Polyolefin microporous membrane and secondary battery

By controlling the pore size distribution of microporous polyolefin membranes with specific ratios of small and large pores, the membrane achieves a balance between high output characteristics and safety, addressing the limitations of conventional separators.

JP7567443B2Active Publication Date: 2024-10-16TORAY INDUSTRIES INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020212078
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-26
Filing Date
2020-12-22
Publication Date
2024-10-16
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

Conventional microporous polyolefin membranes struggle to balance high output characteristics with sufficient strength and safety, particularly in thinner separators used in lithium-ion batteries, leading to issues such as short circuits and membrane rupture due to electrode contact or impact.

Method used

The membrane's pore size distribution is controlled by adjusting the ratio of small and large pores on the surface, with specific ratios of 20-40 nm and less than 20 nm pores to enhance ion permeability, strength, and shrinkage rate, thereby reducing ionic resistance and improving safety.

Benefits of technology

The controlled pore size distribution results in a microporous polyolefin membrane with superior ionic resistance, strength, and shrinkage rate, ensuring high output characteristics and safety as a battery separator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567443000001
    Figure 0007567443000001
  • Figure 0007567443000002
    Figure 0007567443000002
Patent Text Reader

Abstract

To provide a polyolefin microporous film having output properties, strength, and shrinkage rates that are improved compared to the conventional art.SOLUTION: In a polyolefin microporous film, in a pore size distribution obtained by linearization of a surface-scanning electron micrograph, the proportion of pore sizes of 20-40 nm is 28% or more, and the proportion of pore sizes of more than 0 and less than 20 nm is 16% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyolefin microporous membrane that is widely used as a separation membrane for separation, selective permeation, etc. of substances, and as a separator for electrochemical reaction devices such as alkaline batteries, lithium ion batteries, fuel cells, and capacitors, etc. In particular, the present invention relates to a polyolefin microporous membrane that is suitably used as a separator for nonaqueous electrolyte secondary batteries such as lithium ion batteries, and is used as a separator that exhibits superior battery characteristics and has high safety compared to conventional polyolefin microporous membranes. [Background technology]

[0002] Polyolefin microporous membranes are used as filters, fuel cell separators, capacitor separators, etc. In particular, they are suitably used as separators for nonaqueous electrolyte secondary batteries such as lithium ion batteries that are widely used in notebook personal computers, mobile phones, digital cameras, etc. This is because polyolefin microporous membranes have excellent mechanical strength, shutdown properties, and ion permeability.

[0003] In recent years, lithium-ion batteries have come to be used in vehicles, so there is a need to shorten charging times and improve acceleration, and battery characteristics such as rapid charging (high current charging) and increased power consumption (high current discharging) are required. Accordingly, there is an increased demand for separators to improve output characteristics.

[0004] Furthermore, as the driving range of automobiles increases, the capacity of batteries is increasing, and there is an even greater demand for thinner separators. However, thinner separators have lower strength, which makes them more susceptible to short circuits caused by electrodes or foreign objects (reduced resistance to foreign objects) and to membrane rupture (reduced impact resistance) when the battery is subjected to impact, reducing the safety of the battery. In addition, high-output charging and discharging generates a lot of heat in the battery, making it more likely for the separator to shrink and short circuit the battery. For this reason, there is a demand for separators that simultaneously have higher strength, lower shrinkage, and higher output characteristics than ever before.

[0005] As a method for improving output characteristics, Patent Document 1 discloses a method for blending polyethylene (PE) and polypropylene (PP) to increase porosity and control the number of holes, average pore size, and tortuosity to improve ionic conductivity.

[0006] Patent Document 2 discloses a method for improving battery characteristics such as cycle characteristics by controlling the surface and internal pore structure to improve wettability with an electrolyte and retention of the electrolyte in the membrane.

[0007] Patent Documents 3 to 5 propose separators with a bimodal pore size distribution, having large pores or relatively coarse pores (coarse pores) and small pores or relatively fine pores (micropores) in the cross-sectional direction of the separator, and disclose methods for improving cycle characteristics by realizing good air permeability through the coarse pores and good electrolyte permeability and retention through the micropores. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2017-140840 A [Patent Document 2] JP 2012-48987 A [Patent Document 3] JP 2014-74146 A [Patent Document 4] JP 2008-81513 A [Patent Document 5] JP 2000-195490 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, in conventional microporous membranes such as those described in Patent Documents 1 and 2, in order to improve output characteristics, it is necessary to increase the porosity and control the pore structure by increasing the number of holes and through-holes, etc. As a result, sufficient strength and shrinkage rate cannot be obtained, and it is insufficient to achieve both output characteristics and safety.

[0010] Even in the methods of controlling the pore size distribution inside the separator described in Patent Documents 3 to 5, sufficient strength is not obtained because the separator has large pores of several hundred nm or more inside, and further improvements are required to achieve both high output characteristics and safety.

[0011] In view of the above circumstances, an object of the present invention is to provide a microporous polyolefin membrane having better output characteristics, strength, and shrinkage rate than conventional ones. [Means for solving the problem]

[0012] Therefore, the present inventors focused on the relationship between the pore size and resistance of the surface of a separator having a fibrous network structure composed of a resin component. As a result, they found that there are surface pore size components of the separator that affect mechanical properties and thermal properties, and surface pore size components of the separator that affect ion permeability. They found that by appropriately controlling the ratio of small pores and large pores on the surface of the separator, a polyolefin microporous membrane with superior output properties, strength, and shrinkage rate compared to conventional ones can be obtained, and thus completed the present invention.

[0013] That is, the present invention employs the following configuration.

[0014] The polyolefin microporous membrane according to an embodiment of the present invention is characterized in that, in a pore size distribution obtained by binarizing a surface scanning electron microscope image, the proportion of pores having a pore size of 20 to 40 nm is 28% or more, and the proportion of pores having a pore size of more than 0 and less than 20 nm is 16% or more. Effect of the Invention

[0015] An embodiment of the present invention uses a microporous membrane having an appropriately controlled surface pore size distribution, thereby obtaining a polyolefin microporous membrane that is superior in ionic resistance, strength, and shrinkage rate compared to conventional polyolefin microporous membranes, and that provides high output characteristics and safety even when used as a separator for a secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The polyolefin microporous membrane according to the embodiment of the present invention is useful as a battery separator because of its excellent ionic resistance, strength, and shrinkage rate, and has excellent safety and output characteristics. The present invention can be realized by satisfying the surface pore size distribution described below. Specifically, as a result of studying the problem of achieving both output characteristics and safety when a polyolefin microporous membrane having a mesh-like fibril structure is used as a battery separator, it was found that the pore size of the surface of the polyolefin microporous membrane affects the ion permeability, strength, and shrinkage rate. It was also found that by controlling the surface pore size distribution, the ionic resistance at the electrode-separator interface can be reduced without deteriorating the strength and shrinkage rate of the polyolefin microporous membrane, leading to the achievement of both the output characteristics and safety of the battery, which have been in a trade-off relationship in the past.

[0017] The present invention will be described in further detail below. [1] Polyolefin microporous membrane The polyolefin microporous membrane according to an embodiment of the present invention (hereinafter sometimes simply referred to as "microporous membrane") is characterized in that, in a pore size distribution in a surface SEM observation image measured by a scanning electron microscope (SEM) described below, the proportion of the number of pores having a pore diameter of 20 to 40 nm on at least one side is 28% or more of the pore distribution in the entire observation field, and the proportion of the number of pores having a pore diameter of more than 0 and less than 20 nm is 16% or more of the pore distribution in the entire observation field. It is preferable that the proportion of the number of pores having a pore diameter of 20 to 40 nm on both sides is 28% or more of the pore distribution in the entire observation field, and it is particularly preferable that the proportion of the number of pores having a pore diameter of 20 to 40 nm on both sides is 28% or more of the pore distribution in the entire observation field, and the proportion of the number of pores having a pore diameter of more than 0 and less than 20 nm is 16% or more of the pore distribution in the entire observation field. By satisfying the above range, the wettability and retention of the electrolyte are improved, the uniformity of the battery reaction is enhanced, and the resistance at the interface between the electrode and the microporous membrane is reduced, achieving good output characteristics, while also obtaining good strength and shrinkage rate, making it possible to achieve both the output characteristics and safety of the battery, which were previously in a trade-off relationship.

