Aqueous dispersion and method for producing the same, as well as ink, printing method and printing device
An aqueous dispersion with pigment-encapsulated resin particles of specific size and aspect ratio, combined with a surfactant, stabilizes pigment distribution, maintaining high image density on low ink absorption media during heat drying.
Patent Information
- Application Number
- JP2020142542
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-08-26
AI Technical Summary
Existing aqueous inks struggle to maintain high image density during heat drying due to pigment detachment and aggregation, leading to decreased image quality on low ink absorption recording media.
The development of an aqueous dispersion containing pigment-encapsulated resin particles with a specific size range (200 nm to 500 nm) and aspect ratio (1.0 to 1.5) to stabilize the pigment within the resin, using a surfactant to enhance dispersion stability and prevent resin detachment.
The solution achieves high image density and suppresses image density loss during heat drying, ensuring consistent image quality on low ink absorption media.
Smart Images

Figure 0007567286000007 
Figure 0007567286000008 
Figure 0007567286000009
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous dispersion and a method for producing the same, as well as an ink, a printing method, and a printing apparatus. [Background technology]
[0002] In recent years, inkjet technology has been used not only for home use but also for commercial and industrial use. In commercial and industrial use, low ink-absorbent coated printing paper and non-ink-absorbent plastic film are used as recording media. Therefore, there is a demand for inkjet recording methods to achieve the same level of image quality as conventional offset printing for such recording media. For example, Patent Documents 1 to 3 propose water-based pigment dispersions in which pigment particles are coated with a specific resin. Summary of the Invention [Problem to be solved by the invention]
[0003] An object of the present invention is to provide an aqueous dispersion which can provide a high image density and can suppress a decrease in image density during drying by heating. [Means for solving the problem]
[0004] The aqueous dispersion of the present invention as a means for solving the above problems contains pigment-encapsulated resin particles that encapsulate a pigment and a surfactant, and has a cumulative 50% volume particle diameter (D 50 ) is 200 nm or more and 500 nm or less, and the aspect ratio of the pigment-encapsulating resin particles is 1.0 or more and 1.5 or less. Effect of the Invention
[0005] According to the present invention, it is possible to provide an aqueous dispersion which can obtain a high image density and can suppress a decrease in image density during drying by heating. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a schematic diagram showing an example of a printing apparatus of the present invention. [Diagram 2] FIG. 2 is a TEM image of the aqueous dispersion containing the pigment-encapsulated resin particles obtained in Example 1. [Diagram 3] FIG. 3 is a TEM image of the aqueous dispersion obtained in Comparative Example 2. [Figure 4] FIG. 4 is a TEM image of the aqueous dispersion obtained in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] (aqueous dispersion) The aqueous dispersion of the present invention contains pigment-encapsulated resin particles that encapsulate a pigment and a surfactant, and the pigment-encapsulated resin particles have a cumulative 50% volume particle diameter (D 50 ) is 200 nm or more and 500 nm or less, the aspect ratio of the pigment-encapsulating resin particles is 1.0 or more and 1.5 or less, and further contains other components as necessary.
[0008] In the conventional technology, it is difficult to simultaneously form pigment-encapsulated resin particles in which a pigment is encapsulated in a resin and obtain a particle size of the pigment-encapsulated resin particles suitable for an inkjet recording method. In addition, in the pigment-encapsulated resin particles, the resin that coats the pigment is highly hydrophilic, so that the resin is easily detached from the pigment surface, the stability of the pigment composite resin particles is reduced, and the pigment aggregates due to heat drying, which deteriorates the uniform dispersion of the pigment or the surface roughness of the coating film, resulting in a decrease in image density compared to before heat drying. As a result, there is a problem that conventional water-based inks cannot satisfy the high image density that has been required in recent years.
[0009] In the present invention, a pigment-encapsulated resin particle containing a pigment and a surfactant is included, and the cumulative 50% volume particle diameter (D 50By using an aqueous dispersion in which the average particle diameter is 200 nm or more and 500 nm or less and the aspect ratio of the pigment-encapsulating resin particles is 1.0 or more and 1.5 or less, a high image density can be obtained and a decrease in image density during drying by heating can be suppressed.
[0010] <Pigment-encapsulated resin particles> The pigment-encapsulated resin particles are resin particles in which the entire surface of the pigment is coated with resin, and do not have any unencapsulated pigment dispersed therein or any part of the pigment exposed on the surface of the resin particles. The pigment-encapsulated resin particles are preferably spherical. In this specification, the pigment-encapsulated resin particles means that the pigment is entirely contained (encapsulated) in the resin particles in the resin emulsion. For example, JP-A-2016-196621, JP-A-2002-322396, JP-A-2019-099819, and JP-A-2005-120136 propose coated pigments and microencapsulated pigments, but these are not in the form of a pigment encapsulated in a resin particle in a resin emulsion, and are different from pigment-encapsulated resin particles. The pigment-encapsulated resin particles are preferably in the form of a resin emulsion from the viewpoint of ease of handling. By encapsulating the pigment in the resin particles in the resin emulsion, it is possible to suppress the detachment of the pigment dispersion resin into the medium. The resin emulsion refers to a state in which the resin particles are dispersed in water or ink, and it does not matter whether the resin particles are solid or liquid.
[0011] The method of confirming that the particles are pigment-encapsulating resin particles can be performed by observation with a transmission electron microscope (TEM) as described below. First, a water-based dispersion containing pigment-encapsulated resin particles is diluted with ion-exchanged water so that the solid content concentration is 0.1% by mass to prepare a sample solution. Next, 1 μL of the sample solution is placed on a hydrophilically treated collodion membrane-attached mesh (manufactured by Nissin EM Co., Ltd., collodion membrane-attached mesh Cu150 mesh) using a micropipette, and the sample solution is immediately absorbed with a triangular filter paper. Next, 1 μL of EM stainer diluted 10 times is placed using a micropipette, and the sample solution is immediately absorbed with a triangular filter paper. After drying under reduced pressure, observation is performed with a transmission electron microscope (manufactured by JEOL Ltd., JEM-2100F) at an accelerating voltage of 200 kV and a magnification of 40,000 times. As a result of the observation, if a resin layer is present so as to completely cover the pigment (the pigment is encapsulated in the resin particles in the resin emulsion) (for example, see FIG. 2), it can be confirmed that the pigment-encapsulated resin particles of the present invention are the same.
[0012] The cumulative 50% volume particle diameter of the pigment-encapsulated resin particles (D 50 The cumulative 50% volume particle diameter (D 50 When the diameter of the pigment particles is 200 nm or more and 500 nm or less, a plurality of pigment primary particles can be encapsulated, thereby making it possible to increase the image density. Cumulative 50% volume particle diameter of pigment-encapsulated resin particles (D 50 ) can be measured, for example, using a zeta potential / particle measurement system (ELSZ-1000, manufactured by Otsuka Electronics Co., Ltd.).
[0013] The ratio of pigment-encapsulated resin particles is not particularly limited, and the ratio of pigment-encapsulated resin particles to resin particles that do not contain pigment can be appropriately selected. The amount of pigment-encapsulated resin particles is determined by taking five or more images of a field of view containing three or more particles with a volume diameter of 100 nm or more at any desired location, and the ratio of the pigment-encapsulated resin particles to the total particles with a volume diameter of 100 nm or more for each image, and the average value is preferably 30% or more, more preferably 50% or more. When the ratio of pigment-encapsulated resin particles is 30% or more, the image density can be increased by increasing the ratio of pigment-encapsulated resin particles. The pigment-encapsulated resin particles preferably contain two or more primary pigment particles, and thus the pigment density in the pigment-encapsulated resin particles is increased, thereby making it possible to increase the image density.
[0014] The aspect ratio of the pigment-encapsulated resin particles is determined by obtaining multiple images of a field of view including the pigment-encapsulated resin particles, calculating the ratio of the major axis to the minor axis (major axis / minor axis) of 20 arbitrarily selected pigment-encapsulated particles, and averaging the ratios (average aspect ratio) to be in the range of 1.0 to 1.5, preferably 1.0 to 1.2. When the aspect ratio of the pigment-encapsulated resin particles is 1.0 to 1.5, there is an advantage that the smoothness of the coating surface is improved and the image density is improved. In calculating the major axis / minor axis, the length of the axis that is the longest from end to end of the particle (major axis) is taken as the major axis, and the length of the particle in the direction perpendicular to the major axis at the center of the major axis is taken as the minor axis.
[0015] The degree of pigment encapsulation in the pigment-encapsulated resin particles can be evaluated by quantifying the amount of pigment that is exposed without being encapsulated (pigment exposure rate). The pigment exposure rate can be calculated, for example, using a scanning electron microscope (SEM). The specific calculation method for the pigment exposure rate is as follows. An aqueous dispersion containing pigment-encapsulated resin particles is prepared using ion-exchanged water so that the solid content concentration is 10.75% by mass. Then, coated paper (Lumia Art Gloss 130, manufactured by STORA ENSO) is coated with a bar coater having a diameter of 0.15 mm, and dried at 25°C to form a coating film having an average thickness of 2 μm. This coating film is cut out and fixed to a stub for SEM observation using carbon tape. This is observed using a scanning electron microscope (manufactured by ZEISS, Merlin) without conducting a conductive treatment, with an accelerating voltage of 0.75 kV, a backscattered electron detector, and a magnification of 2,000 times to 20,000 times. This observation method makes it possible to distinguish the exposed pigment from the difference in the contrast of the SEM image due to the difference in the amount of backscattered electrons emitted by the carbon black and the resin. The ratio of the area occupied by the pigment on the coating surface at 20,000x magnification (pigment exposure rate) is preferably 8% or less, more preferably 5% or less, and even more preferably 0% to 3%. The area occupied by the pigment on the coating surface is determined by binarizing the SEM observation image, and it is preferable to take the average of three or more visual fields observed at random locations. Under these observation conditions, those that cannot be observed due to charge-up tend to have a low pigment exposure rate, and are easily observed when the pigment exposure rate is 3% or less.
