Liquid composition set and method for producing porous resin
The liquid composition set ensures porosity and substance permeability by using specific compatibility and phase separation conditions, addressing the issue of suppressed porosity in composite porous bodies formed by combining liquid compositions.
Patent Information
- Application Number
- JP2020197906
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-11-30
AI Technical Summary
Existing liquid compositions for forming porous resins face issues when combined, leading to suppressed porosity in the contact area, impairing substance permeability in composite porous bodies.
A liquid composition set comprising a polymerizable compound X and a solvent X, and a solvent Y, where the composition X contains a polymerizable compound and solvent X, and composition Y contains solvent Y, with specific compatibility and phase separation conditions to ensure porosity even when combined.
The liquid composition set maintains porosity in the contact area, enhancing substance permeability and preventing impairment of the porous structure when used with another liquid composition.
Smart Images

Figure 0007567406000014 
Figure 0007567406000015 
Figure 0007567406000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid composition set , and and a method for producing a porous resin. [Background technology]
[0002] In general, porous resins can be used in a variety of applications. For example, by appropriately selecting the shape of the pores, the size of the pores, and the surface characteristics of the skeleton portion in the porous resin, a separation layer that transmits or blocks only a specific substance can be provided. In another example, by utilizing the vast surface area and void volume of the porous resin, an efficient reaction field or storage field for gas or liquid taken in from the outside can be provided. Therefore, if a liquid composition for forming a porous resin that is easy to handle and can be easily applied to various locations can be provided, the range of applications of the porous resin will be greatly expanded.
[0003] As an example of a liquid composition for forming such a porous resin, Patent Document 1 discloses a porous-forming photocurable resin composition containing, as essential components, a photopolymerizable monomer (A), an organic compound (B) that is incompatible with the photopolymerizable monomer (A), a common solvent (C) that is compatible with the photopolymerizable monomer (A) and the organic compound (B), and a photopolymerization initiator (D). Summary of the Invention [Problem to be solved by the invention]
[0004] However, when a liquid composition for forming a porous resin is used in combination with another liquid composition, there is a problem that contact between the liquid composition for forming a porous resin and the other liquid composition suppresses the resin formed in the contact area from becoming porous. [Means for solving the problem]
[0005] The present invention provides a liquid composition set including a liquid composition X containing a polymerizable compound X and a solvent X, and a liquid composition Y containing a solvent Y, the liquid composition X forming a porous resin, and when a liquid composition Z consisting of 10.0 mass % of the liquid composition X and 90.0 mass % of the liquid composition Y is prepared, the liquid composition Z is At 300 rpm The liquid composition Z has a light transmittance of 30% or more at a wavelength of 550 nm as measured while stirring; and The liquid composition Z was filled between two non-alkali glass substrates. The present invention relates to a liquid composition set, characterized in that the increase rate of the haze value measured using a haze measuring element is 1.0% or more. (Note that the rate of increase in haze value is the ratio of the measurement value of the haze measurement element after UV irradiation under conditions in which the polymerizable compound X contained in the haze measurement element can be polymerized to the measurement value of the haze measurement element before UV irradiation, with the measurement value of the haze measurement element before UV irradiation being used as a reference.) Effect of the Invention
[0006] According to the present invention, when a liquid composition for forming a porous resin is used in combination with another liquid composition, even if the liquid composition for forming a porous resin comes into contact with the other liquid composition, a liquid composition set can be provided that is excellent in making the resin porous in the contact area. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic diagram showing an example of a porous resin production apparatus for implementing the porous resin production method of this embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a material jet type molding apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, one embodiment of the present invention will be described.
[0009] [Liquid composition set] The liquid composition set includes liquid composition X and liquid composition Y, and may include other liquid compositions as necessary. In addition, the liquid composition set is not limited to the case where the container filled with liquid composition X and the container filled with liquid composition Y are integrated as long as liquid composition X and liquid composition Y are present in an independent liquid state. For example, even if liquid composition X and liquid composition Y are filled in independent containers, the liquid composition set is included in the concept of the liquid composition set if it is assumed that liquid composition X and liquid composition Y are used in combination, or if it substantially induces liquid composition X and liquid composition Y to be used in combination. Note that liquid composition X and liquid composition Y are liquids with different compositions.
[0010] The liquid composition set forms a porous resin by hardening (polymerizing) a polymerizable compound or the like, which is a component of the liquid composition constituting the liquid composition set. Therefore, the liquid composition set is preferably used for forming a porous resin. In addition, the liquid composition set forming a porous resin is not particularly limited as long as a porous resin is formed as a result of using the liquid composition set so that liquid composition X and liquid composition Y come into contact with each other. Specifically, for example, when liquid composition X and liquid composition Y are applied so that they come into contact with each other, even if a porous resin is formed only in the region where liquid composition X is applied and the contact region of liquid composition X and liquid composition Y, and a porous resin is not formed in the region where liquid composition Y is applied (excluding the contact region of liquid composition X and liquid composition Y), the liquid composition set is considered to form a porous resin. More specifically, for example, even if a material that forms a porous resin by being hardened (polymerized), such as a polymerizable compound, is included in liquid composition X but not included in liquid composition Y, if a porous resin is formed as a result of using the liquid composition set, the liquid composition set is considered to form a porous resin. In addition, when the liquid composition set forms a porous resin, it is meant that the porous resin is formed by hardening (polymerizing) some of the components of the liquid compositions that make up the liquid composition set (such as a polymerizable compound), and the other components of the liquid compositions that make up the liquid composition set (such as a solvent) are not hardened to form a porous resin.
[0011] The liquid composition set is used for applications that assume that the liquid composition for forming a porous resin, which is a component of the liquid composition set, is brought into contact with another liquid composition. The reason why it is preferable to use the liquid composition set of the present disclosure in such cases will be described. When the liquid composition for forming a porous resin contacts with another liquid composition, there is a concern that the resin formed in the contact area is suppressed from becoming porous. More specifically, the above concern becomes apparent, for example, when the liquid composition for forming a porous resin is applied to a porous substrate to form a porous resin on the porous substrate. In such a case, a method of applying another liquid composition to the porous substrate in advance is effective for the purpose of suppressing the penetration of the liquid composition for forming a porous resin into the porous substrate and forming a porous resin on the porous substrate. However, the liquid composition for forming a porous resin contacts with another liquid composition, which may suppress the resin formed in the contact area from becoming porous. In such a case, the communication between the pores in the porous substrate and the pores in the porous resin is impaired by the resin formed in the contact area in which the porosity is suppressed, and the material permeability of the composite porous body having the porous substrate and the porous resin is reduced. Hereinafter, details of a liquid composition set that is excellent in making the resin porous in the contact area even when the liquid composition for forming a porous resin comes into contact with another liquid composition will be described in detail, specifically, details of liquid composition X, which is a liquid composition for forming a porous resin, and liquid composition Y, which is another liquid composition, will be described in detail.
[0012] <<Liquid composition X>> Liquid composition X is a liquid used in combination with liquid composition Y. Liquid composition X is preferably applied to the area where liquid composition Y is applied. Liquid composition X is a liquid that can form a porous resin even when used alone (in other words, even when not used together with liquid composition Y), and the liquid composition set can form a porous resin by having liquid composition X. In the following description, the resin formed when liquid composition X is used alone is referred to as resin X, and the porous body of resin X is referred to as porous resin X. In addition, liquid composition X forms porous resin X, which also means that some components (polymerizable compound X, etc.) constituting liquid composition X are cured (polymerized) to form porous resin X, and other components (solvent X, etc.) constituting liquid composition X are not cured to form porous resin X, and the like. The liquid composition X contains a polymerizable compound X, a solvent X, and, if necessary, other components such as a polymerization initiator.
[0013] <Polymerizable compound X> The polymerizable compound X forms a resin X by polymerization, and when polymerized in the liquid composition X, a porous resin X is formed. The resin X formed by the polymerizable compound X is preferably a resin having a mesh-like structure formed by applying active energy rays (for example, by applying light or heat), and examples thereof include acrylate resins, methacrylate resins, urethane acrylate resins, vinyl ester resins, unsaturated polyester resins, epoxy resins, oxetane resins, vinyl ether resins, and resins formed by ene-thiol reactions. In addition, since it is preferable to use radical polymerization with high reactivity, acrylate resins, methacrylate resins, urethane acrylate resins, etc., which are resins formed by a polymerizable compound X having a (meth)acryloyl group, and vinyl ester resins, etc., which are resins formed by a polymerizable compound X having a vinyl group, are more preferable from the viewpoint of productivity. These may be used alone or in combination of two or more. When two or more types are used in combination, the combination of resins is not particularly limited and can be appropriately selected according to the purpose, but for example, it is preferable to mix other resins with a urethane acrylate resin as the main component in order to impart flexibility. In the present disclosure, a polymerizable compound having an acryloyl group or a methacryloyl group is referred to as a polymerizable compound having a (meth)acryloyl group. The active energy ray is not particularly limited as long as it can provide the energy required to proceed with the polymerization reaction of the polymerizable compound X in the liquid composition X, and examples of the active energy ray include ultraviolet rays, electron beams, α rays, β rays, γ rays, and X-rays. Among these, ultraviolet rays are preferable. In particular, when a high-energy light source is used, the polymerization reaction can proceed without using a polymerization initiator.
[0014] The polymerizable compound X preferably has at least one radically polymerizable functional group. Examples thereof include monofunctional, bifunctional, trifunctional or higher functional radically polymerizable compounds, functional monomers, and radically polymerizable oligomers. Among these, bifunctional or higher functional radically polymerizable compounds are preferred.
[0015] Examples of the monofunctional radical polymerizable compound include 2-(2-ethoxyethoxy)ethyl acrylate, methoxypolyethylene glycol monoacrylate, methoxypolyethylene glycol monomethacrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, tetrahydrofurfuryl acrylate, 2-ethylhexyl carbitol acrylate, 3-methoxybutyl acrylate, benzyl acrylate, cyclohexyl acrylate, isoamyl acrylate, isobutyl acrylate, methoxytriethylene glycol acrylate, phenoxytetraethylene glycol acrylate, cetyl acrylate, isostearyl acrylate, stearyl acrylate, and styrene monomer. These may be used alone or in combination of two or more.
[0016] Examples of bifunctional radically polymerizable compounds include 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, neopentyl glycol diacrylate, EO-modified bisphenol A diacrylate, EO-modified bisphenol F diacrylate, neopentyl glycol diacrylate, tricyclodecane dimethanol diacrylate, etc. These may be used alone or in combination of two or more.
[0017] Examples of the radical polymerizable compound having three or more functionalities include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETTA), glycerol triacrylate, ECH-modified glycerol triacrylate, EO-modified glycerol triacrylate, PO-modified glycerol triacrylate, trimethylolpropane triacrylate, trimeth ... Examples of the acrylates include (acryloxyethyl) isocyanurate, dipentaerythritol hexaacrylate (DPHA), caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, alkyl-modified dipentaerythritol tetraacrylate, alkyl-modified dipentaerythritol triacrylate, dimethylolpropane tetraacrylate (DTMPTA), pentaerythritol ethoxy tetraacrylate, EO-modified phosphoric acid triacrylate, and 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate. These may be used alone or in combination of two or more.
[0018] The content of the polymerizable compound X in the liquid composition X is preferably 5.0% by mass or more and 70.0% by mass or less, more preferably 10.0% by mass or more and 50.0% by mass or less, and even more preferably 20.0% by mass or more and 40.0% by mass or less, based on the total amount of the liquid composition X. When the content of the polymerizable compound X is 70.0% by mass or less, the size of the pores of the obtained porous resin X is not too small, such as several nm or less, and the porous resin X has an appropriate porosity, and the tendency of the penetration of liquids and gases to be difficult to occur can be suppressed, which is preferable. In addition, when the content of the polymerizable compound X is 5.0% by mass or more, the three-dimensional network structure of the resin X is sufficiently formed, a porous structure is sufficiently obtained, and the strength of the obtained porous structure also tends to be improved, which is preferable.
[0019] <Solvent X> Solvent X (hereinafter, solvent X is also referred to as "porogen") is a liquid compatible with polymerizable compound X. Solvent X is a liquid that becomes incompatible with polymerized material (resin X) (phase separation occurs) in the process of polymerizing polymerizable compound X in liquid composition X. That is, the meaning of "solvent X" in this disclosure is distinguished from the meaning of "solvent" which is a commonly used term. By including solvent X in liquid composition X, polymerizable compound X forms porous resin X when polymerized in liquid composition X. In addition, it is preferable that solvent X is capable of dissolving a compound (polymerization initiator described later) that generates radicals or acid by light or heat. Solvent X may be used alone or in combination of two or more kinds. In addition, solvent X does not have polymerizability in this disclosure.
[0020] The boiling point of one type of porogen alone or the boiling point of two or more types in combination is preferably 50°C or more and 250°C or less, more preferably 70°C or more and 200°C or less, at normal pressure. By having a boiling point of 50°C or more, vaporization of the porogen at around room temperature is suppressed, making the liquid composition X easy to handle and facilitating control of the content of the porogen in the liquid composition X. In addition, by having a boiling point of 250°C or less, the time required for the step of drying the porogen after polymerization is shortened, improving the productivity of the porous resin X. In addition, since the amount of porogen remaining inside the porous resin X can be suppressed, the quality is improved when the porous resin X is used as a functional layer such as a material separation layer that separates substances or a reaction layer as a reaction field. The boiling point of the porogen alone or in the case of using two or more porogens in combination is preferably 120° C. or higher at normal pressure.
