LAMINATE, METHOD FOR PRODUCING SAME, AND DISPLAY DEVICE

A laminate with a fine uneven structure and adhesive layer on a light-transmissive substrate addresses adhesion and bubble issues, ensuring effective and cost-efficient manufacturing for display devices.

JP7567187B2Active Publication Date: 2024-10-16MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020055418
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-27
Filing Date
2020-03-26
Publication Date
2024-10-16
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing methods for manufacturing laminates with printed layers on light-transmitting substrates, such as those used in display devices, suffer from issues like air bubbles and blisters due to differences in printing layer levels and outgassing, which increase costs and reduce adhesion.

Method used

A laminate structure is developed with a light-transmissive substrate and a film having a fine uneven structure on one side, bonded with a light-transmissive adhesive layer, where the film's surface opposite to the uneven structure is laminated with the substrate, and a printing layer is formed on the uneven structure, ensuring good adhesion and preventing bubbles and blisters.

Benefits of technology

The laminate achieves improved adhesion between layers, prevents lifting or bubbles due to printing layer differences, and reduces outgas-induced blisters, while being cost-effective to manufacture, enhancing visibility and design quality in display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567187000003
    Figure 0007567187000003
  • Figure 0007567187000004
    Figure 0007567187000004
  • Figure 0007567187000001
    Figure 0007567187000001
Patent Text Reader

Abstract

To provide a laminate without having floating and air bubbles due to the step of a printed layer and swelling and air bubbles due to out gas, and a method for simply manufacturing the same.SOLUTION: A laminate 1 comprises: a light transmissive substrate 2; a film 3 having a fine unevenness structure 4a consisting of a plurality of projections formed at a period equal to or less than a wavelength in a visible light region on one surface; and a printed layer 6 formed on the surface having the fine unevenness structure 4a of the film 3. The one surface of the substrate 2 and the surface on the side opposite to the surface having the fine unevenness structure 4a of the film 3 are laminated through an adhesive material layer 5 having light transmissivity.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a manufacturing method thereof, and a display device. [Background technology]

[0002] Various designs can be applied by providing a printed layer on a light-transmitting substrate using various methods. For example, the substrate constituting the cover member placed on the front of an image display device may have a light-transmitting thin film (optical film) adhered to the printed layer in order to improve the visibility and color reproducibility of the image display and design (FIG. 1). In such cases, the printed layer may lift up or generate air bubbles due to unevenness. As a method for solving this problem, for example, Patent Document 1 discloses a method for suppressing the generation of air bubbles due to unevenness in the printing by providing a smoothing layer between the printed layer and an optical film (moth-eye film) having an adhesive layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-35422 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, this method requires an additional step of providing a smoothing layer, which increases costs. Also, when an optical film is adhered to a printed layer, gas (outgassing) emitted from the printed layer can cause swelling or bubbles to form on the adhesive layer side of the film.

[0005] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a laminate that is free of lifting or air bubbles due to steps in the printed layer and free of bulging or air bubbles due to outgassing, and a method for easily producing such a laminate. [Means for solving the problem]

[0006] The present invention has the following aspects. [1] A laminate comprising a light-transmitting substrate, a film having on one side a fine uneven structure consisting of a plurality of convex portions formed at a period not greater than the wavelength of visible light, and a printed layer formed on the surface of the film having the fine uneven structure, in which one side of the substrate and the surface of the film opposite to the surface having the fine uneven structure are laminated via a light-transmitting adhesive layer. [2] The laminate described above, wherein the surface of the film having a fine uneven structure has an area where no printed layer is formed. [3] The laminate, wherein the surface of the fine uneven structure has a water contact angle of 30° or less. [4] The laminate, wherein the surface of the fine uneven structure has a water contact angle of 120° or more. [5] The laminate, wherein the thickness of the adhesive layer is 50 μm or less. [6] The laminate as described above, wherein the material of the light-transmitting substrate is at least one of polycarbonate and acrylic resin. [7] A display device having the laminate. [8] The display device as described above, wherein a surface of the light-transmitting substrate opposite to a surface in contact with the adhesive layer is disposed facing toward the outside of the device. [9] A method for producing a laminate, comprising forming a printing layer on a surface of a film having a fine uneven structure on one side thereof, the surface being composed of a plurality of convex portions formed at a period not greater than the wavelength of visible light, and then laminating one surface of a light-transmitting substrate and the surface of the film opposite the surface having the fine uneven structure via a light-transmitting adhesive layer.

[10] A method for producing a laminate, comprising: preparing a film having, on one side thereof, a fine uneven structure consisting of a plurality of convex portions formed at a period not greater than the wavelength of visible light; forming a light-transmitting adhesive layer on the side opposite to the side having the fine uneven structure; forming a printing layer on the side having the fine uneven structure; and bonding and laminating one side of a light-transmitting substrate and the side of the film having the adhesive layer. Effect of the Invention

[0007] The laminate of the present invention has good adhesion between the layers, no lifting or bubbles due to steps in the printed layer, and no swelling or bubbles due to outgassing. According to the method for producing the laminate of the present invention, a laminate can be produced easily and at low cost, in which the layers have good adhesion between the layers, no lifting or bubbles due to steps in the printed layer, and no swelling or bubbles due to outgassing. Furthermore, the display device of the present invention has improved visibility. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a conventional laminate. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below. In this specification, the term "light transmissive" means that at least visible light, that is, light with a wavelength of 400 to 800 nm, is transmitted. In addition, the term "active energy rays" as used herein means visible light, ultraviolet rays, electron beams, plasma, heat rays (infrared rays, etc.), and the like. In addition, in this specification, "(meth)acrylate" is a general term for acrylate and methacrylate, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid, "(meth)acrylonitrile" is a general term for acrylonitrile and methacrylonitrile, and "(meth)acrylamide" is a general term for acrylamide and methacrylamide. In Figures 1 and 2, each layer is shown at a different scale so that each layer is large enough to be recognizable on the drawing.

[0010] First Embodiment <Laminate> 2 is a cross-sectional view showing an example of a laminate according to a first embodiment of the present invention. The laminate 1 of this example is a laminate including a light-transmitting substrate, a film having on one side thereof a fine uneven structure consisting of a plurality of convex portions formed at a period equal to or shorter than the wavelength of visible light, and a printed layer formed on the surface of the film having the fine uneven structure, in which one surface of the substrate and the surface of the film opposite to the surface having the fine uneven structure are laminated via a light-transmitting adhesive layer.

[0011] (light-transparent substrate) Examples of materials for the light-transmitting substrate 2 include acrylic resin, polycarbonate, polystyrene resin, polyester, cellulose resin (such as triacetyl cellulose), polyolefin, alicyclic polyolefin, glass, etc. From the viewpoints of transparency, durability, etc., it is preferable to use at least one of polycarbonate and acrylic resin. The light-transmitting substrate may be colored and transparent or colorless and transparent, and may be appropriately selected in consideration of design and light transmittance depending on the application. The surface of the light-transmitting substrate 2 may be subjected to a coating or corona treatment for the purpose of improving properties such as adhesion, antistatic properties, scratch resistance, and weather resistance.