[0016] By covering two or more primary pigment particles into a spherical shape with resin, it is possible to make the pigment dispersion in the coating film after heat drying uniform and reduce the surface roughness of the coating film, thereby improving the image density (OD). The surface roughness of the coating film is preferably 20 nm or less, and more preferably 15 nm or less. By making the surface roughness of the coating film 20 nm or less, a decrease in image density after heat drying can be suppressed. The surface roughness of the coating film is calculated, for example, using a scanning probe microscope (SPM) as follows. First, an aqueous dispersion containing pigment-encapsulated resin particles is prepared using ion-exchanged water so that the solid content concentration is 10.75% by mass. Next, the dispersion is applied to coated paper (Lumia Art Gloss 130, manufactured by STORA ENSO) using a 0.15 mm bar coater, and heated and dried in an oven at 100° C. for 5 minutes to form a coating film with an average thickness of 2 μm. This coating film is cut out and observed under the following conditions to calculate the surface roughness. Observation is performed in three fields of view to determine the average surface roughness. [Measurement conditions] Equipment: Scanning probe microscope (Bruker, DimensionIcon) Cantilever: Olympus Corporation, OMCL-AC240TS Measurement mode: Tapping mode Observation area: 2μm square
[0017] <Resin> The resin preferably has an anionic group. Examples of the anionic group include a carboxyl group, a carboxylate group, a sulfonic acid group, and a sulfonate group. Among these, a carboxylate group or a sulfonate group partially neutralized with a basic compound is preferred. Examples of neutralizing agents that can be used to neutralize the anionic groups include basic compounds such as organic amines such as ammonia, triethylamine, pyridine, and morpholine, and alkanolamines such as monoethanolamine, and metal basic compounds including Na, K, Li, and Ca. The resin is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include polyester resin, polyurethane resin, acrylic resin, etc. Among these, polyester resin is particularly preferred.
[0018] -Polyester resin- The polyester resin is obtained by polycondensation of a polyhydric alcohol with a polycarboxylic acid, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, and / or a derivative thereof, and has an aromatic unit in a part or all of its composition. That is, the aromatic-containing polyester has a polyhydric alcohol and a polycarboxylic acid, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, and / or a derivative thereof, as constituent components.
[0019] -Polyhydric alcohol component- The polyhydric alcohol component may be a dihydric alcohol (diol), specifically, an alkylene glycol having 2 to 36 carbon atoms (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, trimethylolpropane, etc.); an alkylene ether glycol having 4 to 36 carbon atoms (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, etc.); Examples of the alkylene oxides include alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.); adducts (number of moles added: 1 to 30) of the alicyclic diols with alkylene oxides having 2 to 4 carbon atoms (ethylene oxide (hereinafter abbreviated as "EO"), propylene oxide (hereinafter abbreviated as "PO"), butylene oxide (hereinafter abbreviated as "BO"), etc.)); and adducts (number of moles added: 2 to 30) of bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.) with alkylene oxides having 2 to 4 carbon atoms (EO, PO, BO, etc.). In addition to the dihydric diol, the alcohol component may contain a trihydric or higher (trihydric to octahydric or higher) alcohol component. Specifically, aliphatic polyhydric alcohols having 3 to 36 carbon atoms and trihydric to octahydric or higher (alkane polyols and their intramolecular or intermolecular dehydration products, for example, glycerin, triethylolethane, trimethylolpropane, pentaerythritol, sorbitol, sorbitan, polyglycerin, dipentaerythritol; sugars and their derivatives, for example, sucrose and methyl glucoside, etc.) ); adducts of the above aliphatic polyhydric alcohols with alkylene oxides (EO, PO, BO, etc.) having 2 to 4 carbon atoms (number of moles added: 1 to 30); adducts of trisphenols (trisphenol PA, etc.) with alkylene oxides (EO, PO, BO, etc.) having 2 to 4 carbon atoms (number of moles added: 2 to 30); adducts of novolak resins (phenol novolak, cresol novolak, etc.: average degree of polymerization: 3 to 60) with alkylene oxides (EO, PO, BO, etc.) having 2 to 4 carbon atoms (number of moles added: 2 to 30). These may be used alone or in combination of two or more.
[0020] -Polycarboxylic acid component- Examples of the polyvalent carboxylic acid component include divalent carboxylic acids (dicarboxylic acids), specifically, alkane dicarboxylic acids having 4 to 36 carbon atoms (e.g., succinic acid, apidic acid, sebacic acid, etc.), alkenyl succinic acids (e.g., dodecenyl succinic acid, etc.); alicyclic dicarboxylic acids having 4 to 36 carbon atoms [e.g., dimer acid (dimerized linoleic acid)]; alkene dicarboxylic acids having 4 to 36 carbon atoms (e.g., maleic acid, fumaric acid, citraconic acid, mesaconic acid, etc.); aromatic dicarboxylic acids having 8 to 36 carbon atoms (e.g., phthalic acid, isophthalic acid, terephthalic acid or derivatives thereof, naphthalenedicarboxylic acid, etc.). These may be used alone or in combination of two or more. Among these, alkanedicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred. The polyvalent carboxylic acid component may also be an acid anhydride or a lower alkyl (having 1 to 4 carbon atoms) ester (e.g., methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned compounds. In addition, ring-opening polymerization systems such as polylactic acid and polycarbonate diol may also be suitably used.
[0021] The polyester resin can be isolated, for example, by drying a dispersion of pigment-encapsulated resin particles by heating and placing the resulting dried product in a tetrahydrofuran (THF) solution to dissolve the polyester resin. The pigment is then removed by centrifugation, filtration, or the like, and the THF is then removed to isolate the polyester resin. In addition, recycled GPC can be used as necessary.
[0022] The molecular weight of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but the weight average molecular weight (Mw) measured by GPC is preferably from 2,000 to 15,000, more preferably from 4,000 to 12,000. The glass transition temperature (Tg) of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 30° C. to 100° C., more preferably from 50° C. to 80° C. The softening temperature of the polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably from 60° C. to 180° C., more preferably from 80° C. to 150° C. The molecular structure of the polyester resin can be confirmed by NMR measurement of a solution or solid, as well as GC / MS, LC / MS, IR measurement, and the like.
[0023] The polyester resin can be synthesized by a method that has been generally used, for example, the following method. First, the polyhydric alcohol and the polycarboxylic acid can be polycondensed in the absence of a solvent or in the presence of an organic solvent.
[0024] <Pigments> Examples of the pigment include organic pigments and inorganic pigments. Among these, inorganic pigments are preferred. Examples of the inorganic pigment include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, carbon black (CI Pigment Black 7) produced by a known method such as furnace black, lamp black, acetylene black, channel black, and metals such as copper and iron (CI Pigment Black 11), etc. Among these, carbon black is preferable.
[0025] The carbon black preferably has a primary particle size of 15 nm or more and 100 nm or less. By setting the primary particle size within the above range, color development is improved. The DBP absorption of carbon black is preferably 30 mL / 100 g or more and 150 mL / 100 g or less. By setting the DBP absorption in the above range, the pigment dispersibility in an organic solvent can be improved. A self-dispersing pigment may also be used, and the self-dispersing pigment refers to a pigment that has been stabilized by introducing a functional group directly or via another atomic group onto the pigment surface. As the pigment before dispersion stabilization, for example, various conventionally known pigments described in WO 2009 / 014242 can be used.
[0026] <Pigment dispersant> In order to improve the dispersibility of the pigment-encapsulated resin particles, it is preferable to add a pigment dispersant to the aqueous dispersion.
[0027] The hydrophilicity / hydrophobicity of the pigment dispersant is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable to use a hydrophobic pigment dispersant in order to facilitate encapsulation of the pigment in the resin and improve image density. The hydrophilicity / hydrophobicity of the pigment dispersant is hydrophobic if the pigment dispersant is insoluble in water, and hydrophilic if the pigment dispersant is soluble in water.
[0028] The pigment dispersant is not particularly limited and can be appropriately selected depending on the purpose. For example, a polymer dispersant can be used. Examples of pigment dispersants include (meth)acrylic resins, styrene-(meth)acrylic resins, hydroxyl group-containing carboxylic acid esters, salts of long-chain polyaminoamides and high molecular weight acid esters, salts of high molecular weight polycarboxylic acids, salts of long-chain polyaminoamides and polar acid esters, high molecular weight unsaturated acid esters, polymer copolymers, modified polyurethanes, modified polyacrylates, polyether ester-type anionic surfactants, naphthalenesulfonic acid formalin condensate salts, aromatic sulfonic acid formalin condensate salts, polyoxyethylene alkyl phosphate esters, polyoxyethylene nonylphenyl ethers, stearylamine acetates, etc. These may be used alone or in combination of two or more. Commercially available pigment dispersants can be used, and examples of the commercially available products include Joncryl (manufactured by Johnson Polymers), Anti-Terra-U (manufactured by BYK Chemie), Disperbyk (manufactured by BYK Chemie), Efka (manufactured by Efka Chemicals), Flourene (manufactured by Kyoeisha Chemical Co., Ltd.), Disparlon (manufactured by Kusumoto Chemicals Co., Ltd.), Ajisper (manufactured by Ajinomoto Fine-Techno Co., Ltd.), Demol (manufactured by Kao Corporation), Homogenol, Emulgen (all manufactured by Kao Corporation), Solsperse (manufactured by Lubrizol), and Nikkol (manufactured by Nikko Chemical Co., Ltd.). These may be used alone or in combination of two or more.
[0029] <Surfactant> Examples of the surfactant include anionic surfactants such as alkylbenzenesulfonates, α-olefinsulfonates, and phosphoric acid esters; amine salts such as alkylamine salts, aminoalcohol fatty acid derivatives, polyamine fatty acid derivatives, and imidazolines; cationic surfactants of quaternary ammonium salts such as alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, pyridinium salts, alkylisoquinolinium salts, and benzethonium chloride; and nonionic surfactants such as fatty acid amide derivatives and polyhydric alcohol derivatives, for example, alanine, dodecyldi(aminoethyl)glycine, di(octylaminoethyl)glycine, and N-alkyl-N,N-dimethylammonium betaine. Among these, anionic surfactants are preferred, and alkylbenzenesulfonates are more preferred from the viewpoint of increasing dispersion stability.