[0021] Examples of the porogen include ethylene glycols such as diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisopropyl ether, and dipropylene glycol monomethyl ether, esters such as γ-butyrolactone and propylene carbonate, and amides such as NN dimethylacetamide. In addition, liquids with relatively large molecular weights such as methyl tetradecanoate, methyl decanoate, methyl myristate, and tetradecane can also be used. In addition, liquids such as acetone, 2-ethylhexanol, and 1-bromonaphthalene can also be used. In the present disclosure, the above-mentioned liquids do not necessarily correspond to porogens. As described above, the porogen in the present disclosure is a liquid that is compatible with the polymerizable compound X and that becomes incompatible with the polymer (resin X) (causes phase separation) during the polymerization of the polymerizable compound X in the liquid composition X. In other words, whether or not a certain liquid corresponds to a porogen is determined by the relationship between the polymerizable compound X and the polymer (resin X formed by polymerization of the polymerizable compound). Furthermore, since the liquid composition X of the present disclosure only needs to contain at least one type of porogen having the above-mentioned specific relationship with the polymerizable compound X, the range of material selection when preparing the liquid composition X is broadened, and the design of the liquid composition X is facilitated. By broadening the range of material selection when preparing the liquid composition X, the range of response is broadened when there are characteristics required of the liquid composition X from a viewpoint other than the formation of a porous structure. For example, when the liquid composition X is discharged by an inkjet method, the liquid composition X is required to have discharge stability and the like from a viewpoint other than the formation of a porous structure, and the wide range of material selection makes it easy to design the liquid composition X. As described above, the liquid composition X of the present disclosure is only required to contain at least one type of porogen having the above-mentioned specific relationship with the polymerizable compound X, and may additionally contain a liquid (liquid that is not a porogen) that does not have the above-mentioned specific relationship with the polymerizable compound X. However, the content of the liquid (liquid that is not a porogen) that does not have the above-mentioned specific relationship with the polymerizable compound X is preferably 10.0 mass % or less, more preferably 5.0 mass % or less, even more preferably 1.0 mass % or less, and particularly preferably not contained, based on the total amount of the liquid composition X.
[0022] The content of the porogen in the liquid composition X is preferably 30.0% by mass or more and 95.0% by mass or less, more preferably 50.0% by mass or more and 90.0% by mass or less, and even more preferably 60.0% by mass or more and 80.0% by mass or less, based on the total amount of the liquid composition X. When the content of the porogen is 30.0% by mass or more, the size of the pores of the obtained porous body is not too small, such as several nm or less, and the porous body has an appropriate porosity, and the tendency of the penetration of liquids and gases to be difficult can be suppressed, which is preferable. In addition, when the content of the porogen is 95.0% by mass or less, the three-dimensional network structure of the resin X is sufficiently formed, the porous structure is sufficiently obtained, and the strength of the obtained porous structure also tends to be improved, which is preferable.
[0023] The mass ratio of the content of the polymerizable compound X to the content of the porogen in the liquid composition X (polymerizable compound X:porogen) is preferably 1.0:0.4 to 1.0:19.0, more preferably 1.0:1.0 to 1.0:9.0, and even more preferably 1.0:1.5 to 1.0:4.0.
[0024] <Polymerization initiator> The polymerization initiator is a material capable of generating active species such as radicals and cations by energy such as light and heat, and initiating polymerization of the polymerizable compound X. As the polymerization initiator, known radical polymerization initiators, cationic polymerization initiators, base generators, etc. may be used alone or in combination of two or more kinds, and among them, it is preferable to use a photoradical polymerization initiator.
[0025] As the photoradical polymerization initiator, a photoradical generator can be used. For example, photoradical polymerization initiators such as Michler's ketone and benzophenone, known under the trade names Irgacure and Darocure, and more specific compounds include benzophenone and acetophenone derivatives, such as α-hydroxy- or α-aminocetophenone, 4-aroyl-1,3-dioxolane, benzil ketal, 2,2-diethoxyacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, and pp'-dichlorobenzo. Phen, pp'-bisdiethylaminobenzophenone, Michler's ketone, benzil, benzoin, benzil dimethyl ketal, tetramethylthiuram monosulfide, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, azobisisobutyronitrile, benzoin peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-one, 1-(4-isopropylphenyl)-2-hydroxy -2-Methylpropan-1-one, methylbenzoyl formate, benzoin isopropyl ether, benzoin methyl ether, benzoin ethyl ether, benzoin ether, benzoin isobutyl ether, benzoin n-butyl ether, benzoin n-propyl, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1 ,2-Diphenylethan-1-one, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Darocur 1173), bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one monoacylphosphine oxide, bisacylphosphine oxide or titanocene, fluorescene, anthraquinone, thioxanthone or xanthone, lophine dimer, trihalomethyl compounds or dihalomethyl compounds, active ester compounds, organic boron compounds, and the like are preferably used. Furthermore, a photocrosslinking radical generator such as a bisazide compound may be simultaneously contained. When polymerization is performed by heat alone, a thermal polymerization initiator such as azobisisobutyronitrile (AIBN), which is a typical radical generator, can be used.
[0026] In order to obtain a sufficient curing rate, the content of the polymerization initiator is preferably from 0.05% by mass to 10.0% by mass, and more preferably from 0.5% by mass to 5.0% by mass, when the total mass of the polymerizable compound X is taken as 100.0% by mass.
[0027] <Conditions for making resin X porous> Porous resin X, which is a porous body of resin X, is formed by polymerization-induced phase separation occurring in liquid composition X. Polymerization-induced phase separation refers to a state in which polymerizable compound X and porogen are compatible, but the polymer (resin X) generated in the process of polymerizing polymerizable compound X and porogen are not compatible (phase separation occurs). There are other methods for obtaining a porous body by phase separation, but by using the polymerization-induced phase separation method, a porous body having a network structure can be formed, and therefore a porous body with high resistance to chemicals and heat can be expected. In addition, compared to other methods, there are also advantages such as a shorter process time and easier surface modification.
[0028] Next, a process for forming porous resin X using polymerization-induced phase separation will be described. Polymerizable compound X undergoes a polymerization reaction by light irradiation or the like to form resin X. During this process, the solubility of porogen in the growing resin X decreases, and phase separation occurs between resin X and porogen. Finally, resin X forms a mesh-like porous structure in which porogen or the like fills the pores. When this is dried, porogen or the like is removed, and porous resin X remains. Therefore, in order to form porous resin X, conditions that represent the compatibility between polymerizable compound X and porogen, and conditions that represent the compatibility between resin X and porogen are examined.
[0029] -Conditions expressing compatibility between polymerizable compound X and porogen- An example of a condition indicating that the polymerizable compound X and the porogen are compatible with each other is that the transmittance of light at a wavelength of 550 nm of the liquid composition X is 30% or more when the liquid composition X is measured while stirring the liquid composition X. The measurement method for determining whether or not this condition is satisfied is as follows. First, liquid composition X is poured into a quartz cell, and while stirring at 300 rpm using a stirrer, the transmittance of light (visible light) at a wavelength of 550 nm through liquid composition X is measured. At this time, when the light transmittance is 30% or more, it is determined that the polymerizable compound X and the porogen are in a compatible state, and when it is less than 30%, it is determined that the polymerizable compound X and the porogen are in an incompatible state. The conditions for measuring the light transmittance are as follows. Quartz cell: Special microcell with screw cap (Product name: M25-UV-2) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Measure the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air. (Transmittance: 100%)
[0030] -Conditions expressing compatibility between resin X and porogen- An example of a condition indicating that the resin X and the porogen are not compatible (phase separation occurs) is that the increase rate of the haze value in a haze measurement element prepared using the liquid composition X is 1.0% or more. The measurement method for determining whether or not this condition is satisfied is as follows. First, resin particles are uniformly dispersed on a non-alkali glass substrate by spin coating to form a gap agent. Then, the substrate coated with the gap agent is bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Then, liquid composition X is filled between the bonded substrates by utilizing capillary action to prepare a "pre-UV haze measurement element". Next, the pre-UV haze measurement element is irradiated with UV light to harden the liquid composition X. Finally, the periphery of the substrate is sealed with a sealant to prepare a "haze measurement element". The various conditions during fabrication are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Amount of liquid composition filled: 160μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond) Next, the haze value (cloudiness) is measured using the prepared haze measuring element before UV irradiation and the haze measuring element. The measured value in the haze measuring element before UV irradiation is used as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measuring element relative to the measured value in the haze measuring element before UV irradiation is calculated. The haze value in the haze measuring element increases as the compatibility between the resin X formed by polymerization of the polymerizable compound X and the porogen decreases, and decreases as the compatibility increases. In addition, the higher the haze value, the easier it is for the resin X formed by polymerization of the polymerizable compound X to form a porous structure. At this time, when the increase rate of the haze value is 1.0% or more, it is determined that the resin X and the porogen are incompatible, and when it is less than 1.0%, it is determined that the resin X and the porogen are compatible. The apparatus used for the measurement is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0031] <Method of producing liquid composition X> The liquid composition X is preferably prepared through a process including a step of dissolving a polymerization initiator in a polymerizable compound X, a step of further dissolving a porogen and other components, and a step of stirring to obtain a homogeneous solution.
[0032] <Physical properties of liquid composition X> From the viewpoint of workability when applying liquid composition X, the viscosity of liquid composition X at 25°C is preferably 1.0 mPa·s or more and 150.0 mPa·s or less, more preferably 1.0 mPa·s or more and 30.0 mPa·s or less, and particularly preferably 1.0 mPa·s or more and 25.0 mPa·s or less. When the viscosity of liquid composition X is 1.0 mPa·s or more and 30.0 mPa·s or less, good ejection properties can be obtained even when liquid composition X is applied to an inkjet method. Here, the viscosity can be measured using, for example, a viscometer (device name: RE-550L, manufactured by Toki Sangyo Co., Ltd.) or the like.
[0033] <<Liquid composition Y>> The liquid composition Y is a liquid used in combination with the liquid composition X that forms the porous resin. The liquid composition Y is preferably used, for example, to suppress the diffusion of the liquid composition X and form the porous resin at a predetermined position. Specifically, for example, in the case of forming a porous resin on a porous substrate, the liquid composition Y is preferably applied to the porous substrate before the liquid composition X is applied, and is used to suppress the penetration of the liquid composition X into the porous substrate. By suppressing the penetration of the liquid composition X into the porous substrate, a part of the porous resin is formed in the porous substrate, and the deterioration of the function of the porous substrate can be suppressed.
[0034] Liquid composition Y contains solvent Y and other components as necessary. It is preferable that liquid composition Y does not form a porous resin when used alone (in other words, when not used together with liquid composition X). That is, it is preferable that liquid composition Y does not substantially contain a polymerizable compound. Note that "substantially does not contain a polymerizable compound" means that when the presence or absence of a polymerizable compound in liquid composition Y is confirmed by a method that is publicly known and is common technical knowledge in this technical field, no polymerizable compound can be detected.
[0035] <Solvent Y> The solvent Y is not particularly limited as long as it satisfies the specific requirements described below in the liquid composition Z consisting of the liquid composition X and the liquid composition Y. The solvent Y may be used alone or in combination of two or more kinds. In the present disclosure, unlike the solvent X, the solvent Y is not called a porogen.
[0036] The boiling point of the solvent Y alone or the boiling point of the solvent Y in combination is preferably 50°C or more and 250°C or less, more preferably 70°C or more and 200°C or less, at normal pressure. By having a boiling point of 50°C or more, the evaporation of the solvent Y at around room temperature is suppressed, making the liquid composition Y easy to handle, and the content of the solvent Y in the liquid composition Y easy to control. In addition, by having a boiling point of 250°C or less, the time required for the step of drying the solvent Y after the porous resin is formed is shortened, improving productivity. In addition, since the amount of the solvent Y remaining inside the porous resin can be suppressed, the quality is improved when the porous resin is used as a functional layer such as a material separation layer that separates substances or a reaction layer as a reaction field. The boiling point of the solvent Y alone or in the case of using two or more kinds in combination is preferably 120° C. or higher at normal pressure.
[0037] Examples of the solvent Y include ethylene glycols such as ethylene glycol monobutyl ether, ketones such as cyclohexanone, esters such as diethyl carbonate, amides such as NN dimethylacetamide, etc. Also included are liquids such as ethanol and 1,3-butanediol. In the present disclosure, the above-mentioned exemplified liquids do not necessarily correspond to the solvent Y. As described above, the solvent Y in the present disclosure is a liquid that satisfies the specific requirements described below in the liquid composition Z consisting of the liquid composition X and the liquid composition Y.
[0038] The content of the solvent Y in the liquid composition Y is preferably 60.0 mass% or more, more preferably 70.0 mass% or more, still more preferably 80.0 mass% or more, and particularly preferably 90.0 mass% or more, based on the total amount of the liquid composition Y. In addition, the total amount of the liquid composition Y (100 mass%) may be the solvent Y.
[0039] <Physical Properties of Liquid Composition Y> From the viewpoint of workability when applying the liquid composition Y, the viscosity of the liquid composition Y at 25°C is preferably from 1.0 mPa·s to 150.0 mPa·s, more preferably from 1.0 mPa·s to 30.0 mPa·s, and particularly preferably from 1.0 mPa·s to 25.0 mPa·s. When the viscosity of the liquid composition Y is from 1.0 mPa·s to 30.0 mPa·s, good ejection properties can be obtained even when the liquid composition Y is applied to an inkjet method. Here, the viscosity can be measured using, for example, a viscometer (device name: RE-550L, manufactured by Toki Sangyo Co., Ltd.) or the like.
[0040] <<Liquid composition Z>> Liquid composition Z is a liquid used in a test to present conditions under which the resin formed in the contact area between liquid composition X and liquid composition Y is excellent in terms of porosity even when liquid composition X and liquid composition Y come into contact with each other. Thus, liquid composition Z itself is different from liquid composition X and liquid composition Y and is not a component of the liquid composition set.
[0041] Liquid composition Z is a liquid consisting of a mixture of 10.0 mass % of liquid composition X and 90.0 mass % of liquid composition Y. Thus, liquid composition Z contains components derived from liquid composition X, such as polymerizable compound X, solvent X, and a polymerization initiator, and components derived from liquid composition Y, such as solvent Y. In the present disclosure, the polymerizable compound contained in the liquid composition Z is referred to as the polymerizable compound Z, and the solvent contained in the liquid composition Z is referred to as the solvent Z. That is, the polymerizable compound Z represents the polymerizable compound X, etc., and the solvent Z represents the solvent X and the solvent Y, etc.
[0042] First, the reason for conducting a test using liquid composition Z to present conditions under which the resin formed in the contact region between liquid composition X and liquid composition Y is excellent in terms of porosity will be described. By using liquid composition X and liquid composition Y in combination, when liquid composition X and liquid composition Y come into contact with each other, liquid composition X and liquid composition Y are partially mixed in the contact area (near the interface between liquid composition X and liquid composition Y), and a concentration gradient of liquid composition X and liquid composition Y is generated. In order to be able to form a porous resin using polymerizable compound X contained in liquid composition X as a material even in the contact area where this concentration gradient occurs, it is sufficient to specify the conditions for forming a porous resin even when the concentration of the component derived from liquid composition X is low and the concentration of the component derived from liquid composition Y is high. Therefore, the conditions for forming a porous resin in liquid composition Z consisting of 10.0 mass% liquid composition X and 90.0 mass% liquid composition Y are described in detail below. In the following description, the resin formed when liquid composition Z is used is referred to as resin Z, and the porous body of resin Z is referred to as porous resin Z.