[0018] When the ratio of the number of pores having a pore size of 20 to 40 nm on at least one surface is 28% or more, good ion permeability can be obtained and an increase in resistance can be suppressed when the separator is used as a nonaqueous electrolyte secondary battery such as a lithium ion battery. That is, from the viewpoint of ion permeability related to output characteristics, the ratio of pores having a pore size of 20 to 40 nm is preferably 29% or more, more preferably 30% or more.

[0019] On the other hand, the strength of the microporous membrane depends on the number of fibrils per unit volume. Therefore, an increase in the ratio of the number of pores having a pore diameter of 20 to 40 nm in the polyolefin microporous membrane leads to a decrease in the number of fibrils per unit volume, leading to a decrease in strength. In addition, an increase in the ratio of the number of pores having a pore diameter of 20 to 40 nm leads to a relative decrease in the ratio of pore diameters greater than 0 and less than 20 nm, resulting in a non-uniform polyolefin microporous membrane. This leads to a deterioration in the shrinkage rate and non-uniform reactions in the battery, leading to a decrease in safety. Therefore, from the viewpoint of high strength and low shrinkage rate among the objects of the present invention, the ratio of the number of pores having a pore diameter of 20 to 40 nm is preferably 50% or less, more preferably 34% or less, even more preferably 31% or less, and particularly preferably 30% or less.

[0020] The polyolefin microporous membrane according to the embodiment of the present invention is characterized in that, in the pore size distribution measured by surface SEM, the ratio of the number of pores having a pore size of more than 0 and less than 20 nm on at least one surface is 16% or more of the pore distribution in the entire observation field. When the ratio of pore sizes of more than 0 and less than 20 nm is 16% or more, the number of fibrils per unit volume increases, and good strength is obtained. In addition, pore sizes of more than 0 and less than 20 nm are formed by the advancement of fineness of the fibril structure by stretching. The fine fibril structure has a stable structure with a highly oriented high melting point, so that a low shrinkage rate can be achieved. From the viewpoint of strength and shrinkage rate, the ratio of pore sizes of more than 0 and less than 20 nm in the entire membrane is preferably 18% or more, more preferably 20% or more, and even more preferably 24% or more.

[0021] On the other hand, an increase in the ratio of the number of pores having a pore size of more than 0 and less than 20 nm in the polyolefin microporous membrane is advantageous from the viewpoints of dendrite resistance and self-discharge characteristics, but the surface pore size becomes finer, which reduces the impregnation and retention of the electrolyte, leading to deterioration of battery characteristics such as cycle tests. In addition, a decrease in the ratio of pore sizes of 20 to 40 nm leads to deterioration of ion permeability and deterioration of output characteristics. Therefore, from the viewpoint of reducing ion resistance among the objects of the present invention, the ratio of pore sizes of more than 0 and less than 20 nm is preferably 30% or less, more preferably 25% or less.

[0022] The ratio of the number of pores having a pore diameter of more than 0 and less than 20 nm to the number of pores having a pore diameter of 20 to 40 nm on at least one surface of the polyolefin microporous membrane in the entire observation field (the ratio of pore diameters of more than 0 and less than 20 nm / the ratio of pore diameters of 20 to 40 nm) is preferably less than 0.75. When it is less than 0.75, the non-uniformity of the microporous membrane is improved and a good shrinkage rate is obtained, and the uniformity of the battery reaction is improved and good safety is obtained, leading to a balance between the output characteristics and safety of the battery, which have been in a trade-off relationship in the past. In addition, during the charge and discharge process of a battery, the electrolyte is usually electrochemically decomposed inside the battery, generating solid products such as organic substances and gases such as ethylene and hydrogen. These products block the pores in the polyolefin microporous membrane, leading to deterioration of the battery characteristics. When the ratio of the number of pores having a pore size of more than 0 and less than 20 nm to the number of pores having a pore size of 20 to 40 nm (the ratio of pore sizes of more than 0 and less than 20 nm / pore size of 20 to 40 nm) is less than 0.75, blocking of pores by decomposition products can be suppressed, leading to improved battery characteristics. Therefore, such a ratio is more preferably 0.7 or less, and even more preferably 0.65 or less.

[0023] In this embodiment, the average pore size of at least one surface of the polyolefin microporous membrane measured by surface SEM observation described later is preferably 30 nm or more, and preferably 45 nm or less. When the average pore size is 45 nm or less, short circuits due to dendrite growth can be suppressed, and a good number of holes can be obtained, increasing the ion permeation path and obtaining excellent battery characteristics. From the viewpoint of ion permeability and strength, the average pore size is preferably 45 nm or less, more preferably 42 nm or less, and even more preferably less than 40 nm. On the other hand, when the average pore size is 30 nm or more, a good opening ratio can be obtained and high ion permeability can be obtained. Therefore, the average pore size is preferably 30 nm or more, and more preferably 33 nm or more.

[0024] A polyolefin microporous membrane has many micropores inside, and the micropores are connected within the membrane. The average pore size measured by a porometer is the pore size of the neck portion in the cross-sectional direction of the polyolefin microporous membrane, and therefore affects the electrolyte retention and ion permeability in the microporous membrane. From the viewpoint of ion permeability, the average pore size measured by a porometer is preferably 10 nm or more. When the average pore size is 10 nm or more, good opening property and number of pores are obtained, and excellent battery characteristics are obtained.

[0025] As the average pore size measured by a porometer increases, the number of ion permeation paths decreases and the strength of the microporous membrane decreases due to the coarse pores in the inward direction, so the average pore size measured by a porometer is preferably less than 40 nm, more preferably less than 35 nm, even more preferably less than 30 nm, even more preferably 28 nm or less, and most preferably 25 nm or less.

[0026] In the present embodiment, the difference between the average pore size (calculated by SEM) obtained from the surface SEM image of the polyolefin microporous membrane and the average pore size (calculated by porometer) obtained using a porometer (average pore size (calculated by SEM) - average pore size (calculated by porometer)) is preferably 21 nm or less. When the difference in pore size is 21 nm or less, the wettability and retention of the electrolyte, and the balance between the strength and shrinkage of the microporous membrane are excellent, and good battery characteristics and safety are obtained. Since the pore size calculated by the porometer is the pore size of the neck portion in the cross-sectional direction, the difference between the average pore size obtained from the surface SEM image and the average pore size obtained using the porometer indicates the uniformity of the pore size. If there are large pores with large pore sizes inside the separator, the injectability of the electrolyte due to capillary phenomenon and the retention of the electrolyte against pressure are reduced. If the surface has relatively large pores, the resistance at the interface between the electrode and the microporous membrane is reduced, and good output characteristics can be achieved. Therefore, from the viewpoints of the injectability and retention of the electrolyte, and the interface resistance, the difference between the average pore diameter obtained from the surface SEM image and the average pore diameter obtained using a porometer is more preferably 20 nm or less, even more preferably 18 nm or less, and even more preferably 15 nm or less.

[0027] The porosity of the polyolefin microporous membrane according to the embodiment of the present invention is preferably 35% or more, more preferably 40% or more, and even more preferably 45% or more, from the viewpoint of permeability and electrolyte content. When the porosity is 35% or more, the balance between permeability, strength, and electrolyte content is good, and the non-uniformity of the battery reaction is eliminated. As a result, the generation of dendrites is suppressed, and the membrane can be used without impairing the conventional battery performance, and can be suitably used as a separator for a secondary battery. In addition, by increasing the porosity, good output characteristics can be obtained, but the safety of the battery is reduced due to a decrease in puncture strength and an increase in shrinkage rate. Therefore, the porosity is preferably 50% or less, more preferably 48% or less. The porosity is represented by the following formula and can be measured by the method described in the Examples.

