associated disadvantages due to ellipticity can be kept very low, and it can be predictable that high precision of the anti-resonant element and precise positioning within the hollow-core fiber can be reproducibly achieved.
[0022] Additionally, a capillary blank is provided having low ellipticity which facilitates accurate positioning of the sleeve tube at a given azimuthal position and repeatable prediction of the draw results.
[0023] Additionally, it is an object of the present invention to identify a preform from which an anti-resonant hollow-core fiber can be drawn having geometrically precise anti-resonant elements that are positioned as precisely as possible.
[0024] Regarding the method for producing an anti-resonant hollow core fiber, the objective is to produce a hollow core fiber having a cross-sectional dimension OD NE , ID NE , O.D. ARE , ID ARE And O.D. ARE_cap and W.T. ARE_cap is achieved according to the invention based on a method of the aforementioned type in that the ARE outer capillary (11) of the capillary blank (5) is adjusted in such a way that it has an ovality of less than 1.025.
[0025] The starting point for manufacturing an anti-resonant hollow-core fiber is a preform, referred to herein as the "primary preform". Typically, the manufacture of the primary preform includes the placement and connection of an anti-resonant element preform to a sleeve tube. At least a part of the anti-resonant element preform is present in the form of a pre-fabricated capillary blank with a nested anti-resonant element. In the present specification, this is understood to mean a blank with an ARE outer capillary, to whose inner surface at least one NE inner capillary is fixed, the ARE outer capillary extending parallel to its longitudinal axis. In the case of a multi-nested anti-resonant element, at least one further inner NE inner capillary, also extending parallel to the longitudinal axis of the outer capillary, is fixed to the inner surface of the outer NE inner capillary. The ARE outer capillary and the NE inner capillary(s) are fused together to form the anti-resonant element preform.
[0026] The primary preform produced using the prefabricated capillary blank can be directly drawn to form a hollow core fiber. In principle, the primary preform can be further processed to produce therefrom a preform, referred to herein as a "secondary preform". Optionally, a hollow core fiber is drawn from the secondary preform. The production of the secondary preform includes a step in which the output elements of the hollow core fiber are produced and positioned relative to each other, and at least one hot forming step.
[0027] The primary and secondary preforms are either monolithic bodies or parts of a coaxial collection of components having one or more collecting cylinders that are drawn to directly form a hollow-core fiber. The general term "preform" is understood herein to mean the component or coaxial collection of components from which a hollow-core fiber is ultimately drawn.
[0028] The addition of sheath material is accomplished, for example, by collapsing a collecting cylinder onto the primary preform, where the coaxial arrangement of the primary preform and collecting cylinder is stretched or not stretched as the collecting cylinder collapses, where the anti-resonant element preforms change their shape or arrangement or do not change their shape or arrangement.
[0029] To manufacture a capillary blank with a simple nested NE inner capillary, output tubes with circular cross section, referred to herein as the outer ARE tube and the inner NE tube, are used. The inner NE tube is fixed to the inner surface of the outer ARE tube. They are preferably connected on the two opposite end face ends of the assembly, for example by means of structural retention means, preferably by local spot bonding or thermal bonding (spot welding).
[0030] This component assembly is softened and stretched (elongated) zone by zone to form a prefabricated capillary blank with a fixed, predetermined and verifiable position and orientation of the ARE outer capillary and the NE inner capillary relative to one another. Prefabrication eliminates positioning and alignment means that would otherwise be required during assembly to produce the primary preform. In this respect, these assembly steps are facilitated and the dimensional stability of the antiresonant element preform is improved.
[0031] However, it has been found that when stretching the component assembly, oval (elliptical) deformation of the initially circular tube cross-section is likely to occur. This is relevant for the NE inner capillary as well, but particularly for the ARE outer capillary. The degree of oval deformation of the ARE outer capillary depends on the cross-sectional geometry of the output tube (OD NE , ID NE , O.D. ARE , ID ARE ) and the cross-sectional geometry of the ARE outer capillary (OD ARE_cap , W.T. ARE_cap It has been found that the ovality of the ARE outer capillary is substantially determined by the taper ratio during hot drawing (but also as a function of the cross-sectional geometry of the output tube and the ARE outer capillary). In contrast, drawing parameters such as temperature, infeed and draw rates have relatively little effect on the ovality. However, other drawing parameters such as pressure and gas flow have a significant effect on the ovality of the ARE outer capillary. For example, gas flow can cause localized cooling, which affects the geometry of the ARE outer capillary. For otherwise given drawing parameters, the ovality of the ARE outer capillary is primarily a function of the cross-sectional geometric dimensions of the output tube and the ARE outer capillary.
[0032] The present invention specifies teachings on how to adjust said geometric parameters so that a given maximum ellipticity of the ARE outer capillary, e.g. 1.025, can be reproducibly maintained in capillary blanks produced by hot drawing.