[0043] <Conditions for making resin Z porous> Porous resin Z, which is a porous body of resin Z, is formed by polymerization-induced phase separation that occurs in liquid composition Z. Polymerization-induced phase separation refers to a state in which polymerizable compound Z and solvent Z are compatible with each other, but the polymer (resin Z) generated in the process of polymerization of polymerizable compound Z is not compatible with solvent Z (phase separation occurs).
[0044] Next, a process for forming the porous resin Z using polymerization-induced phase separation will be described. The polymerizable compound Z undergoes a polymerization reaction by light irradiation or the like to form the resin Z. During this process, the solubility of the growing resin Z in the solvent Z decreases, and phase separation occurs between the resin Z and the solvent Z. Finally, the resin Z forms a mesh-like porous structure in which the pores are filled with the solvent Z or the like. When this is dried, the solvent Z or the like is removed, and the porous resin Z remains. Therefore, in order to form the porous resin Z, conditions that represent the compatibility between the polymerizable compound Z and the solvent Z, and conditions that represent the compatibility between the resin Z and the solvent Z are examined.
[0045] -Conditions expressing compatibility between polymerizable compound Z and solvent Z- An example of a condition indicating that the polymerizable compound Z and the solvent Z are compatible with each other is that the transmittance of the liquid composition Z at a wavelength of 550 nm measured while stirring the liquid composition Z is 30% or more. The measurement method for determining whether or not this condition is satisfied is as follows. First, liquid composition Z is poured into a quartz cell, and while stirring at 300 rpm with a stirrer, the transmittance of light (visible light) at a wavelength of 550 nm of liquid composition Z is measured. At this time, when the light transmittance is 30% or more, it is determined that polymerizable compound Z and solvent Z are in a compatible state, and when it is less than 30%, it is determined that polymerizable compound Z and solvent Z are in an incompatible state. The conditions for measuring the light transmittance are as follows. Quartz cell: Special microcell with screw cap (Product name: M25-UV-2) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Measure the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air. (Transmittance: 100%)
[0046] -Conditions expressing compatibility between resin Z and solvent Z- An example of a condition indicating that the resin Z and the solvent Z are not compatible (phase separation occurs) is that the increase rate of the haze value in a haze measurement element prepared using the liquid composition Z is 1.0% or more. The measurement method for determining whether or not this condition is satisfied is as follows. First, resin particles are uniformly dispersed on a non-alkali glass substrate by spin coating to form a gap agent. Next, the substrate coated with the gap agent is bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Then, liquid composition Z is filled between the bonded substrates by utilizing capillary action to prepare a "pre-UV haze measurement element". Next, the pre-UV haze measurement element is irradiated with UV light to harden the liquid composition Z. Finally, the periphery of the substrate is sealed with a sealant to prepare a "haze measurement element". The various conditions during fabrication are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Amount of liquid composition Z filled: 160μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond) Next, the haze value (cloudiness) is measured using the prepared haze measurement element and haze measurement element before UV irradiation. The measured value in the haze measurement element before UV irradiation is used as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation is calculated. The haze value in the haze measurement element increases as the compatibility between the resin Z formed by polymerization of the polymerizable compound Z and the solvent Z decreases, and decreases as the compatibility increases. In addition, the higher the haze value, the easier it is for the resin Z formed by polymerization of the polymerizable compound Z to form a porous structure. At this time, when the increase rate of the haze value is 1.0% or more, it is determined that the resin Z and the solvent Z are incompatible, and when it is less than 1.0%, it is determined that the resin Z and the solvent Z are compatible. The apparatus used for the measurement is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0047] <Method for providing conditions for making resin Z porous> An example of a method satisfying the conditions for making the resin Z porous will be described. In order to form the porous resin Z, as described above, it is required that the compatibility between the polymerizable compound Z and the solvent Z is high and the compatibility between the resin Z and the solvent Z is low. This compatibility can be predicted through the Hansen solubility parameter (HSP), and therefore the Hansen solubility parameter (HSP) will be described.
[0048] -Hansen Solubility Parameter (HSP)- Hansen Solubility Parameter (HSP) is a useful tool for predicting the compatibility of two substances, and was discovered by Charles M. Hansen. Hansen Solubility Parameter (HSP) is expressed by combining the following three parameters (δD, δP, and δH) derived experimentally and theoretically. The unit of Hansen Solubility Parameter (HSP) is MPa. 0.5 or (J / cm 3 ) 0.5 In this disclosure, (J / cm 3 ) 0.5 was used. · δD: Energy resulting from London dispersion forces. · δP: Energy resulting from dipole-dipole interactions. · δH: Energy derived from hydrogen bonding forces. Hansen Solubility Parameter (HSP) is a vector quantity expressed as (δD, δP, δH) and is plotted in a three-dimensional space (Hansen space) with three parameters as coordinate axes. The Hansen Solubility Parameter (HSP) of commonly used substances is available from publicly known information sources such as databases, so the Hansen Solubility Parameter (HSP) of a desired substance can be obtained, for example, by referring to the database. For substances whose Hansen Solubility Parameter (HSP) is not registered in the database, the Hansen Solubility Parameter (HSP) can be calculated from the chemical structure of the substance or the Hansen Solubility Sphere method described below, for example, by using computer software such as Hansen Solubility Parameters in Practice (HSPiP). The Hansen Solubility Parameter (HSP) of a mixture containing two or more substances is calculated as the vector sum of the Hansen Solubility Parameter (HSP) of each substance multiplied by the volume ratio of each substance to the entire mixture. In this disclosure, the Hansen Solubility Parameter (HSP) of solvent Z obtained based on a publicly known information source such as a database is referred to as the "Hansen Solubility Parameter of the solvent." In addition, the relative energy difference (RED) based on the Hansen solubility parameters (HSP) of a solute and a solution is expressed by the following formula:
number
[0049] -Hansen dissolving ball method- First, the substance for which Ro is to be calculated and several dozen evaluation solvents with known Hansen Solubility Parameters (HSP) are prepared, and a compatibility test of the target substance with each evaluation solvent is performed. In the compatibility test, the Hansen Solubility Parameters (HSP) of the evaluation solvents that showed compatibility and the Hansen Solubility Parameters (HSP) of the evaluation solvents that showed no compatibility are each plotted in Hansen space. Based on the plotted Hansen Solubility Parameters (HSP) of each evaluation solvent, a virtual sphere (Hansen sphere) is created in Hansen space that includes the Hansen Solubility Parameters (HSP) of the evaluation solvents that showed compatibility, but does not include the Hansen Solubility Parameters (HSP) of the evaluation solvents that showed no compatibility. The radius of the Hansen sphere is the interaction radius R of the substance. 0 The center is the Hansen solubility parameter (HSP) of the substance. Note that the interaction radius R 0 The evaluation criteria for compatibility (criteria for determining whether or not compatibility exists) between a substance for which the Hansen Solubility Parameter (HSP) is to be calculated and a solvent for evaluation whose Hansen Solubility Parameter (HSP) is known is set by the evaluator himself. The evaluation criteria in this disclosure will be described later.
[0050] -Hansen solubility parameter (HSP) and interaction radius of polymerizable compound Z- The Hansen solubility parameter (HSP) of the polymerizable compound Z in the present disclosure and the interaction radius of the polymerizable compound Z are determined by the Hansen dissolved ball method. As described above, the evaluation criteria for compatibility in the Hansen dissolved ball method are set by the evaluator himself, so the Hansen solubility parameter (HSP) of the polymerizable compound Z in the present disclosure obtained by the following criteria is represented as the "Hansen solubility parameter C of the polymerizable compound Z", and the interaction radius of the polymerizable compound Z is represented as the "interaction radius D of the polymerizable compound Z". In other words, the "Hansen solubility parameter C of the polymerizable compound Z" and the "interaction radius D of the polymerizable compound Z" are obtained based on the Hansen solubility parameter C of the polymerizable compound Z" and the "interaction radius D of the polymerizable compound Z", unlike the "Hansen solubility parameter of the solvent Z" obtained based on a publicly known information source such as a database, and are obtained based on the Hansen dissolved ball method including the evaluation criteria for compatibility set by the evaluator himself.
[0051] The Hansen solubility parameter C of the polymerizable compound Z and the interaction radius D of the polymerizable compound Z are determined by evaluating the compatibility of the polymerizable compound Z with the evaluation solvent (based on the "transmittance of light at a wavelength of 550 nm of a transmittance measurement composition, which is measured while stirring a transmittance measurement composition containing the polymerizable compound Z and the evaluation solvent") in accordance with the following [1-1] and [1-2].
[0052] [1-1] Preparation of composition for transmittance measurement First, prepare the polymerizable compound Z for which the Hansen solubility parameter (HSP) is to be calculated and several dozens of evaluation solvents with known Hansen solubility parameters (HSP), and mix the polymerizable compound Z, each evaluation solvent, and polymerization initiator in the ratio shown below to prepare a composition for transmittance measurement. As several dozens of evaluation solvents with known Hansen solubility parameters (HSP), the following 21 evaluation solvents are used. ~Composition ratio for transmittance measurement~ Polymerizable compound Z for which Hansen solubility parameter (HSP) is to be calculated: 28.0% by mass Solvent for evaluation with known Hansen Solubility Parameters (HSP): 70.0% by mass Polymerization initiator (Irgacure 819, manufactured by BASF): 2.0% by mass ~Solvents for evaluation (21 types)~ Ethanol, 2-propanol, mesitylene, dipropylene glycol monomethyl ether, N-methyl 2-pyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, propylene carbonate, ethyl acetate, tetrahydrofuran, acetone, n-tetradecane, ethylene glycol, diethylene glycol monobutyl ether, diethylene glycol butyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 2-ethylhexanol, diisobutyl ketone, benzyl alcohol, 1-bromonaphthalene
[0053] [1-2] Measurement of light transmittance The prepared composition for transmittance measurement is poured into a quartz cell, and the transmittance of the composition for transmittance measurement at a wavelength of 550 nm (visible light) is measured while stirring with a stirrer at 300 rpm. In the present disclosure, a light transmittance of 30% or more is determined to be a compatible state between the polymerizable compound Z and the evaluation solvent, and a light transmittance of less than 30% is determined to be a non-compatible state between the polymerizable compound Z and the evaluation solvent. The conditions for measuring the light transmittance are as follows. Quartz cell: Special microcell with screw cap (Product name: M25-UV-2) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Measure the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air. (Transmittance: 100%)
[0054] -Hansen solubility parameter (HSP) and interaction radius of resin Z formed by polymerization of polymerizable compound Z- The Hansen solubility parameter (HSP) of the resin Z formed by polymerization of the polymerizable compound Z in the present disclosure and the interaction radius of the resin Z formed by polymerization of the polymerizable compound Z are determined by the Hansen dissolved ball method. As described above, the evaluation criteria for compatibility in the Hansen dissolved ball method are set by the evaluator himself, so the Hansen solubility parameter (HSP) of the resin Z formed by polymerization of the polymerizable compound Z in the present disclosure obtained by the following criteria is represented as the "Hansen solubility parameter A of the resin Z", and the interaction radius of the resin Z formed by polymerization of the polymerizable compound Z is represented as the "interaction radius B of the resin Z". In other words, the "Hansen solubility parameter A of the resin Z" and the "interaction radius B of the resin Z" are obtained based on the Hansen solubility parameter of the solvent Z" obtained based on a publicly known information source such as a database, and are obtained based on the Hansen dissolved ball method including the evaluation criteria for compatibility set by the evaluator himself.
[0055] The Hansen solubility parameter A of the resin Z and the interaction radius B of the resin Z are determined by evaluating the compatibility of the resin Z with the evaluation solvent (based on the "rate of increase in the haze value (cloudiness) in a haze measurement element prepared using a haze measurement composition containing the polymerizable compound Z and the evaluation solvent") in accordance with the following [2-1], [2-2], and [2-3].