[0028] Porosity (%) = (volume-mass / film density) / volume x 100 The puncture strength of the polyolefin microporous membrane according to the embodiment of the present invention is preferably as high as possible since it affects safety such as suppression of short circuit caused by foreign matter in the battery. From the viewpoint of preventing rupture due to electrode active material, etc., the puncture strength of the polyolefin microporous membrane converted into a membrane thickness of 10 μm (10 μm converted puncture strength) is preferably 4.0 N or more, more preferably 5.0 N or more, and even more preferably 6.0 N or more. When the puncture strength is 4.0 N or more, short circuit caused by foreign matter in the battery is suppressed, and good battery safety is obtained. In addition, the higher the puncture strength, the more preferable, but it is usually 10 N or less.

[0029] In order to increase the puncture strength, it is recommended to use ultra-high molecular weight polyolefin and increase the number of tie molecules connecting the lamellae from the viewpoint of the fibril crystal structure. Also, it is recommended to have fine fibrils as the fibril structure. The fine fibril structure is a highly oriented structure, and can be obtained by applying the raw materials, resin concentration, and stretch ratio described below.

[0030] The pin puncture strength calculated based on a film thickness of 10 μm refers to the pin puncture strength L2 calculated by the formula: L2 = (L1 × 10) / T1 when the pin puncture strength of a polyolefin microporous film with a film thickness of T1 (μm) is L1. In the following, unless otherwise specified regarding the film thickness, the term "pin puncture strength" is used to mean "pin puncture strength calculated based on a film thickness of 10 μm."

[0031] In a battery, tension is applied in the MD direction (machine length direction), so if the shrinkage rate in the MD direction is high, the membrane will break and lead to a short circuit. Therefore, the polyolefin microporous membrane according to the embodiment of the present invention preferably has a MD shrinkage rate of 25% or less at 105°C / 8h. In addition, such a shrinkage rate is preferably 3.0% or more. When the MD shrinkage rate is within this range, the balance between the shape stability and shutdown properties of the polyolefin microporous membrane is improved. By setting the shrinkage rate to 25% or less, it is possible to prevent deterioration of shape stability at high temperatures and suppress a decrease in safety due to internal short circuits when abnormal heat is generated locally. In addition, if the shrinkage rate is 3.0% or more, it is possible to suppress deterioration of the fluidity of the polyolefin and prevent a decrease in the shutdown properties. The MD shrinkage rate is more preferably 20% or less, even more preferably 15% or less, and even more preferably 10% or less.

[0032] In addition, the polyolefin microporous membrane according to the embodiment of the present invention has a shrinkage rate in the TD direction (machine width direction) at 105°C / 8h of preferably 1.0% or more from the viewpoint of heat resistance such as stress relaxation properties, and preferably 30% or less. When the shrinkage rate is within this range, the balance between the shape stability and shutdown properties of the polyolefin microporous membrane is improved. If the shrinkage rate is 1.0% or more, the deterioration of the fluidity of the polyolefin can be suppressed, and the deterioration of the shutdown properties can be prevented. If the shrinkage rate is 30% or less, the deterioration of the shape stability at high temperatures can be suppressed, and the occurrence of an internal short circuit when abnormal heat is generated locally can be prevented, and safety can be maintained. The shrinkage rate in the TD direction is more preferably 20% or less, and even more preferably 10% or less. In particular, the polyolefin microporous membrane according to the present embodiment has an improved balance between ion permeability, strength, and shrinkage by controlling the ratio of the number of pores having a pore diameter of more than 0 and less than 20 nm to the number of pores having a pore diameter of 20 to 40 nm, and a microporous membrane excellent in safety and output properties can be obtained.

[0033] The shrinkage rates in the MD and TD directions at 105° C. / 8 h can be measured by the method described in the Examples.

[0034] The tensile (break) strength in both the MD and TD directions (hereinafter simply referred to as "MD strength" and "TD strength") is preferably 150 MPa or more, more preferably 180 MPa or more, and even more preferably 200 MPa or more. When the MD strength and TD strength are 150 MPa or more, short circuit caused by foreign matter in the battery can be prevented, and the safety of the battery can be maintained. From the viewpoint of improving safety, the higher the tensile strength, the better, but since there is often a trade-off between tensile strength and shrinkage rate, it is preferable that the tensile strength is 300 MPa or less, and more preferably 280 MPa or less. To set the tensile strength in the above range, it is preferable that the raw material composition of the polyolefin microporous membrane and the above-mentioned membrane-forming conditions are within the ranges described below.

[0035] Moreover, the tensile (break) elongation in both the MD and TD directions (hereinafter simply referred to as "MD elongation" and "TD elongation") is preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. When the MD elongation and TD elongation are 30% or more, short circuits caused by foreign matter in the battery or during winding are suppressed, and good safety is obtained, which is preferable. Furthermore, both the MD elongation and TD elongation are preferably 100% or less, more preferably 80% or less, and even more preferably 70% or less. When the MD elongation and TD elongation are 100% or less, a good balance between strength and elongation can be achieved, and a microporous membrane with excellent safety can be obtained.

[0036] The tensile strength and tensile elongation in the MD and TD directions can be measured by the methods described in the Examples.

[0037] In this embodiment, the direction parallel to the film-forming direction of the polyolefin microporous membrane is referred to as the film-forming direction, longitudinal direction or MD direction, and the direction perpendicular to the film-forming direction within the plane of the polyolefin microporous membrane is referred to as the width direction or TD direction.

[0038] In the polyolefin microporous membrane according to the embodiment of the present invention, the air permeability is a value measured in accordance with JIS P 8117 (2009). In this specification, unless otherwise specified regarding the membrane thickness, the term "air permeability" is used to mean "air permeability when the membrane thickness is 10 μm". When the measured air permeability is p1, the air permeability p2 calculated by the formula: p2 = (p1 × 10) / T1 is regarded as the air permeability when the membrane thickness is 10 μm.

[0039] Air permeability (Gurley value) is 200sec / 100cm 3 It is preferable that the speed is less than 150sec / 100cm. 3 More preferably, it is 100sec / 100cm or less. 3 It is more preferable that the air permeability is 200 sec / 100 cm or less. 3 If the air permeability is less than 50 sec / 100 cm, good ion permeability can be obtained and electrical resistance can be reduced. The lower the air permeability, the better. 3 That's all.

[0040] In the polyolefin microporous membrane according to the embodiment of the present invention, the resistance increases with an increase in the membrane thickness, and the output characteristics of the battery decrease. From the viewpoint of the output characteristics of the battery, the membrane thickness is preferably 12 μm or less, more preferably 10 μm or less, and even more preferably 7 μm or less. On the other hand, the thinner the membrane, the lower the strength and the lower the safety. From the viewpoint of safety, the membrane thickness is preferably 3 μm or more, and more preferably 5 μm or more. [2] Polyolefin resin The polyolefin microporous membrane according to an embodiment of the present invention is a porous film mainly composed of a polyolefin resin, and the term "main component" means that the polyolefin resin accounts for preferably 80% by mass or more, and more preferably 90% by mass or more of the total mass of the polyolefin microporous membrane.

[0041] The resin raw material for the polyolefin microporous membrane may be a single composition, a composition of a main raw material and a sub-raw material, or a polyolefin resin mixture (polyolefin resin composition) consisting of two or more polyolefin resins. The raw material form for the polyolefin microporous membrane is preferably a polyolefin resin, and examples of the polyolefin resin include polyethylene and polypropylene. It is more preferable that the polyolefin is a single composition, since the uniformity of the openings is improved and good output characteristics and membrane strength can be obtained.