[0012] (film) The material of the film 3 may be the same as that of the light-transmitting substrate. A cured resin layer having a fine uneven structure is formed on one surface of the film 3. The surface of the film 3 may be subjected to various coatings or corona treatments, as in the case of the surface of the light-transmitting substrate. Examples of materials for the film 3 include acrylic resins such as ACRYPLEN HBS010P, HBS006, and HBA002P (manufactured by Mitsubishi Chemical Corporation), Technoloy S000, S020, S001G, S014G, TSF001, TSF002, MX001M30, and MXS001M60 (manufactured by S-Carbosheet Co., Ltd.), Sunduren SD009 and SD010 (manufactured by Kaneka Corporation), and Acriview FZ, FV, and HV (manufactured by Nippon Shokubai Co., Ltd.). Specific examples of polycarbonates include Panlite PC-1151, PC-2151, PC-1141, PC-2141, NJ-5100, NK-5101 (manufactured by Teijin Limited), C000, C001, C003, C101, C103, C010 (manufactured by S-Carbosheet Co., Ltd.), PC-10, AW-10, PW-10 (manufactured by Shine Techno Co., Ltd.), and Elmec R Film (manufactured by Kaneka Corporation). Specific examples of polyesters include Diafoil T910E, T600E (manufactured by Mitsubishi Chemical Corporation), Lumirror U343, U483, U403, U413, UD03, UH13, UF83, QTH0, SF20 (manufactured by Toray Industries, Inc.), Cosmoshine A4300, A2330, TA017, TA015, TA042, TA044, TA048, Softshine TA009 (manufactured by Toyobo Co., Ltd.), etc. Specific examples of cellulose-based materials include Fujitac TD80U, TD80UL, T80UZ, T80SE, TD60ULP (manufactured by Fujifilm Corporation), TAC Film KC4UA (manufactured by Konica Minolta, Inc.), etc. Specific examples of alicyclic polyolefins include ZEONOR ZF14 and ZF16 (manufactured by Zeon Corporation), ARTON FILM (manufactured by JSR Corporation), and TOPAS (manufactured by Polyplastics Co., Ltd.). The surface of the film may be coated with a primer for the purpose of improving properties such as increasing adhesion and adjusting the refractive index.

[0013] From the viewpoints of ease of handling and stability of thermodynamic properties, the thickness of the film is preferably 10 μm or more, more preferably 20 μm or more, and is preferably 700 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.

[0014] (cured resin layer) The cured resin layer 4 is a film made of a cured product of an active energy ray-curable resin composition described below, and has a fine uneven structure made up of a plurality of protrusions 4a on its surface.

[0015] The method for forming the fine uneven structure is not particularly limited, and examples thereof include a method of directly forming the structure on a molded body, a method of transferring the structure from a mold having a fine uneven structure (transfer method), etc. In the case of the transfer method, the fine uneven structure is preferably formed by transferring a plurality of pores of anodized alumina, which will be described later. The fine uneven structure formed by transferring a plurality of pores of anodized alumina can be formed at low cost and can be made large in area.

[0016] The average interval (period) P between adjacent convex portions 4a of the fine uneven structure is equal to or less than the wavelength of visible light, i.e., 400 nm or less, preferably 300 nm or less, and more preferably 250 nm or less. When convex portions 4a are formed by transferring a plurality of pores of anodized alumina, a high voltage is required to increase the pore interval, which makes industrial production difficult, and therefore the average interval P between convex portions 4a is particularly preferably 200 nm or less. If the average interval P between convex portions 4a is equal to or less than the wavelength of visible light, the reflectance is low and the wavelength dependency of the reflectance is small. From the viewpoint of ease of forming the protrusions 4a, the average interval P between the protrusions 4a is preferably 20 nm or more, and more preferably 80 nm or more. The average spacing P between the protrusions 4a was determined by measuring the spacing between adjacent protrusions 4a (the distance from the center of a protrusion 4a to the center of an adjacent protrusion 4a) at 50 points using an electron microscope and averaging these values.

[0017] The average height H of the protrusions 4a is preferably 100 nm or more, and more preferably 130 nm or more. If the average height H of the protrusions 4a is 100 nm or more, the reflectance is low and the wavelength dependency of the reflectance is small. In addition, the adhesion between the layers can be sufficiently ensured. If it is 180 nm or more and 300 nm or less, the reflection in the visible light region and the near infrared light region can be effectively reduced. From the viewpoint of ease of forming the protrusion structure, the average height H of the protrusions 4a is preferably 400 nm or less, and more preferably 300 nm or less. The average height H of the convex portions 4a was determined by measuring the distance between the top of the convex portion 4a and the bottom of the concave portion between the convex portions 4a at 50 points using an electron microscope, and averaging these values.

[0018] The aspect ratio (H / P) of the protrusions 4a is preferably 0.8 to 5, more preferably 1.2 to 4, and further preferably 1.5 to 3. When the aspect ratio of the protrusions 4a is 0.8 or more, the reflectance is sufficiently low. Also, the adhesion between layers can be sufficiently ensured. When the aspect ratio of the protrusions 4a is 5 or less, the scratch resistance of the protrusions 4a is good.

[0019] The shape of the protrusion 4a may be a substantially conical shape, a pyramidal shape, a bell shape, a cylindrical shape, or the like.

[0020] (Printing layer) The printed layer 6 is preferably a layer containing a resin ink, but is not limited to this resin ink. Hereinafter, "ink" may also be referred to as "ink". The printed layer 6 may have a single-layer structure or a multi-layer structure. Usually, multiple printed layers of different colors are formed on the back surface of the light-transmitting substrate 2 to form printed images such as photographs, pictures, letters, and numbers.

[0021] The resin ink contains a resin, a colorant, and a solvent. The resin ink may also contain additives as necessary. The resin ink used in the present invention may be either oil-based or water-soluble, but the oil-based ink is preferred because it has excellent compatibility with the cured resin layer 4. As the oil-based ink or water-soluble ink, known inks used for forming printed images can be used. Commercially available products may also be used. Specific examples of oil-based inks include Jujo Chemical Co., Ltd.'s product number 762, Raycure series, Teikoku Ink Co., Ltd.'s IPX-HF series, MIX-HF series, IRX-HF series, Seiko Advance Co., Ltd.'s HF-HSD series, HF-GV3 series, HF-GV2 series, IR BLACK series, Roland Co., Ltd.'s EUV-BK (90) Black, etc. In addition, oil-based markers (e.g. Zebra's Mackie) can also form a printing layer. An example of each component contained in the oil-based ink and the water-soluble ink will be specifically described below.

[0022] Oil-based inks: Examples of resins contained in oil-based inks include thermoplastic resins such as acrylic resins, maleic acid resins, rosin-based resins, epoxy resins, silicone resins, and butyral resins. Examples of colorants contained in oil-based inks include dyes such as azo-based metal complexes and phthalocyanines; and pigments such as carbon black and organic pigments. The solvent contained in the oil-based ink is an organic solvent such as ketone, alcohol, ethyl acetate, etc. In particular, alcohol having permeability is preferable, and it is possible to reduce the difference in refractive index at the interface with the cured resin layer 4. Examples of additives contained in oil-based inks include a conductivity imparting agent, a plasticizer, an antioxidant, and an ultraviolet absorbing agent.