[0056] [2-1] Preparation of composition for haze measurement First, prepare a precursor of resin Z (polymerizable compound Z) for which the Hansen solubility parameter (HSP) is to be calculated, and several dozen types of evaluation solvents with known Hansen solubility parameters (HSP), and mix polymerizable compound Z, each evaluation solvent, and a polymerization initiator in the ratio shown below to prepare a composition for haze measurement. As several dozen types of evaluation solvents with known Hansen solubility parameters (HSP), the 21 types of evaluation solvents shown below are used. ~Composition ratio for haze measurement~ Precursor of resin Z (polymerizable compound Z) for which you want to calculate the Hansen solubility parameter (HSP): 28.0% by mass Solvent for evaluation with known Hansen Solubility Parameters (HSP): 70.0% by mass Polymerization initiator (Irgacure 819, manufactured by BASF): 2.0% by mass ~Solvents for evaluation (21 types)~ Ethanol, 2-propanol, mesitylene, dipropylene glycol monomethyl ether, N-methyl 2-pyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, propylene carbonate, ethyl acetate, tetrahydrofuran, acetone, n-tetradecane, ethylene glycol, diethylene glycol monobutyl ether, diethylene glycol butyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 2-ethylhexanol, diisobutyl ketone, benzyl alcohol, 1-bromonaphthalene
[0057] [2-2] Preparation of element for haze measurement Resin particles are uniformly dispersed on a non-alkali glass substrate by spin coating to form a gap agent. Next, the substrate coated with the gap agent is bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Next, the haze measurement composition prepared in [2-1] is filled between the bonded substrates by utilizing capillary action to prepare a "pre-UV haze measurement element". Next, the pre-UV haze measurement element is irradiated with UV light to harden the haze measurement composition. Finally, the periphery of the substrate is sealed with a sealant to prepare a "haze measurement element". The various conditions during fabrication are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Amount of haze measurement composition filled: 160μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond)
[0058] [2-3] Haze value (cloudiness) measurement The haze value (cloudiness) is measured using the prepared haze measurement element and haze measurement element before UV irradiation. The measured value in the haze measurement element before UV irradiation is used as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation is calculated. The haze value in the haze measurement element increases as the compatibility between the resin Z formed by polymerization of the polymerizable compound Z and the evaluation solvent decreases, and decreases as the compatibility increases. In addition, the higher the haze value, the easier it is for the resin Z formed by polymerization of the polymerizable compound Z to form a porous structure. In the present disclosure, when the increase rate of the haze value is 1.0% or more, it is determined that the resin Z and the evaluation solvent are incompatible, and when it is less than 1.0%, it is determined that the resin Z and the evaluation solvent are compatible. The apparatus used for the measurement is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0059] -Relative energy difference (RED) based on Hansen solubility parameters (HSP) between resin Z and solvent Z- As described above, the relative energy difference (RED) calculated based on the Hansen solubility parameter A of the resin Z formed by polymerization of the polymerizable compound Z, which is determined based on the rate of increase in the haze value (cloudiness) in a haze measurement element prepared using a haze measurement composition containing the polymerizable compound Z and an evaluation solvent, the interaction radius B of the resin Z, and the Hansen solubility parameter of the solvent Z according to the following formula 1 is preferably 1.00 or more, more preferably 1.10 or more, even more preferably 1.20 or more, and particularly preferably 1.30 or more.
number
[0060] -Relative energy difference (RED) based on Hansen solubility parameters (HSP) between polymerizable compound Z and solvent Z- As described above, the Hansen solubility parameter C of the polymerizable compound Z, which is determined based on the transmittance of light at a wavelength of 550 nm of the transmittance measurement composition containing the polymerizable compound Z and the evaluation solvent, measured while stirring the transmittance measurement composition containing the polymerizable compound Z and the evaluation solvent, the interaction radius D of the polymerizable compound Z, which is determined based on the compatibility of the polymerizable compound Z with the evaluation solvent, and the Hansen solubility parameter of the solvent Z, are calculated based on the following formula 2. The relative energy difference (RED) is preferably 1.05 or less, more preferably 0.90 or less, even more preferably 0.80 or less, and particularly preferably 0.70 or less.
number
[0061] [Porous resin manufacturing equipment, porous resin manufacturing method] FIG. 1 is a schematic diagram showing an example of a porous resin production apparatus for implementing the porous resin production method of the present disclosure.
[0062] <<Porous resin manufacturing equipment>> The porous resin manufacturing apparatus 100 is an apparatus for manufacturing a porous resin using the above-mentioned liquid composition X and liquid composition Y. The porous resin manufacturing apparatus 100 includes a printing process section 10 including a process of applying liquid composition X and liquid composition Y, respectively, onto a printing substrate 4 to form a layer of liquid composition X and a layer of liquid composition Y, a polymerization process section 20 including a polymerization process of activating a polymerization initiator in the layer of liquid composition X to polymerize a polymerizable compound to obtain a porous resin precursor 6, and a heating process section 30 including a heating process of heating the porous resin precursor 6 to obtain a porous resin. The porous resin manufacturing apparatus 100 includes a conveying section 5 for conveying the printing substrate 4, and the conveying section 5 conveys the printing substrate 4 at a preset speed in the order of the printing process section 10, the polymerization process section 20, and the heating process section 30.
[0063] <Printing process department> The printing process section 10 includes a printing device 1a, which is an example of an application means for realizing an application step of applying liquid composition X and liquid composition Y onto the printing substrate 4, a storage container 1b for storing liquid composition X and liquid composition Y, respectively, and a supply tube 1c for supplying liquid composition X and liquid composition Y stored in storage container 1b to the printing device 1a. Among the application means, a means for applying liquid composition X is referred to as application means X, and a means for applying liquid composition Y is referred to as application means Y. Among the application steps, a step of applying liquid composition X is referred to as application step X, and a step of applying liquid composition Y is referred to as application step Y.
[0064] The storage container 1b stores liquid composition X and liquid composition Y, respectively (in FIG. 1, liquid composition X and liquid composition Y are simply indicated as liquid composition 7), and the printing process unit 10 ejects liquid composition X and liquid composition Y, respectively, from the printing device 1a and applies liquid composition X and liquid composition Y, respectively, onto the printing substrate 4 to form a layer of liquid composition X and a layer of liquid composition Y in the form of a thin film. At this time, the order of the application process X and the application process Y in the present disclosure is such that the application process Y is performed first, and the application process X is performed afterwards. However, when the application process Y is performed first, it is preferable that in the application process X, liquid composition X is applied so as to at least partially overlap the area where liquid composition Y is applied. The storage container 1b may be integrated with the porous resin manufacturing apparatus 100, or may be removable from the porous resin manufacturing apparatus 100. Also, the storage container 1b may be a container used for adding to a storage container integrated with the porous resin manufacturing apparatus 100 or a storage container removable from the porous resin manufacturing apparatus 100.
[0065] The printing device 1a is not particularly limited as long as it can apply liquid composition X and liquid composition Y, and any printing device suitable for various printing methods such as spin coating, casting, microgravure coating, gravure coating, bar coating, roll coating, wire bar coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing can be used.
[0066] The container 1b and the supply tube 1c can be selected arbitrarily as long as they can stably store and supply the liquid compositions X and Y, respectively. The materials constituting the container 1b and the supply tube 1c preferably have a light-shielding property in the relatively short wavelength region of ultraviolet and visible light. This prevents the liquid composition X from being polymerized by external light.
[0067] <Polymerization process section> 1, the polymerization process section 20 has a light irradiation device 2a, which is an example of a curing means for realizing a curing process in which the liquid composition is cured by irradiating it with active energy rays such as heat or light, and a polymerization inert gas circulation device 2b for circulating a polymerization inert gas. The light irradiation device 2a irradiates the layer of liquid composition X and the layer of liquid composition Y formed by the printing process section 10 with light in the presence of a polymerization inert gas, thereby initiating photopolymerization in the layer of liquid composition X to obtain a porous resin precursor 6.
[0068] The light irradiation device 2a is appropriately selected according to the absorption wavelength of the photopolymerization initiator, and is not particularly limited as long as it can initiate and advance the polymerization of the polymerizable compound in the layer of the liquid composition X, and examples of such light irradiation device include ultraviolet light sources such as high-pressure mercury lamps, metal halide lamps, hot cathode tubes, cold cathode tubes, and LEDs. However, since light with a shorter wavelength generally tends to reach deeper parts, it is preferable to select a light source according to the thickness of the porous film to be formed.
[0069] Regarding the irradiation intensity of the light source of the light irradiation device 2a, if the irradiation intensity is too strong, polymerization will proceed rapidly before phase separation has sufficiently occurred, and it will be difficult to obtain a porous structure. On the other hand, if the irradiation intensity is too weak, phase separation will proceed to a microscale or greater, and porosity will tend to vary and become coarse. In addition, the irradiation time will be long, and productivity will tend to decrease. For this reason, the irradiation intensity is set to 10 mW / cm 2 More than 1W / cm 2 Less than 30mW / cm is preferable. 2 More than 300mW / cm 2 The following is more preferred:
[0070] Next, the polymerization inert gas circulation device 2b plays a role of lowering the concentration of polymerization active oxygen contained in the atmosphere, and allowing the polymerization reaction of the polymerizable compound X near the surface of the layer of the liquid composition X to proceed without being hindered. Therefore, the polymerization inert gas used is not particularly limited as long as it satisfies the above-mentioned functions, and examples thereof include nitrogen, carbon dioxide, and argon.
[0071] In addition, the flow rate is set to O, taking into consideration the effect of effectively reducing inhibition. 2 The concentration is preferably less than 20% (an environment with a lower oxygen concentration than the atmosphere), more preferably 0% to 15%, and even more preferably 0% to 5%. In addition, the polymerization inert gas circulation device 2b is preferably provided with a temperature control means capable of controlling the temperature in order to realize stable polymerization progress conditions.
[0072] <Heating process section> 1, the heating process section 30 has a heating device 3a and includes a solvent removal step of heating and drying and removing the solvent X and solvent Y remaining in the porous resin precursor 6 formed in the polymerization process section 20 by the heating device 3a. This makes it possible to form a porous resin. The heating process section 30 may perform the solvent removal step under reduced pressure.
[0073] The heating process section 30 also includes a polymerization promotion step in which the porous membrane precursor 6 is heated by the heating device 3a to further promote the polymerization reaction carried out in the polymerization process section 20, and an initiator removal step in which the photopolymerization initiator remaining in the porous membrane precursor 6 is heated by the heating device 3a, dried, and removed. Note that the polymerization promotion step and the initiator removal step may be carried out before or after the solvent removal step, rather than simultaneously with the solvent removal step.
[0074] Furthermore, the heating process section 30 includes a polymerization completion process of heating the porous material under reduced pressure after the solvent removal process. The heating device 3a is not particularly limited as long as it satisfies the above-mentioned functions, and examples thereof include an IR heater and a hot air heater.
[0075] The heating temperature and time can be appropriately selected depending on the boiling points of the solvent X and the solvent Y contained in the porous film precursor 6 and the thickness of the formed film.
[0076] <Printing base material> Any material, whether transparent or opaque, can be used for the printing substrate 4. In other words, various substrates can be used, such as glass substrates, resin film substrates such as various plastic films, and composite substrates thereof, as transparent substrates, and silicon substrates, metal substrates such as stainless steel, and laminates of these, as opaque substrates. The printing substrate 4 may be a recording medium such as plain paper, glossy paper, special paper, or cloth. The recording medium may also be a low-permeability substrate (low-absorbency substrate). A low-permeability substrate means a substrate having a surface with low water permeability, absorbency, or adsorption, and includes materials that have many cavities inside but are not open to the outside. Examples of low-permeability substrates include coated paper used in commercial printing and recording media such as paperboard coated with recycled paper pulp in the middle and back layers. As described above, the printing substrate 4 is preferably a porous substrate. This is because the effects of the present invention become more pronounced when the substrate is a porous substrate. Specific examples of the porous substrate include an active material layer used in an electricity storage element, and a porous sheet used as an insulating layer in an electricity storage element or a power generation element.
[0077] In addition, as for the shape, any substrate that can be used in the printing process section 10 and the polymerization process section 20 may be used, regardless of whether it has a curved surface or an uneven surface.
[0078] [Porous resin] The film thickness of the porous resin formed by the liquid composition set is not particularly limited, but is preferably 0.01 μm or more and 500 μm or less in consideration of the uniformity of hardening during polymerization, more preferably 0.01 μm or more and 100 μm or less, even more preferably 1 μm or more and 50 μm or less, and particularly preferably 10 μm or more and 20 μm or less. By having a film thickness of 0.01 μm or more, the surface area of the obtained porous resin is increased, and the function of the porous resin can be fully obtained. In addition, by having a film thickness of 500 μm or less, unevenness of light and heat used during polymerization in the film thickness direction is suppressed, and a uniform porous resin can be obtained in the film thickness direction. By producing a uniform porous resin in the film thickness direction, the structural unevenness of the porous resin can be suppressed, and the decrease in permeability of liquids and gases can be suppressed. The film thickness of the porous resin is appropriately adjusted according to the application in which the porous resin is used. For example, when the porous resin is used as an insulating layer for a storage element, it is preferable that the film thickness is 10 μm or more and 20 μm or less. The porous resin formed is not particularly limited, but from the viewpoint of ensuring good permeability of liquids and gases, it is preferable that the porous resin has a three-dimensional branched network structure of the cured resin as a skeleton and has a co-continuous structure (also called a monolith structure) in which a plurality of pores in the porous resin are continuously connected. That is, it is preferable that the porous resin has a large number of pores, and each pore has a connectivity with other pores around it and spreads three-dimensionally. When the pores are connected to each other, the penetration of liquids and gases occurs sufficiently, and functions such as substance separation and reaction field can be efficiently expressed. One of the physical properties obtained by having a bicontinuous structure is air permeability. The air permeability of the porous resin is measured, for example, in accordance with JIS P8117, and is preferably 500 seconds / 100 mL or less, and more preferably 300 seconds / 100 mL or less. In this case, the air permeability is measured, for example, using a Gurley densometer (manufactured by Toyo Seiki Seisakusho). The cross-sectional shape of the pores in the porous resin formed may be various shapes and sizes, such as a substantially circular shape, a substantially elliptical shape, a substantially polygonal shape, etc. Here, the size of the pores refers to the length of the longest part in the cross-sectional shape. The size of the pores can be obtained from a cross-sectional photograph taken with a scanning electron microscope (SEM). The size of the pores in the porous resin is not particularly limited, but is preferably 0.01 μm or more and 10 μm or less from the viewpoint of the permeability of liquids and gases. In addition, the porosity of the porous resin is preferably 30% or more, and more preferably 50% or more. The method for adjusting the size and porosity of the pores in the porous resin to these ranges is not particularly limited, but examples thereof include a method of adjusting the content of the polymerizable compound X in the liquid composition X, a method of adjusting the content of the porogen in the liquid composition X, and a method of adjusting the irradiation conditions of the active energy rays.
[0079] <<Applications of porous resin>>
[0080] <For use as an energy storage element or power generation element> The porous resin formed using the liquid composition set of the present disclosure can be used, for example, as an insulating layer for an electricity storage element or a power generating element. In other words, the liquid composition set of the present disclosure can be used as a liquid composition set for producing an insulating layer in an electricity storage element or a power generating element. When used for these applications, it is preferable to form an insulating layer (separator) by, for example, applying liquid composition Y and liquid composition X in that order onto an active material layer previously formed on an electrode substrate. As an insulating layer for an electric storage element or a power generating element, for example, a film-like porous insulating layer having a predetermined size of pores or porosity is known to be used. On the other hand, when the liquid composition set of the present disclosure is used, the pores or porosity can be appropriately changed by appropriately adjusting the content of the polymerizable compound X, the content of the porogen, the irradiation conditions of the active energy rays, etc., and the design freedom in terms of the performance of the electric storage element and the power generating element can be improved. In addition, since the liquid composition set of the present disclosure can be applied in various application methods, for example, it can be applied by an inkjet method, and the design freedom in terms of the shape of the electric storage element and the power generating element can be improved. In addition, since the liquid composition set of the present disclosure applies the liquid composition X to the region of the active material layer to which the liquid composition Y is applied, the porous resin formed by the curing of the liquid composition X is formed without excessively penetrating into the active material layer. This suppresses the deterioration of the function of the active material layer. In addition, since the resin formed in the contact region of the liquid composition X and the liquid composition Y is excellently porous, the deterioration of the function of the insulating layer (separator) is also suppressed. The insulating layer is a member that separates the positive electrode from the negative electrode and ensures ion conductivity between the positive electrode and the negative electrode. In the present application, the insulating layer is not limited to a layered shape. The liquid composition set of the present disclosure can be applied onto an insulating layer (first insulating layer) for an electricity storage element or a power generation element to additionally form an insulating layer (second insulating layer) made of a porous resin layer. By forming the second insulating layer on the first insulating layer, various functions such as heat resistance, impact resistance, and high-temperature shrinkage resistance of the insulating layer as a whole can be added or improved.