[0042] The polyolefin resin is preferably a homopolymer of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, or the like, and a homopolymer of ethylene (polyethylene) is particularly preferred.

[0043] Polyethylene may be a homopolymer of ethylene and a copolymer containing other α-olefins such as propylene, butene-1, hexene-1, pentene-1, 4-methylpentene-1, octene, or alkenes having a higher carbon number, vinyl acetate, methyl methacrylate, styrene, etc.

[0044] The type of polyolefin resin used is preferably polyethylene, and has a density of 0.94 g / cm 3 High density polyethylene with a density of 0.93 to 0.94 g / cm 3 Medium density polyethylene, with a density in the range of 0.93 g / cm 3 Examples of the low density polyethylene include lower low density polyethylene and linear low density polyethylene.

[0045] In particular, from the viewpoint of pore size distribution observed by surface SEM, it is preferable to use an ultra-high molecular weight polyolefin having a weight average molecular weight (Mw) of 1 million or more alone as the polyolefin resin, more preferably an ultra-high molecular weight polyolefin having a weight average molecular weight of 1.5 million or more alone, and even more preferably an ultra-high molecular weight polyolefin having a weight average molecular weight of 2 million or more alone. By using a polyolefin having a weight average molecular weight of 100 or more alone, a uniform structure with few coarse pores is formed by applying a uniform stress to the polyethylene resin layer in the stretching process, and a polyolefin microporous membrane with a small difference in pore size distribution between the front and back as measured by surface SEM observation can be obtained, resulting in excellent output characteristics.

[0046] Ultra-high molecular weight polyolefin has a weight average molecular weight of 1.0×10 6 More than 1.0×10 is preferable. 7 The weight average molecular weight is preferably 1.0×10 or less. 6 If the weight average molecular weight is 1.0×10 or more, the entanglement density of the amorphous region increases, and stress is uniformly applied to the polyethylene resin layer during the stretching process, so that a uniform structure with few coarse pores can be formed, and good output characteristics can be obtained. 6 By using the above polyolefin resins, the number of tie molecules increases, resulting in high strength. This improves the trade-off between ion resistance and strength, making it possible to achieve both battery safety and output characteristics.

[0047] Therefore, the weight average molecular weight of the ultra-high molecular weight polyolefin is preferably 1.0×10 6 More preferably, it is 1.5×10 6More preferably, 2.0×10 6 More preferably, 3.0×10 6 More than 6.0×10, most preferably 6 The weight average molecular weight is preferably 1.0×10 7 Less than or equal to 8.0×10 6 Less than 6.0×10, more preferably 6 The following is the result.

[0048] The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the ultra-high molecular weight polyolefin is preferably 3.0 or more, and preferably 100 or less. The narrower the molecular weight distribution, the more uniform the system and the easier it is to obtain uniform micropores, so the narrower the molecular weight distribution, the more preferable it is, but the narrower the distribution, the lower the molding processability. Therefore, the lower limit of the molecular weight distribution is more preferably 4.0 or more, even more preferably 5.0 or more, and even more preferably 6.0 or more. If the molecular weight distribution increases, the amount of low molecular weight components increases, so that the strength decreases and the melting and fusion of fine fibrils during stretching and heat setting tends to occur. Therefore, the upper limit is more preferably 80 or less, even more preferably 50 or less, even more preferably 20 or less, and particularly preferably 10 or less. By setting it in the above range, good molding processability can be obtained, and uniform micropores can be obtained because the system is unified.

[0049] The ultra-high molecular weight polyolefin has a weight average molecular weight (Mw) of 1.0×10 from the viewpoints of pore size distribution, membrane strength, and shrinkage rate. 6 It is preferable that the polyethylene be ultra-high molecular weight polyethylene having a molecular weight of 1.5×10 or more. 6 More preferably, 2.0×10 6 The above is even more preferable.

[0050] In the manufacturing process of the polyolefin microporous film according to the embodiment of the present invention, it is preferable to add a plasticizer in order to improve the molding processability. The blending ratio of the polyolefin resin and the plasticizer may be appropriately adjusted within a range that does not impair the molding processability, but the ratio of the polyolefin resin is preferably 10% by mass or more, and preferably 50% by mass or less, with the total of the polyolefin resin and the plasticizer being 100% by mass. By making the ratio of the polyolefin resin 10% by mass or more, i.e., making the ratio of the plasticizer 90% by mass or less, swelling and necking at the outlet of the die can be suppressed when forming into a sheet, and the moldability and film formability of the sheet are improved. On the other hand, by making the ratio of the polyolefin resin 50% by mass or less, i.e., making the ratio of the plasticizer 50% by mass or more, the pressure increase in the film formation process can be suppressed, and good molding processability can be obtained.

[0051] When the total of the polyolefin resin and the plasticizer is 100% by mass, the proportion of the polyolefin resin is preferably 10% by mass or more, more preferably 16% by mass or more, even more preferably 17% by mass or more, and particularly preferably 20% by mass or more. By increasing the proportion of the polyolefin resin, the overlap density of the molecular chains in the presence of the plasticizer increases, the uniformity of the stretching is improved, and the formation of coarse pores is suppressed, and it becomes possible to control the proportion of the number of pores having a pore diameter of more than 0 and less than 20 nm and the number of pores having a pore diameter of 20 to 40 nm. In addition, by increasing the proportion of the polyolefin resin, the increase in the stretching ratio and "hole collapse" during the washing and drying process are suppressed, and a good pore size distribution with few coarse pores is obtained.

[0052] When using a polyolefin resin with Mw of 1 million or more, from the viewpoint of the pressure and stretching stress in the film-forming process, the proportion of the polyolefin resin is preferably 30 mass% or less, more preferably less than 28.5 mass%, and even more preferably less than 25 mass%, based on 100 mass% of the total of the polyolefin resin and plasticizer.

[0053] In addition, the polyolefin microporous membrane according to an embodiment of the present invention may contain various additives such as antioxidants, heat stabilizers, antistatic agents, ultraviolet absorbers, antiblocking agents, fillers, etc., within the scope that does not impair the effects of the present invention. In particular, it is preferable to add an antioxidant for the purpose of suppressing oxidative deterioration of the polyolefin resin due to its thermal history.

[0054] As the antioxidant, it is preferable to use one or more selected from hindered phenol-based antioxidants such as 2,6-di-t-butyl-p-cresol (BHT: molecular weight 220.4), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., BASF's "Irganox" (registered trademark) 1330: molecular weight 775.2), and tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., BASF's "Irganox" (registered trademark) 1010: molecular weight 1177.7), and thiol-based antioxidants.

[0055] Appropriate selection of the type and amount of antioxidant and heat stabilizer is important for adjusting or enhancing the properties of the microporous polyolefin membrane.

[0056] The layer structure of the polyolefin microporous membrane according to the embodiment of the present invention may be a single layer or a laminate, and is preferably a laminate from the viewpoint of the balance of physical properties. When the microporous membrane obtained by the above-mentioned raw material formulation is laminated and used as a high-power characteristic layer, the high-power characteristic layer preferably accounts for 50 mass% or more of the total mass of the membrane. [3] Manufacturing method of polyolefin microporous membrane Next, the method for producing a polyolefin microporous membrane according to an embodiment of the present invention will be specifically described. The method for producing a polyolefin microporous membrane according to an embodiment of the present invention preferably includes the following steps (a) to (e) in this order. (a) Preparation of a polyolefin resin solution: A process of melt-kneading a polymer material containing one or more polyolefin resins and, if necessary, a solvent to prepare a polyolefin resin solution. (b) Formation of extrudate and gel-like sheet: A process of extruding the obtained polyolefin resin solution, forming it into a sheet, and cooling and solidifying it. (c) Stretching step: A step of stretching the obtained sheet by a roll method or a tenter method to obtain a stretched film. (d) Plasticizer extraction (washing) and drying process: A process for extracting the plasticizer from the obtained stretched film and drying the film. (e) Heat treatment / re-stretching process: a process for performing heat treatment / re-stretching Each step will be described below.