[0023] Water-soluble inks: Water-soluble inks are generally composed of colorants, dispersants (resins, etc.), additives, and hydrophilic solvents. Examples of resins contained in water-soluble inks include acrylic block copolymers. Examples of colorants contained in the water-soluble ink include dyes such as anionic azo dyes and phthalocyanine; and pigments such as carbon black and organic pigments. The main solvent in water-soluble ink is water. The water may also contain glycerin or glycol, which acts as an anti-drying agent, or alcohol or glycol ether, which acts as a penetrating agent. In particular, if the water contains a penetrating agent, the refractive index difference at the interface with the light-transmitting substrate 2 can be reduced. Examples of additives contained in the water-soluble ink include pH adjusters such as alcohol amines and sodium hydroxide, chelating agents such as EDTA, surfactants such as nonionic surfactants, cationic surfactants, and anionic surfactants, antibacterial and antifungal agents, etc. As the water-soluble ink, for example, commercially available printing inks for plastics can be used.

[0024] The refractive index difference between the printed layer 6 and the cured resin layer 4 is preferably within a range of -0.2 to 0.2. If the refractive index difference between the printed layer 6 and the cured resin layer 4 is within the above range, the fine uneven structure formed in the cured resin layer 4 can suppress reflection of external light when the laminate 1 is viewed from the light-transmitting substrate 2 side, and the printed image by the printed layer 6 can be made to look clear.

[0025] It is preferable that the surface of the film having the fine uneven structure has an area where no printed layer is formed. The area where the printed layer is formed has a clear printed image, and the transparent area where no printed layer is formed has improved visibility of background images (electronic displays, paintings, etc.) due to the reduction in light reflection caused by the fine uneven structure, making it useful as an excellent design material.

[0026] <Method of manufacturing laminate> The laminate of the present invention can be produced by forming a printed layer on the surface of a film having a fine uneven structure on one surface thereof, the fine uneven structure consisting of a plurality of convex portions formed at a period not exceeding the wavelength of visible light, and then laminating one surface of a light-transmitting substrate and the surface of the film opposite the surface having the fine uneven structure via a light-transmitting adhesive layer. The laminate of the present invention can also be produced by preparing a film having a fine uneven structure on its surface consisting of a plurality of convex portions formed at a period not greater than the wavelength of visible light, then forming a light-transmitting adhesive layer on the side opposite to the side having the fine uneven structure, forming a printing layer on the side having the fine uneven structure, and laminating one side of a light-transmitting substrate and the side of the film having the adhesive layer. Although the present invention is not limited to the above-mentioned production methods, the above-mentioned production methods are preferable from the viewpoints of ease of handling in the production process, the size of the production lot, and the like, and these can be appropriately selected. The laminate 1 shown in FIG. 2 can be produced, for example, by forming a cured resin layer 4 on the surface of a film 3, printing a printed layer 6 using a resin ink on the fine uneven structure on the surface of the cured resin layer 4, and then laminating one side of a light-transmitting substrate and the side of the film opposite the side having the fine uneven structure via a light-transmitting adhesive layer. The method for printing the printing layer 6 on the surface of the fine uneven structure is not particularly limited, and a known method can be used. Specific examples include plateless printing such as inkjet printing, thermal transfer (ink ribbon) printing, and laser printer printing; stencil printing such as screen printing; lithographic printing such as offset printing; relief printing such as letterpress printing and flexographic printing; and intaglio printing such as gravure printing. In addition, the printing layer 6 may be formed using a seal or stamp, or may be formed by simple drawing, and such cases of forming the printing layer 6 are also included in printing.

[0027] The method for forming the cured resin layer 4 on the surface of the film 3 is not particularly limited, but may be, for example, the method disclosed in JP 2015-116819 A. Specifically, the method is as follows. An active energy ray-curable resin composition is supplied from a tank between the surface of a roll-shaped mold on which anodized alumina having a plurality of pores is formed and the surface of a film-shaped light-transmitting substrate (hereinafter referred to as "film substrate") that moves along the surface of the mold in synchronization with the rotation of the mold.

[0028] The film substrate and the active energy ray-curable resin composition are nipped between the mold and a nip roll whose nip pressure is adjusted by an air pressure cylinder, and the active energy ray-curable resin composition is uniformly distributed between the film substrate and the mold and simultaneously filled into the pores of the mold.

[0029] With the active energy ray-curable resin composition sandwiched between the mold and the film substrate, an active energy ray irradiation device installed below the mold is used to irradiate the active energy ray-curable resin composition with active energy rays from the film substrate side, thereby curing the active energy ray-curable resin composition, thereby forming a cured resin layer 4 having, on its surface, an uneven structure consisting of a plurality of convex portions to which the plurality of pores on the surface of the mold have been transferred. The film substrate having the cured resin layer 4 formed on its surface is peeled off with a peel roll to obtain a film having a fine uneven structure in which the cured resin layer 4 is laminated on the surface of the film substrate.

[0030] The active energy ray irradiation device is preferably a high pressure mercury lamp, a metal halide lamp, an electrodeless UV lamp (fusion UV), a UV-LED, etc. The integrated light amount is preferably 100 to 10000 mJ / cm2.

[0031] (Mold) The mold is not particularly limited, and examples thereof include a mold having a concave-convex structure formed by lithography or laser processing, a mold having anodized alumina on the surface, etc., but considering the inexpensive increase in area, a mold having anodized alumina on the surface is preferred. A mold having anodized alumina on the surface can be increased in area and is easy to fabricate.

[0032] Anodized alumina is a porous oxide film of aluminum (anodized aluminum) with multiple pores on its surface.

[0033] A mold having anodized alumina on its surface can be manufactured, for example, through the following steps (a) to (f). Although the regularity of the arrangement of the pores will be somewhat reduced, it is also possible to skip steps (a) and (b) and start with step (c), to carry out only step (a), or to carry out steps (c) and (d) without carrying out steps (a), (b), and (f). (a) A process for forming an oxide film by anodizing an aluminum substrate in an electrolyte. (b) A process for removing the oxide film and forming pore initiation points for anodization. (c) A process of anodizing the aluminum substrate again in an electrolyte to form an oxide film having pores at the pore generation points. (d) A step of enlarging the pore size. (e) after step (d), a step of anodizing again in an electrolyte; (f) Repeating steps (d) and (e).

[0034] Process (a): When an aluminum substrate is anodized, an oxide film having fine pores is formed. The purity of aluminum is preferably 99% or more, more preferably 99.5% or more, and particularly preferably 99.8% or more. If the purity of aluminum is low, the regularity of the pores obtained by anodization may decrease. Examples of the electrolyte include an aqueous solution of sulfuric acid, an aqueous solution of oxalic acid, and an aqueous solution of phosphoric acid.

[0035] Process (b): The oxide film is temporarily removed and used as the pore generating points 40 for the anodic oxidation, thereby improving the regularity of the pores.

[0036] The oxide film can be removed by dissolving it in a solution that does not dissolve aluminum but selectively dissolves the oxide film, for example, a mixed solution of chromic acid and phosphoric acid.

[0037] Process (c): When the aluminum base material from which the oxide film has been removed is anodized again, an oxide film having cylindrical pores is formed. The electrolyte may be the same as that used in step (a).

[0038] Process (d): A process for enlarging the diameter of the pores (hereinafter referred to as pore size enlargement process) is carried out. The pore size enlargement process is a process for enlarging the diameter of the pores obtained by anodization by immersing in a solution that dissolves the oxide film. An example of such a solution is an aqueous solution of phosphoric acid with a concentration of about 5% by mass.