[0081] The electrode substrate is not particularly limited as long as it is a conductive substrate, and generally, aluminum foil, copper foil, stainless steel foil, titanium foil, and etched foils made by etching them to make fine holes, which are suitable for use in secondary batteries and capacitors, which are electric storage devices, and especially lithium ion secondary batteries, as well as perforated electrode substrates used in lithium ion capacitors, are used. In addition, carbon paper fibrous electrodes used in power generation devices such as fuel cells that have been made flat in a non-woven or woven form, and the above-mentioned perforated electrode substrates with fine holes can also be used. Furthermore, in the case of solar devices, in addition to the above-mentioned electrodes, a transparent semiconductor thin film such as indium-titanium oxide or zinc oxide can be formed on a flat substrate such as glass or plastic, or a conductive electrode film can be thinly evaporated on the substrate.
[0082] The active material layer is formed by dispersing a powdered active material or catalyst composition in a liquid, applying the liquid onto the electrode substrate, fixing the liquid, and drying the liquid. Usually, printing using a spray, dispenser, die coater, or pull-up coating is used, and the active material layer is formed by applying the liquid and then drying the liquid.
[0083] The positive electrode active material is not particularly limited as long as it is a material that can reversibly absorb and release alkali metal ions. Typically, an alkali metal-containing transition metal compound can be used as the positive electrode active material. For example, a lithium-containing transition metal compound can be a composite oxide containing lithium and at least one element selected from the group consisting of cobalt, manganese, nickel, chromium, iron, and vanadium. For example, lithium-containing transition metal oxides such as lithium cobalt oxide, lithium nickel oxide, and lithium manganate, LiFePO 4Examples of the lithium-containing transition metal oxide include olivine-type lithium salts such as titanium disulfide and molybdenum disulfide, chalcogen compounds such as manganese dioxide, etc. The lithium-containing transition metal oxide is a metal oxide containing lithium and a transition metal, or a metal oxide in which a part of the transition metal in the metal oxide is replaced by a different element. Examples of the different elements include Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, etc., and among them, Mn, Al, Co, Ni, and Mg are preferable. The different elements may be one type or two or more types. These positive electrode active materials can be used alone or in combination of two or more types. Examples of the active materials in nickel-metal hydride batteries include nickel hydroxide, etc.
[0084] The negative electrode active material is not particularly limited as long as it is a material that can reversibly absorb and release alkali metal ions. Typically, a carbon material containing graphite having a graphite crystal structure can be used as the negative electrode active material. Examples of such carbon materials include natural graphite, spherical or fibrous artificial graphite, non-graphitizable carbon (hard carbon), and graphitizable carbon (soft carbon). Examples of materials other than carbon materials include lithium titanate. In addition, from the viewpoint of increasing the energy density of a lithium ion battery, high-capacity materials such as silicon, tin, silicon alloys, tin alloys, silicon oxide, silicon nitride, and tin oxide can also be suitably used as the negative electrode active material.
[0085] As the active material in the nickel-metal hydride battery, the hydrogen storage alloy may be, for example, an AB2-based or A2B-based hydrogen storage alloy.
[0086] For example, PVDF, PTFE, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylic acid methyl ester, polyacrylic acid ethyl ester, polyacrylic acid hexyl ester, polymethacrylic acid, polymethacrylic acid methyl ester, polymethacrylic acid ethyl ester, polymethacrylic acid hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene butadiene rubber, carboxymethyl cellulose, etc. can be used as the binder for the positive electrode or the negative electrode. In addition, a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene may be used. In addition, two or more materials selected from these may be mixed and used. Examples of the conductive agent contained in the electrode include graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fiber and metal fiber, metal powders such as carbon fluoride and aluminum, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and organic conductive materials such as phenylene derivatives and graphene derivatives.
[0087] In general, the active material in a fuel cell is a catalyst for the cathode electrode or the anode electrode, in which metal particles such as platinum, ruthenium, or a platinum alloy are supported on a catalyst carrier such as carbon. To support catalyst particles on the surface of a catalyst carrier, for example, the catalyst carrier is suspended in water, and a precursor of the catalyst particle (containing alloy components such as chloroplatinic acid, dinitrodiamino platinum, platinic chloride, platinous chloride, bisacetylacetonato platinum, dichlorodiammine platinum, dichlorotetramine platinum, platinic sulfate chlororuthenic acid, chloroiridic acid, chlororhodium acid, ferric chloride, cobalt chloride, chromium chloride, gold chloride, silver nitrate, rhodium nitrate, palladium chloride, nickel nitrate, iron sulfate, and copper chloride) is added and dissolved in the suspension, and an alkali is added to generate a hydroxide of the metal and obtain a catalyst carrier supported on the surface of the catalyst carrier. Such a catalyst carrier is applied to an electrode and reduced under a hydrogen atmosphere, etc., to obtain an electrode with catalyst particles (active material) applied on the surface.
[0088] In the case of solar cells, the active material is tungsten oxide powder, titanium oxide powder, and SnO 2 , ZnO, ZrO 2 , Nb 2 O 5 , CEO 2 , SiO 2 , Al 2 O 3 The semiconductor layer is supported with a dye, and examples of such dyes include compounds such as ruthenium-tris type transition metal complexes, ruthenium-bis type transition metal complexes, osmium-tris type transition metal complexes, osmium-bis type transition metal complexes, ruthenium-cis-diaqua-bipyridyl complexes, phthalocyanines and porphyrins, and organic-inorganic perovskite crystals.
[0089] -Solvent X, Solvent Y, and Electrolytes for Energy Storage Devices- When the porous resin formed by the liquid composition set is used as an insulating layer for a storage element, it is preferable that the solvent X and the solvent Y are also used as components contained in the electrolyte that constitutes the storage element. In other words, the electrolyte is preferably a solution containing the solvent X, the solvent Y, and an electrolyte described below. By selecting the solvent X and the solvent Y that are suitable not only for forming the porous resin but also as components contained in the electrolyte, it is possible to omit a process of removing the solvent X and the solvent Y by a heating process or the like after forming the porous resin and a separate process of impregnating the electrolyte into the porous resin. When the heating step can be omitted, it is possible to suppress damage to the porous resin that may be caused by heating and damage to components other than the porous resin (e.g., the electrode substrate, the active material layer, etc.) In particular, suppressing damage to the porous resin can suppress short circuits in the electricity storage element and uneven reactions during operation of the electricity storage element, thereby further improving the performance of the electricity storage element. Even when a step of removing the solvent X and the solvent Y is performed by a heating step, some of the solvent X and the solvent Y may remain in the porous material. Such remaining solvent X and solvent Y may generate gas due to an unexpected side reaction inside the energy storage element, thereby reducing the performance of the energy storage element. However, by selecting a solvent X and a solvent Y that can also be used as components contained in the electrolyte (e.g., a solvent that is unlikely to reduce the performance of the energy storage element due to a side reaction, etc.), the reduction in performance can be suppressed.
[0090] Solvent X and solvent Y suitably selected when the porous resin is used as an insulating layer for a storage element are preferably those that suppress decomposition reactions and gas generation during use of the storage element (during charging and discharging), and examples thereof include propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, ethylene carbonate, acetonitrile, γ-butyrolactone, sulfolane, dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,2-dimethoxyethane, 1,2-ethoxymethoxyethane, polyethylene glycol, alcohols, and mixtures thereof. Among these, it is preferable to use at least one selected from propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, and ethylene carbonate.
[0091] The boiling points of the solvent X and the solvent Y, which are omitted from the process of removing them by a heating process or the like after the porous resin is formed, are preferably higher than the boiling points of the solvent X and the solvent Y, which require a process of removing them by a heating process or the like. By having a high boiling point, the evaporation of the solvent X and the solvent Y during the production is suppressed, and the composition of the electrolyte is suppressed from changing from the composition originally expected. Specifically, the boiling point is preferably 80°C or higher, more preferably 85°C or higher, and even more preferably 90°C or higher. The boiling point of propylene carbonate (propylene carbonate) is 240°C, the boiling point of ethyl methyl carbonate (ethyl methyl carbonate) is 107°C, the boiling point of dimethyl carbonate (dimethyl carbonate) is 90°C, and the boiling point of ethylene carbonate (ethylene carbonate) is 244°C.
[0092] As described above, when using the solvent X and the solvent Y that also function as components contained in the electrolyte constituting the electricity storage element, it is preferable that the porous resin manufacturing apparatus 100 in FIG.
[0093] As described above, the electrolyte is a component used when the porous resin formed by the liquid composition set is used as an insulating layer for an electric storage element. Examples of the electrolyte include solid electrolytes and liquid electrolytes such as ionic liquids that are soluble in the solvent X and the solvent Y. By including an electrolyte in the liquid composition X or the liquid composition Y, the solvent X, the solvent Y, and the electrolyte that constitute the remaining components after the porous resin is formed can function as an electrolytic solution in the electric storage element. This makes it possible to omit a step of removing the solvent X and the solvent Y by a heating step or the like after the porous resin is formed, and a separate step of impregnating the porous resin with an electrolytic solution. When the heating step can be omitted, it is possible to suppress damage to the porous resin that may be caused by heating and damage to components other than the porous resin (e.g., the electrode substrate, the active material layer, etc.) In particular, suppressing damage to the porous resin can suppress short circuits in the electricity storage element and uneven reactions during operation of the electricity storage element, thereby further improving the performance of the electricity storage element. Even if a step of removing the solvent X and the solvent Y by a heating step is performed, some of the solvent X and the solvent Y may remain in the porous material. Such remaining solvent X and solvent Y may generate gas due to an unexpected side reaction inside the energy storage element, thereby reducing the performance of the energy storage element. However, by selecting a solvent X and a solvent Y that can also be used as components contained in the electrolyte (e.g., a solvent that is unlikely to reduce the performance of the energy storage element due to a side reaction, etc.), the reduction in performance can be suppressed.
[0094] The solid electrolyte is not particularly limited as long as it is soluble in the solvent X and the solvent Y. For example, inorganic ion salts such as alkali metal salts and alkaline earth metal salts, quaternary ammonium salts, supporting salts of acids, and supporting salts of alkalis can be used. More specifically, LiClO 4 , LiBF 4 , LiAsF 6 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 COO, KCl, NaClO 3 , NaCl, NaBF4 , NaSCN, KBF 4 , Mg(ClO 4 ) 2 , Mg(BF 4 ) 2 etc.
[0095] Examples of the liquid electrolyte include various ionic liquids containing a cationic component and an anionic component. The ionic liquid is preferably one that can maintain a liquid state over a wide temperature range including room temperature. Examples of the cationic component include imidazole derivatives such as N,N-dimethylimidazole salt, N,N-methylethylimidazole salt, and N,N-methylpropylimidazole salt; aromatic salts such as pyridinium derivatives such as N,N-dimethylpyridinium salt and N,N-methylpropylpyridinium salt; and aliphatic quaternary ammonium compounds such as tetraalkylammoniums such as trimethylpropylammonium salt, trimethylhexylammonium salt, and triethylhexylammonium salt. As the anion component, for example, a compound containing fluorine is preferable in terms of stability in the atmosphere, and BF 4 - , C.F. 3 SO 3 - , P.F. 4 - , (CF 3 SO 2 ) 2 N - , B(CN 4 ) - etc.
[0096] The content of the electrolyte is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.7 mol / L or more and 4.0 mol / L or less in the electrolyte solution, more preferably 1.0 mol / L or more and 3.0 mol / L or less, and from the viewpoint of achieving both the capacity and output of the energy storage element, more preferably 1.0 mol / L or more and 2.5 mol / L or less.
[0097] <For white ink use> The liquid composition set of the present disclosure is whitened by forming a porous resin and then removing the solvent X and the solvent Y, and can be used, for example, as a liquid composition set for imparting a white image onto a recording medium. In the present application, the liquid composition set for imparting a white image is not particularly limited as long as it can form a white image, and includes those other than white when used as ink (for example, those that are transparent or those with a color other than white). In the present application, the liquid composition set for imparting a white image is also referred to as a white ink.
[0098] White inks that exhibit whiteness by containing inorganic pigments such as titanium oxide as coloring materials are generally known. However, such white inks have a problem that sedimentation is likely to occur due to the large specific gravity of the coloring materials, and that the storage stability and ejection stability are poor. In this respect, the white ink of the present disclosure can exhibit whiteness without containing white coloring materials such as pigments and dyes, and therefore can improve the storage stability and ejection stability. The white ink of the present disclosure may contain a white coloring material, but preferably does not substantially contain a white coloring material. When the white ink does not substantially contain a white coloring material, the content of the white coloring material is preferably 0.1% by mass or less, more preferably 0.05% by mass or less, even more preferably 0.01% by mass or less, even more preferably below the detection limit, and particularly preferably not contained. In this way, when the white ink does not substantially contain a white coloring material, the white image formed by the white ink can be made lighter, and the white ink can be suitably used, for example, as a white ink for painting aircraft, a white ink for painting automobiles, etc.
[0099] Also, there are known white inks that contain multiple types of polymerizable compounds and become cloudy due to phase separation of these polymers during curing. However, such white inks have the problem of poor whiteness because the white color is achieved by phase separation between the polymers, not by an air layer. In this regard, when the liquid composition set of the present disclosure is used as a white ink, the white color is achieved by a porous resin having pores as air layers, and therefore high whiteness can be achieved. Note that white is the color commonly referred to as "white" in social terms, and whiteness is measured, for example, by measuring the lightness (L * For example, when the ink is applied at 100% duty or in an amount that sufficiently covers the surface of the recording medium, the lightness (L * ) and chromaticity (a * , b * ) but 70≦L * ≦100, -4.5≦a * ≦2, -6≦b * It is preferable to indicate a range of ≦2.5.