[0033] In a preferred method variant, the geometric dimensions are determined by the following factors (F1) to (F4): (F1) Equilibrium pressure p of the NE inner pipe eg_NE Ratio of and equilibrium pressure p of the ARE outer tube eq_ARE The ratio of (F2) Distance between the ARE outer tube and the NE inner tube relative to the inner diameter of the ARE outer tube (ID ARE -OD NE ) / ID ARE , (F3) Taper ratio OD during hot drawing of the capillary blank assembly according to step (b2) ARE / OD ARE_cap , and (F4) Ratio of outer diameter to wall thickness of the capillary blank OD ARE_cap / WT ARE_cap is adjusted in relation to
[0034] Equilibrium pressure p eq is the pressure required during elongation of the glass tube so that it neither collapses nor expands. The equilibrium pressure of the inner tube, p eq;NE teeth, p eq;NE =(2 / OD NE +2 / ID NE )×σ (1), is required by Equilibrium pressure p of the ARE outer tube eq;ARE teeth, p eq,ARE =(2 / OD ARE +2 / ID ARE ×σ (2), is required by where σ is the surface tension at the drawing temperature that can be applied to quartz glass at 0.4 N / m.
[0035] Advantageously, the diameter of the ARE outer tube made of quartz glass or the NE inner tube made of quartz glass is such that the equilibrium pressure p eq,NE is in the range of 60 to 90 Pa, preferably in the range of 65 to 80 Pa, and the equilibrium pressure p eq_ARE is selected to be in the range of 25 to 50 Pa, preferably in the range of 30 to 40 Pa.
[0036] Ratio of equilibrium pressures according to factor (F1) p eq;NE / p eq;ARE is a measure of the effectiveness of the surface tension of a single capillary in the capillary blank. The higher this value, the greater the influence of the inner capillary (NE) on the ellipticity of the outer capillary (ARE).
[0037] Therefore, the equilibrium pressure p eq;NE and p eq;ARE is adjusted so that the factor (F1) advantageously assumes a value in the range of 1.5 to 2.5, preferably in the range of 1.5 to 2.
[0038] On the one hand, the larger the free distance between the ARE outer tube and the NE inner tube, the larger the inner diameter ID NE_cap As the NE inner tube becomes smaller, the final processing of the fiber becomes more complex and more difficult. Therefore, for example, high temperature resistant joints with pressure joints are technically more complex. Secondly, the ratio of the equilibrium pressures increases with the increase in the free distance of the AR outer tube from the NE inner tube.
[0039] From this point of view, it has proven advantageous to adjust the factor (F2) to a value in the range of 0.2 to 0.5, preferably to a value in the range of 0.3 to 0.4.
[0040] In order to reduce the absolute geometric shape error, a large taper ratio OD is used during hot drawing. ARE / OD ARE_cap On the other hand, large drawdown ratios are associated with correspondingly large molding processes and material transfers that can easily result in undesirable deformations in the delicate anti-resonant element preforms.
[0041] Setting the taper ratio according to factor (F3) to a value in the range of 5 to 10, preferably in the range of 5 to 8, has proven to be a good compromise.
[0042] Ratio of outer diameter to wall thickness of the capillary blank (OD) ARE_cap / WTARE_cap is a measure of the dimensional stability of the capillary blank. The thinner the wall compared to the outside diameter, the more prone it is to deformation.
[0043] With regard to the lowest possible ellipticity, adjusting the factor (F4) to a value in the range of 15-25, preferably in the range of 15-20, has proven successful.
[0044] In addition, the measurements provide an indication of the dimensional stability of the capillary draw.
[0045] In a particularly preferred method variant, factors (F1) to (F4) are adjusted so that the capillary blank has an ellipticity of less than 1.020.
[0046] It turns out that the mathematical product of factors (F1)–(F4) is a measure of ellipticity. The smaller the product, the less ellipticity of the ARE outer capillary in the capillary blank. This measure is referred to below as the “geometric parameter” (P(geom.)).
[0047]
number
[0048] Each individual factor of factors (F1)-(F4) has an influence on the geometrical parameters. The smaller the factor, the smaller the contribution of the ARE outer capillary to the ellipticity. Based on the geometrical parameters, a person skilled in the art can reliably estimate how the cross-sectional dimensions of the output tubes (NE inner tube and ARE outer tube) will result in an ellipticity with the planned taper ratio. Thus, empirical tests and failures can be prevented or at least their number can be reduced. For example, if the geometrical parameter is 94, an ellipticity of 1.04 is expected. If the ellipticity is less than 1.025, the geometrical parameter should not exceed 77.5. If only an ellipticity of 1.010 is acceptable, the geometrical parameter should be set to 55 or less.
[0049] Therefore, to achieve the minimum ellipticity, the geometric parameter is set to a value in the range of 35-75, preferably in the range of 40-60.
[0050] In particular, with such multi-nested capillary blanks, the positioning and alignment efforts are significantly reduced as compared to individual components.
[0051] During further processing to form a primary preform, a plurality of pre-manufactured capillary blanks are attached to the inner surface of the sleeve tube.
[0052] The primary preform produced with the aid of this method preferably has an outer diameter in the range of 26 to 230 mm, particularly preferably in the range of 30 to 200 mm.
[0053] During the elongation of the primary preform, additional sheath material or no additional sheath material is applied to form the hollow core fiber or to form the secondary preform. During the elongation, the primary preform is heated zone by zone in the heating zone. The larger the diameter, the slower the advance speed into the heating zone and the longer the duration that each axial part of the preform is exposed to the high temperature of the heating zone. However, if the advance speed is too slow during the elongation, the anti-resonant element preform will deform. Therefore, the diameter of the primary preform is preferably at most 230 mm, preferably at most 200 mm. Also, the diameter of the primary preform is preferably at least 26 mm, preferably at least 30 mm. This is because it has been found that for smaller diameters, the thermal inertia of the preform is too low to compensate for any temperature fluctuations in the heating zone.