[0039] Process (e): Re-anodization results in the formation of additional cylindrical pores of smaller diameter extending downward from the bottom of the cylindrical pores. The electrolyte may be the same as that used in step (a).

[0040] Process (f): By repeating the pore diameter enlargement treatment in step (d) and the anodization in step (e), a mold 20 is obtained in which anodized alumina (a porous oxide film of aluminum (anodized aluminum)) is formed with pores whose diameters decrease continuously from the openings in the depth direction. It is preferable to finish with step (d).

[0041] The surface of the anodized alumina may be treated with a release agent so as to facilitate separation from the cured resin layer. Examples of the treatment method include a method of coating with a silicone resin or a fluorine-containing polymer, a method of vapor-depositing a fluorine-containing compound, and a method of coating with a fluorine-containing silane compound.

[0042] Examples of the shape of the pores include a substantially conical shape, a pyramidal shape, a bell shape, and a cylindrical shape.

[0043] The average spacing between the pores is equal to or smaller than the wavelength of visible light, i.e., 400 nm or less, preferably 300 nm or less, more preferably 250 nm or less, and particularly preferably 200 nm. The average spacing between the pores 36 is preferably 20 nm or more, more preferably 80 nm or more. The average depth of the pores is preferably 100 nm or more, and more preferably 130 nm or more. The average depth of the pores 36 is preferably 400 nm or less, and more preferably 300 nm or less.

[0044] (Active energy ray-curable resin composition) The active energy ray-curable resin composition contains a polymerizable compound and a polymerization initiator. Examples of the polymerizable compound include monomers, oligomers, and reactive polymers having a radically polymerizable bond and / or a cationic polymerizable bond in the molecule.

[0045] Polymerizable compound: The monomer having a radically polymerizable bond may be a monofunctional monomer or a polyfunctional monomer. Examples of monofunctional monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, alkyl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, and the like. Examples of such acrylates include (meth)acrylate derivatives such as acrylate, tetrahydrofurfuryl (meth)acrylate, allyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, and 2-ethoxyethyl (meth)acrylate; (meth)acrylic acid, (meth)acrylonitrile; styrene derivatives such as styrene and α-methylstyrene; (meth)acrylamide derivatives such as (meth)acrylamide, N-dimethyl (meth)acrylamide, N-diethyl (meth)acrylamide, and dimethylaminopropyl (meth)acrylamide. These may be used alone or in combination of two or more.

[0046] Examples of polyfunctional monomers include ethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, isocyanuric acid ethylene oxide modified di(meth)acrylate, triethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, and polybutylene glycol. Di(meth)acrylate, 2,2-bis(4-(meth)acryloxypolyethoxyphenyl)propane, 2,2-bis(4-(meth)acryloxyethoxyphenyl)propane, 2,2-bis(4-(3-(meth)acryloxy-2-hydroxypropoxy)phenyl)propane, 1,2-bis(3-(meth)acryloxy-2-hydroxypropoxy)ethane, 1,4-bis(3-(meth)acryloxy-2-hydroxypropoxy)butane, dimethyloltricyclodecane di(meth)acrylate, ethylene oxide of bisphenol A Bifunctional monomers such as side adduct di(meth)acrylate, propylene oxide adduct di(meth)acrylate of bisphenol A, hydroxypivalic acid neopentyl glycol di(meth)acrylate, divinylbenzene, methylene bisacrylamide; pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethylene oxide modified tri(meth)acrylate, trimethylolpropane propylene oxide modified triacrylate, trimethylolpropane trifunctional monomers such as ethylene oxide-modified triacrylate and ethylene oxide-modified tri(meth)acrylate with isocyanuric acid; tetrafunctional or higher monomers such as a condensation reaction mixture of succinic acid / trimethylolethane / acrylic acid, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane tetraacrylate, and tetramethylolmethane tetra(meth)acrylate; difunctional or higher urethane acrylates, difunctional or higher polyester acrylates, etc. These may be used alone or in combination of two or more.

[0047] Examples of the monomer having a cationically polymerizable bond include monomers having an epoxy group, an oxetanyl group, an oxazolyl group, a vinyloxy group, etc., and monomers having an epoxy group are particularly preferred.

[0048] Examples of the oligomer or reactive polymer include unsaturated polyesters such as condensates of unsaturated dicarboxylic acids and polyhydric alcohols; polyester (meth)acrylates, polyether (meth)acrylates, polyol (meth)acrylates, epoxy (meth)acrylates, urethane (meth)acrylates, cationic polymerization type epoxy compounds, and homopolymers or copolymers of the above-mentioned monomers having radically polymerizable bonds in their side chains.

[0049] Polymerization initiator: When a photocuring reaction is used, examples of the photopolymerization initiator include carbonyl compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzil, benzophenone, p-methoxybenzophenone, 2,2-diethoxyacetophenone, α,α-dimethoxy-α-phenylacetophenone, methylphenyl glyoxylate, ethylphenyl glyoxylate, 4,4'-bis(dimethylamino)benzophenone, and 2-hydroxy-2-methyl-1-phenylpropan-1-one; sulfur compounds such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide; 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and benzoyldiethoxyphosphine oxide. These may be used alone or in combination of two or more.

[0050] In the case of using an electron beam curing reaction, examples of the polymerization initiator include thioxanthones such as benzophenone, 4,4-bis(diethylamino)benzophenone, 2,4,6-trimethylbenzophenone, methyl orthobenzoyl benzoate, 4-phenylbenzophenone, t-butylanthraquinone, 2-ethylanthraquinone, 2,4-diethylthioxanthone, isopropylthioxanthone, and 2,4-dichlorothioxanthone; diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 1-hydroxycyclohexyl-phenyl ketone, and 2-methyl-2-morpholino(4-thiomethylphenyl)propane. acetophenones such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone; benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; methylbenzoyl formate, 1,7-bisacridinylheptane, and 9-phenylacridine. These may be used alone or in combination of two or more.

[0051] In the case of utilizing a thermosetting reaction, examples of the thermal polymerization initiator include organic peroxides such as methyl ethyl ketone peroxide, benzoyl peroxide, dicumyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyoctoate, t-butyl peroxybenzoate, and lauroyl peroxide; azo compounds such as azobisisobutyronitrile; and redox polymerization initiators in which the organic peroxides are combined with amines such as N,N-dimethylaniline and N,N-dimethyl-p-toluidine.

[0052] The amount of the polymerization initiator is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the polymerizable compound. If the amount of the polymerization initiator is less than 0.1 parts by mass, the polymerization does not proceed easily. If the amount of the polymerization initiator is more than 10 parts by mass, the cured resin layer may become discolored or the mechanical strength may decrease.

[0053] Internal release agent: By including an internal release agent in the active energy ray-curable resin composition, continuous transferability can be improved. The internal mold release agent is not particularly limited in composition as long as it improves the releasability between the cured product of the active energy ray-curable resin composition and the surface of a metal mold and is compatible with the active energy ray-curable resin composition.

[0054] Examples of internal release agents include (poly)oxyalkylene alkyl phosphate compounds, fluorine-containing compounds, silicone compounds, phosphate ester compounds (excluding (poly)oxyalkylene alkyl phosphate compounds), compounds having long-chain alkyl groups, polyalkylene waxes, amide waxes, Teflon powder (Teflon is a registered trademark), and the like. These may be used alone or in combination of two or more kinds. Among these, those containing a (poly)oxyalkylene alkyl phosphate compound as the main component are preferred.