[0057] (a) Preparation of polyolefin resin solution The above polymer material is dissolved in a plasticizer under heating to prepare a polyolefin resin solution. The plasticizer is not particularly limited as long as it is a solvent that can sufficiently dissolve the polyolefin resin, but it is preferable that the solvent is liquid at room temperature in order to enable stretching at a relatively high ratio.

[0058] Examples of the solvent include aliphatic, alicyclic or aromatic hydrocarbons such as nonane, decane, decalin, paraxylene, undecane, dodecane, and liquid paraffin, as well as mineral oil fractions having boiling points corresponding thereto, and phthalate esters that are liquid at room temperature, such as dibutyl phthalate and dioctyl phthalate.

[0059] In order to obtain a gel-like sheet with a stable liquid solvent content, it is preferable to use a non-volatile liquid solvent such as liquid paraffin.

[0060] When the polymer material is melt-kneaded, a solvent that is miscible with the polyolefin resin but is solid at room temperature may be mixed with the liquid solvent. Examples of such solid solvents include stearyl alcohol, ceryl alcohol, paraffin wax, etc. However, if only a solid solvent is used, there is a risk of uneven stretching.

[0061] The viscosity of the liquid solvent is preferably 20 cSt or more at 40°C, and is preferably 200 cSt or less. If the viscosity at 40°C is 20 cSt or more, the sheet extruded from the die of the polyolefin resin solution is less likely to be non-uniform. On the other hand, if the viscosity at 40°C is 200 cSt or less, the liquid solvent is easily removed. The viscosity of the liquid solvent is measured at 40°C using an Ubbelohde viscometer.

[0062] The method of homogeneously melt-kneading the polyolefin resin solution is not particularly limited, but when preparing a high-concentration polyolefin resin solution, it is preferable to carry out the melt-kneading in a twin-screw extruder. If necessary, known additives such as metal soaps such as calcium stearate, ultraviolet absorbers, light stabilizers, and antistatic agents may be added within a range that does not impair the film-forming properties and does not impair the effects of the present invention. In particular, it is preferable to add an antioxidant to prevent oxidation of the polyolefin resin.

[0063] In the extruder, the polyolefin resin solution is mixed uniformly at a temperature at which the polyolefin resin is completely melted. The melt-kneading temperature varies depending on the polyolefin resin used, but is preferably (melting point of polyolefin resin + 10°C) or higher and preferably (melting point of polyolefin resin + 120°C) or lower. More preferably, it is (melting point of polyolefin resin + 20°C) or higher and (melting point of polyolefin resin + 100°C) or lower.

[0064] The melting point herein refers to a value measured by DSC (Differential Scanning Calorimetry) based on JIS K7121 (1987) (hereinafter the same).

[0065] For example, when the polyolefin resin is polyethylene, the melt-kneading temperature of the polyethylene resin is preferably 140° C. or higher, more preferably 160° C. or higher, and most preferably 170° C. or higher. The melt-kneading temperature is preferably 250° C. or lower, more preferably 230° C. or lower, and most preferably 200° C. or lower. Specifically, since the polyethylene composition has a melting point of about 130 to 140° C., the melt-kneading temperature is preferably 140° C. or higher, most preferably 180° C. or higher, and is preferably 250° C. or lower, and most preferably 230° C. or lower.

[0066] From the viewpoint of suppressing the deterioration of the polyolefin resin, the melt-kneading temperature is preferably low, but if the temperature is lower than the above, unmelted material may occur in the extrudate extruded from the die, which may cause film breakage in the subsequent stretching process. If the temperature is higher than the above, the thermal decomposition of the polyolefin resin becomes intense, and the physical properties of the obtained polyolefin microporous film, such as strength and porosity, may deteriorate. In addition, the decomposition product may precipitate on the chill roll or the roll in the stretching process, and adhere to the sheet, leading to deterioration of the appearance. Therefore, it is preferable to knead the melt-kneading temperature within the above range.

[0067] (b) Forming an extrudate and forming a gel-like sheet Next, the melt obtained in step (a) is extruded, and the resulting extrudate is cooled to obtain a gel-like sheet, and further cooling can fix the microphase of the polyolefin resin separated by the solvent.

[0068] In the cooling step, the gel-like sheet is preferably cooled to 10 to 50°C. This is to make the final cooling temperature below the crystallization end temperature, and by making the high-order structure consisting of polyolefin crystals finer, it becomes easier to perform uniform stretching in the subsequent stretching. Therefore, it is preferable to cool at least to the gelation temperature at a rate of 30°C / min or more.

[0069] Generally, when the cooling rate is slow, relatively large crystals are formed, which results in a coarse higher-order structure of the gel-like sheet, and the gel structure that forms the coarse crystals is also large. This makes it easier for coarse pores to form, making it difficult to obtain good output characteristics. In contrast, when the cooling rate is fast, small and uniform crystals are formed, which results in a dense higher-order structure of the gel-like sheet, leading to a uniform pore structure.

[0070] The cooling method may be a method of directly contacting the material with cold air, cooling water or other cooling medium, a method of contacting the material with a roll cooled with a cooling medium, or a method using a casting drum or the like.

[0071] Although the polyolefin microporous membrane has been described so far as a single layer, the polyolefin microporous membrane according to an embodiment of the present invention is not limited to a single layer and may be a laminate.

[0072] The number of layers is not particularly limited, and may be two layers or three or more layers. In addition to the polyolefin resin as described above, the laminated portion may contain desired resins to the extent that the effect of the present invention is not impaired.

[0073] Conventional methods can be used to laminate the polyolefin microporous membrane, for example, by preparing desired resins as needed, separately feeding these resins to an extruder and melting them at a desired temperature, joining them in a polymer tube or die, and extruding them through a slit die to the desired thickness of each layer to form a laminate.

[0074] (c) Stretching process The gel-like sheet (including the laminated sheet) thus obtained is stretched by a method such as uniaxial stretching in the sheet conveying direction (MD) by rolling or a roll stretching machine, uniaxial stretching in the sheet width direction (TD) by a tenter, sequential biaxial stretching by a combination of a roll stretching machine and a tenter or a combination of a tenter and a tenter, and simultaneous biaxial stretching by a simultaneous biaxial tenter.

[0075] The stretching ratio varies depending on the thickness of the gel-like sheet from the viewpoint of thickness uniformity, but it is preferable to stretch the sheet 7 times or more in any direction.

[0076] The area ratio of the stretching is preferably 45 times or more, more preferably 60 times or more, even more preferably 80 times or more, and particularly preferably 100 times or more. By setting the area ratio to 45 times or more, it is possible to prevent the formation of coarse pores due to insufficient stretching. On the other hand, the area ratio is preferably 150 times or less. If the area ratio is large, breakage tends to occur frequently during the production of the polyolefin microporous membrane, and productivity decreases.

[0077] From the viewpoint of improving the stretching uniformity in the stretching process and controlling the pore size distribution observed by surface SEM, the preferred form of the stretching ratio and raw material composition is to wet-stretch a raw material having a Mw of 1 million or more at an areal magnification of 60 times or more, more preferably at 80 times or more, and even more preferably at 100 times or more. A particularly preferred form is to wet-stretch a raw material having a Mw of 2 million or more at an areal magnification of 80 times or more, and most preferably to wet-stretch in MD direction x TD direction = 10 x 10 times or more.

[0078] The stretching temperature is preferably set to (melting point of the gel-like sheet + 10° C.) or lower, and more preferably within the range of (crystal dispersion temperature Tcd of the polyolefin resin) to (melting point of the gel-like sheet + 5° C.).