[0054] When drawing the primary or secondary preform according to step (d) to form a hollow-core fiber, an overpressure is preferably generated and maintained in the ARE outer capillary and in the NE inner capillary relative to the elongated hollow core region. The pressure in the ARE outer capillary is generally different from the pressure in the NE inner capillary. A hollow-core fiber is obtained with a hollow core region and an inner sheath region, the former ARE outer capillary forming an anti-resonant element, preferably with a circular or slightly oval cross section.
[0055] The accuracy of the positioning of the preform on the inner surface of the sleeve tube is further improved by manufacturing the inside of the sleeve tube and / or the outside of the sleeve tube and / or the inside of the outer ARE tube and / or the outside of the outer ARE tube by machining, in particular drilling, milling, grinding, honing and / or polishing.
[0056] Compared to other known forming techniques, the machining technique provides more precise and finer structures by using heat and pressure and avoids contamination of the surface by forming tools such as nozzles, presses or molten dies.
[0057] Furthermore, a procedure in which the ARE outer tube is made of quartz glass containing at least one dopant that reduces the viscosity of the quartz glass and / or a procedure in which at least one NE inner tube is made of quartz glass containing at least one dopant that increases the viscosity of the quartz glass has proven effective.
[0058] The dopants used to reduce the viscosity of the quartz glass are preferably fluorine, chlorine and / or hydroxyl groups. The dopants that increase the viscosity of the quartz glass are preferably Al. 2 O 3 (maximum concentration of 15 ppm by weight) and nitrogen.
[0059] Doping allows for matching the thermal expansion coefficients of adjacent preform components to avoid or reduce stresses, and can also be used to reduce the thermal stability of the ARE outer tube relative to that of the at least one nested NE inner tube.
[0060] In this regard, it is advantageous, for example, if at a measuring temperature of 1250°C, the quartz glass of the ARE outer tube has a viscosity that is at least 0.1 dPa·s lower, preferably at least 0.2 dPa·s lower (when the viscosity is given as the logarithmic value in dPa·s) than the quartz glass of the nested NE inner tube.
[0061] In a preferred method, the positioning accuracy of the capillary blank in the sleeve tube is further improved in that the ARE outer capillary has a wall thickness in the range of 0.2-3 mm, preferably in the range of 0.25-1 mm, and a sleeve tube is used having an outer diameter in the range of 90-230 mm, preferably in the range of 120-200 mm. The components each have a length of at least 700 mm, preferably at least 1 m. The components are structural elements of relatively large volume that simplify their handling. In addition, in the case of a vertical arrangement of the sleeve tube and the capillary blank, gravity supports the parallelism and vertical alignment of the longitudinal axes of the capillaries when the capillary blanks are each positioned and fixed at the target position of their upper ends.
[0062] With regard to the manufacture of preforms for hollow core fibers, the above technical objective is to obtain the geometric dimension OD NE , ID NE , O.D. ARE , ID ARE And O.D. ARE_cap and W.T. ARE_cap is achieved by the present invention based on a method of the type described above in that the ARE outer capillary of the capillary blank is constructed to have an ovality of less than 1.025.
[0063] For this purpose, a prefabricated capillary blank is provided in which an ARE outer capillary is fused to at least one NE inner capillary, the ARE outer capillary and the NE inner capillary having fixed, predetermined and verifiable positions and orientations relative to each other.
[0064] Pre-fabrication eliminates positioning and alignment means that would otherwise be required during assembly to produce the primary preform, facilitating these assembly steps and improving the dimensional stability of the anti-resonant element preform.
[0065] The manufacture of the prefabricated capillary blank involves the hot drawing of a component assembly consisting of an outer ARE tube and an inner NE tube, which may tend to result in oval (elliptical) deformation of the initially circular tube cross-section. This is relevant for the NE inner capillary, but especially for the ARE outer capillary. The degree of oval deformation of the ARE outer capillary depends on the cross-sectional geometry (OD) of the output tube. NE , ID NE , O.D. ARE , ID ARE ) and the cross-sectional geometry of the ARE outer capillary (OD ARE_cap , W.T. ARE_cap It has been found that the ovality is substantially determined by the taper ratio during hot drawing (but also as a function of the cross-sectional geometry of the output tube and the ARE outer capillary). In contrast, drawing parameters such as temperature, infeed and draw rates have relatively little effect on the ovality. However, other drawing parameters such as pressure and gas flow have a significant effect on the ovality of the ARE outer capillary. For example, gas flow can cause localized cooling, which affects the geometry of the ARE outer capillary. However, for otherwise given drawing parameters, the ovality of the ARE outer capillary is primarily a function of the geometric cross-sectional dimensions of the output tube and of the stretched ARE outer capillary.
[0066] The present invention specifies teachings on how to adjust said geometric parameters so that a given maximum ellipticity of the ARE outer capillary, e.g. 1.025, can be reproducibly maintained in capillary blanks produced by hot drawing.
[0067] Means for producing the preform have been described above in connection with the manufacture of hollow-core fibers, and these descriptions are included herein.