[0055] By containing the same (poly)oxyalkylene alkyl phosphate compound as the mold release agent as the internal mold release agent, the mold releasability between the cured resin layer, which is the cured product, and the mold is particularly good. In addition, since the load during mold release is extremely low, the fine uneven structure is less damaged, and as a result, the fine uneven structure of the mold can be efficiently and accurately transferred.

[0056] As the (poly)oxyalkylene alkyl phosphate compound, a compound represented by the following formula (1) is preferred from the viewpoint of releasability. (HO)3-t(O=)P[-O-(R2O)s-R1]t ···(1). Here, R1 represents an alkyl group, R2 represents an alkylene group, s represents an integer of 1 to 20, and t represents an integer of 1 to 3.

[0057] R1 is preferably an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 3 to 18 carbon atoms. R2 is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably an alkylene group having 2 to 3 carbon atoms. s is preferably an integer of 1 to 10.

[0058] The (poly)oxyalkylene alkyl phosphate compound may be any of a monoester (t=1), a diester (t=2), and a triester (t=3). In the case of a diester or triester, the (poly)oxyalkylene alkyl groups in one molecule may be different from each other.

[0059] Examples of commercially available (poly)oxyalkylene alkyl phosphate compounds include the following: Johoku Chemical Co., Ltd.: JP-506H (t ≒ 1 to 2, s ≒ 1, R1 = butyl group, R2 = ethylene group), Axel: Moldwith INT-1856 (structure not disclosed), Nikko Chemicals: TDP-10 (t≒3, s≒10, R1=C12-15, R2=ethylene group), TDP-8 (t≒3, s≒8, R1=C12-15, R2=ethylene group), TDP-6 (t≒3, s≒6, R1=C12-15, R2=ethylene group), TDP-2 (t≒3, s≒2, R1=C12-15, R2=ethylene group), DDP-10 (t≒2, s≒10, R1=C12-15, R2=ethylene group), DDP-8 (t≒2, s≒8, R1=C12-15, R2 = ethylene group), DDP-6 (t ≒ 2, s ≒ 6, R1 = C12-15, R2 = ethylene group), DDP-4 (t ≒ 2, s ≒ 4, R1 = C12-15, R2 = ethylene group), DDP-2 (t ≒ 2, s ≒ 2, R1 = C12-15, R2 = ethylene group), TLP-4 (t ≒ 3, s ≒ 4, R1 = lauryl group, R2 = ethylene group), TCP-5 (t ≒ 3, s ≒ 5, R1 = cetyl group, R2 = ethylene group), DLP-10 (t ≒ 3, s ≒ 10, R1 = lauryl group, R2 = ethylene group). The (poly)oxyalkylene alkyl phosphate compounds may be used alone or in combination of two or more kinds.

[0060] The amount of the (poly)oxyalkylene alkyl phosphate compound is preferably 0.01 to 1 part by mass, more preferably 0.05 to 0.5 parts by mass, and even more preferably 0.05 to 0.1 parts by mass, relative to 100 parts by mass of the polymerizable compound. When the amount of the (poly)oxyalkylene alkyl phosphate compound is 1 part by mass or less, the deterioration of the performance of the cured resin layer is suppressed. In addition, the deterioration of the adhesion to the film substrate is suppressed, and as a result, the resin residue on the mold (poor release) and the peeling of the cured resin layer from the article are suppressed. When the amount of the (poly)oxyalkylene alkyl phosphate compound is 0.01 part by mass or more, the mold releasability from the mold is sufficient, and the resin residue on the mold (poor release) is suppressed.

[0061] Other Ingredients: The active energy ray-curable resin composition may contain, as necessary, a non-reactive polymer, an active energy ray sol-gel reactive composition, an antistatic agent, an additive such as a fluorine compound for improving antifouling properties, fine particles, and a small amount of a solvent.

[0062] Examples of non-reactive polymers include acrylic resins, styrene resins, polyurethanes, cellulose resins, polyvinyl butyral, polyesters, and thermoplastic elastomers. Examples of the active energy ray sol-gel reactive composition include alkoxysilane compounds and alkyl silicate compounds.

[0063] The alkoxysilane compound includes a compound represented by the following formula (2). R11xSi(OR12)y ···(2). Here, R11 and R12 each represent an alkyl group having 1 to 10 carbon atoms, and x and y represent integers that satisfy the relationship x+y=4.

[0064] Examples of the alkoxysilane compound include tetramethoxysilane, tetra-i-propoxysilane, tetra-n-propoxysilane, tetra-n-butoxysilane, tetra-sec-butoxysilane, tetra-t-butoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltributoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, trimethylmethoxysilane, trimethylpropoxysilane, and trimethylbutoxysilane.

[0065] The alkyl silicate compound may be the compound represented by the following formula (3). R21O[Si(OR23)(OR24)O]zR22 ···(3). Here, R21 to R24 each represent an alkyl group having 1 to 5 carbon atoms, and z represents an integer of 3 to 20.

[0066] Examples of the alkyl silicate compound include methyl silicate, ethyl silicate, isopropyl silicate, n-propyl silicate, n-butyl silicate, n-pentyl silicate, and acetyl silicate.

[0067] The cured product of the active energy ray curable resin composition may be hydrophobic or hydrophilic. By changing the cured product of the active energy ray curable resin composition to be hydrophobic or hydrophilic, it is possible to impart properties (for example, water resistance, fingerprint wiping property, anti-fogging property) as required.

[0068] (hydrophilic material) From the viewpoints of ink wettability, adhesion to a printing layer, and anti-fogging properties, the surface of the fine unevenness structure is preferably hydrophilic. Specifically, the contact angle of water on the surface of the fine unevenness structure is preferably 30° or less, more preferably 20° or less. As an active energy ray curable resin composition capable of forming a hydrophilic material, it is preferable to use a composition containing a polyfunctional (meth)acrylate having 4 or more functional groups, a hydrophilic (meth)acrylate having 2 or more functional groups, and, if necessary, a monofunctional monomer.

[0069] Examples of polyfunctional (meth)acrylates having 4 or more functional groups include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol ethoxytetra(meth)acrylate, dipentaerythritol hydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, a condensation reaction mixture of succinic acid / trimethylolethane / acrylic acid in a molar ratio of 1:2:4, and urethane acrylates (manufactured by Daicel-Cytec: EBECRYL220, EBECRYL1290, EBECRYL1290K ... L5129, EBECRYL8210, EBECRYL8301, KRM8200), polyether acrylates (manufactured by Daicel-Cytec: EBECRYL81), modified epoxy acrylates (manufactured by Daicel-Cytec: EBECRYL3416), polyester acrylates (manufactured by Daicel-Cytec: EBECRYL450, EBECRYL657, EBECRYL800, EBECRYL810, EBECRYL811, EBECRYL812, EBECRYL1830, EBECRYL845, EBECRYL846, EBECRYL1870), etc. These may be used alone or in combination of two or more. As the tetrafunctional or higher polyfunctional (meth)acrylate, a pentafunctional or higher polyfunctional (meth)acrylate is more preferable.