[0079] Specifically, since the polyethylene composition has a crystal dispersion temperature of about 90 to 110° C., the stretching temperature is preferably 100° C. or higher, more preferably 110° C. or higher, and preferably 130° C. or lower, more preferably 125° C. or lower, and even more preferably 120° C. or lower. The crystal dispersion temperature Tcd is determined from the temperature characteristics of dynamic viscoelasticity measured in accordance with ASTM D 4065 (2012).

[0080] When the stretching temperature is 90°C or higher, the pores are sufficiently opened due to low-temperature stretching, and the membrane is easily uniform and has a high porosity. On the other hand, when the stretching temperature is 130°C or lower, the gel-like sheet melts, which can prevent the pores from becoming blocked.

[0081] The above-mentioned stretching causes the higher-order structure of the gel-like sheet to be cleaved, the polyolefin crystal phase to be finer, and a large number of fibrils are formed. The fibrils have a three-dimensionally irregularly connected network structure, and stretching improves the mechanical strength and forms uniform pores with few coarse pores. Therefore, the polyolefin microporous membrane according to the embodiment of the present invention is suitable for battery separators. Furthermore, since the membrane has a uniform fine structure, there is less bleeding out of plasticizers and the like even when stretched at a higher stretching temperature than in the conventional technology, and process stability is improved.

[0082] In addition, by stretching before removing the plasticizer, the polyolefin resin is in a sufficiently plasticized and softened state, so that the higher-order structure is smoothly cleaved and the crystal phase can be uniformly refined. In addition, since the higher-order structure is easily cleaved, distortion during stretching is unlikely to remain, and the shrinkage rate can be reduced compared to the case of stretching after removing the plasticizer.

[0083] (d) Plasticizer extraction (washing) and drying process Next, the plasticizer (solvent) remaining in the gel-like sheet is removed using a cleaning solvent. Since the polyolefin resin phase and the solvent phase are separate, a microporous polyolefin membrane is obtained by removing the solvent.

[0084] Examples of the cleaning solvent include saturated hydrocarbons such as pentane, hexane, and heptane; chlorinated hydrocarbons such as methylene chloride and carbon tetrachloride; ethers such as diethyl ether and dioxane; ketones such as methyl ethyl ketone; and chain fluorocarbons such as ethane trifluoride.

[0085] These cleaning solvents have low surface tension (for example, 24 mN / m or less at 25°C). By using a cleaning solvent with low surface tension, the network structure that forms the micropores is prevented from shrinking due to the surface tension at the air-liquid interface during drying after cleaning, and a polyolefin microporous membrane with excellent porosity and permeability is obtained. These cleaning solvents are appropriately selected depending on the plasticizer, and are used alone or in combination.

[0086] The cleaning method may be a method of immersing the gel-like sheet in a cleaning solvent and extracting it, a method of showering the cleaning solvent onto the gel-like sheet, or a combination of these methods. The amount of cleaning solvent used varies depending on the cleaning method, but is generally preferably 300 parts by mass or more per 100 parts by mass of the gel-like sheet.

[0087] The washing temperature may be 15 to 30° C., and is heated to 80° C. or lower as necessary. In this case, the longer the time for which the gel-like sheet is immersed in the washing solvent, the better from the viewpoints of increasing the washing effect of the washing solvent, preventing the physical properties (e.g., physical properties in the TD and / or MD) of the obtained polyolefin microporous membrane from becoming non-uniform, and improving the mechanical and electrical properties of the polyolefin microporous membrane.

[0088] The above-mentioned washing is preferably carried out until the residual solvent in the washed gel-like sheet, ie, the polyolefin microporous membrane, becomes less than 1 mass %.

[0089] Thereafter, the solvent in the polyolefin microporous membrane is removed by drying in a drying step. The drying method is not particularly limited, and may be a method using a metal heating roll or a method using hot air.

[0090] The drying temperature is preferably 40 to 100° C., more preferably 40 to 80° C. If the drying is insufficient, the porosity of the polyolefin microporous membrane decreases in the subsequent heat treatment, and the permeability deteriorates.

[0091] (e) Heat treatment / re-stretching process Subsequently, heat treatment / re-stretching may be performed. That is, the dried polyolefin microporous membrane may be stretched (re-stretched) at least uniaxially. The re-stretching may be performed by a tenter method or the like while heating the polyolefin microporous membrane, similarly to the above-mentioned stretching. The re-stretching may be uniaxial or biaxial. In the case of multi-stage stretching, it is preferable to perform simultaneous biaxial or sequential stretching in combination.

[0092] The re-stretching temperature is preferably equal to or lower than the melting point of the polyolefin resin composition, and more preferably within the range of (Tcd of the polyolefin resin composition - 20°C) to the melting point of the polyolefin resin composition. Specifically, in the case of a polyethylene composition, the re-stretching temperature is preferably equal to or higher than 70°C, more preferably equal to or higher than 110°C, even more preferably equal to or higher than 125°C, and even more preferably equal to or higher than 130°C. The re-stretching temperature is preferably equal to or lower than 135°C.

[0093] In particular, the weight average molecular weight is 1.0×10 6 If the weight average molecular weight is less than 1.0×10, the relaxation time is short, so when heat treatment / re-stretching is performed at a temperature of 130°C or higher, the fibrils melt and fuse, increasing the number of coarse pores and decreasing the porosity and number of pores, leading to a decrease in output characteristics. 6 The above polyethylene has a long relaxation time, so even if it is stretched and heat-set at a temperature of 130°C or higher, the melting and fusion of fibrils is suppressed, resulting in a microporous membrane with few coarse pores, and it is easy to control the pore size observed by surface SEM. As a result, good shrinkage rate and output characteristics are obtained. Weight average molecular weight is 1.0×10 6 When using the above polyethylene, it is preferable to heat fix it at a temperature of 130° C. or higher.

[0094] In the case of uniaxial stretching, the re-stretching ratio is preferably 1.01 to 2.0 times, and in particular, the ratio in the TD direction is preferably 1.1 times or more, more preferably 1.2 times or more, and is preferably 1.6 times or less, more preferably 1.4 times or less. In the case of biaxial stretching, it is preferable to stretch in the MD direction and the TD direction, respectively, by 1.01 to 2.0 times. The re-stretching ratio may be different between the MD direction and the TD direction. By re-stretching within the above-mentioned range, the porosity and permeability are increased, and the aggregation of fibrils due to necks can be suppressed, resulting in a uniform polyolefin microporous membrane with few coarse pores.

[0095] From the viewpoint of shrinkage rate and wrinkles and sagging, the relaxation rate from the maximum re-stretching ratio is preferably 20% or less, more preferably 10% or less, and even more preferably 5% or less. When the relaxation rate is 20% or less, a uniform fibril structure is easily obtained.

[0096] (f) Other processes Furthermore, depending on other applications, the polyolefin microporous membrane may be subjected to a hydrophilization treatment. The hydrophilization treatment may be performed by monomer grafting, surfactant treatment, corona discharge, etc. The monomer grafting is preferably performed after the crosslinking treatment.

[0097] The microporous polyolefin membrane is preferably crosslinked by irradiation with ionizing radiation such as α-rays, β-rays, γ-rays, or electron beams. In the case of electron beam irradiation, the electron beam dose is preferably 0.1 to 100 Mrad, and the acceleration voltage is preferably 100 to 300 kV. The crosslinking treatment increases the meltdown temperature of the microporous polyolefin membrane.

[0098] In the case of surfactant treatment, any of nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants can be used, but nonionic surfactants are preferred. The treatment can be performed by immersing the polyolefin microporous membrane in a solution prepared by dissolving the surfactant in water or a lower alcohol such as methanol, ethanol, or isopropyl alcohol, or by applying the solution to the polyolefin microporous membrane by a doctor blade method.