[0030] The content of the surfactant is preferably from 1% by mass to 20% by mass, and more preferably from 2% by mass to 10% by mass, based on the total amount of the aqueous dispersion. When the surfactant content is within the above range, the dispersion stability is good. Inks using aqueous dispersions with a surfactant content of 20% by mass or more tend to have poor ejection stability due to nozzle clogging, ejection deflection, etc. The method for measuring the surfactant content in the aqueous dispersion is not particularly limited and can be appropriately selected depending on the purpose. For example, the surfactant content can be measured using a high performance liquid chromatograph (LC-20, manufactured by Shimadzu Corporation).
[0031] <Other ingredients> The other components are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other components include organic solvents, antioxidants, and ultraviolet protection agents.
[0032] (Method of manufacturing pigment-encapsulated resin particles) The method for producing pigment-encapsulated resin particles of the present invention includes a step of mixing an organic solvent and a pigment to prepare a pigment pre-dispersion (hereinafter referred to as the "pigment pre-dispersion preparation step"), a step of mixing the obtained pigment pre-dispersion with a resin to prepare a pigment dispersion resin solution (hereinafter referred to as the "pigment dispersion resin solution preparation step"), a step of mixing the obtained pigment dispersion resin solution with a surfactant-containing liquid to prepare a pigment-encapsulated resin particle dispersion liquid (hereinafter referred to as the "pigment-encapsulated resin particle dispersion preparation step"), and a step of removing the organic solvent from the obtained pigment-encapsulated resin particle dispersion liquid (hereinafter referred to as the "organic solvent removal step"), and may further include other steps as necessary.
[0033] <Pigment pre-dispersion preparation process> The pigment pre-dispersion preparation step is a step of mixing an organic solvent and a pigment to prepare a pigment pre-dispersion. As the pigment, the same pigment as that in the above-mentioned aqueous dispersion can be used. The organic solvent is not particularly limited as long as it can dissolve the resin in the next pigment dispersion resin solution preparation step, and can be appropriately selected depending on the purpose, and examples thereof include ethyl acetate, methyl ethyl ketone, acetone, etc. Among these, ethyl acetate is preferred. The apparatus used in the pigment pre-dispersion preparation step is not particularly limited and can be appropriately selected depending on the purpose. For example, a dispersing machine can be used.
[0034] The cumulative volume particle size of the pigment in the pigment pre-dispersion is 50% (D 50 ) is preferably from 10 nm to 150 nm, and more preferably from 20 nm to 120 nm, in order to reduce the particle size of the pigment-encapsulated resin particles. The cumulative volume particle size of the pigment is 50% (D 50 ) can be measured, for example, using a zeta potential / particle measurement system (ELSZ-1000, manufactured by Otsuka Electronics Co., Ltd.).
[0035] The content of the pigment in the pigment pre-dispersion is not particularly limited and can be appropriately selected depending on the purpose. In the pigment pre-dispersion preparation step, it is preferable to use a pigment dispersant. As the pigment dispersant, the same pigment dispersant as that in the above-mentioned aqueous dispersion can be used, and a hydrophobic pigment dispersant is particularly preferable. The ratio of the pigment to the pigment dispersant in the pigment pre-dispersion is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of improving the dispersibility of the pigment pre-dispersion, however, the ratio of the pigment to the pigment dispersant is preferably 4:0.2 to 4:4, and more preferably 4:0.5 to 4:3. It is preferable that the pigment pre-dispersion is filtered, if necessary, with a filter, a centrifugal separator or the like to remove coarse particles.
[0036] The pigment pre-dispersion can be produced by dissolving or suspending a pigment dispersant in an organic solvent as necessary, adding a resin and a pigment, stirring the mixture, and then using a commonly used known dispersing machine. The dispersing machine is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include anchor blades, dispersing blades, homomixers, ball mills, roll mills, beads mills, sand mills, attritors, pearl mills, Dyno Mills, high-pressure homogenizers, ultrasonic dispersers, agitator mills, paint shakers, grain mills, cobol mills, jet mills, etc. Among these, from the viewpoint of dispersion efficiency, roll mills, beads mills, sand mills, Dyno Mills, high-pressure homogenizers, and paint shakers are preferred.
[0037] <Pigment dispersion resin solution preparation process> The pigment dispersion resin solution preparation step is a step of mixing the obtained pigment pre-dispersion with a resin to prepare a pigment dispersion resin solution. The pigment dispersion resin solution can be obtained by mixing and stirring the pigment pre-dispersion obtained in the pigment pre-dispersion preparation step, a resin, and, if necessary, a basic compound, an organic solvent, and additives. As the resin, the same resin as that in the above-mentioned aqueous dispersion can be used. The mixing and stirring device used in the pigment dispersion resin solution preparation step is not particularly limited and can be appropriately selected depending on the purpose, but examples thereof include the devices described in the pigment pre-dispersion preparation step. Among these, a homomixer or a high-speed stirring device equipped with a dispersing blade is preferably used from the viewpoints of uniform stirring of a high-viscosity solution and efficient dissolution of the resin powder. The procedure for preparing the pigment dispersion resin solution is not particularly limited. The resin may be added to the pigment pre-dispersion obtained in the pigment pre-dispersion preparation step, or may be added after the resin is solubilized in an organic solvent. The cumulative volume particle size of the pigment in the pigment dispersion resin solution is 50% (D 50 ) is the same as the cumulative volume particle size 50% (D 50 ), and it is more preferable that no change occurs between the pigment pre-dispersion preparation step and the pigment dispersion resin solution preparation step. The resin is used to encapsulate the pigment in the pigment-encapsulated resin particle dispersion preparation step, and preferably has a nonionic, anionic or cationic hydrophilic group, and more preferably has an anionic hydrophilic group. When the resin is an anionic resin, it is preferable that the resin forms an emulsion in an aqueous medium and that a part or all of the anionic groups are neutralized with a basic compound in order to maintain dispersion stability in the aqueous medium.
[0038] The ratio of the pigment to the resin is preferably 0.2 to 0.75, more preferably 0.3 to 0.6. When the ratio of the pigment to the resin is 0.2 or more, the pigment concentration is appropriate, and the image density of the printed matter is high. When the ratio of the pigment to the resin is 0.75 or less, most of the pigment can be encapsulated in the resin, and the surface roughness of the coating film after heat drying is suppressed, thereby improving the image density. The ratio of the pigment to the resin can be calculated from the charge ratio or the obtained dispersion. The calculation method from the aqueous dispersion can be, for example, by thermal analysis of the dried and solidified film of the aqueous dispersion using a thermogravimetric differential thermal analyzer (TG-DTA). Specifically, the dried and solidified film of the aqueous dispersion can be heated and held in a nitrogen gas atmosphere to the thermal decomposition temperature of the resin using a thermogravimetric differential thermal analyzer, and the decomposed weight can be calculated as the resin and the weight of the residue as the pigment. In addition, for highly heat-resistant resins that cannot be completely decomposed by thermal decomposition in a nitrogen gas atmosphere, the heat loss can be calculated using a calibration curve of the pigment ratio to the resin. Specifically, a plurality of mixtures of pigment and resin mixed at any ratio are prepared, and each mixture is heated to a certain temperature and held, to create the above calibration curve, and the ratio of pigment to resin can be calculated based on the weight loss rate obtained from the measurement results of unknown samples.
[0039] <Pigment-encapsulated resin particle dispersion preparation process> The pigment-encapsulated resin particle dispersion liquid preparation step is a step of mixing the obtained pigment dispersion resin solution with a surfactant-containing liquid to prepare a pigment-encapsulated resin particle dispersion liquid. The mixing and stirring device used in the pigment-encapsulated resin particle dispersion preparation step is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include the devices described in the pigment pre-dispersion preparation step. Among these, a high-speed stirring device equipped with a homomixer or a dispersing blade is preferred in terms of uniform stirring in a high-viscosity solution, and the higher the energy required for dispersion, the smaller the particle size of the generated pigment-encapsulated resin particles can be, but if the energy is too high, the generated pigment-encapsulated resin particles may be crushed and the encapsulation state may not be maintained. There is no particular limitation on the procedure for mixing the pigment dispersion resin solution and the surfactant-containing liquid, and the surfactant-containing liquid may be added to the pigment dispersion resin solution, or the pigment dispersion resin solution may be added to the surfactant-containing liquid. As the surfactant, the same surfactant as that in the above-mentioned aqueous dispersion can be used. From the viewpoint of dispersion stability of the pigment-encapsulated resin particles, the content of the surfactant-containing liquid is preferably 70 parts by mass or more and 700 parts by mass or less, and more preferably 100 parts by mass or more and 500 parts by mass or less, relative to 100 parts by mass of the resin used in the pigment dispersion resin solution preparation process. From the viewpoint of dispersion stability, the surfactant is preferably added to a solvent in an amount of 1.0% by mass to 20% by mass with respect to the aqueous dispersion, and then added to the pigment dispersion resin solution.
[0040] <Organic solvent removal process> The organic solvent removing step is a step of removing the organic solvent from the obtained pigment-encapsulated resin particle dispersion liquid. By removing the organic solvent from the pigment-encapsulated resin particle dispersion liquid, the aqueous dispersion of the present invention is obtained. The method for removing the organic solvent is not particularly limited, and any known removal device can be used. It is preferable to heat the organic solvent at a temperature equal to or higher than the boiling point of the organic solvent under reduced pressure, and examples of such devices include a rotary evaporator. The reduced pressure is preferably 200 mmHg or less, more preferably 100 mmHg or less, and the heating temperature is preferably 20°C to 80°C, more preferably 30°C to 60°C. If necessary, the obtained aqueous dispersion can be filtered to remove coarse particles using a filter, a centrifugal separator, etc. Furthermore, if necessary, it is also possible to remove the surfactant using an ultrafiltration device.
[0041] (ink) The ink of the present invention contains water, pigment-encapsulated resin particles that encapsulate a pigment, a surfactant, and an organic solvent, and further contains other components as required.