[0068] Regarding the prefabricated capillary blank as an intermediate product for manufacturing an antiresonant hollow-core fiber, the above mentioned technical objectives are achieved according to the present invention based on a capillary blank of the initially mentioned type, in that the ARE outer capillary has an ellipticity of less than 1.025.
[0069] In a prefabricated capillary blank, at least two capillaries are integrally connected to each other to form a tubular component. Prefabrication eliminates positioning and alignment means that would otherwise be required during assembly to produce the primary preform. In this respect, these assembly steps are facilitated and the dimensional stability of the antiresonant element preform is improved.
[0070] The cross section of the ARE outer capillary of the capillary blank is circular or has a low opacity of at most 1.025, preferably at most 1.020, which facilitates accurate positioning of the capillary blank on the inner wall of the sleeve tube and fixing of the outer diameter of the sleeve tube for the subsequent drawing process, as well as accurate and reproducible prediction of the drawing results and more precise manufacturing of hollow-core fibers.
[0071] Means for producing capillary blanks and preforms have been described above in the context of making hollow-core fibers, and these descriptions are incorporated herein.
[0072] With regard to the preform, the above mentioned technical object is achieved by the invention on the basis of a preform of the above mentioned type in that at least a part of the anti-resonant element preform is designed as a capillary blank according to the invention.
[0073] The preform is a primary preform in the sense of the present invention. The sheath region of the preform comprises a sleeve tube which may be surrounded by at least one further sheath tube. The antiresonant element preform is arranged inside the sleeve tube and connected to it, for example by gluing or thermal bonding. At least a part of said antiresonant element preforms, preferably all of the antiresonant element preforms, is in the form of a prefabricated capillary blank, in which at least two capillaries are integrally connected to each other. The prefabrication eliminates positioning and alignment means that would otherwise be necessary during assembly to manufacture the primary preform. In this respect, these assembly steps are facilitated and the dimensional stability of the antiresonant element preforms is improved.
[0074] The cross section of the ARE outer capillary of the capillary blank is circular or has a low opacity of less than 1.025 at most, preferably less than 1.020, which facilitates accurate positioning of the capillary blank on the inner wall of the sleeve tube and fixing of the outer diameter of the sleeve tube for the subsequent drawing process, as well as accurate and reproducible prediction of the drawing results and more precise manufacturing of hollow-core fibers.
[0075] Means for producing capillary blanks and preforms have been described above in the context of making hollow-core fibers, and these descriptions are incorporated herein.
[0076] definition The individual method steps and terms in the above description are further defined below. The definitions form part of the description of the present invention. In the event of a factual contradiction between one of the following definitions and the remaining description, the remaining description is conclusive.
[0077] anti-resonance element The anti-resonant element may be a simple structural element of the hollow-core fiber or may be a nested structural element. The anti-resonant element has at least two walls that have negative curvature (convex) or no curvature (planar, straight) when viewed in the direction of the hollow core. The anti-resonant element is generally made of a material transparent to the operating light, such as glass, especially doped SiO 2 or undoped SiO 2 , made of a plastic, in particular a polymer, a composite material or a crystalline material.
[0078] Preform for anti-resonance element What is referred to as an anti-resonant element preform is a preform component or constituent that will become an effective anti-resonant element in a hollow-core fiber by simple stretching during the fiber drawing process. A nested anti-resonant element preform forms a nested anti-resonant element in a hollow-core fiber. The nested anti-resonant element is composed of an outer ARE tube and at least one further structural element disposed in the inner bore of the outer ARE tube. The further structural element can be a further tube that is in contact with the inner surface of the outer tube. The further tube is referred to as a "nested element" or "NE inner tube" for short, or also as a "nested NE inner tube".
[0079] In the case of a multiple nested anti-resonant element preform, at least one further structural element, e.g., a third tube abutting the inner surface of the nested NE inner tube, may be disposed within the inner bore of the NE inner tube. When multiple nested anti-resonant element preforms are present, an "outer NE inner tube" and an "inner NE inner tube" are optionally distinguished to distinguish between the multiple tubes disposed within the ARE outer tube.
[0080] In connection with cylindrical anti-resonant element preforms and their cylindrical structural elements as well as capillary blanks, the term "cross section" always refers to a cross section perpendicular to the associated longitudinal axis of the cylinder, i.e., a cross section of the outer contour (and not a cross section of the inner contour) of the tubular component, unless otherwise indicated.
[0081] Further processing of the primary preform, in particular by a hot forming step, can result in an intermediate product, in which the original anti-resonant element preform is present in a changed shape compared to its original shape, the changed shape also being referred to herein as the anti-resonant element preform.
[0082] Preform / Primary preform / Secondary preform / Core preform (Cane) The preform is the component from which the anti-resonant hollow-core fiber is drawn. The preform can be a primary preform or a secondary preform produced by further processing of the primary preform. The primary preform can be present as an assembly consisting of at least one sleeve tube and a preform or precursor for the anti-resonant element, loosely housed or firmly fixed therein. The further processing of the primary preform into a secondary preform from which the hollow-core fiber is drawn can be performed by the following hot forming process: (i) elongation, (ii) Collapse, (iii) collapse and simultaneous extension; (iv) Collapse of additional sheath material; (v) collapse and subsequent expansion of additional sheath material; (vi) Collapse and simultaneous expansion of additional sheath material. The present invention may include a single execution or repeated execution of one or more of the following:
[0083] By cane, this specification refers to a preform obtained by collapse and / or elongation of a primary preform, thus falling within the definition of a secondary preform. Typically, the cane is coated with an additional sheath material before or during drawing of the hollow-core fiber.