[0099] The polyolefin microporous membrane according to the embodiment of the present invention may be surface-coated with a fluorine-based resin porous body such as polyvinylidene fluoride or polytetrafluoroethylene, a porous body such as polyimide or polyphenylene sulfide, or an inorganic coating such as ceramic, for the purpose of improving the meltdown property or heat resistance when used as a battery separator. In particular, the polyolefin porous membrane obtained by the present embodiment has a fine and uniformly controlled pore size and fibril structure, so that clogging by coating materials can be suppressed and the like, and the membrane has excellent coatability.

[0100] The polyolefin microporous membrane obtained as described above can be used in various applications such as filters, fuel cell and lithium ion battery separators, and capacitor separators. In particular, when used as a separator for a nonaqueous electrolyte secondary battery, it has excellent safety and output characteristics. Therefore, the polyolefin microporous membrane can be preferably used as a battery separator for nonaqueous electrolyte secondary batteries that require high energy density, high capacity, and high output, such as electric vehicles. Therefore, the present invention also relates to a nonaqueous electrolyte secondary battery having the polyolefin microporous membrane. EXAMPLES

[0101] The present invention will be described in more detail with reference to examples, but the embodiments of the present invention are not limited to these examples.

[0102] The evaluation and analysis methods used in the examples are as follows.

[0103] The molecular weight distribution of the polyolefin (weight average molecular weight, molecular weight distribution, content of specific components, etc.) was measured by high-temperature gel permeation chromatography (GPC) under the following measurement conditions.

[0104] Equipment: High temperature GPC equipment (Equipment No. HT-GPC, manufactured by Polymer Laboratories, PL-220) Detector: Differential refractive index detector RI Guard column: Shodex G-HT Column: Shodex HT806M (2 columns) (φ7.8mm×30cm, Showa Denko) Solvent: 1,2,4-trichlorobenzene (TCB, Wako Pure Chemical Industries, Ltd.) (0.1% BHT added) Flow rate: 1.0mL / min Column temperature: 145℃ Sample preparation: 5 mL of the measurement solvent was added to 5 mg of sample, and the mixture was heated and stirred at 160 to 170°C for about 30 minutes, after which the resulting solution was filtered through a metal filter (pore size 0.5 um).

[0105] Injection volume: 0.200mL Standard sample: Monodisperse polystyrene (manufactured by Tosoh) (PS) Data processing: TRC GPC data processing system The obtained Mw and Mn were then converted into polyethylene (PE) values ​​using the following conversion formula:

[0106] Mw (PE equivalent) = Mw (PS equivalent measurement value) x 0.468 Mn (PE conversion) = Mn (PS conversion measurement value) x 0.468 (2) Film thickness (μm) The thickness of the polyolefin microporous membrane was measured at five points within a 50 mm x 50 mm area using a contact thickness gauge, Litematic VL-50 (10.5 mmφ ultrahard spherical probe, measuring load 0.01 N) manufactured by Mitutoyo Corporation, and the average value was recorded as the thickness (μm). (3) Air permeability (sec / 100cm 3 ) For a polyolefin microporous membrane with a thickness of T1 (μm), the air permeability (sec / 100 cm) was measured in an atmosphere of 25°C using an Oken air permeability meter (manufactured by Asahi Seiko Co., Ltd., EGO-1T) in accordance with JIS P-8117. 3 The air permeability (converted to 10 μm) (sec / 100 cm) when the membrane thickness was 10 μm was also measured using the following formula: 3 ) was calculated.

[0107] Formula: Air permeability (10μm conversion) (sec / 100cm3 ) = Air permeability (sec / 100cm 3 )×10(μm) / polyolefin microporous membrane thickness(μm) (4) Porosity (%) A sample of 50 mm × 50 mm square was cut from the polyolefin microporous membrane, and its volume (cm) at room temperature (25°C) was measured. 3 ) and mass (g). These values ​​and the film density (g / cm 3 ) The porosity of the polyolefin microporous membrane was calculated from the following formula.

[0108] Porosity (%) = (volume-mass / film density) / volume x 100 The film density is 0.99 g / cm 3 The calculations were performed assuming a constant value of (5) 10μm equivalent puncture strength (N) The puncture strength was measured in accordance with JIS Z 1707 (2019), except that the test speed was 2 mm / sec. Using a force gauge (IMADA Co., Ltd., DS2-20N), the maximum load (N) was measured (L1) when a polyolefin microporous membrane was punctured in an atmosphere of 25°C with a 1.0 mm diameter needle with a spherical tip (radius of curvature R: 0.5 mm), and the puncture strength (L2) converted to a film thickness of 10 μm was calculated using the following formula. Formula: L2 = L1 × 10 (μm) / polyolefin microporous membrane thickness (μm) (6) Tensile breaking strength (MPa) A tensile test was performed using a tensile tester (Shimadzu Autograph AGS-J type), and the strength at the time of sample breakage was divided by the cross-sectional area of ​​the sample before the test to obtain the tensile breakage strength (MPa). The measurement conditions were: temperature; 23 ± 2°C, sample shape; width 10 mm × length 50 mm, chuck distance; 20 mm, and tensile speed; 100 mm / min. The above measurements were performed at three points each in the MD and TD directions at different locations on the same film, and the average value of the three points was used as the tensile breakage strength in each direction (MD tensile breakage strength, TD tensile breakage strength). (7) Tensile elongation at break (%) A tensile test was performed using a tensile tester (Shimadzu Autograph AGS-J type), and the tensile breaking elongation was calculated from the gauge length L0 (mm) of the test piece before the test and the gauge length L (mm) at break using the following formula. The measurement conditions were: temperature: 23 ± 2°C, sample shape: width 10 mm × length 50 mm, chuck distance: 20 mm, and tensile speed: 100 mm / min. The above measurements were performed at three points each in the MD and TD directions at different locations on the same film, and the average value of the three points was taken as the tensile breaking elongation in each direction (MD tensile breaking elongation, TD tensile breaking elongation).

[0109] Tensile elongation at break (%) = ((L-L0) / L) x 100 (7) Shrinkage rate (%) at 105℃ / 8h Three 50 mm square test pieces were cut from the center of the width of the polyolefin microporous membrane, and the shrinkage (heat shrinkage) in the MD direction was measured for each of them when they were kept at 105°C for 8 hours, and the average value was taken as the shrinkage in the MD direction (MD shrinkage). The same measurement was also performed in the TD direction to obtain the shrinkage in the TD direction (TD shrinkage). (8) Porometer calculated pore size (nm) Using a perm porometer (CFP-1500A, manufactured by PMI), the maximum pore size and average pore size were measured in the order of dry-up and wet-up. For wet-up, pressure was applied to a polyolefin microporous membrane sufficiently soaked in Galwick (trade name) manufactured by PMI, which has a surface tension of 15.6 dynes / cm, and the pore size calculated from the pressure at which air begins to penetrate was taken as the maximum pore size calculated by the porometer.

[0110] The average pore size calculated by the porometer was calculated from the pressure at the point where the curve showing half the slope of the pressure-flow curve in the dry-up measurement intersects with the curve in the wet-up measurement. The following formula was used to convert between pressure and average pore size.

[0111] d=C·γ / P (In the above formula, "d (μm)" is the average pore size of the polyolefin microporous membrane, "γ (mN / m)" is the surface tension of the liquid, "P (Pa)" is the pressure, and "C" is a constant. (9) Surface SEM calculated pore diameter (nm) The secondary electron images of the surface of the Pt-deposited polyolefin microporous membrane were observed using a scanning electron microscope (SEM) at an accelerating voltage of 2 kV, a magnification of 10,000 times, and a field of view of 11.7 μm × 9.4 μm. The captured surface SEM image was binarized using HALCON 13 from MVTec Software to extract voids.

[0112] The images before binarization were images with an accelerating voltage of 2 kV, a magnification of 10,000 times, 11.7 μm × 9.4 μm (1280 pixels × 1024 pixels), and 8-bit (256 gradations) grayscale.

[0113] The image processing method involved removing noise from the above surface SEM image by averaging 3 pixels x 3 pixels, and then performing dynamic binarization processing from the 21 pixel x 21 pixel average image using a threshold value of -30 gradations to extract dark areas (image processing 1), and counting independent dark areas as holes.