[0070] Examples of the difunctional or higher hydrophilic (meth)acrylate include polyfunctional acrylates having long-chain polyethylene glycol, such as ARONIX M-240, ARONIX M260 (manufactured by Toagosei Co., Ltd.), NK Ester AT-20E, NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd.), polyethylene glycol dimethacrylate, etc. These may be used alone or in combination of two or more. In the polyethylene glycol dimethacrylate, the average total number of repeating units of the polyethylene glycol chain present in one molecule is preferably 6 to 40, more preferably 9 to 30, and particularly preferably 12 to 20. When the average number of repeating units of the polyethylene glycol chain is 6 or more, hydrophilicity is sufficient and antifouling properties are improved. When the average number of repeating units of the polyethylene glycol chain is 40 or less, compatibility with polyfunctional (meth)acrylates having 4 or more functionalities is good, and the active energy ray-curable resin composition is less likely to separate.

[0071] The monofunctional monomer is preferably a hydrophilic monofunctional monomer. Examples of hydrophilic monofunctional monomers include monofunctional (meth)acrylates having a polyethylene glycol chain on an ester group, such as M-20G, M-90G, and M-230G (manufactured by Shin-Nakamura Chemical Co., Ltd.), monofunctional (meth)acrylates having a hydroxyl group on an ester group, such as hydroxyalkyl (meth)acrylates, monofunctional acrylamides, and cationic monomers such as methacrylamide propyl trimethyl ammonium methyl sulfate and methacryloyloxyethyl trimethyl ammonium methyl sulfate. In addition, as the monofunctional monomer, a viscosity modifier such as acryloylmorpholine or vinylpyrrolidone, or an adhesion improver such as acryloyl isocyanates that improves adhesion to a film substrate may be used.

[0072] The monofunctional monomer may be blended in the active energy ray curable resin composition as a low polymerization degree polymer obtained by (co)polymerizing one or more kinds of monofunctional monomers. Examples of the low polymerization degree polymer include a 40 / 60 copolymer oligomer of monofunctional (meth)acrylates having a polyethylene glycol chain on an ester group such as M-230G (manufactured by Shin-Nakamura Chemical Co., Ltd.) and methacrylamide propyl trimethyl ammonium methyl sulfate (manufactured by MCC Unitech Co., Ltd., "MG Polymer"). In the case of a hydrophilic material, the ink for forming the printed layer is preferably an oil-based ink as described above, but a wide range of inks, including water-soluble inks, can be used depending on the conditions of use.

[0073] (Hydrophobic material) When the surface of the fine unevenness structure is required to be hydrophobic, for example to prevent adhesion of water droplets, it is preferable to use a composition containing at least one of a fluorine-containing compound and a silicone-based compound as an active energy ray curable resin composition capable of forming a hydrophobic material. In this case, the contact angle of water on the surface of the fine unevenness structure is preferably 120° or more, more preferably 130° or more.

[0074] Examples of the fluorine-containing compound include a fluorine-containing monomer, a fluorine-containing silane coupling agent, a fluorine-containing surfactant, and a fluorine-containing polymer.

[0075] Examples of the fluorine-containing monomer include a fluoroalkyl group-substituted vinyl monomer and a fluoroalkyl group-substituted ring-opening polymerizable monomer. Examples of the fluoroalkyl group-substituted vinyl monomer include fluoroalkyl group-substituted (meth)acrylates, fluoroalkyl group-substituted (meth)acrylamides, fluoroalkyl group-substituted vinyl ethers, and fluoroalkyl group-substituted styrenes.

[0076] Examples of the fluoroalkyl group-substituted ring-opening polymerizable monomer include a fluoroalkyl group-substituted epoxy compound, a fluoroalkyl group-substituted oxetane compound, and a fluoroalkyl group-substituted oxazoline compound.

[0077] Examples of the fluorine-containing silane coupling agent include 3,3,3-trifluoropropyltrimethoxysilane, 3,3,3-trifluoropropyltriacetoxysilane, dimethyl-3,3,3-trifluoropropylmethoxysilane, and tridecafluoro-1,1,2,2-tetrahydrooctyltriethoxysilane.

[0078] Examples of the fluorine-containing surfactant include a fluoroalkyl group-containing anionic surfactant and a fluoroalkyl group-containing cationic surfactant.

[0079] The fluorine-containing polymer includes a polymer of a fluoroalkyl group-containing monomer, Examples of the fluorine-containing polymer include a copolymer of an alkyl group-containing monomer and a poly(oxyalkylene) group-containing monomer, a copolymer of a fluoroalkyl group-containing monomer and a crosslinking reactive group-containing monomer, etc. The fluorine-containing polymer may be a copolymer with other copolymerizable monomers.

[0080] Examples of the silicone-based compound include (meth)acrylic acid-modified silicone, silicone resin, and silicone-based silane coupling agent. Examples of the (meth)acrylic acid modified silicone include silicone (di)(meth)acrylates, and for example, silicone diacrylates "x-22-164" and "x-22-1602" manufactured by Shin-Etsu Chemical Co., Ltd. are preferably used. In the case of a hydrophobic material, it is preferable to use an oil-based ink as the ink for forming the printed layer. If a water-soluble ink is used, the ink tends to have poor coatability, such as "repellency," as described below.

[0081] (Adhesive layer) The adhesive layer is a layer containing an adhesive material, and may be colored and transparent or colorless and transparent, and may be appropriately adjusted in consideration of design and light transmittance depending on the application. Examples of adhesives include rubber-based adhesives, acrylic-based adhesives, ethylene-vinyl acetate copolymer (EVA)-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinyl pyrrolidone-based adhesives, polyacrylamide-based adhesives, cellulose-based adhesives, etc. Among these, acrylic-based adhesives are preferred because of their excellent transparency. Specific examples of adhesives include the LUCIACS CS986 series (manufactured by Nitto Denko Corporation), the OCA8146 series (manufactured by 3M Corporation), the PD-S1 series, the RD-R5 series (manufactured by Panac Corporation), the EW1500 series (manufactured by Daio Paper Corporation), and the TD06 series (manufactured by Tomoegawa Paper Co., Ltd.).

[0082] In addition to pressure-sensitive adhesive resins, adhesive materials containing heat-sensitive adhesive resins can be used as adhesive materials. The heat-sensitive adhesive resin is preferably one that becomes soft and molten when heated to 80°C or less, preferably about 60°C, and becomes bonded to the light-transmitting substrate 2 and the film 3 when the temperature drops. Such heat-sensitive adhesive resins are widely used in industrial applications as hot melt adhesives, and general ones having good water resistance and abrasion resistance can be applied in the present invention. For example, ethylene vinyl acetate, ethylene acrylic acid, polyamide, polyolefin, urethane, polyvinyl acetate, acrylic, and other resins are preferred.

[0083] The adhesive layer may contain additives such as a tackifier, a filler, an antioxidant, and a colorant, if necessary, within the range that does not impair transparency. Examples of the colorant include dyes such as anionic azo dyes, azo metal complex salts, and phthalocyanine; and pigments such as carbon black and organic pigments. The adhesive layer may be colored in a single color or in multiple colors. The adhesive layer may be colored entirely or partially, or may be colored to form characters, designs, pictures, etc. An adhesive tape colored in a desired color may be used as the adhesive layer.