[0084] Stretch / Collapse During stretching, the primary preform is hot-drawn. The stretching can be performed without collapsing at the same time. The stretching can be performed to scale, so that, for example, the shape and arrangement of the components or components of the primary preform are reflected in the stretched and elongated final product. However, during stretching, the primary preform may not be drawn to scale and its geometry may be altered.
[0085] During collapse, the inner bore narrows or the annular gap between the tubular components closes or narrows. Generally, collapse occurs by expansion.
[0086] Hollow core / inner sheath region / outer sheath region In this document, an assembly comprising at least one sleeve tube and an ARE preform loosely housed or firmly fixed therein is also called "primary preform". The primary preform comprises a hollow core and a sheath region. This sheath region is also called "inner sheath region" if an "outer sheath region" is also present and if it is to be distinguished, for example produced by collapsing onto the assembly. The terms "inner sheath region" and "outer sheath region" are also used for the corresponding regions in the hollow-core fiber or in an intermediate product obtained by further processing of the primary preform.
[0087] The designation "inside the tube" is also used as a synonym for "inner surface of the tube," and the designation "outside the tube" is also used as a synonym for "outer surface of the tube." The term "inner bore" in reference to a tube does not imply that the inner bore has been produced by a drilling process.
[0088] Equilibrium Pressure Equilibrium pressure p eq is the pressure required during extension of the glass tube so that it neither collapses nor expands.
[0089] The calculations were done according to K. Schuster, J. Kobelke, A. Schwuchow, M. Leich, M. Becker, M. Rothhardt, U. Ropke, J. Kirchhof, H. Bartelt, T. Geernaert, "Preparation and applications of germanium and fluorine doped microstructured fibers", Proc. SPIE 6588, Photonic Crystal Fibers, 658804 (May 22, 2007), doi:10.1117 / 12.722470, and the inner radius of the glass tube (r internal ) and outer radius (r external ) is as follows:
[0090] p eq =(1 / r external +1 / r internal )×σ (4), where σ is the surface tension at the drawing temperature. For quartz glass at the drawing temperature, σ=0.4 N / m can be applied.
[0091] Ellipticity For a tube with a circular cross section, the ellipticity is 1. For a tube with an elliptical cross section, the ellipticity is the ratio of the longest cross-sectional axis A L and the shortest cross-sectional axis A K The ovality of the capillary blank is determined from the ovality of its ARE outer capillary. EXAMPLES
[0092] [Brief description of the drawings]
[0093] The present invention will now be described in more detail with reference to the following examples, the details of which are as follows. [Figure 1] 13 shows a cross-sectional photograph of a loose assembly of an outer ARE tube and an inner NE tube for producing a capillary blank. [Diagram 2] 2 shows a photograph of the assembly of the outer ARE tube and the inner NE tube of FIG. 1 after the ends of the tubes have been secured together using a thermal bonding process. [Diagram 3] 3 shows a schematic diagram for explaining a process for producing a capillary blank using the assembly of FIG. 2. [Figure 4a] 1 shows a cross section of multiple assemblies for producing an ideally shaped capillary blank. [Figure 4b] 4 shows a photograph of a cross section of a capillary blank manufactured using the assembly of FIG. 4a. [Diagram 5] FIG. 1 is a diagram illustrating the relationship between ellipticity and geometric parameters. [Figure 6] 1 shows a schematic cross-sectional view of a primary preform manufactured using multiple capillary blanks.
[0094] Figure 1 shows a precursor for producing a prefabricated capillary blank. The precursor is in the form of a loose assembly 4 of several nested output tubes, i.e., an outer ARE tube 1 and an inner NE tube 2. All tubes (1, 2) are made of quartz glass and have a circular cross section. The longitudinal axes of these tubes run parallel and, in the given figure, perpendicular to the plane of the paper. The outer surface of the inner NE tube 2 abuts against the inner surface of the outer ARE tube 1. The output tubes (1, 2) have different diameters, but substantially the same wall thickness and length. Figure 4a and table 1 contain detailed information regarding the radial dimensions of the output tubes (1, 2) and of the further assemblies.
[0095] The power tubes (1, 2) are fused to one another in a point-like manner in the region of their two end faces. The local connection points are designated by the reference number 6 in FIG.
[0096] Figure 3 shows diagrammatically the steps for further processing the assembly 4 to form a capillary blank 5. The output tube assembly 4, fixed with the connection points 6, is fed from top to bottom with its vertically oriented longitudinal axis into an annular heating zone 7, where it is softened zone by zone, and the strands (5) are removed from the softened areas with drawing rollers 8, from which the strand capillary blanks 5 are cut. During the drawing process, a constant helium gas flow of 25 ml / min is flowed through the internal bores of the capillary blanks. The inner bores of the output tubes (1, 2) remain open during this process, so that approximately the same internal pressure is established inside.