[0114] Furthermore, the diameter of the hole equivalent to a circle is calculated from the area of ​​each independent hole, and a cumulative frequency distribution is created from the frequency distribution of the hole diameters. 50 The pore size calculated by SEM was determined as the average pore size. Number of holes with a given diameter Percentage (SEM calculated pore size ratio of 0 to less than 20 nm), 20 to 40 nm Number of holes with a given diameter The ratio of the pore size ratio of more than 0 and less than 20 nm to the pore size ratio of 20 to 40 nm (pore size ratio of more than 0 and less than 20 nm / 20 to 40 nm) was calculated as the pore size ratio of more than 0 and less than 20 nm / the pore size ratio of 20 to 40 nm calculated from the frequency distribution. (11)Resistance value (Ω) In order to evaluate the ionic resistance when the polyolefin microporous membrane was used as a separator for a nonaqueous electrolyte secondary battery, a charge-discharge test was performed by incorporating the polyolefin microporous membrane as a separator in a nonaqueous electrolyte secondary battery consisting of a positive electrode, a negative electrode, a separator, and an electrolyte.

[0115] Weight of 9.5mg / cm on aluminum foil measuring 38mm wide x 33mm long x 20μm thick2 NMC532 (Lithium Nickel Manganese Cobalt Complex Oxide (Li 1.05 Ni 0.50 Mn 0.29 Co 0.21 O2)) on a positive electrode and a copper foil with a density of 1.45 g / cm 3 of natural graphite with a unit area mass of 5.5 mg / cm 2 The positive and negative electrodes were dried in a vacuum oven at 120°C before use.

[0116] The resulting microporous polyolefin membrane having a length of 50 mm and a width of 50 mm was dried in a vacuum oven at room temperature and used as a separator.

[0117] The electrolyte was prepared by dissolving vinylene carbonate (VC) and LiPF6 in a mixture of ethylene carbonate / ethyl methyl carbonate / dimethyl carbonate (volume ratio: 30 / 35 / 35) to prepare a solution with a VC concentration of 0.5 mass% and a LiPF6 concentration of 1 mol / L.

[0118] The positive electrode, separator and negative electrode were stacked in this order, and the resulting laminate was placed in a laminate pouch. An electrolyte was poured into the laminate pouch, and the laminate pouch was vacuum-sealed to prepare a nonaqueous electrolyte secondary battery.

[0119] The internal resistance of the fabricated nonaqueous electrolyte secondary battery was determined by low-frequency AC-IR measurement.

[0120] Specifically, impedance measurements were performed under the conditions of a frequency range of 0.1 to 316227 Hz, an amplitude voltage of 20 mV, and a measurement temperature of 25° C., and the point of Z″=0 in the obtained Cole-Cole plot was taken as the resistance value. [Example 1] Raw material Mw is 20 x 10 5 30 parts by mass of ultra-high molecular weight polyethylene having Mw of 5×10 571.5 parts by mass of liquid paraffin was added to 28.5 parts by mass of a polyethylene mixture blended in a ratio of 70 parts by mass of high density polyethylene, and 0.5 parts by mass of 2,6-di-t-butyl-p-cresol and 0.7 parts by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, based on the mass of the ultra-high molecular weight polyethylene, were further added and mixed as antioxidants to prepare a polyethylene resin solution.

[0121] The obtained polyethylene resin solution was charged into a twin-screw extruder and kneaded at 180°C, and then fed to a T-die. The extrudate was cooled with a cooling roll controlled at 15°C to form a gel-like sheet.

[0122] The obtained gel-like sheet was simultaneously biaxially stretched 10 times in both the longitudinal and transverse directions at 115°C using a batch-type tenter stretching machine, and the sheet width was fixed in the tenter stretching machine and held at 115°C for 10 seconds.

[0123] The stretched gel-like sheet was then immersed in a methylene chloride bath in a washing tank to remove the liquid paraffin, and then dried to obtain a polyolefin microporous membrane.Finally, the sheet was heat-set in an oven at 125°C for 10 minutes without stretching.

[0124] The raw material formulation and film-forming conditions of the polyolefin microporous membrane are as shown in the production method in Table 1. The evaluation results of the polyolefin microporous membrane are shown in the physical properties in Table 1. In the table, "MD" means MD direction, and "TD" means TD direction. [Examples 2 to 8, Comparative Examples 1 to 9] A polyolefin microporous membrane was produced in the same manner as in Example 1, except that the raw material formulation and film-forming conditions were changed as described in the manufacturing method in Table 1 or Table 2. In addition, in the "wet stretching method" and "dry re-stretching method" in Tables 1 and 2, "sequential" means sequential stretching, that is, uniaxial stretching in the MD direction and then uniaxial stretching in the TD direction. In addition, "simultaneous" means simultaneous biaxial stretching, that is, simultaneous stretching in the MD direction and the TD direction. The "dry re-stretching method" means stretching after removing liquid paraffin and drying after wet stretching.

[0125] The physical properties of the obtained microporous polyolefin membrane are shown in Table 2.

[0126] In Tables 1 and 2, "UHPE" means ultra-high molecular weight polyethylene, and "HDPE" means high density polyethylene. The evaluation results of the obtained polyolefin microporous membrane are shown in Table 1. In the wet stretching step, the upper surface of the sample when it was set in the tenter stretching machine was Side A, and the opposite surface was Side B.

[0127] [Table 1]

[0128] [Table 2]

[0129] The above results suggest that the polyolefin microporous membrane according to the present embodiment has high strength while maintaining a low shrinkage rate, and that when used as a separator for a nonaqueous electrolyte secondary battery, the internal resistance of the battery can be reduced and good output characteristics of the secondary battery can be obtained.

Claims

1. A polyolefin microporous membrane, in which, in a pore size distribution obtained by binarizing a surface scanning electron microscope image, the proportion of the number of pores having a pore size of 20 to 40 nm is 28% or more and 50% or less, and the proportion of the number of pores having a pore size of more than 0 and less than 20 nm is 16% or more and 30% or less, and the average pore size obtained using a porometer is less than 40 nm.

2. The polyolefin microporous membrane according to claim 1, wherein a ratio of the pore size ratio of more than 0 and less than 20 nm to the pore size ratio of 20 to 40 nm (pore size ratio of more than 0 and less than 20 nm / pore size ratio of 20 to 40 nm) is less than 0.

75.

3. The polyolefin microporous membrane according to claim 1 or 2, having a 10 μm converted pin puncture strength of 4.0 N or more.

4. The polyolefin microporous membrane according to any one of claims 1 to 3, having a shrinkage rate in the MD direction of 25% or less at 105°C / 8h.

5. The microporous polyolefin membrane according to any one of claims 1 to 4, having an average pore size of 45 nm or less, obtained by binarizing a surface scanning electron microscope image.

6. A polyolefin microporous membrane described in any one of claims 1 to 5, wherein the difference between the average pore diameter obtained by binarizing a surface scanning electron microscope image and the average pore diameter obtained using a porometer is 20 nm or less.

7. The microporous polyolefin membrane according to any one of claims 1 to 6, having a porosity of 50% or less.

8. The polyolein microporous membrane according to any one of claims 1 to 7, having a membrane thickness of 12 µm or less.

9. A non-aqueous electrolyte secondary battery comprising the polyolefin microporous membrane according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Separator for battery and its manufacture

    JP2000195490A

  • Microporous polyethylene membrane and method for producing the same, and battery separator

    JP2007106992A

  • Polyolefin microporous membrane and method for producing the same

    JP2008081513A

  • Polyolefin multilayer microporous membrane, method for producing the same, separator for battery and battery

    JP2008255306A

  • Polyolefin microporous film, nonaqueous secondary battery separator, and nonaqueous secondary battery

    JP2012048987A