[0084] The thickness of the adhesive layer, which is an adhesive resin, is preferably 1 μm or more, more preferably 5 μm or more. Also, it is preferably 250 μm or less, more preferably 50 μm or less. If the thickness of the adhesive layer is too large, the manufacturing cost may become excessive, and processing such as punching may become difficult. Also, if the thickness is too small, the adhesion between the light-transmitting substrate 2 and the film 3 may not be sufficient.

[0085] There are no particular limitations on the method for laminating the adhesive layer 5 on the surface of the film 3 on which the fine uneven structure is not formed, and any known method can be used. Specific examples include a method of laminating an adhesive material, a method of attaching a transparent adhesive tape, and a method of coating an adhesive material.

[0086] <Action and effect> The laminate of the first embodiment of the present invention described above has a fine uneven structure on the surface of the laminate, and therefore has excellent anti-reflection properties. Moreover, the laminate of the first embodiment of the present invention has a printed layer formed on the surface of the fine uneven structure, so there is no lifting or bubbles due to the steps of the printed layer, and since the printed layer and the adhesive layer are not in contact with each other, there is no swelling or bubbles due to outgassing in the adhesive layer. These properties can be easily imparted, for example, by changing the compounding composition of the active energy ray curable resin composition constituting the cured resin layer, the period or height of the convex portions, etc. In addition, the laminate of the first embodiment of the present invention has good adhesion between the layers. The laminate of the first embodiment of the present invention can be easily produced by forming a cured resin layer on the surface of a film substrate in advance to prepare a laminate body, and then forming a printed layer on the surface of the cured resin layer having a fine uneven structure.

[0087] In Fig. 2, the printing layer 6 is printed directly on the surface of the cured resin layer 4 having the fine uneven structure, but another layer (such as a transparent adhesive layer) may be interposed between the fine uneven structure surface and the printing layer. Also, a light-transmitting adhesive layer 5 may be provided on the surface of the printing layer 6 opposite to the surface in contact with the fine uneven structure, i.e., on the surface of the laminate. If the adhesive layer is provided, the laminate can be easily attached to a desired location.

[0088] A laminate 1 shown in FIG. 2 is exemplified as the laminate of the first embodiment of the present invention, but the present invention is not limited thereto. "Display device" As described above, the laminate 1 of the present invention is free from lifting or bubbles due to steps in the printed layer, and is also free from swelling or bubbles due to outgassing, and can therefore be suitably used in various display devices such as liquid crystal display panels. Examples include instrument dials. Furthermore, it can be used in touch panels arranged on the front of image display device bodies such as liquid crystal panels. Examples of image display device bodies include flat display panels (liquid crystal panels, plasma display panels, organic EL display panels, etc.), CRTs, etc. In the laminate 1 of the present invention used in a display device, the surface opposite to the surface in contact with the adhesive layer 5 of the light-transmitting substrate 2 is preferably disposed facing the outside of the device from the viewpoints of the texture, color reproducibility, and design of the printed layer. Here, the "outside of the device" refers to the side from which the display of the display device is observed. A display device having the laminate 1 of the present invention has improved visibility. In addition, for example, in a region that appears black when the power supply of the image display device is turned off, by making the printed layer 6 black, the black color of the region where the printed layer 6 is formed becomes clear, and in a transparent region where the printed layer is not formed, the visibility and color reproducibility of the black color of the image display part such as a liquid crystal panel arranged in the image display device are improved due to the reduction of light reflection by the fine uneven structure, so that an excellent design member can be provided. EXAMPLES

[0089] The present invention will now be described in further detail with reference to examples. The various measurement and evaluation methods, the mold manufacturing method, and the components used in each example are as follows.

[0090] "Measurement and Evaluation" (Measurement of mold pores) A portion of the mold was cut out, and platinum was evaporated onto the surface and longitudinal section for 1 minute. The portion was then observed using a field emission scanning electron microscope (manufactured by JEOL, "JSM-7400F") at an acceleration voltage of 3.00 kV. The distance between adjacent pores (the distance from the center of a pore to the center of an adjacent pore) was measured at 50 points, and the average value was taken as the average distance between adjacent pores. In addition, the vertical cross section of the mold was observed, the distance between the bottom of the pores and the top of the protrusions present between the pores was measured at 50 points, and the average value was taken as the average pore depth.

[0091] (Measurement of convex parts of fine uneven structure) Platinum was evaporated onto the vertical cross section of the cured resin layer for 10 minutes, and the cross section was observed using a field emission scanning electron microscope (manufactured by JEOL, "JSM-7400F") at an acceleration voltage of 3.00 kV. The distance between adjacent protrusions (the distance from the center of a protrusion to the center of an adjacent protrusion) was measured at 50 points, and the average value was taken as the average distance between adjacent protrusions. In addition, the cross section of the measurement sample was observed, the distance between the bottom of a convex portion and the top of a concave portion present between convex portions was measured at 50 points, and the average value was taken as the average height of the convex portions.

[0092] (Evaluation of print adhesion) The adhesion of the printed layer formed on the surface of the microrelief structure was evaluated by a cross-cut test. A grid-shaped cut was made in the printed layer at 2 mm intervals, and cellophane adhesive tape (CT-24, manufactured by Nichiban Co., Ltd.) was attached and then peeled off. Cross-cut test (compliant with JIS K5600-5-6) ○: Peeling of the printed layer was less than 15%. ×: Peeling of the printed layer was 15% or more.

[0093] (Evaluation of print gap tracking) The edge portions of the printed layer of the laminate were visually inspected to check for air bubbles or gaps at thickness step portions of the printed layer. ○: No step, or no air bubbles or gaps were found in the step area. ×: Air bubbles or gaps were observed in the stepped portion.

[0094] (Evaluation of outgassing resistance) The laminate was placed in a thermostatic chamber and exposed to an environment of 85° C. for 100 hours, after which the appearance was visually evaluated. ○: No change. ×: Air bubbles or floating occurs in the adhesive layer or in the interface of the layer in contact with the adhesive layer.

[0095] (Evaluation of ink application properties) An oil-based or water-based marker was applied as ink to the surface of the moth-eye film having the fine uneven structure, and then the appearance was evaluated visually. ◯: A uniform coating film is formed. ×: Repelling occurred and it was difficult to form a uniform coating film.

[0096] "Production of a film having a microrelief structure on one side" (Manufacturing of mold a) The above-mentioned steps (a) to (f) were carried out to obtain a plate-shaped mold a having anodized alumina on its surface, the anodized alumina having a plurality of approximately conical pores with an average interval of 100 nm and an average depth of 200 nm. Mold a was immersed in a 0.1% by mass diluted solution of Optool DSX (manufactured by Daikin Industries, Ltd.) and air-dried overnight, and the surface of the anodized alumina was treated with a mold release agent.

[0097] (Preparation of active energy ray-curable resin composition A) 25 parts by mass of dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd., "Kayarad DPHA"), 25 parts by mass of pentaerythritol triacrylate (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "PET-3"), 25 parts by mass of EO-modified dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd., "Kayarad DPEA-12"), 25 parts by mass of polyethylene glycol diacrylate (manufactured by Toagosei Co., Ltd., "Aronix M260"), 0.1 parts by mass of a (poly)oxyalkylene alkyl phosphate ester compound (manufactured by Nikko Chemicals Co., Ltd., "NIKKOL TDP-2"), 1 part by mass of 1-hydroxycyclohexyl phenyl ketone (manufactured by IGM Resins BV, "Omnirad184"), 0.5 parts by mass of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (manufactured by IGM Resins BV, "Omnirad819") was mixed in to obtain an active energy ray-curable resin composition A.