[0097] After a softening and drawing process, in which the former output tubes (1, 2) are stretched and fused together along their contact surfaces, a capillary blank 5 is obtained. As a result of the effective surface tension forces in the softened regions, they change their cross-sectional shape to an oval shape.
[0098] This shows an idealized representation of the assembly 4 of samples 1-6 in Fig. 4a compared to a photograph of a capillary blank produced therefrom in Fig. 4b. In the capillary blank 5, the former ARE outer tube (1) forms the ARE outer capillary 11 and the former NE inner tube (2) forms the nested NE inner capillary 12. All capillaries (11, 12) exhibit more or less oval cross-sectional areas. For one of the capillary blanks, dimensional arrows are drawn as an example, dimensional arrow A radial denotes the outer diameter of the ARE outer capillary 11 as measured at the point of contact with the nested NE inner capillary 12. Here, this is simultaneously the maximum outer diameter of the ARE outer capillary 11. The arrow A indicates the dimension tangential A radialARE outer capillary 11. This dimension also corresponds to the minimum outer diameter of the ARE outer capillary 11. For the other capillary blanks, A radial and A tangential is determined in the same manner.
[0099] Table 1 shows the geometric cross-sectional dimensions of the output tubes (1, 2) for samples 1-6 and capillary blanks stretched therefrom, as well as factors 1-4 of equation (3) above for the geometric parameters calculated based on these data.
[0100] [Table 1]
[0101] [Table 2] *1) These are not measured data, but rather calculated diameter targets assuming a specific stretch (the to-scale diameter reduction due to elongation).
[0102] In Samples 1 and 2, the geometric parameter is less than 77.5 and the ellipticity is less than 1.025. These are examples of the present invention. Samples 3 to 6 are comparative examples.
[0103] In the diagram of FIG. 5, the ellipticity "O" determined for the capillary blanks of samples 1-6 is plotted against the dimensionless geometric parameter "P(geom.)". It can be seen that the ellipticity and the geometric parameter scale very well, i.e. almost independently of the draw temperature and the infeed and withdrawal speeds. The linear equation of the regression line is y=0.9682+0.008x, where R 2 =0.9886. By specifying the geometric cross-sectional dimensions, this relationship thereby allows for specific adjustment or prediction of the expected ellipticity of the capillary blank.
[0104] Samples 1 to 7 that follow the linear relationship have medium to large wall thicknesses. More specifically, they range from 238.8 to 863.9 mm 2 The cross-sectional area of the ARE outer capillary is 5.95 to 15.17 mm. 2 The cross-sectional area ratio (CSA_ARE / CSA_ARE) _cap ) ranges from 28.75 to 57.68.
[0105] For very thin-walled samples with larger (surface / volume) ratios, it cannot be excluded that other effects come into play, such as, for example, the heating and cooling behavior of the sample, which may result in somewhat different regression lines. Also, using the linear equation above, the linear regression line for cross-sectional area ratios (CSA_ARE / CSA_ARE) above 25, and especially above 28, is not consistent. _cap ) can also be predicted very well.
[0106] For samples 1-6, the output tube is made of undoped quartz glass. The linear relationship according to equation (3) also applies to doped quartz glass. Optionally, different surface tensions result in different equilibrium pressures according to factor (F1).
[0107] Figure 6 shows a schematic cross-section of a primary preform 15 constructed using the capillary blank 5 of sample 1 (table 1). It represents an intermediate product for manufacturing a hollow core fiber. The primary preform 15 consists of a sleeve tube 14 made of quartz glass with a length of 1000 mm, an outer diameter of 30 mm and an inner diameter of 24 mm. All capillary blanks 5 are in each case present as a joined assembly of nested structural elements consisting of an ARE outer capillary 11 and a nested NE inner capillary 12. The ARE outer tube 11 has an outer diameter of 7.46 mm, the nested NE inner tube 12 has an outer diameter in the region of 4.6 mm. The wall thickness of all structural elements (11, 12) is the same, 0.37 mm. The length of the ARE outer tube 11 and the nested ARE inner tube 12 corresponds to the length of the sleeve tube 14.
[0108] The sleeve tube 14 is manufactured without forming tools in a vertical drawing process by a two-stage elongation process. In the first stage, a hollow output cylinder made of glass is machined to set the final dimensions of the hollow output cylinder. Per final dimensions, the outer diameter is 90 mm and the diameter ratio of the outer diameter to the inner diameter is 2.5. In the first elongation process, the output cylinder with a vertically oriented longitudinal axis is continuously fed to a heating zone with a heating zone length of 200 mm, softened in the inner region, and an intermediate cylinder is drawn from the softening region. In the second elongation process, the intermediate cylinder with a vertically oriented longitudinal axis is continuously fed to a different heating zone with a heating zone length of 100 mm, softened in the inner region, and a tube section is drawn from the softening region. The sleeve tube is obtained from a continuous tube by cutting the continuous tube to a predetermined length.
[0109] Capillary blank 5 is SiO 2 The capillary blanks 5 are fixed to the inner wall of the sleeve tube 14 using a bonding compound 16 based on . The bonding compound 16 is applied locally to the inner surface of the sleeve tube in the region of the ends, on which the capillary blanks 5 are placed using a positioning template with a structurally predetermined star-shaped arrangement of holding arms for the individual capillary blanks 5. In this case, the positioning template is limited to the area around the two end face ends of the sleeve tube.