[0100] Furthermore, the white ink of the present disclosure forms a layer composed of a porous resin when applied onto a recording medium, and therefore may be used as a primer ink to create a base layer (primer layer) that improves the adhesion of another ink (such as an ink containing a colorant) that is subsequently applied. In general, when a low-permeability or non-permeability substrate such as coated paper, glass substrate, resin film substrate, or metal substrate is used as a recording medium, there is a problem that the fixability of the ink to the substrate decreases. In this respect, when the white ink (primer ink) of the present disclosure is used, the fixability of the white ink (primer ink) to the low-permeability or non-permeability substrate is high, so that the fixability of another ink applied later on the undercoat layer can be improved. In addition, even if the other ink (ink containing a coloring material, etc.) applied later is a permeability ink (water-based ink, etc.) that is difficult to use on a low-permeability or non-permeability substrate, the ink components can be permeated and diffused into the porous resin while the coloring material can be fixed to the porous resin surface. In addition, the white ink (primer ink) forms a white receiving layer, which conceals the color and transparency of the recording medium and can improve the image density of another ink (such as an ink containing a coloring material) that is applied later.
[0101] <3D modeling use> The liquid composition set of the present disclosure can form a porous resin layer having a layer thickness in the height direction, so that a three-dimensional object can be formed by stacking a plurality of the porous resin layers. That is, the liquid composition set of the present disclosure can be used as a liquid composition set for forming a three-dimensional object. In general, in three-dimensional modeling, a problem is distortion of the three-dimensional object caused by curing shrinkage. In this regard, the liquid composition set of the present disclosure forms a porous body having a network structure in association with polymerization-induced phase separation, so that the network structure relieves the internal stress during polymerization, and distortion of the object caused by curing shrinkage is suppressed.
[0102] Next, a modeling apparatus and a modeling method for modeling a three-dimensional object will be described with reference to FIG. 2. FIG. 2 is a schematic diagram showing an example of a material jet modeling apparatus. The modeling apparatus in FIG. 2 has a discharge means (an example of an application means) for discharging liquid composition X and liquid composition Y by an inkjet method or the like, and a curing means for curing the discharged liquid composition X by irradiating it with active energy rays, and is an apparatus for modeling a three-dimensional object by sequentially repeating the discharge by the discharge means and the curing by the curing means. In addition, the modeling method realized by the modeling apparatus in FIG. 2 has a discharge step (an example of a discharge step) for discharging liquid composition X and liquid composition Y by an inkjet method, and a curing step for curing the discharged liquid composition X by irradiating it with active energy rays, and is a method for modeling a three-dimensional object by sequentially repeating the discharge step and the curing step. The modeling apparatus and modeling method will be described in detail. The modeling apparatus 39 in Fig. 2 uses a head unit (movable in the AB direction) having an array of inkjet heads to discharge a first composition for three-dimensional modeling from a modeling object discharge head unit 30 and a second composition for three-dimensional modeling, which has a different composition from the first composition for three-dimensional modeling, from support member discharge head units 31 and 32, and laminates these compositions for three-dimensional modeling while curing them with adjacent ultraviolet ray irradiation means 33 and 34. More specifically, for example, the second composition for three-dimensional modeling is discharged from the support head units 31 and 32 onto the object support substrate 37, and the composition is solidified by irradiating it with active energy rays to form a first support layer having a reservoir. The first composition for three-dimensional modeling is then discharged from the support head unit 30 into the reservoir, and the first object layer is formed by irradiating it with active energy rays to form a first object layer. This process is repeated several times while lowering the stage 38 movable in the vertical direction according to the number of layers, thereby laminating the support layer and the object layer to produce a three-dimensional object 35. Thereafter, the support layer 36 is removed as necessary. Note that, although only one object ejection head unit 30 is provided in FIG. 2, two or more object ejection head units 30 may be provided.
[0103] <Laminate applications> The liquid composition set of the present disclosure can be applied to various objects such as a substrate to laminate a porous resin layer on various objects such as a substrate. In other words, the liquid composition set of the present disclosure is preferably used as a liquid composition set for forming a laminate having an object such as a substrate and a porous resin layer formed on the object. Specifically, as described above, liquid composition sets used for storage elements or power generation elements, liquid composition sets used for white ink, and liquid composition sets used for three-dimensional modeling can be mentioned. The liquid composition set used for storage elements or power generation elements is applied to an active material layer to laminate a porous resin layer as an insulating layer, the liquid composition set used for white ink is applied to a recording medium to laminate a porous resin layer as a white image, and the liquid composition set used for three-dimensional modeling is applied to a porous resin layer after a curing process to laminate a porous resin layer as a predetermined layer of a three-dimensional model. Generally, when a layer is laminated on an object such as a substrate, an interface exists between the object and the layer, so that when the adhesion at the interface is weak, peeling between the object and the layer is likely to occur. In particular, when layers are formed by polymerization reaction and laminated, the polymer is likely to be distorted during polymerization, which is likely to cause peeling of the target and the layer. In this respect, when the liquid composition set of the present disclosure is used for a laminate, a porous body having a network structure is formed with polymerization-induced phase separation, and the network structure relieves internal stress during polymerization, suppresses distortion of the shaped object due to cure shrinkage, and as a result, suppresses peeling of the target and the layer, which is preferable.
[0104] <Support Use> When the liquid composition set of the present disclosure is mixed with a functional substance to form a porous resin, a support in which the functional substance is supported on the surface of the porous resin can be produced. In other words, the liquid composition set of the present disclosure can be used as a liquid composition set for forming a support to manufacture a support carrying a functional substance. Here, the surface of the porous resin includes not only the outer surface of the porous resin but also the inner surface that communicates with the outside. In this way, the functional substance can be supported in the voids that communicate with the outside, so that the surface area that can support the functional substance is increased.
[0105] When the liquid composition set for forming a support of the present disclosure is used, the pores and porosity can be changed by appropriately adjusting the content of the polymerizable compound X, the content of the porogen, the irradiation conditions of the active energy ray, etc., and the degree of freedom in designing the performance of the support can be improved. In addition, since the liquid composition set for forming a support of the present disclosure can be applied in various application methods, for example, it can be applied by an inkjet method, and the degree of freedom in designing the shape of the support can be improved. Specifically, the support can be uniformly formed not only on a flat surface but also on a curved surface, and the time and effort required to adjust the shape by cutting the support to match the target shape can be omitted. In addition, a support having a particle shape can be formed by discharging the liquid droplets by the inkjet method, and the liquid droplets in flight or independent liquid droplets attached to a substrate are irradiated with active energy rays to form a liquid droplet.
[0106] The functional substance is preferably a substance that exerts a predetermined function directly or indirectly, and the function increases or improves with an increase in the area supported on the porous resin, and more preferably the supported functional substance is a substance that exerts the function when located on the external surface or an internal surface that communicates with the outside (in other words, a substance whose exertion of the function is suppressed when located on an internal surface that does not communicate with the outside). The functional substance may be a substance that dissolves or disperses in the liquid composition X or liquid composition Y, but is preferably a dispersible substance. Examples of functional substances include, but are not limited to, photocatalysts, biologically active substances, and the like.
[0107] Photocatalysts are substances that exhibit photocatalytic activity when irradiated with light in a specific wavelength range (excitation light with energy equal to or greater than the band gap between the valence band and conduction band of the photocatalyst).By exhibiting this photocatalytic activity, photocatalysts can exert various effects, such as antibacterial action, deodorizing and odor eliminating action, and decomposing harmful substances such as volatile organic compounds (VOCs).
[0108] Examples of photocatalysts include anatase or rutile titanium oxide (IV) (TiO 2 ), tungsten(III) oxide (W 2 O 3 ), tungsten(IV) oxide (WO 2 ), tungsten(VI) oxide (WO 3 ), zinc oxide (ZnO), iron(III) oxide (Fe 2 O 3 ), strontium titanate (SrTiO 3 ), bismuth(III) oxide (Bi 2 O 3 ), bismuth vanadate (BiVO 4 ), tin(II) oxide (SnO), tin(IV) oxide (SnO 2 ), tin(VI) oxide (SnO 3 ), zirconium oxide (ZrO 2 ), cerium(II) oxide (CeO), cerium(IV) oxide (CeO 2 ), barium titanate (BaTiO 3 ), indium(III) oxide (In 2 O 3 ), copper(I) oxide (Cu 2 O), copper(II) oxide (CuO), potassium tantalate (KTaO 3 ), potassium niobate (KNbO 3 ); metal sulfides such as cadmium sulfide (CdS), zinc sulfide (ZnS), and indium sulfide (InS); cadmium selenate (CdSeO 4 ), metal selenides such as zinc selenide (ZnSe); and metal nitrides such as gallium nitride (GaN).2 ), tin(IV) oxide (SnO 2 ), tungsten(III) oxide (W 2 O 3 ), tungsten(IV) oxide (WO 2 ), and tungsten(VI) oxide (WO 3 ), and anatase type titanium(IV) oxide (TiO 2 ) is more preferably included.
[0109] A physiologically active substance is an active ingredient used to exert a physiological effect on a living body, and examples of such substances include low molecular weight compounds including pharmaceutical compounds, food compounds, and cosmetic compounds, as well as high molecular weight compounds including proteins such as antibodies and enzymes, and biopolymers such as nucleic acids such as DNA and RNA. The term "physiological effect" refers to an effect caused by a physiologically active substance exerting its physiological activity at a target site, and is, for example, a quantitative and / or qualitative change or effect on a living body, tissue, cell, protein, DNA, RNA, etc. The term "physiological activity" refers to a physiologically active substance acting on a target site (e.g., a target tissue, etc.) to cause a change or effect. The target site is preferably, for example, a receptor present on the cell surface or inside the cell. In this case, a signal is transmitted to the cell by the physiological activity of the physiologically active substance binding to a specific receptor, and as a result, a physiological effect is exerted. The physiologically active substance may be a substance that is converted to a mature form by an enzyme in the living body and then binds to a specific receptor to exert a physiological effect. In this case, in the present application, the substance before being converted to a mature form is also included in the physiologically active substance. The physiologically active substance may be a substance produced by a living organism (human or non-human organism) or may be an artificially synthesized substance. When a sheet-shaped carrier is formed using liquid composition X or liquid composition Y containing such a physiologically active substance, it can be used as a sustained release sheet that continues to release a drug for a long period of time.
[0110] <Surface modification applications> The outer surface of the porous resin formed by the liquid composition set of the present disclosure has fine unevenness due to the porosity, which allows wettability to be controlled. Specifically, when the resin constituting the porous resin is hydrophilic, the outer surface of the porous resin can be functionally imparted with hydrophilicity higher than that of the planar surface formed by the resin. In addition, when the resin constituting the porous resin is water-repellent, the outer surface of the porous resin can be functionally imparted with water-repellency higher than that of the planar surface formed by the resin. Therefore, by applying the liquid composition set of the present disclosure to the surface of the object, a surface modification layer can be formed, and the wettability of the surface of the object can be easily modified.
[0111] In addition, when the liquid composition set of the present disclosure is used, the unevenness (unevenness due to holes or porosity) on the porous outer surface can be changed by appropriately adjusting the content of the polymerizable compound X, the content of the porogen, the irradiation conditions of the active energy rays, etc., and the design freedom in terms of the performance of the surface modification layer can be improved. In addition, since the liquid composition set of the present disclosure can be applied in various ways, for example, it can be applied by the inkjet method, and the design freedom in terms of the shape of the surface modification layer can be improved. Specifically, the surface modification layer can be uniformly formed not only on flat surfaces but also on curved surfaces.
[0112] <Separation layer or reaction layer use> In the case where a fluid such as a liquid or gas can permeate the porous resin formed by the liquid composition set of the present disclosure, the porous resin can be used as a flow path for the fluid. In the case where the porous resin can be used as a flow path for the fluid, the porous resin can be used as a separation layer for separating a predetermined substance from a fluid, or as a reaction layer (microreactor) for providing a microscopic reaction field for the fluid. In other words, the liquid composition of the present disclosure can be used as a liquid composition set for forming a separation layer or a reaction layer. It is preferable that the porous resin used for these applications is capable of uniformly and efficiently permeating the fluid inside the porous resin. In this regard, the porous resin formed by the liquid composition set of the present disclosure has a structure in which the pores are formed by phase separation, and the voids are continuously connected to each other and can uniformly and efficiently permeate the fluid. The porous resin is not particularly limited in the case where it is permeable to fluids such as liquids and gases, but for example, the air permeability measured in accordance with JIS P8117 is preferably 500 sec / 100 mL or less, and more preferably 300 sec / 100 mL or less. In this case, the air permeability is measured using, for example, a Gurley densometer (manufactured by Toyo Seiki Seisakusho) or the like. Note that separation refers to the removal or concentration of a specific substance contained in a fluid mixture. Furthermore, removal is not limited to the complete removal of a specific substance from a fluid mixture, and may involve only a partial removal. The reaction field refers to a place where a predetermined chemical reaction progresses as a result of a predetermined substance contained in a fluid passing through the reaction field.
[0113] When used for a separation layer, the liquid composition X of the present disclosure preferably contains a polymerizable compound X having a functional group capable of interacting with a predetermined substance contained in a fluid. When a porous resin is formed using a liquid composition set containing the liquid composition X, a functional group capable of interacting with a predetermined substance is arranged on the surface (internal surface and external surface) of the porous resin, and the predetermined substance can be effectively separated. The polymerizable compound X having a functional group capable of interacting with a predetermined substance contained in a fluid may be a part or the whole of the polymerizable compound X contained in the liquid composition. In this application, the functional group capable of interacting with a predetermined substance includes not only the case where the functional group itself is capable of interacting with the predetermined substance, but also the case where the functional group becomes capable of interacting with the predetermined substance by additional graft polymerization.
[0114] When used for a reaction layer application, the liquid composition X of the present disclosure preferably contains a polymerizable compound X having a functional group that provides a reaction field for a fluid. When a porous resin is formed using a liquid composition set containing the liquid composition X, a functional group that provides a reaction field for a fluid is arranged on the surface (internal surface and external surface) of the porous resin, and a reaction field can be effectively provided. The polymerizable compound X having a functional group that provides a reaction field for a fluid may be a part or the whole of the polymerizable compound X contained in the liquid composition. In this application, the functional group that provides a reaction field for a fluid includes not only a case where the functional group itself can provide a reaction field, but also a case where a reaction field can be provided by additionally performing graft polymerization.