[0098] (Preparation of active energy ray-curable resin composition B) 70 parts by mass of 1,9-nonanediol diacrylate (Osaka Organic Chemical Industry Co., Ltd., "V#260"), 20 parts by mass of a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate (Toagosei Co., Ltd., "Aronix M305"), 10 parts by mass of silicone acrylate (BYK Japan K.K., "BYK-UV3570"), 0.5 parts by mass of a (poly)oxyalkylene alkyl phosphate ester compound (Nikko Chemicals Co., Ltd., "NIKKOL TDP-8"), 1 part by mass of 1-hydroxycyclohexyl phenyl ketone (IGM Resins B.V., "Omnirad184"), and 0.5 parts by mass of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins BV, "Omnirad819") were mixed to obtain an active energy ray-curable resin composition B.

[0099] (Production of Moth Eye Film 1) The active energy ray-curable resin composition A was applied to the surface of the mold a, and then covered with a PET film having a thickness of 80 μm (Cosmoshine "super birefringent type" manufactured by Toyobo Co., Ltd.) as a light-transmitting substrate. Using an ultraviolet irradiator (Fusion Lamp D bulb), ultraviolet light was irradiated through the film at an integrated light dose of 1000 mJ / cm2 to cure the active energy ray curable resin composition A, and then the composition was separated from the mold a to obtain a film (hereinafter referred to as "Moth Eye Film 1") having a hydrophilic micro-convex structure formed on the surface of a light-transmitting substrate, on one side of which was a 5 μm-thick cured resin layer having a micro-convex structure consisting of a plurality of convex portions in the shape of a truncated cone. The contact angle of the surface was 14°. The average spacing between the protrusions was 100 nm, the average height of the protrusions was 200 nm, and the average width of the base of the protrusions was 100 nm.

[0100] (Moth Eye Film 2 Production) In the production of the moth-eye film 1, the active energy ray-curable resin composition B was used instead of the active energy ray-curable resin composition A to obtain a film having a hydrophobic fine uneven structure formed on the surface of a light-transmitting substrate on one side (hereinafter, referred to as "moth-eye film 2"). The contact angle of the surface was 137°.

[0101] "Example 1" A printed layer (thickness 13 μm) was formed by screen printing using a two-component curing ink (black, manufactured by Jujo Chemical Co., Ltd., product number 762) on the surface having the fine uneven structure of the moth-eye film 1. Next, an optical adhesive (manufactured by Daio Paper Co., Ltd., product number EW1502-G1) was applied to the surface opposite to the surface having the fine uneven structure of the film to form an adhesive layer (thickness 25 μm), and then the adhesive layer was attached to a 0.5 mm-thick polycarbonate plate (manufactured by Teijin Co., Ltd., product number PC1151) to produce a laminate. The obtained laminate was evaluated for print adhesion, print step conformity, and outgassing resistance. The results are shown in Table 1.

[0102] "Comparative Example 1" A printed layer (thickness 13 μm) was formed on a polycarbonate plate (manufactured by Teijin, product number PC1151) by screen printing using a two-component curing ink (black, manufactured by Jujo Chemical Co., Ltd., product number 762). Next, an optical adhesive (manufactured by Daio Paper Co., Ltd., product number EW1502-G1) was applied to the surface of the moth-eye film 1 opposite to the surface having the fine uneven structure to form an adhesive layer (thickness 25 μm), and the surface on which the adhesive layer was formed was attached to the surface of the polycarbonate plate on which the printed layer was formed to produce a laminate. The obtained laminate was evaluated for print step conformability and outgassing resistance, and the results are shown in Table 1.

[0103] [Table 1]

[0104] As is clear from the results in Table 1, the laminate obtained in Example 1 had excellent print adhesion, print step conformability, and outgassing resistance, and had good adhesion between the layers. Moreover, these laminates could be easily produced. On the other hand, the laminate obtained in Comparative Example 1 was poor in print step conformability and outgassing resistance.

[0105] "Example 2" A laminate was produced in the same manner as in Example 1, except that the moth-eye film 2 was used instead of the moth-eye film 1, and an oil-based marker (Zebra's Maki) was applied as ink to the surface having the fine uneven structure. As a result, a uniform coating film was formed. The results are shown in Table 2.

[0106] "Reference example" A laminate was produced in the same manner as in Example 2, except that an aqueous pigment marker (Zebra Paper Markie) was used as the ink. As a result, repellency occurred at the applied area, making it difficult to form a uniform coating film. The results are shown in Table 2.

[0107] [Table 2] As is clear from the results in Table 2, when ink was applied to a hydrophobic surface with fine projections and recesses, a uniform and good coating film was formed with oil-based ink, but a uniform coating film was not formed with water-based ink. [Industrial Applicability]

[0108] The laminate of the present invention has excellent printing adhesion, printing step followability, outgassing resistance, and the like, and has good adhesion between each layer. Therefore, the laminate is suitable for use as front cover members for image display devices, cel drawings, photographs, bromides, amusement-related boards and cards, interior materials such as wall materials and partitions, cosmetic cases, decorative items, various interior products, framing, cover members and housings for sensors and the like, and other applications in which design is particularly desired. The method for producing a laminate of the present invention can easily produce a laminate having excellent print adhesion, print step conformability, outgassing resistance, and the like, and having good adhesion between layers. The display device of the present invention has good adhesion between the layers, is free of floating or air bubbles due to steps in the printed layer, and is also free of swelling or air bubbles due to outgassing, making it suitable for use in display devices. [Explanation of symbols]

[0109] 1. Laminate 2 Light-transparent substrate 3. Film 4 Cured resin layer 4a Convex part of fine uneven structure 5 Adhesive layer 6 printing layer

Claims

1. A light-transmitting substrate and a micro-recessed structure including a plurality of protrusions formed at a period equal to or smaller than the wavelength of visible light. A film having a convex structure on one side and a film formed on the side having a fine concave-convex structure of the film A display device having a laminate including a printed layer, The laminate has one surface of the light-transmitting substrate and a surface of the film having a fine uneven structure. a laminate in which the opposite surface is laminated via a light-transmitting adhesive layer, The surface of the light-transmitting substrate opposite to the surface in contact with the adhesive layer is disposed facing the outside of the display device. A display device.

2. The surface of the film having the fine uneven structure has an area where a printing layer is not formed.

2. The display device according to claim 1.

3. The display device according to claim 1 or 2, wherein the surface of the fine uneven structure has a water contact angle of 30° or less. Place.

4. The display according to claim 1 or 2, wherein the surface of the fine uneven structure has a water contact angle of 120° or more. Device.

5. The display device according to any one of claims 1 to 4, wherein the thickness of the adhesive layer is 50 µm or less. .

6. The material of the light-transmitting substrate is at least one of polycarbonate and acrylic resin. The display device according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Patterned film and display body

    JP2014071220A

  • Display body

    JP2015138042A

  • Dial plate for meter and vehicular display device

    JP2016035422A

  • Three-dimensional printing method and decorative plate and light box manufactured by the method