[0042] <Pigment-encapsulated resin particles> The pigment-encapsulating resin particles encapsulating the pigment are the same as the pigment-encapsulating resin particles encapsulating the pigment in the aqueous dispersion of the present invention. The cumulative 50% volume particle diameter of the pigment-encapsulated resin particles (D 50) is 200 nm or more and 500 nm or less, and the aspect ratio of the pigment-encapsulating resin particles is 1.0 or more and 1.5 or less.
[0043] <Organic solvent> The organic solvent used in the present invention is not particularly limited, and any water-soluble organic solvent can be used. Examples of the organic solvent include polyhydric alcohols, ethers such as polyhydric alcohol alkyl ethers and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds. Examples of the water-soluble organic solvent include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, and the like. Diol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, petriol and other polyhydric alcohols; ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diene Examples of the alkyl ethers include polyhydric alcohols such as ethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; polyhydric alcohols such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether; nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone; amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; amines such as monoethanolamine, diethanolamine, and triethylamine; sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol, propylene carbonate, and ethylene carbonate. It is preferable to use an organic solvent having a boiling point of 250° C. or less, since this not only functions as a wetting agent but also provides good drying properties.
[0044] Polyol compounds having 8 or more carbon atoms and glycol ether compounds are also suitably used. Specific examples of polyol compounds having 8 or more carbon atoms include 2-ethyl-1,3-hexanediol and 2,2,4-trimethyl-1,3-pentanediol. Specific examples of the glycol ether compound include polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; and polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether.
[0045] Polyol compounds having 8 or more carbon atoms and glycol ether compounds can improve the permeability of ink when paper is used as the recording medium.
[0046] The content of the organic solvent in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, the content is preferably from 10% by mass to 60% by mass, and more preferably from 20% by mass to 60% by mass.
[0047] <Water> The water is not particularly limited and can be appropriately selected depending on the purpose. Examples of the water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, and ultrapure water. The water content in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, it is preferably from 10% by mass to 90% by mass, and more preferably from 20% by mass to 60% by mass.
[0048] The particle size of the solid content in the ink is not particularly limited and can be appropriately selected depending on the purpose, but in terms of improving image quality such as ejection stability and image density, the maximum frequency in terms of maximum number is preferably 20 nm or more and 1000 nm or less, more preferably 20 nm or more and 150 nm or less. The solid content includes resin particles, pigment particles, etc. The particle size can be measured using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac Bell Co., Ltd.).
[0049] <Surfactant> As the surfactant, any of silicone-based surfactants, fluorine-based surfactants, amphoteric surfactants, nonionic surfactants, and anionic surfactants can be used. The silicone surfactant is not particularly limited and can be appropriately selected according to the purpose. Among them, those that do not decompose even at high pH are preferable. Examples of silicone surfactants include side chain modified polydimethylsiloxane, both end modified polydimethylsiloxane, one end modified polydimethylsiloxane, and both end modified polydimethylsiloxane of side chain. Those having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modified group are particularly preferable because they show good properties as an aqueous surfactant. In addition, polyether modified silicone surfactants can also be used as silicone surfactants, and examples thereof include compounds in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylpolysiloxane. As the fluorosurfactant, for example, perfluoroalkylsulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in the side chain are particularly preferred because they have low foaming properties. As the perfluoroalkylsulfonic acid compounds, for example, perfluoroalkylsulfonic acid, perfluoroalkyl sulfonate, etc. are included. As the perfluoroalkyl carboxylic acid compounds, for example, perfluoroalkyl carboxylic acid, perfluoroalkyl carboxylate, etc. are included. As the polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in the side chain, sulfate ester salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups in the side chains, salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups in the side chains, etc. are included. As the counter ions of the salts in these fluorosurfactants, Li, Na, K, NH4, NH3CH2CH2OH, NH2(CH2CH2OH)2, NH(CH2CH2OH)3, etc. are included. Examples of amphoteric surfactants include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine. Examples of nonionic surfactants include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and ethylene oxide adducts of acetylene alcohol. Examples of the anionic surfactant include polyoxyethylene alkyl ether acetates, dodecylbenzene sulfonates, laurates, and polyoxyethylene alkyl ether sulfates. These may be used alone or in combination of two or more.
[0050] The silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the silicone surfactant include side-chain modified polydimethylsiloxane, both-end modified polydimethylsiloxane, one-end modified polydimethylsiloxane, and both-end side-chain modified polydimethylsiloxane. Polyether-modified silicone surfactants having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modifying group are particularly preferred because they exhibit good properties as an aqueous surfactant. Such surfactants may be appropriately synthesized or commercially available products, such as those available from BYK-Chemie Co., Ltd., Shin-Etsu Chemical Co., Ltd., Dow Corning Toray Silicone Co., Ltd., Nippon Emulsion Co., Ltd., and Kyoeisha Chemical Co., Ltd. The polyether-modified silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, it can be one in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylpolysiloxane, as represented by the general formula (S-1).
[0051] [ka] (In the general formula (S-1), m, n, a, and b each independently represent an integer, R represents an alkylene group, and R' represents an alkyl group.)
[0052] As the polyether-modified silicone surfactant, commercially available products can be used, such as KF-618, KF-642, KF-643 (manufactured by Shin-Etsu Chemical Co., Ltd.), EMALEX-SS-5602, SS-1906EX (manufactured by Nippon Emulsion Co., Ltd.), FZ-2105, FZ-2118, FZ-2154, FZ-2161, FZ-2162, FZ-2163, FZ-2164 (manufactured by Dow Corning Toray Silicone Co., Ltd.), BYK-33, BYK-387 (manufactured by BYK-Chemie Co., Ltd.), TSF4440, TSF4452, TSF4453 (manufactured by Toshiba Silicon Co., Ltd.), and the like.
[0053] The fluorine-based surfactant is preferably a compound having 2 to 16 fluorine-substituted carbon atoms, and more preferably a compound having 4 to 16 fluorine-substituted carbon atoms. Examples of the fluorine-based surfactant include perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chains. Among these, polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in the side chains are preferred because they have low foaming properties, and fluorine-based surfactants represented by any of general formulas (F-1) and (F-2) are particularly preferred.
[0054] [ka] In the compound represented by the above general formula (F-1), m is preferably an integer of 0 to 10, and n is preferably an integer of 0 to 40 in order to impart water solubility.
[0055] [General formula (F-2)] C n F 2n+ -CH2CH(OH)CH2-O-(CH2CH2O) a -Y In the compound represented by the above general formula (F-2), Y is H or C m F 2m+1 m is an integer from 1 to 6, or CH2CH(OH)CH2-C m F 2m+1 m is an integer between 4 and 6, or C p H 2P+1 where p is an integer from 1 to 19. n is an integer from 1 to 6. a is an integer from 4 to 14. As the above fluorosurfactant, a commercially available product may be used.
[0056] Examples of commercially available products include Surflon S-111, S-112, S-113, S-121, S-131, S-132, S-141, and S-145 (all manufactured by Asahi Glass Co., Ltd.); Fullard FC-93, FC-95, FC-98, FC-129, FC-135, FC-170C, FC-430, and FC-431 (all manufactured by Sumitomo 3M Limited); Megaf FAC F-470, F-1405, F-474 (all manufactured by DIC Corporation); Zonyl TBS, FSP, FSA, FSN-100, FSN, FSO-100, FSO, FS-300, UR, Capstone FS-30, FS-31, FS-3100, FS-34, FS-35 (all manufactured by Chemours); FT-110, FT-250 , FT-251, FT-400S, FT-150, FT-400SW (all manufactured by NEOS Corporation), Polyfox PF-136A, PF-156A, PF-151N, PF-154, PF-159 (manufactured by OMNOVA), Unidyne DSN-403N (manufactured by Daikin Industries, Ltd.), and the like. Among these, FS-3100, FS-34, FS-300 manufactured by Chemours, FT-110, FT-250, FT-251, FT-400S, FT-150, FT-400SW manufactured by NEOS Corporation, Polyfox PF-151N manufactured by OMNOVA, and Unidyne DSN-403N manufactured by Daikin Industries, Ltd. are particularly preferred from the viewpoint of achieving good printing quality, particularly improved color development, penetration into paper, wettability, and dye uniformity.
[0057] The content of the surfactant in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of excellent wettability and ejection stability and improved image quality, the content is preferably from 0.001% by mass to 5% by mass, and more preferably from 0.05% by mass to 5% by mass.
[0058] <Other ingredients> Other components include, as required, antifoaming agents, antiseptics, antifungals, rust inhibitors, pH adjusters, and the like.
[0059] - Defoaming agent - The defoaming agent is not particularly limited, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, and fatty acid ester-based defoaming agents. These may be used alone or in combination of two or more. Among these, silicone-based defoaming agents are preferred because of their excellent foam breaking effect.
[0060] -Preservative and fungicidal agent- The antiseptic and antifungal agent is not particularly limited, and examples thereof include 1,2-benzisothiazolin-3-one.
[0061] -Rust inhibitor- The rust inhibitor is not particularly limited, and examples thereof include acid sulfite and sodium thiosulfate.
[0062] -pH adjuster- There are no particular limitations on the pH adjuster, so long as it is capable of adjusting the pH to 7 or higher, and examples of the pH adjuster include amines such as diethanolamine and triethanolamine. isn't it.
[0063] The physical properties of the ink are not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are within the following ranges. The viscosity of the ink at 25°C is preferably from 5 mPa·s to 30 mPa·s, more preferably from 5 mPa·s to 25 mPa·s, in order to improve print density and character quality and to obtain good ejection properties. Here, the viscosity can be measured using, for example, a rotational viscometer (RE-80L, manufactured by Toki Sangyo Co., Ltd.). The measurement conditions are 25°C, a standard cone rotor (1°34' x R24), a sample liquid volume of 1.2 mL, a rotation speed of 50 rpm, and 3 minutes. The surface tension of the ink is preferably 35 mN / m or less, and more preferably 32 mN / m or less at 25° C., in order to ensure that the ink is appropriately leveled on the recording medium and the drying time of the ink is shortened. The pH of the ink is preferably from 7 to 12, and more preferably from 8 to 11, from the viewpoint of preventing corrosion of metal members that come into contact with the ink.