[0115] The separation layer and reaction layer are formed, for example, by filling a container capable of forming a fluid inlet and a fluid outlet, such as a glass tube, with liquid composition X and liquid composition Y and curing the liquid composition. In addition, a separation layer and reaction layer having a flow path of a desired shape formed of a porous resin can be produced (drawn) by printing liquid composition X and liquid composition Y on a substrate by an inkjet method or the like. Since the flow paths of the separation layer and reaction layer can be printed, it is possible to provide a separation layer and reaction layer whose flow paths can be appropriately changed according to the purpose.
[0116] Furthermore, when the liquid composition set for forming a separation layer and a reaction layer according to the present disclosure is used, the content of the polymerizable compound X, the content of the porogen, the irradiation conditions of the active energy rays, and the like can be appropriately adjusted to change the pores and porosity of the porous resin, thereby improving the design freedom in terms of the performance of the separation layer and the reaction layer. EXAMPLES
[0117] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0118] <Calculation of Hansen solubility parameter C and interaction radius D of polymerizable compounds> According to the following procedure, the Hansen solubility parameter C and the interaction radius D were calculated for the following two types of polymerizable compounds. Polymerizable compound P1: Tricyclodecane dimethanol diacrylate (manufactured by Daicel-Allnex Corporation) Polymerizable compound P2: ε-caprolactone-modified tris-(2-acryloxyethyl) isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd.)
[0119] -Preparation of composition for transmittance measurement- First, a polymerizable compound for which the Hansen solubility parameter C and interaction radius D are to be calculated and the following 21 types of evaluation solvents with known Hansen solubility parameters (HSP) were prepared. The polymerizable compound, each evaluation solvent, and polymerization initiator were mixed in the ratio shown below to prepare a composition for transmittance measurement. ~Composition ratio for transmittance measurement~ Polymerizable compound for which Hansen solubility parameter C is to be calculated: 28.0% by mass Solvent for evaluation with known Hansen Solubility Parameters (HSP): 70.0% by mass Polymerization initiator (Irgacure 819, manufactured by BASF): 2.0% by mass ~Solvents for evaluation (21 types)~ Ethanol, 2-propanol, mesitylene, dipropylene glycol monomethyl ether, N-methyl 2-pyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, propylene carbonate, ethyl acetate, tetrahydrofuran, acetone, n-tetradecane, ethylene glycol, diethylene glycol monobutyl ether, diethylene glycol butyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 2-ethylhexanol, diisobutyl ketone, benzyl alcohol, 1-bromonaphthalene
[0120] -Measurement of light transmittance (compatibility evaluation)- The prepared transmittance measurement composition was poured into a quartz cell, and the transmittance of the transmittance measurement composition at a wavelength of 550 nm (visible light) was measured while stirring at 300 rpm using a stirrer. In this example, it was determined that the polymerizable compound and the evaluation solvent were in a compatible state when the light transmittance was 30% or more, and that the polymerizable compound and the evaluation solvent were in an incompatible state when the light transmittance was less than 30%. The conditions for measuring the light transmittance are shown below. Quartz cell: Special microcell with screw cap (Product name: M25-UV-2) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Measure the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air. (Transmittance: 100%) In Table 1, the results of the compatibility evaluation between the polymerizable compound and the evaluation solvent are shown according to the following evaluation criteria. (Evaluation Criteria) a: The polymerizable compound and the evaluation solvent are compatible with each other. b: The polymerizable compound and the evaluation solvent are not compatible.
[0121] [Table 1]
[0122] -Calculated using the Hansen dissolving sphere method- In the compatibility evaluation, the Hansen solubility parameters (HSP) of the evaluation solvents that showed compatibility and those that showed no compatibility were plotted on the Hansen space. Based on the plotted Hansen solubility parameters (HSP) of each evaluation solvent, a virtual sphere (Hansen sphere) was created in the Hansen space that encompassed the Hansen solubility parameters (HSP) of the evaluation solvents that showed compatibility, but did not encompass the Hansen solubility parameters (HSP) of the evaluation solvents that showed no compatibility. The center of the Hansen sphere was calculated as the Hansen solubility parameter C, and the radius of the Hansen sphere was calculated as the interaction radius D.
[0123] -Calculated Hansen solubility parameter C and interaction radius D- The calculated Hansen solubility parameter C and interaction radius D of the polymerizable compound are shown below. Polymerizable compound P1: Hansen solubility parameter C (17.21, 8.42, 7.98), interaction radius D (11.8) Polymerizable compound P2: Hansen solubility parameter C (18.51, 9.04, 4.75), interaction radius D (9.5)
[0124] <Calculation of Hansen solubility parameter A and interaction radius B of resin formed by polymerization of polymerizable compound> According to the following procedure, the Hansen solubility parameter A and the interaction radius B were calculated for a resin formed by polymerizing the following two types of polymerizable compounds. Polymerizable compound P1: Tricyclodecane dimethanol diacrylate (manufactured by Daicel-Allnex Corporation) Polymerizable compound P2: ε-caprolactone-modified tris-(2-acryloxyethyl) isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd.)
[0125] -Preparation of composition for haze measurement- First, a precursor of a resin (polymerizable compound) for which the Hansen solubility parameter A and the interaction radius B are to be calculated, and 21 types of evaluation solvents with known Hansen solubility parameters (HSP) were prepared. The polymerizable compound, each evaluation solvent, and polymerization initiator were mixed in the ratio shown below to prepare a composition for haze measurement. ~Composition ratio for haze measurement~ Precursor of the resin for which you want to calculate the Hansen solubility parameter A (polymerizable compound): 28.0% by mass Solvent for evaluation with known Hansen Solubility Parameters (HSP): 70.0% by mass Polymerization initiator (Irgacure 819, manufactured by BASF): 2.0% by mass ~Solvents for evaluation (21 types)~ Ethanol, 2-propanol, mesitylene, dipropylene glycol monomethyl ether, N-methyl 2-pyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, propylene carbonate, ethyl acetate, tetrahydrofuran, acetone, n-tetradecane, ethylene glycol, diethylene glycol monobutyl ether, diethylene glycol butyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 2-ethylhexanol, diisobutyl ketone, benzyl alcohol, 1-bromonaphthalene
[0126] - Fabrication of haze measurement element - On an alkali-free glass substrate, resin particles were uniformly dispersed on the substrate by spin coating to form a gap agent. Then, the substrate coated with the gap agent was bonded to an alkali-free glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Next, the prepared haze measurement composition was filled between the bonded substrates by utilizing the capillary phenomenon, and a pre-UV haze measurement element was produced. Next, the pre-UV haze measurement element was irradiated with UV to harden the haze measurement composition. Finally, the periphery of the substrate was sealed with a sealant to produce a haze measurement element. The various conditions during production are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Amount of haze measurement composition filled: 160μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond)
[0127] -Haze value (cloudiness) measurement (compatibility evaluation)- The haze value (cloudiness) was measured using the prepared haze measurement element and haze measurement element before UV irradiation. The measured value in the haze measurement element before UV irradiation was used as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation was calculated. In this example, when the increase rate of the haze value was 1.0% or more, it was determined that the resin and the evaluation solvent were in a non-compatible state, and when it was less than 1.0%, it was determined that the resin and the evaluation solvent were in a compatible state. The apparatus used for the measurement is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. In Table 2, the results of the compatibility evaluation between the resin formed by polymerization of the polymerizable compound and the evaluation solvent are shown according to the following evaluation criteria. (Evaluation Criteria) a: The resin formed by polymerization of the polymerizable compound is not compatible with the evaluation solvent. b: The resin formed by polymerization of the polymerizable compound is compatible with the evaluation solvent.
[0128] [Table 2]
[0129] -Calculated using the Hansen dissolving sphere method- In the measurement of the haze value (cloudiness) (compatibility evaluation), the Hansen solubility parameters (HSP) of the evaluation solvents that showed compatibility and the Hansen solubility parameters (HSP) of the evaluation solvents that showed no compatibility were plotted on the Hansen space. Based on the plotted Hansen solubility parameters (HSP) of each evaluation solvent, a virtual sphere (Hansen sphere) was created in the Hansen space that encompassed the Hansen solubility parameters (HSP) of the evaluation solvent group that showed compatibility, but did not encompass the Hansen solubility parameters (HSP) of the evaluation solvent group that showed no compatibility. The center of the Hansen sphere was calculated as the Hansen solubility parameter A, and the radius of the Hansen sphere was calculated as the interaction radius B.
[0130] -Calculated Hansen solubility parameter A and interaction radius B- The calculated Hansen solubility parameter A and interaction radius B of the resin formed by polymerization of the polymerizable compound are shown below. Resin formed by polymerization of polymerizable compound P1: Hansen solubility parameter A (20.02, 5.22, 6.15), interaction radius B (8.3) Resin formed by polymerization of polymerizable compound P2: Hansen solubility parameter A (19.89, 10.47, 7.32), interaction radius B (8.2)
[0131] <Example 1> The materials were mixed in the ratios shown below to prepare liquid compositions X and Y. In this example, liquid composition Y, which is the liquid applied first, is also referred to as a pre-coating liquid, and liquid composition X, which is the liquid applied later, is also referred to as a post-coating liquid. -Liquid composition X (post-coating liquid)- ·Polymerizable compound X (polymerizable compound P1): 28.0% by mass Solvent X (2-propanol): 70.0% by mass Polymerization initiator (Irgacure 819 (BASF)): 2.0% by mass -Liquid composition Y (pre-coating liquid)- Solvent Y (ethanol): 100.0% by mass
[0132] Next, a liquid composition Z consisting of 10.0% by mass of liquid composition X and 90.0% by mass of liquid composition Y was prepared. When the polymerizable compound contained in the liquid composition Z is polymerizable compound Z and the solvent contained in the liquid composition Z is solvent Z, the polymerizable compound Z is polymerizable compound P1 (tricyclodecane dimethanol diacrylate), and the solvent Z is a mixture of solvent X (2-propanol) and solvent Y (ethanol). Therefore, the Hansen solubility parameter C of the polymerizable compound Z is the same as the Hansen solubility parameter C of the above-mentioned polymerizable compound P1, and the interaction radius D of the polymerizable compound Z is the same as the interaction radius D of the above-mentioned polymerizable compound P1. In addition, the Hansen solubility parameter A of the resin Z is the same as the Hansen solubility parameter A of the resin formed by polymerizing the above-mentioned polymerizable compound P1, and the interaction radius B of the resin Z is the same as the interaction radius B of the resin formed by polymerizing the above-mentioned polymerizable compound P1. In addition, the Hansen solubility parameter of the solvent Z is calculated by dividing the Hansen solubility parameter of the solvent X by the following HSP X The Hansen solubility parameter of solvent Y is expressed as HSP Y If you express it as HSP as follows: Z This is expressed as: Highly Sensitive People X =(δD X , δP X , δH X ) Highly Sensitive People Y =(δD Y , δP Y , δH Y ) Highly Sensitive People Z =0.1(δD X , δP X , δH X )+0.9(δD Y , δP Y , δH Y ) At this time, the relative energy difference (RED) calculated from the Hansen solubility parameter C of the polymerizable compound Z, the interaction radius D of the polymerizable compound Z, and the Hansen solubility parameter of the solvent Z based on the following formula 2 was 0.972.
number
number
[0133] Furthermore, the viscosities of Liquid Compositions X and Y at 25° C. were measured using a viscometer (device name: RE-550L, manufactured by Toki Sangyo Co., Ltd.) and were found to be 30.0 mPa·s or less.
[0134] <Various Examples and Comparative Examples> Liquid compositions X and Y of various Examples and Comparative Examples were obtained in the same manner as in the preparation of Example 1, except that the compositions in Example 1 were changed to those shown in Tables 3 to 4. The units of the numbers in the compositions in Tables 3 to 4 are "mass %". In addition, in Tables 3 to 4, the relative energy difference (RED) calculated based on Formula 2 (represented as "RED between polymerizable compound Z and solvent Z" in Tables 3 to 4) and the relative energy difference (RED) calculated based on Formula 1 (represented as "RED between resin Z and solvent Z" in Tables 3 to 4) are also shown for liquid composition Z, as in Example 1. The viscosities of liquid compositions X and Y in Examples 1 to 11 at 25°C were measured using a viscometer (device name: RE-550L, manufactured by Toki Sangyo Co., Ltd.) and were 30.0 mPa s or less except for liquid composition Y in Example 7. The viscosity of liquid composition Y in Example 7 at 25°C was greater than 30.0 mPa s and less than 100.0 mPa s.
[0135] [Table 3]
[0136] [Table 4]
[0137] Next, for the liquid compositions X of Examples 1 to 11, the light transmittance and the rate of change in haze were evaluated.
[0138] [Light transmittance] Using the prepared liquid composition X of each example, the light transmittance was measured according to the following procedure. The prepared liquid composition X was poured into a quartz cell, and the transmittance of light (visible light) at a wavelength of 550 nm of the liquid composition X was measured while stirring with a stirrer at 300 rpm. In this example, a light transmittance of 30% or more was determined to be a compatible state between the polymerizable compound X and the porogen, and a light transmittance of less than 30% was determined to be a non-compatible state between the polymerizable compound X and the porogen. The conditions for measuring the light transmittance are shown below. Quartz cell: Special microcell with screw cap (Product name: M25-UV-2) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Measure the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air. (Transmittance: 100%) The light transmittance results are shown in Table 5 according to the following evaluation criteria. (Evaluation Criteria) A: Light transmittance is 30% or more b: Light transmittance is less than 30%
[0139] [Haze change rate] Using the prepared liquid composition X of each example, a haze measuring element was produced and the haze value (cloudiness) was measured according to the following procedures.