[0110] The primary preform 15 thus produced is hot-drawn in a drawing process to form a so-called "cane" with an outer diameter of 20 mm. In this case, the capillary blank 5 connects over its entire length to the inner wall of a sleeve tube 14. The drawn sleeve tube 14 is then collected using a collecting cylinder made of quartz glass, which collapses onto the drawn sleeve tube 14, while at the same time the assembly is drawn to form a secondary preform. The collecting cylinder has an outer diameter of 75 mm and a wall thickness of 25 mm.
[0111] In the collapse and expansion process, the coaxial arrangement of sleeve tube 1 and buffer tube extending from below on a vertically oriented longitudinal axis is fed into a temperature controlled heating zone where it is softened zone by zone starting from the top end of the arrangement.
[0112] The heating zone is kept at a target temperature of 1600°C with a control accuracy of + / - 0.1°C, thereby limiting temperature variations during the hot forming process to less than + / - 0.5°C.
[0113] During the collapsing and extending steps, a vacuum is drawn in the gap between the collection cylinder and the cane.
[0114] The secondary preform thus formed during the collapse and elongation process has an outer diameter of 50 mm and a sheath wall thickness consisting of the outer sheath and the inner sheath of 19.55 mm (inner diameter: 10.9 mm). The secondary preform is elongated to form an anti-resonant hollow-core fiber. For this purpose, all structural elements of the previous capillary blank 5 are closed using the sealing or bonding compound mentioned above. The sealing compound is applied only to the end face of the capillary blank that faces up during the fiber drawing process.
[0115] The same end face is then connected to a holding tube made of quartz glass, which simultaneously serves as a gas connection. The retainer is fixed to the collecting cylinder and the sleeve tube with a sealing or joining compound. In the fiber drawing process, the secondary preform is fed from above, with a vertically oriented longitudinal axis, into a temperature-controlled heating zone, in which it is softened zone by zone starting from the lower end. The heating zone is kept at a target temperature of about 2100°C with a control accuracy of + / -0.1°C. Thereby, the temperature fluctuations in the hot forming process can be limited to less than + / -0.5°C. At the same time, gas is supplied to the core region (hollow core) so that an internal pressure of 4 mbar is established in the core region.
[0116] Using such a controlled fiber drawing process, an anti-resonant hollow-core fiber having an anti-resonant element embedded therein with a circular cross-sectional shape is obtained.
Claims
1. 1. A method of manufacturing an anti-resonant hollow-core fiber, the anti-resonant hollow-core fiber comprising a hollow core extending along a longitudinal axis of the fiber and an inner sheath region surrounding the hollow core, the sheath region comprising a plurality of anti-resonant elements, the method comprising: (a) providing a sleeve tube (14), the sleeve tube having an inner bore (16) and a sleeve tube longitudinal axis along which a sleeve tube wall defined by an inner side and an outer side extends; (b) providing a tubular anti-resonant element preform (5), at least a portion of which exists as a capillary blank (5) comprising at least one ARE outer capillary (11) and at least one nested NE inner capillary (12) connected to an inner surface of the ARE outer capillary (11), said manufacturing of said capillary blank comprising: (b1) Outer diameter OD ARE and inner diameter ID ARE On the inner surface of the ARE outer tube (1), an outer diameter OD NE and inner diameter ID NE to form a capillary blank assembly (4); (b2) The capillary blank assembly (4) is thermally stretched to a maximum outer diameter OD ARE_cap and maximum wall thickness WT ARE_cap forming the capillary blank (5) having and (c) mounting the capillary blank (5) at a target location inside the sleeve wall to form a primary preform (15) having a hollow core region (16) and a sheath region; (d) stretching the primary preform (15) to form the hollow-core fiber or further processing the primary preform to form a secondary preform from which the hollow-core fiber is drawn; Including, Said geometric dimension OD NE , I.D. NE , O.D. ARE , I.D. ARE , and O.D. ARE_cap and W.T. ARE_cap are adjusted relative to each other in such a way that the ARE outer capillary (11) of the capillary blank (5) has an ellipticity of less than 1.025, and the diameter dimensions of the ARE outer tube (1) made of quartz glass or the NE inner tube (2) made of quartz glass are such that the equilibrium pressure p eq_ARE of the ARE outer tube (1) is in the range of 25 to 50 Pa, and p eq_ARE = (2 / OD ARE +2 / ID ARE) x σ and the equilibrium pressure p eq_NE of the NE inner pipe (2) is within a range of 60 to 90 Pa, p eq_NE = (2 / OD NE +2 / ID NE) x σ where σ is the surface tension at the draw temperature. A method for fabricating an anti-resonant hollow-core fiber.
2. The geometric dimensions are determined based on the following factors (F1) to (F4): (F1) The ratio of the equilibrium pressure p eq_NE of the NE inner pipe (2) to the equilibrium pressure p eq_NE of the ARE outer pipe (1) eq_ARE The ratio of (F2) The distance (ID) between the ARE outer pipe (1) and the NE inner pipe (2) relative to the inner diameter of the ARE outer pipe (1) ARE -OD NE ) / ID ARE , (F3) Taper ratio OD during hot drawing of the capillary blank assembly (4) according to step (b2) ARE / OD ARE_cap , and (F4) the ratio OD of the outer diameter to the wall thickness of the capillary blank (5) ARE_cap / W.T. ARE_cap 2. The method of claim 1, wherein the method is adjusted relative to
3. The diameter dimension of the ARE outer pipe or the NE inner pipe is such that the equilibrium pressure p eq_NE is in the range of 65 to 80 Pa, and the equilibrium pressure p eq_ARE 3. The method according to claim 2, characterized in that is selected to be in the range of 30 to 40 Pa.