[0064] <Pretreatment solution> The pretreatment liquid contains a flocculant, an organic solvent, and water, and may contain, as necessary, a surfactant, an antifoaming agent, a pH adjuster, an antiseptic / fungal agent, an antirust agent, and the like. The organic solvent, surfactant, defoamer, pH adjuster, antiseptic and antifungal agent, and rust inhibitor may be the same as those used in ink, and other materials used in known treatment liquids may be used. The type of the flocculant is not particularly limited, and examples thereof include water-soluble cationic polymers, acids, and polyvalent metal salts.
[0065] <Post-processing solution> The post-treatment liquid is not particularly limited as long as it can form a transparent layer. The post-treatment liquid is obtained by selecting and mixing organic solvents, water, resins, surfactants, defoamers, pH adjusters, antiseptics, antifungals, rust inhibitors, etc. as necessary. The post-treatment liquid may be applied to the entire recording area formed on the recording medium, or may be applied only to the area where the ink image is formed.
[0066] <Recording Media> There are no particular limitations on the recording medium, and although plain paper, glossy paper, special paper, cloth, etc. can be used, good image formation is also possible using a non-permeable substrate. The non-permeable substrate is a substrate having a surface with low water permeability and absorbency, and includes materials that have many cavities inside but are not open to the outside. More quantitatively, in the Bristow method, 1 / 2 Water absorption up to 10mL / m 2 The term "substrate" refers to a substrate that is: As the impermeable substrate, for example, a plastic film such as a polyvinyl chloride resin film, a polyethylene terephthalate (PET) film, a polypropylene film, a polyethylene film, or a polycarbonate film can be suitably used.
[0067] The recording medium is not limited to those generally used as recording media, and may be wallpaper, flooring, building materials such as tiles, cloth for clothing such as T-shirts, textiles, leather, etc. By adjusting the configuration of the path for conveying the recording medium, ceramics, glass, metal, etc. may also be used.
[0068] <Recordings> The recorded matter of the present invention comprises an image formed on a recording medium using the ink of the present invention. A recorded matter can be obtained by recording using an inkjet recording apparatus and an inkjet recording method.
[0069] <Recording device and recording method> The ink of the present invention can be suitably used in various recording devices using the ink jet recording method, such as printers, facsimile machines, copying machines, printer / fax / copier combination machines, and three-dimensional modeling devices. In the present invention, the recording apparatus and recording method refer to an apparatus capable of ejecting ink, various treatment liquids, etc. onto a recording medium, and a method of recording using the apparatus. The recording medium refers to an object onto which ink or various treatment liquids can be attached even temporarily. This recording device can include not only a head portion that ejects ink, but also means related to feeding, transporting, and discharging the recording medium, as well as other devices called pre-processing devices and post-processing devices. The recording apparatus and the recording method may have a heating means used in the heating step and a drying means used in the drying step. The heating means and the drying means include, for example, a means for heating and drying the printed surface and the back surface of the recording medium. The heating means and the drying means are not particularly limited, but for example, a hot air heater or an infrared heater can be used. Heating and drying can be performed before, during, or after printing. In addition, the recording device and recording method are not limited to those that visualize meaningful images such as characters and figures with ink. For example, those that form patterns such as geometric designs and those that create three-dimensional images are also included. Furthermore, unless otherwise specified, the recording apparatus includes both a serial type apparatus in which the ejection head moves and a line type apparatus in which the ejection head does not move. Furthermore, this recording device includes not only desktop types, but also wide-width recording devices capable of printing on A0-sized recording media, and continuous-feed printers that can use, for example, continuous paper wound into a roll as a recording medium.
[0070] An example of a recording apparatus will be described with reference to Fig. 1. Fig. 1 is a schematic explanatory diagram of a printing apparatus which is an apparatus that ejects liquid.
[0071] The printing apparatus 1 includes an input section 10, a pre-processing section 50, a printing section 20, a drying section 30, and an unloading section 40. In the printing apparatus 1, a processing liquid is applied to the sheet material P loaded from the input section 10 in the pre-processing section 50, the printing section 20 applies the liquid to perform the required printing, the drying section 30 dries the liquid attached to the sheet material P, and the sheet material P is then discharged to the unloading section 40.
[0072] The carry-in section 10 includes an input tray 11 on which a plurality of sheet materials P are stacked, a feeding device 12 that separates and sends out the sheet materials P one by one from the input tray 11, and a pair of registration rollers 13 that sends the sheet materials P to the printing section 20.
[0073] Any feeding device can be used as the feeding device 12, such as a device using rollers or a device using air suction. After the leading edge of the sheet material P sent out from the input tray 11 by the feeding device 12 reaches the pair of registration rollers 13, the pair of registration rollers 13 is driven at a predetermined timing to send it out to the printing section 20.
[0074] The pre-treatment section 50 has a treatment liquid container 51 that contains a treatment liquid for reacting with liquid to suppress bleeding, and a pre-coating treatment rotor as a treatment liquid application means that applies the treatment liquid to the sheet material P. The pre-coating treatment rotor has a pumping roller that pumps up the treatment liquid, an application roller 52 that receives the treatment liquid adhering to the pumping roller and applies the treatment liquid to the surface of the sheet material being transported, and a roller 53 that holds the sheet material by being pressed against the application roller. After the treatment liquid is applied to the lower surface of the sheet material P by the application roller 52, the sheet material P is turned upside down and conveyed to a pair of registration rollers 13 constituting the conveying section .
[0075] The printing unit 20 includes a sheet conveying device 21 that conveys the sheet material P. The sheet conveying device 21 includes a belt that supports and conveys the sheet material P, and a suction device that generates a suction force on the belt surface.
[0076] The printing unit 20 also includes a liquid ejection unit 22 that ejects and applies liquid onto the treatment liquid-applied surface of the sheet material P that is carried and transported by the belt of the sheet transport device 21 .
[0077] The liquid discharge section 22 includes discharge units 23 (23A to 23F) which are liquid application means. For example, the discharge unit 23A discharges cyan (C) liquid, the discharge unit 23B discharges magenta (M) liquid, the discharge unit 23C discharges yellow (Y) liquid, and the discharge unit 23D discharges black (K) liquid. The discharge units 23F, 23F are used to discharge any of YMCK, or special liquids such as white and gold (silver). Furthermore, a discharge unit that discharges a treatment liquid such as a surface coating liquid can also be provided.
[0078] The ejection unit 23 is, for example, a full-line type head configured with a plurality of liquid ejection heads (hereinafter simply referred to as "heads") each having a nozzle row in which a plurality of nozzles are arranged.
[0079] The discharge operation of each discharge unit 23 of the liquid discharge section 22 is controlled by a drive signal corresponding to the printing information. When the sheet material P supported on the drum passes through an area facing the liquid discharge section 22, liquid of each color is discharged from the discharge unit 23, and an image corresponding to the printing information is printed.
[0080] The sheet material P onto which the liquid has been applied by the liquid discharger 22 is delivered to a suction transport mechanism 31 of the drying section 30 .
[0081] The drying section 30 includes a suction conveying mechanism section 31, which is a conveying means for conveying (suction conveying) the sheet material P in a suctioned state, and a drying mechanism section 32 for drying the liquid on the sheet material P conveyed by the suction conveying mechanism section 31.
[0082] The sheet material P to which the liquid has been applied in the printing section 20 is dried by the drying mechanism section 32 while being transported by the suction transport mechanism section 31, and then delivered to the discharge section .
[0083] The discharge section 40 includes a discharge tray 41 on which a plurality of sheet materials P are stacked. The sheet materials P conveyed from the drying section 30 are successively stacked and held on the discharge tray 41.
[0084] Although the pre-treatment unit 50 is configured to apply treatment liquid to one side of the sheet material P, the present invention is not limited to this. Another treatment liquid container may be provided downstream in the transport direction of the treatment liquid container 51 to apply treatment liquid to the back side of the sheet material P, or the sheet material P that has passed through the treatment liquid container 51 may be turned over and passed through the treatment liquid container 51 again to apply treatment liquid to the back side of the sheet material P.
[0085] The ink can be used in a wide variety of ways, including, but not limited to, inkjet recording, blade coating, gravure coating, bar coating, roll coating, dip coating, curtain coating, slide coating, die coating, and spray coating.
[0086] The application of the ink of the present invention is not particularly limited and can be appropriately selected depending on the purpose, and can be applied to, for example, printed matter, paint, coating material, undercoat, etc. Furthermore, the ink can be used not only to form two-dimensional characters and images when used as an ink, but also as a material for three-dimensional modeling to form three-dimensional solid images (three-dimensional objects). A known three-dimensional modeling device for forming a three-dimensional object can be used, and is not particularly limited. For example, a device equipped with an ink storage means, supply means, discharge means, drying means, etc. can be used. The three-dimensional object includes a three-dimensional object obtained by applying ink over and over. Also included is a molded product obtained by processing a structure to which ink is applied on a substrate such as a recording medium. The molded product is, for example, a recording material or structure formed in a sheet or film shape, which is molded by heat stretching, punching, etc., and is preferably used for applications in which the surface is molded after decoration, such as meters and operation panel of automobiles, office automation equipment, electric and electronic equipment, cameras, etc.
[0087] In the present invention, the terms image formation, recording, printing, printing, etc. are all synonymous. Recording medium, media, and printed material are all synonymous. EXAMPLES
[0088] Examples of the present invention will be described below, but the present invention is not limited to these examples. The methods for measuring various physical properties in the examples will be described below.
[0089] <Measurement of number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn)> Equipment: GPC (Tosoh Corporation) Detector: RI ·Measurement temperature: 40℃ Mobile phase: Tetrahydrofuran ·Flow rate: 0.45mL / min. The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) are the number average molecular weight, weight average molecular weight, and molecular weight distribution measured by GPC (gel permeation chromatography) using a calibration curve prepared from polystyrene samples of known molecular weight as the standard. Note that columns with exclusion limits of 60,000, 20,000, and 10,000 connected in series were used.