[0140] - Fabrication of haze measurement element - Resin particles were uniformly dispersed on a non-alkali glass substrate by spin coating to form a gap agent. Then, the substrate coated with the gap agent was bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Next, the prepared liquid composition X was filled between the bonded substrates by utilizing the capillary phenomenon, to prepare a pre-UV haze measurement element. Next, the pre-UV haze measurement element was irradiated with UV light to harden the liquid composition X. Finally, the periphery of the substrate was sealed with a sealant to prepare a haze measurement element. The conditions for preparation are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Filled liquid composition X: 160 μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond)
[0141] - Haze value (cloudiness) measurement - The haze value (cloudiness) was measured using the prepared haze measurement element before UV irradiation and the haze measurement element. The measured value in the haze measurement element before UV irradiation was used as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation was calculated. In this example, when the increase rate of the haze value was 1.0% or more, it was determined that the resin and the porogen were in a non-compatible state, and when it was less than 1.0%, it was determined that the resin and the porogen were in a compatible state. The apparatus used for the measurement is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0142] The results of the increase rate of the haze value are shown in Table 5 according to the following evaluation criteria. (Evaluation Criteria) a: The increase in haze value is 1.0% or more. b: The increase in haze value is less than 1.0%.
[0143] [Table 5]
[0144] As shown in Table 5, the liquid compositions X in Examples 1 to 11 had a light transmittance of 30% or more and an increase in haze value of 1.0% or more. By satisfying these conditions, the liquid compositions X in Examples 1 to 11 were liquids capable of forming a porous resin even when used alone.
[0145] Next, for the liquid composition Z of each of the examples and comparative examples, the light transmittance and the rate of change in haze were evaluated. In addition, for the porous resin formed using the liquid composition set (liquid composition X and liquid composition Y) of each of the Examples and Comparative Examples, the porosity of the resin formed in the contact area (near the interface between liquid composition X and liquid composition Y) where liquid composition X and liquid composition Y come into contact with each other was evaluated.
[0146] [Light transmittance] The light transmittance of each of the prepared liquid compositions Z of the Examples and Comparative Examples was measured according to the following procedure. The prepared liquid composition Z was poured into a quartz cell, and the transmittance of light (visible light) at a wavelength of 550 nm of the liquid composition Z was measured while stirring with a stirrer at 300 rpm. In this example, a light transmittance of 30% or more was determined to be a compatible state between the polymerizable compound Z and the solvent Z, and a light transmittance of less than 30% was determined to be a non-compatible state between the polymerizable compound Z and the solvent Z. The conditions for measuring the light transmittance are shown below. Quartz cell: Special microcell with screw cap (Product name: M25-UV-2) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Measure the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air. (Transmittance: 100%) The light transmittance results are shown in Table 6 according to the following evaluation criteria. (Evaluation Criteria) A: Light transmittance is 30% or more b: Light transmittance is less than 30%
[0147] [Haze change rate] Using the prepared liquid composition Z of each of the Examples and Comparative Examples, a device for haze measurement was produced and the haze value (cloudiness) was measured according to the following procedures.
[0148] - Fabrication of haze measurement element - On a non-alkali glass substrate, resin particles were uniformly dispersed on the substrate by spin coating to form a gap agent. Then, the substrate coated with the gap agent was bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Next, the prepared liquid composition Z was filled between the bonded substrates by utilizing the capillary phenomenon, and a pre-UV haze measurement element was produced. Next, the pre-UV haze measurement element was irradiated with UV to harden the liquid composition Z. Finally, the periphery of the substrate was sealed with a sealant to produce a haze measurement element. The various conditions during production are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Filled liquid composition Z: 160 μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond)
[0149] - Haze value (cloudiness) measurement - The haze value (cloudiness) was measured using the prepared haze measurement element and haze measurement element before UV irradiation. The measured value in the haze measurement element before UV irradiation was used as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation was calculated. In this example, when the increase rate of the haze value was 1.0% or more, it was determined that the resin Z and the solvent Z were in a non-compatible state, and when it was less than 1.0%, it was determined that the resin Z and the solvent Z were in a compatible state. The apparatus used for the measurement is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0150] The results of the rate of increase in haze value are shown in Table 6 according to the following evaluation criteria. Note that in the above evaluation of light transmittance, for liquid compositions Z in which the components were determined to be incompatible, evaluation was not performed and these are indicated in Table 6 as "-". (Evaluation Criteria) a: The increase in haze value is 1.0% or more. b: The increase in haze value is less than 1.0%.
[0151] [Porosity of resin formed in contact area] First, a porous resin was formed using the liquid composition set (liquid composition X and liquid composition Y) of each Example and Comparative Example. Specifically, 5 mL of liquid composition Y was placed in a glass petri dish having a diameter of 5 cm, and 20 μL of liquid composition X was dropped onto liquid composition Y. 2 A cured product was produced by irradiating UV light under atmospheric conditions. The cured product was held with tweezers and placed on the substrate so that the surface of the cured product on the contact area side was the upper surface. Solvent X and solvent Y were removed by heating at 100°C for 1 minute using a hot plate, and a porous resin was formed. The UV irradiation conditions are as follows: ·Light source: UV-LED (manufactured by Phoseon, product name: FJ800) ·Light source wavelength: 365nm ·Irradiation intensity: 30mW / cm 2 ·Irradiation time: 20s - Device for measuring UV radiation intensity: Ushio Inc., UV integrated light meter UIT-250 Next, the surface of the porous resin on the contact region side was observed by SEM. The porosity of the resin formed in the contact region is shown in Table 6 according to the following evaluation criteria. In addition, in the evaluation of the light transmittance, the liquid composition set in which the components in the liquid composition Z were determined to be incompatible was not evaluated, and is shown as "-" in Table 6. (Evaluation Criteria) a: Pores with diameters of 0.01 μm to 10 μm are observed. b: No pores with diameters of 0.01 μm or more and 10 μm or less are observed
[0152] In addition, the porous resins produced in the evaluation of the above-mentioned [Porosity of the resin formed in the contact area] using the liquid composition sets of Examples 1 to 11 all had a porosity of 30.0% or more and a co-continuous structure in which multiple pores in the resin were continuously connected.
[0153] [Table 6]
[0154] The results in Tables 3 to 4 and 6 show that when the relative energy difference (RED) calculated based on the above formula 2 in the liquid composition Z is 1.05 or less, the compatibility between the polymerizable compound Z and the solvent Z is high. Also, when the relative energy difference (RED) calculated based on the above formula 1 in the liquid composition Z is 1.00 or more, the compatibility between the resin Z and the solvent Z is low. This indicates that by using a liquid composition set having an appropriate combination of liquid composition X and liquid composition Y, it is possible to provide a liquid composition set that is excellent in making the resin porous in the contact area even when liquid composition X and liquid composition Y come into contact with each other.
[0155] <Example of manufacturing an electricity storage element using the liquid composition set> - Preparation of negative electrode - A negative electrode active material dispersion was obtained by uniformly dispersing 97.0 parts by mass of graphite particles (average particle size 10 μm) as a negative electrode active material, 1.0 parts by mass of cellulose as a thickener, and 2.0 parts by mass of acrylic resin as a binder in water. This dispersion was applied to a copper foil having a thickness of 8 μm as a negative electrode substrate, and the resulting coating was dried at 120° C. for 10 minutes and then pressed to obtain an electrode composite part having a thickness of 60 μm. This was then cut into a size of 50 mm×33 mm to prepare a negative electrode.
[0156] - Preparation of positive electrode - A positive electrode active material dispersion was obtained by uniformly dispersing 94.0 parts by mass of mixed particles of nickel, cobalt, and aluminum as a positive electrode active material, 3.0 parts by mass of Ketjen Black as a conductive assistant, and 3.0 parts by mass of polyvinylidene fluoride resin as a binder in N-methylpyrrolidone as a solvent. This dispersion was applied to an aluminum foil having a thickness of 15 μm as an electrode substrate by die coating, and the resulting coating was dried at 120 ° C for 10 minutes and then pressed to obtain an electrode mixture part having a thickness of 50 μm. Next, this was cut into 43 mm × 29 mm to prepare a positive electrode.
[0157] -Making the separator- Liquid composition X and liquid composition Y contained in the liquid composition set of Example 1 were filled into an inkjet ejection device equipped with a GEN5 head (manufactured by Ricoh Printing Systems Co., Ltd.), and liquid composition Y was ejected onto the negative electrode prepared as described above to form a solid image-like coating region. Next, liquid composition X was immediately ejected onto the negative electrode so as to overlap the coating region, forming a solid image-like coating region. Immediately after that, N 2 Under atmospheric conditions, the coating area was irradiated with UV light (light source: UV-LED (manufactured by Phoseon, product name: FJ800), wavelength: 365 nm, irradiation intensity: 30 mW / cm 2 The cured product was then heated at 120° C. for 1 minute using a hot plate to remove the solvent X and the solvent Y, thereby obtaining a negative electrode integrated with the porous resin that functions as a separator.
[0158] - Fabrication of energy storage elements - The negative electrode integrated with the porous resin was placed opposite the positive electrode prepared as above, an electrolyte was injected, and the electrodes were sealed with a laminate exterior material to prepare an energy storage element. The electrolyte was a mixture of ethylene carbonate (EC) and dimethyl carbonate (DMC) (a mixture with a mass ratio of EC:DMC=1:1) with an electrolyte of LiPF 6 A solution containing 1.5 mol / L of [Explanation of symbols]
[0159] 1a: Printing device 1b: Container 1c: Supply tube 2a: Light irradiation device 2b: Polymerization inert gas circulation device 3a: Heating device 4: Printing base material 5: Transport section 6: Porous resin precursor 7:Liquid composition 10: Printing process department 20: Polymerization process section 30: Heating process section [Prior art documents] [Patent documents]
[0160] [Patent Document 1] Patent No. 4426157
Claims
1. A liquid composition set including a liquid composition X containing a polymerizable compound X and a solvent X, and a liquid composition Y containing a solvent Y, The liquid composition X forms a porous resin, A liquid composition set characterized in that, when liquid composition Z is prepared consisting of 10.0 mass % of liquid composition X and 90.0 mass % of liquid composition Y, the liquid composition Z has a light transmittance of 30% or more at a wavelength of 550 nm as measured while stirring the liquid composition Z at 300 rpm, and a rate of increase in haze value in a haze measurement element in which liquid composition Z is filled between two alkali-free glass substrates is 1.0% or more. (Note that the rate of increase in haze value is the ratio of the measured value of the haze measurement element after UV irradiation under conditions in which the polymerizable compound X contained in the haze measurement element can be polymerized to the measured value of the haze measurement element before UV irradiation, with the measured value of the haze measurement element before UV irradiation being used as a reference.)
2. the liquid composition X has a light transmittance of 30% or more at a wavelength of 550 nm as measured while stirring the liquid composition X at 300 rpm; 2. The liquid composition set according to claim 1, wherein an increase in haze value in a haze measuring element having liquid composition X filled between two alkali-free glass substrates is 1.0% or more. (Note that the rate of increase in haze value is the ratio of the measured value of the haze measurement element after UV irradiation under conditions in which the polymerizable compound X contained in the haze measurement element can be polymerized to the measured value of the haze measurement element before UV irradiation, with the measured value of the haze measurement element before UV irradiation being used as a reference.)
3. In the case where the polymerizable compound contained in the liquid composition Z is a polymerizable compound Z and the solvent contained in the liquid composition Z is a solvent Z, The liquid composition set according to claim 1 or 2, wherein the relative energy difference calculated based on the Hansen solubility parameter A of the resin Z formed by polymerization of the polymerizable compound Z, the interaction radius B of the resin Z, and the Hansen solubility parameter of the solvent Z based on the following formula 1 is 1.00 or more. [0010]
4. In the case where the polymerizable compound contained in the liquid composition Z is a polymerizable compound Z and the solvent contained in the liquid composition Z is a solvent Z, The liquid composition set according to any one of claims 1 to 3, wherein the relative energy difference calculated from the Hansen solubility parameter C of the polymerizable compound Z, the interaction radius D of the polymerizable compound Z, and the Hansen solubility parameter of the solvent Z based on the following formula 2 is 1.05 or less. [0025]
5. the polymerizable compound X is contained in the liquid composition X in an amount of 10.0% by mass or more and 50.0% by mass or less; The liquid composition set according to claim 1 , wherein the solvent X is contained in the liquid composition X in an amount of 50.0% by mass or more and 90.0% by mass or less.
6. The liquid composition set according to claim 1 , wherein the liquid composition X and the liquid composition Y each independently have a viscosity at 25° C. of 1 mPa·s or more and 150 mPa·s or less.
7. The liquid composition set according to claim 1 , wherein the polymerizable compound X has a (meth)acryloyl group or a vinyl group.
8. The liquid composition set according to claim 1 , wherein the liquid composition Y is substantially free of a polymerizable compound.
9. A method for producing a porous resin, comprising the steps of: producing a porous resin using a liquid composition X containing a polymerizable compound X and a solvent X; and a liquid composition Y containing a solvent Y, the method comprising the steps of: The method includes an application step Y of applying the liquid composition Y, an application step X of applying the liquid composition X to the area to which the liquid composition Y has been applied, and a curing step of curing the applied liquid composition X, A method for producing a porous resin, characterized in that, when a liquid composition Z consisting of 10.0 mass % of the liquid composition X and 90.0 mass % of the liquid composition Y is prepared, the liquid composition Z has a light transmittance of 30% or more at a wavelength of 550 nm as measured while stirring the liquid composition Z at 300 rpm, and a rate of increase in haze value in a haze measurement element in which the liquid composition Z is filled between two alkali-free glass substrates is 1.0% or more. (Note that the rate of increase in haze value is the ratio of the measured value of the haze measurement element after UV irradiation under conditions in which the polymerizable compound X contained in the haze measurement element can be polymerized to the measured value of the haze measurement element before UV irradiation, with the measured value of the haze measurement element before UV irradiation being used as a reference.)
10. The method for producing a porous resin according to claim 9 , wherein the application step Y is a step of applying the liquid composition Y to a porous substrate.
11. The method for producing a porous resin according to claim 10, wherein the porous substrate is an active material layer.
12. 12. The method for producing a porous resin according to claim 9, wherein the applying step X is a step of ejecting the liquid composition X by an inkjet method.
Citation Information
Patent Citations
Recording material and manufacturing method for the same
JP2001293946A
Photocurable resin composition capable of forming porous material, and porous cured resin
JP2004051783A
Separation system, separation system component and method of making same
JP2005531011A
Laminate manufacturing method, laminate, active energy ray curable composition, ink, ink storage container, and two-dimensional or dimensional image forming apparatus
JP2017131865A
Curable composition, storage container, two-dimensional or three-dimensional image forming apparatus, two-dimensional or three-dimensional image forming method, and cured product
JP2020117586A