4. 4. The method according to claim 2 or 3, characterized in that the equilibrium pressures p eq_NE and p eq_ARE are adjusted such that the factor (F1) advantageously assumes a value in the range of 1.5 to 2.5, preferably in the range of 1.5 to 2.
5. 4. The method according to claim 2, wherein said factor (F2) is adjusted to a value in the range of 0.2 to 0.5, preferably to a value in the range of 0.3 to 0.
4.
6. 4. The method according to claim 2, wherein said factor (F3) is adjusted to a value in the range of 5 to 10, preferably to a value in the range of 5 to 8.
7. 4. The method according to claim 2, wherein said factor (F4) is adjusted to a value in the range of 15 to 25, preferably to a value in the range of 15 to 20.
8. 4. The method according to claim 2, wherein the factors (F1) to (F4) are adjusted so that the capillary blank (5) has an ellipticity of less than 1.
025.
9. A geometric parameter, the mathematical product of factors (F1) to (F4) being in the range of 35 to 75, preferably in the range of 40 to 60; [0010] The method according to any one of claims 2 to 3, characterized in that:
10. Method according to any one of claims 2 to 3, characterized in that the primary preform (15) has an outer diameter in the range of 26 to 230 mm, preferably 30 to 200 mm.
11. A method of manufacturing a preform (15) for an anti-resonant hollow-core fiber, the anti-resonant hollow-core fiber comprising a hollow core extending along a longitudinal axis of the fiber and an inner sheath region surrounding the hollow core, the sheath region comprising a plurality of anti-resonant elements, the method comprising: (a) providing a sleeve tube (14), the sleeve tube having an inner bore (16) and a sleeve tube longitudinal axis along which a sleeve tube wall defined by an inner side and an outer side extends; (b) providing a tubular anti-resonant element preform, at least a portion of which exists as a capillary blank (5) comprising at least one ARE outer capillary (11) and at least one nested NE inner capillary (12) connected to an inner surface of the ARE outer capillary (11), said manufacturing of said capillary blank (5) comprising: (b1) Outer diameter OD ARE and inner diameter ID ARE On the inner surface of the ARE outer tube (1), an outer diameter OD NE and inner diameter ID NE to form a capillary blank assembly (4); (b2) The capillary blank assembly (4) is thermally stretched to a maximum outer diameter OD ARE_cap and maximum wall thickness WT ARE_cap forming the capillary blank (5) having and (c) mounting the capillary blank (5) at a target location inside the sleeve wall to form a primary preform (15) having a hollow core region (16) and a sheath region; (d) optionally further processing said primary preform (15) to form a secondary preform for said hollow-core fiber, said further processing being performed by the following hot forming process: (i) elongation, (ii) collapse, (iii) collapse and simultaneous extension; (iv) collapse of additional sheath material; (v) collapse and subsequent expansion of additional sheath material; (vi) Collapse and simultaneous expansion of additional sheath material and Including, Said geometric dimension OD NE , I.D. NE , O.D. ARE , I.D. ARE , and O.D. ARE_cap and W.T. ARE_cap are adjusted relative to each other in such a way that the ARE outer capillaries of the capillary blank have an ellipticity of less than 1.025, and the diameter dimensions of the ARE outer tube (1) made of quartz glass or the NE inner tube (2) made of quartz glass are such that the equilibrium pressure p eq_ARE of the ARE outer tube (1) is in the range of 25 to 50 Pa, and p eq_ARE = (2 / OD ARE +2 / ID ARE) x σ and the equilibrium pressure p eq_NE of the NE inner pipe (2) is within a range of 60 to 90 Pa, p eq_NE = (2 / OD NE +2 / ID NE) x σ where σ is the surface tension at the draw temperature. A method for manufacturing a preform (15) for an anti-resonant hollow-core fiber.
12. The geometric dimensions are determined based on the following factors (F1) to (F4): (F1) The ratio of the equilibrium pressure p eq_NE of the NE inner pipe (2) to the equilibrium pressure p eq_NE of the ARE outer pipe (1) eq_ARE The ratio of (F2) The distance (ID) between the ARE outer pipe (1) and the NE inner pipe (2) relative to the inner diameter of the ARE outer pipe (1) ARE -OD NE ) / ID ARE , (F3) Taper ratio OD during hot drawing of the capillary blank assembly (4) according to step (b2) ARE / OD ARE_cap , and (F4) the ratio OD of the outer diameter to the wall thickness of the capillary blank (5) ARE_cap / W.T. ARE_cap 12. The method of claim 11, wherein the method is configured in relation to:
Citation Information
Patent Citations
hollow optical fiber
JP2017520804A
Method for manufacturing an optical fiber preform
JP2020525391A
Anti-resonant hollow core preforms and optical fibers and processing methods
JP2020533264A