[0090] (Synthesis Example 1 of Polyester Resin) -Synthesis of polyester resin α- In a 1 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 280 parts by mass of propylene glycol as a diol, 611 parts by mass of terephthalic acid as a dicarboxylic acid, and 109 parts by mass of succinic acid were mixed. Next, the inside of the reaction vessel was thoroughly replaced with nitrogen gas, and then 300 ppm (relative to the monomer) of titanium tetraisopropoxide was added, and the temperature was raised to 200° C. in a nitrogen gas flow for about 4 hours. Next, the temperature was raised to 230°C over 2 hours, and the reaction was continued until no more effluent was produced. After that, the reaction was continued for 1 hour under reduced pressure of 5mmHg to 30mmHg to obtain polyester.
[0091] (Preparation Example of Pigment Pre-Dispersion A) The following ingredients were mixed and poured into a 110 mL glass screw cap bottle, after which 170 parts by mass of 2.0 mm diameter zirconia balls (Nikkato Corporation, YTZ balls) were poured in, the bottle was attached to a shaker (IKA Corporation, Vibrax VXR basic) and dispersed at 1,000 rpm for 24 hours. The media and dispersion were then separated by filtration, and the mixture was filtered through a PTFE membrane filter with an average pore size of 5.0 μm to produce pigment pre-dispersion A. The cumulative 50% volume particle diameter (D 50 ) was 112 nm. [Pigment pre-dispersion formulation] Carbon black (SBX45, Asahi Carbon Co., Ltd., primary particle size: 22 nm, DBP absorption: 55 mL / 100 g): 15.0 parts by mass Pigment dispersant (Ajisper PB821, manufactured by Ajinomoto Fine-Techno Co., Ltd., hydrophobic): 3.8 parts by weight Ethyl acetate: 41.2 parts by weight
[0092] (Preparation Example of Pigment Pre-Dispersion B) The following ingredients were mixed and poured into a 110 mL glass screw cap bottle, after which 170 parts by mass of 2.0 mm diameter zirconia balls (Nikkato Corporation, YTZ balls) were poured in, the bottle was attached to a shaker (IKA Corporation, Vibrax VXR basic) and dispersed at 1,000 rpm for 24 hours. The media and dispersion were then separated by filtration, and the mixture was filtered through a PTFE membrane filter with an average pore size of 5.0 μm to produce pigment pre-dispersion B. The cumulative 50% volume particle diameter (D 50 ) was 113 nm. [Pigment pre-dispersion formulation] Carbon black (SBX45, Asahi Carbon Co., Ltd., primary particle size: 22 nm, DBP absorption: 55 mL / 100 g): 15.0 parts by mass Pigment dispersant (BYKJET-9151, manufactured by BYK Chemie, hydrophilic): 3.8 parts by weight Ethyl acetate: 41.2 parts by weight
[0093] (Preparation Example of Pigment Pre-Dispersion C) The following ingredients were mixed and poured into a 110 mL glass screw cap bottle, after which 170 parts by mass of 2.0 mm diameter zirconia balls (Nikkato Corporation, YTZ balls) were poured in, the bottle was attached to a shaker (IKA Corporation, Vibrax VXR basic) and dispersed at 1,000 rpm for 24 hours. The media and dispersion were then separated by filtration, and the mixture was filtered through a PTFE membrane filter with an average pore size of 5.0 μm to produce pigment pre-dispersion C. The cumulative 50% volume particle diameter (D 50 ) was 159 nm. [Pigment pre-dispersion formulation] Carbon black (Asahi #15, Asahi Carbon Co., Ltd., primary particle size: 122 nm, DBP absorption: 41 mL / 100 g): 15.0 parts by mass Pigment dispersant (Ajisper PB821, manufactured by Ajinomoto Fine-Techno Co., Ltd., hydrophobic): 3.8 parts by weight Ethyl acetate: 41.2 parts by weight
[0094] Example 1 <Preparation of Aqueous Dispersion (1)> 26.7 g of the above pigment pre-dispersion A, 13.4 g of the above polyester resin α, 0.27 g of bis(2-morpholinoethyl)ether (manufactured by Tokyo Chemical Industry Co., Ltd.), and 5.19 g of ethyl acetate were placed in a container and stirred at 3,000 rpm for 1 minute using a TK Robomix (manufactured by Primix Corporation) to obtain a pigment dispersion resin solution. Next, 39.6 g of ion-exchanged water, 7.06 g of a 50% by mass aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.), and 3.7 g of ethyl acetate were mixed to prepare an aqueous layer, to which 29.6 g of the pigment dispersion resin solution prepared above was added, and the mixture was stirred at 5,000 rpm for 10 minutes using a TK Robomix (manufactured by Primix Corporation). Finally, the ethyl acetate was removed, and the mixture was filtered and purified using a nylon mesh with 67 μm openings. The solid content was adjusted to 30 mass% with ion-exchanged water to obtain an aqueous dispersion (1) containing pigment-encapsulated resin particles containing two or more pigment primary particles. FIG. 2 shows a TEM image of the aqueous dispersion (1) containing the pigment-encapsulated resin particles obtained in Example 1. FIG. 2 shows that the aqueous dispersion (1) has a form in which the pigment is encapsulated in spherical resin particles.
[0095] <Preparation of Ink 1> An ink having the following formulation was prepared using the aqueous dispersion (1) obtained above. The viscosity at 25°C was adjusted to 7.5 mPa s, and then the ink was filtered through a membrane filter having an average pore size of 10 μm to prepare Ink 1. "Ink prescription" The above aqueous dispersion (1): 10.75% by mass as solid content Propylene glycol: 40% by mass (adjusted to viscosity 7.5 mPa s) Silicone surfactant (Silface SAG503A, manufactured by Nissin Chemical Industry Co., Ltd.): 1.0% by mass Aliphatic dialcohol surfactant (Nissin Chemical Industry Co., Ltd., Surfynol AD01): 0.1% by mass Water: balance (total: 100% by mass)
[0096] Example 2 <Preparation of Aqueous Dispersion (2)> An aqueous dispersion (2) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of a 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.) was changed from 7.06 g to 1.2 g.
[0097] <Preparation of Ink 2> Ink 2 was prepared in the same manner as in Example 1, except that the aqueous dispersion (2) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0098] Example 3 <Preparation of Aqueous Dispersion (3)> An aqueous dispersion (3) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of a 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.) was changed from 7.06 g to 12.2 g.
[0099] <Preparation of Ink 3> Ink 3 was prepared in the same manner as in Example 1, except that the aqueous dispersion (3) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0100] Example 4 <Preparation of Aqueous Dispersion (4)> An aqueous dispersion (4) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of a 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.) was changed from 7.06 g to 24.6 g.
[0101] <Preparation of Ink 4> Ink 4 was prepared in the same manner as in Example 1, except that the aqueous dispersion (4) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0102] Example 5 <Preparation of Aqueous Dispersion (5)> An aqueous dispersion (5) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of pigment pre-dispersion A was changed from 26.7 g to 18.7 g.
[0103] <Preparation of Ink 5> Ink 5 was prepared in the same manner as in Example 1, except that the aqueous dispersion (5) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0104] Example 6 <Preparation of Aqueous Dispersion (6)> An aqueous dispersion (6) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of pigment pre-dispersion A was changed from 26.7 g to 10.7 g.
[0105] <Preparation of Ink 6> Ink 6 was prepared in the same manner as in Example 1, except that the aqueous dispersion (6) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0106] Example 7 <Preparation of Aqueous Dispersion (7)> An aqueous dispersion (7) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of a 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.) was changed from 7.06 g to 0.84 g.
[0107] <Preparation of Ink 7> Ink 7 was prepared in the same manner as in Example 1, except that the aqueous dispersion (7) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0108] Example 8 <Preparation of Aqueous Dispersion (8)> An aqueous dispersion (8) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of pigment pre-dispersion A was changed from 26.7 g to 40.0 g.
[0109] <Preparation of Ink 8> Ink 8 was prepared in the same manner as in Example 1, except that the aqueous dispersion (8) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0110] Comparative Example 1 <Preparation of Aqueous Dispersion (9)> An aqueous dispersion (9) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that a 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.) was not added.
[0111] <Preparation of Ink 9> Ink 9 was prepared in the same manner as in Example 1, except that the aqueous dispersion (9) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0112] Comparative Example 2 <Preparation of Aqueous Dispersion (10)> An aqueous dispersion (10) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that the amount of 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.) was changed from 7.06 g to 37.2 g in Example 1. FIG. 3 shows a TEM image of the aqueous dispersion (10) obtained in Comparative Example 2. FIG. 3 shows that the aqueous dispersion (10) has a form in which the pigment is encapsulated in non-spherical resin particles.
[0113] <Preparation of Ink 10> Ink 10 was prepared in the same manner as in Example 1, except that the aqueous dispersion (10) obtained above was used instead of the aqueous dispersion (1).
[0114] Comparative Example 3 <Preparation of Aqueous Dispersion (11)> An aqueous dispersion (11) was obtained in the same manner as in Example 1, except that the pigment pre-dispersion A in Example 1 was replaced with the pigment pre-dispersion B. Fig. 4 shows a TEM image of the aqueous dispersion (11) obtained in Comparative Example 3. Fig. 4 shows that in the aqueous dispersion (11), the pigment is not encapsulated in the resin particles.
[0115] <Preparation of Ink 11> Ink 11 was prepared in the same manner as in Example 1, except that the aqueous dispersion (11) obtained above was used instead of the aqueous dispersion (1).
[0116] Comparative Example 4 <Preparation of Aqueous Dispersion (12)> An aqueous dispersion (12) containing pigment-encapsulated resin particles containing two or more pigment primary particles was obtained in the same manner as in Example 1, except that in Example 1, pigment pre-dispersion A was replaced with pigment pre-dispersion C.
[0117] <Preparation of Ink 12> Ink 12 was prepared in the same manner as in Example 1, except that the aqueous dispersion (12) obtained above was used instead of the aqueous dispersion (1) in Example 1.
[0118] Comparative Example 5 Instead of using pigment-encapsulated resin particles, the following resin-only emulsion and water-based pigment dispersion were prepared to prepare Ink 13.
[0119] <Preparation of polyester single resin emulsion> 13.4 g of the polyester resin α, 0.27 g of bis(2-morpholinoethyl)ether (Tokyo Chemical Industry Co., Ltd.), and 5.19 g of ethyl acetate were placed in a container and stirred at 3,000 rpm for 1 minute with a TK Robomix (Primix Corporation) to obtain a resin solution. Next, 29.6 g of the pigment dispersion resin solution prepared above was added to an aqueous layer prepared by mixing 39.6 g of ion-exchanged water, 7.06 g of a 50 mass% aqueous solution of sodium dodecyl phenyl ether disulfonate (Eleminol MON-7, Sanyo Chemical Industries Co., Ltd.), and 3.7 g of ethyl acetate, and the mixture was stirred at 5,000 rpm for 10 minutes with a TK Robomix. Finally, the ethyl acetate was removed, and the mixture was filtered and purified using a nylon mesh with a mesh size of 67 μm. The solid content was adjusted to 30 mass% with ion-exchanged water, and the cumulative 50% volume particle size (D 50 ) A polyester resin emulsion with a diameter of 257 nm was obtained.
[0120] (Production example of pigment dispersant) 62.0 parts by mass of 1,6-hexanediol (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in 700 mL of dichloromethane, and 20.7 parts by mass of pyridine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added and stirred. A solution of 2-naphthalenecarbonyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) dissolved in 100 mL of dichloromethane was dropped into this solution over 2 hours, and then the mixture was stirred at room temperature for 6 hours. The resulting reaction solution was washed with water, and then the organic layer was isolated, dried over magnesium sulfate, and the solvent was distilled off. The residue was purified by silica gel column chromatography using a mixed solvent of dichloromethane / methanol (volume ratio 98 / 2) as an eluent to obtain a compound. Next, 42.1 parts by mass of the obtained compound was dissolved in 80 mL of dry methyl ethyl ketone, and heated to 60° C. while stirring. A solution in which 24.0 parts by mass of Karenz MOI (manufactured by Showa Denko K.K.) was dissolved in 20 mL of dry methyl ethyl ketone was added dropwise to this solution over 1 hour, and then stirred at 70° C. for 12 hours. After cooling to room temperature, the solvent was distilled off. The residue was purified by silica gel column chromatography using a mixed solvent of dichloromethane / methanol (volume ratio 99 / 1) as an eluent to obtain a monomer. Next, 2.30 parts by mass of acrylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), 8.54 parts by mass of the monomer, and 0.31 parts by mass of 2,2'-azobis(isobutyronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 100 mL of methyl ethyl ketone, and the mixture was stirred for 5 hours at a temperature condition of 75°C under a nitrogen gas flow. Thereafter, the reaction solution was cooled to room temperature, and reprecipitation was repeated five times using hexane to purify the copolymer. After the purification process, the copolymer was filtered and dried under reduced pressure to obtain a pigment dispersant.
[0121] <Preparation of Water-Based Pigment Dispersion> 3.8 parts by mass of the pigment dispersant was dissolved in 30.0 parts by mass of an aqueous diethanolamine solution so that the pH was 8.0. Ion-exchanged water was further added to make the total amount of the aqueous solution 45.0 parts by mass. Next, the materials in the following formula were mixed and placed in a 110 mL glass screw tube bottle, after which 170 parts by mass of 2.0 mm diameter zirconia balls (YTZ balls, manufactured by Nikkato Corporation) were added, the bottle was attached to a shaker (Vibrax VXR basic, manufactured by IKA) and dispersed at 1,000 rpm for 24 hours. After that, the media and the dispersion were separated by filtration, and an aqueous pigment dispersion was produced by filtering through a cellulose acetate membrane filter with an average pore size of 5.0 μm. The cumulative 50% volume particle size (D 50 ) was 120 nm. [Water-based pigment dispersion formulation] Carbon black (SBX45, manufactured by Asahi Carbon Co., Ltd.): 15.0 parts by mass The pigment dispersant aqueous solution: 45.0 parts by mass
[0122] <Preparation of Ink 13> An ink was prepared according to the following formulation using the polyester single resin emulsion and water-based pigment dispersion obtained above. The viscosity at 25°C was adjusted to 7.5 mPa s, and then the ink was filtered through a membrane filter with an average pore size of 10 μm to prepare Ink 13. "Ink prescription" Polyester only resin emulsion: 5.375% by weight as solids Water-based pigment dispersion: 5.375% by weight as solids Propylene glycol: 40% by mass (adjusted to viscosity 7.5 mPa s) Silicone surfactant (Silface SAG503A, manufactured by Nissin Chemical Industry Co., Ltd.): 1.0% by mass Aliphatic dialcohol surfactant (Nissin Chemical Industry Co., Ltd., Surfynol AD01): 0.1% by mass Water: balance (total: 100% by mass)
[0123] Next, the properties of each of the prepared aqueous dispersions and inks were evaluated as follows. The results are shown in Tables 1 to 4.
[0124] <Cumulative 50% volume diameter of resin particles (D 50 )> Cumulative 50% volumetric particle size of resin particles (D 50 ) was measured by dynamic light scattering using a zeta potential / particle size measurement system (ELSZ-1000, Otsuka Electronics Co., Ltd.). Specifically, the sample was diluted with ion-exchanged water or an organic solvent as necessary so that the solid content concentration of the measurement sample was 0.01 mass%, and a part of the obtained solution was placed in a quartz cell and set in a sample holder. Then, the measurement was performed under the following conditions: temperature: 25°C, dust cut (number of times: 5, Upper: 5, Lower: 100), cumulative number: 70.
[0125] <Pigment exposure rate> The pigment exposure rate on the coating surface was calculated by observing with a scanning electron microscope (SEM). Specifically, first, an aqueous dispersion was prepared using ion-exchanged water so that the solid content concentration was 10.75% by mass. Then, the dispersion was applied to coated paper (Lumia Art Gloss 130, manufactured by STORA ENSO) using a bar coater having a diameter of 0.15 mm, and dried overnight at 25°C to form a coating film having an average thickness of 2 μm. This coating film was cut out and fixed to a stub for SEM observation using carbon tape. This was observed without conductive treatment using a scanning electron microscope (ZEISS, Merlin) at an acceleration voltage of 0.75 kV, a backscattered electron detector, and a magnification of 2,000 to 20,000 times. This observation method makes it possible to distinguish the exposed pigment from the difference in the amount of backscattered electrons emitted by carbon black and resin. The area occupied by the pigment relative to the entire coating film at a magnification of 20,000 times was defined as the pigment exposure rate, and the pigment exposure rate was classified as follows. The ratio of the area occupied by the pigment on the coating film surface was determined by binarizing the SEM observation image, and the average of three visual fields observed at random locations was taken to determine the pigment exposure rate, which was then evaluated according to the following criteria. [Evaluation Criteria] ◎: 0% or more and 3% or less ○: More than 3% and 5% △: More than 5% and less than 8% ×: More than 8%
[0126] <Surface roughness of coating film> The surface roughness of the coating film was calculated using a scanning probe microscope (SPM) as follows. First, an aqueous dispersion was prepared using ion-exchanged water so that the solid content concentration was 10.75% by mass. Next, the coating was applied to coated paper (Lumia Art Gloss 130, manufactured by STORA ENSO) using a bar coater with a diameter of 0.15 mm, and heated and dried in an oven at 100°C for 5 minutes. This coating film was cut out and observed under the following conditions, and the surface roughness was calculated. The observation was performed by arbitrarily changing the location and taking the average of three visual fields observed to determine the average surface roughness. [Measurement conditions] Equipment: Scanning probe microscope (Bruker, DimensionIcon) Cantilever: Olympus OMCL-AC240TS Measurement mode: Tapping mode Observation area: 2μm square
[0127] <Proportion of pigment-encapsulated resin particles> First, each of the obtained aqueous dispersions was diluted with ion-exchanged water so that the solid content concentration was 0.1% by mass to prepare a sample solution. Next, 1 μL of the sample liquid was placed on a hydrophilized collodion membrane-attached mesh (Nisshin EM Co., Ltd., collodion membrane-attached mesh, Cu150 mesh) using a micropipette, and the sample liquid was immediately absorbed with a triangular filter paper. Next, 1 μL of EM stainer diluted 10 times was placed using a micropipette, and the sample liquid was immediately absorbed with a triangular filter paper. After drying under reduced pressure, observation was performed with a transmission electron microscope (JEM-2100F, JEOL Ltd.) at an acceleration voltage of 200 kV and a magnification of 40,000 times. By this observation method, five or more images of a field of view containing three or more particles with a volume diameter of 100 nm or more were obtained by arbitrarily changing the location, and the ratio of the number of pigment-encapsulated resin particles to the total number of particles with a volume diameter of 100 nm or more was calculated for each image, and the average value was calculated. The obtained ratio was defined as the presence ratio of pigment-encapsulated resin particles, and was evaluated according to the following criteria. [Evaluation Criteria] ◎: 50% or more ○: 30% or more but less than 50% △: 10% to less than 30% ×: 0% or more but less than 10%
[0128] <Aspect ratio of resin particles> The aspect ratio was determined by measuring the long and short sides of 20 pigment-encapsulated resin particles observed according to the above-mentioned method for observing pigment-encapsulated resin particles using a transmission electron microscope (TEM), calculating the average value, and then calculating the aspect ratio from the average value of the long sides / average value of the short sides.
[0129] <Image formation> The exterior of an inkjet printer (IPSiO GXe5500, manufactured by Ricoh Company, Ltd.) was removed, a rear multi-manual feeder was attached, and pure water was passed through the ink supply path including the print head to clean it. The cleaning liquid was passed through sufficiently until it was no longer colored, and then the cleaning liquid was completely drained from the device to prepare a printing device for evaluation. The prepared ink was filled into an ink cartridge to prepare an ink cartridge for evaluation. A filling operation was performed to confirm that all nozzles were filled with the evaluation ink and that no abnormal images were produced. After selecting the glossy paper clean mode in the driver attached to the printer, the print mode was set to color matching off in the user settings. In this mode, the ink deposition amount on the recording medium for a solid image is 20 g / m 2 The discharge amount was adjusted by changing the head drive voltage so as to obtain the following.
[0130] <Image density> A solid image was printed by the above image output method, and then dried at room temperature (25° C.) for 1 day and in an oven at 100° C. for 5 minutes to prepare images. With a sheet of white plain paper placed under the printed image, the total density was measured using a spectrophotometric densitometer (X-Rite939, manufactured by X-Rite Corporation), and the black (K) value was taken as the image density. In addition, the difference in image density between the image obtained by drying at 25°C and the image obtained by drying at 100°C (ΔOD = "OD of image obtained by drying at 25°C" - "OD of image obtained by drying at 100°C") was calculated and evaluated according to the following criteria. [Evaluation Criteria] ○: ΔOD is less than 0% △: ΔOD is 0% ×: ΔOD is greater than 0%
[0131] [Table 1]
[0132] [Table 2]
[0133] [Table 3] *In Table 3, "-" in Comparative Examples 1 to 4 means that measurement was not possible.
[0134] [Table 4]
[0135] From the results in Tables 1 to 4, it was found that in all of Examples 1 to 8, high image density was obtained, and the decrease in image density during drying by heating could be suppressed. In contrast, in Comparative Example 1, numerous nozzle clogging occurred in the inkjet evaluation, making it difficult to print solid images (image density could not be measured). In addition, in Comparative Example 2, numerous nozzle clogging and deflection of ink jet occurred in the inkjet evaluation, making it difficult to print solid images (image density could not be measured). In Comparative Example 3, the surface smoothness of the coating film after drying at 100°C was low, and high image density could not be obtained after drying at 100°C. In addition, in Comparative Example 4, numerous nozzle clogging occurred in the inkjet evaluation, making it difficult to print solid images (image density could not be measured). In Comparative Example 5, the surface smoothness of the coating film after drying at 100°C was low, and high image density could not be obtained after drying at 100°C.
[0136] For example, aspects of the present invention are as follows. <1> The ink contains pigment-encapsulated resin particles that encapsulate a pigment and a surfactant, The cumulative 50% volume particle diameter of the pigment-encapsulated resin particles (D 50 ) is 200 nm or more and 500 nm or less, The aqueous dispersion is characterized in that the aspect ratio of the pigment-encapsulating resin particles is 1.0 or more and 1.5 or less. <2> The content of the surfactant is 1% by mass or more and 20% by mass or less. <1> 2. The aqueous dispersion according to claim 1. <3> The surfactant is an anionic surfactant. <1> from <2> The aqueous dispersion according to any one of the above items. <4> The pigment is an inorganic pigment, and the inorganic pigment is carbon black. <1> from <3> The aqueous dispersion according to any one of the above items. <5> The pigment-encapsulated resin particles contain a polyester resin. <1> from <4> The aqueous dispersion according to any one of the above items. <6> The mass ratio of the pigment to the resin in the pigment-encapsulated resin particles (pigment / resin) is 0.2 or more and 0.75 or less. <1> from <5> The aqueous dispersion according to any one of the above items. <7> a coating film having an average thickness of 2 μm formed using the aqueous dispersion has a pigment exposure rate of 8% or less on the surface thereof; <1> from <6> The aqueous dispersion according to any one of the above items. <8> The surface roughness of a coating film having an average thickness of 2 μm formed using the aqueous dispersion is 20 nm or less. <1> from <7> The aqueous dispersion according to any one of the above items. <9> The ratio of the pigment-encapsulating resin particles to the total number of particles having a volume particle size of 100 nm or more is 30% or more. <1> from <8> The aqueous dispersion according to any one of the above items. <10> mixing an organic solvent and a pigment to prepare a pigment pre-dispersion; A step of mixing the obtained pigment pre-dispersion with a resin to prepare a pigment dispersion resin solution; A step of mixing the obtained pigment-dispersed resin solution with a surfactant-containing liquid to prepare a pigment-encapsulated resin particle dispersion liquid; removing the organic solvent from the obtained pigment-encapsulated resin particle dispersion; The present invention relates to a method for producing an aqueous dispersion comprising the steps of: <11> The cumulative volume particle size of the pigment in the pigment pre-dispersion is 50% (D 50 ) is 10 nm or more and 150 nm or less, <10> 2. A method for producing the aqueous dispersion according to claim 1. <12> In the step of preparing the pigment pre-dispersion, a hydrophobic pigment dispersant is added. <10> from <11> 10. The method for producing the aqueous dispersion according to claim 9, <13> The composition contains water, pigment-encapsulated resin particles that encapsulate a pigment, a surfactant, and an organic solvent, The cumulative 50% volume particle diameter of the pigment-encapsulated resin particles (D 50 ) is 200 nm or more and 500 nm or less, The ink is characterized in that the aspect ratio of the pigment-encapsulating resin particles is 1.0 or more and 1.5 or less. <14> The above <13> A printing method comprising the step of applying the ink according to claim 1. <15> The above <13> an ink storage section that stores the ink according to an ink applying means for applying the ink; The printing device is characterized by having:
[0137] The above <1> from <9> The aqueous dispersion according to any one of the preceding claims. <10> from <12> The method for producing the aqueous dispersion according to any one of the above-mentioned <13> The ink according to <14> The printing method according to claim 1, <15> According to the printing apparatus described in the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0138] 400 Image forming device 401 Exterior of image forming device 401c Device body cover 404 Cartridge Holder 410 Main Tank 410k, 410c, 410m, 410y Main tanks for black (K), cyan (C), magenta (M), and yellow (Y) 411 Ink storage unit 413 Ink outlet 414 Storage container case 420 Mechanism Department 434 Discharge Head 436 Supply Tube [Prior art documents] [Patent documents]
[0139] [Patent Document 1] JP 2016-196621 A [Patent Document 2] JP 2002-322396 A [Patent Document 3] JP 2019-099819 A
Claims
1. A pigment dispersion composition comprising a hydrophobic pigment dispersant, pigment-encapsulated resin particles that encapsulate the pigment, and a surfactant, The cumulative 50% volume particle diameter of the pigment-encapsulated resin particles (D 50 ) is 200 nm or more and 500 nm or less, The aspect ratio of the pigment-encapsulated resin particles is 1.0 or more and 1.5 or less, The aqueous dispersion has a surfactant content of 1% by mass or more and 20% by mass or less.
2. The aqueous dispersion according to claim 1 , wherein the surfactant is an anionic surfactant.
3. 3. The aqueous dispersion according to claim 1, wherein the pigment is an inorganic pigment, and the inorganic pigment is carbon black.
4. The aqueous dispersion according to claim 1 , wherein the pigment-encapsulating resin particles contain a polyester resin.
5. 5. The aqueous dispersion according to claim 1, wherein the mass ratio of the pigment to the resin (pigment / resin) in the pigment-encapsulating resin particles is 0.2 or more and 0.75 or less.
6. 6. The aqueous dispersion according to claim 1, wherein a coating film having an average thickness of 2 μm formed using the aqueous dispersion has a pigment exposure rate of 8% or less on the surface thereof.
7. 7. The aqueous dispersion according to claim 1, wherein a coating film having an average thickness of 2 μm formed using the aqueous dispersion has a surface roughness of 20 nm or less.
8. 8. The aqueous dispersion according to claim 1, wherein the pigment-encapsulating resin particles account for 30% or more of the total number of particles having a volume particle size of 100 nm or more.
9. mixing an organic solvent and a pigment to prepare a pigment pre-dispersion; A step of mixing the obtained pigment pre-dispersion with a resin to prepare a pigment dispersion resin solution; A step of mixing the obtained pigment-dispersed resin solution with a surfactant-containing liquid to prepare a pigment-encapsulated resin particle dispersion liquid; removing the organic solvent from the obtained pigment-encapsulated resin particle dispersion; Including, In the step of preparing the pigment pre-dispersion, a hydrophobic pigment dispersant is added, A method for producing an aqueous dispersion, wherein the amount of the surfactant added is 1.0% by mass or more and 20% by mass or less based on the aqueous dispersion obtained in the step of removing the organic solvent.
10. The cumulative volume particle size of the pigment in the pigment pre-dispersion is 50% (D 50 10. The method for producing an aqueous dispersion according to claim 9, wherein the average particle diameter is from 10 nm to 150 nm.
11. The ink contains water, a hydrophobic pigment dispersant, pigment-encapsulated resin particles that encapsulate a pigment, and a surfactant, and an aqueous dispersion containing the surfactant and an organic solvent; The cumulative 50% volume particle diameter of the pigment-encapsulated resin particles (D 50 ) is 200 nm or more and 500 nm or less, The aspect ratio of the pigment-encapsulated resin particles is 1.0 or more and 1.5 or less, The ink is characterized in that the surfactant contained in the aqueous dispersion is from 1% by mass to 20% by mass.
12. A printing method comprising the step of applying the ink according to claim 11.
13. an ink storage section that stores the ink according to claim 11; an ink applying means for applying the ink; A printing device comprising:
Citation Information
Patent Citations
Aqueous colored particle dispersion for use in ink jet printing liquid, its manufacturing method and ink jet printing liquid
JP2002322396A
Fine particles of colored resin, method for producing water dispersion of fine particles of colored resin, dispersion of fine particles of colored resin, method for producing fine particles of colored resin, ink, recording unit, ink cartridge, ink-jet recording device and ink-jet printing method
JP2003327895A
Microencapsulated pigment and its production process, aqueous dispersion, and ink for inkjet recording
JP2005097476A
Resin composition for inkjet system color filter, color filter, and method for manufacturing color filter
JP2006301307A
Method for producing aqueous dispersion of pigment-containing polymer particle and water-based pigment ink composition
JP2008163059A