The container design addresses the issue of lid peeling by using a cup and lid laminate structure with specific resin compositions, ensuring strong adhesion and clean peeling, maintaining heat resistance and reliability.
Patent Information
- Application Number
- JP2021030659
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-02-26
AI Technical Summary
The existing paper cups with heat-sealable lids made of polypropylene resin face issues with the lid material not peeling off cleanly due to insufficient adhesion or the paper peeling off during heating.
A container design using a cup and lid laminate structure where the cup's flange is sealed with a lid material containing a polypropylene resin sealant layer with a melt flow rate of 15-60 g/10 min and a polyethylene resin base layer, and the lid material has a polyethylene resin sealant layer with a tackifier or polystyrene resin, ensuring a sealing strength of 8 kPa or more.
The design provides a container with good peeling characteristics, maintaining heat resistance and ensuring reliable bonding without deformation or peeling issues during heating.
Smart Images

Figure 0007567553000003 
Figure 0007567553000004 
Figure 0007567553000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a container comprising a cup having a lid. In a vessel Regarding. [Background technology]
[0002] Conventionally, containers such as paper cups have been made of a laminate with a sealant layer applied to a paper base material, and polyethylene (PE) resin has been mainly used for the sealant layer to ensure heat sealability and flexibility of the laminate. Recently, there has been a demand for such containers to be heated in a microwave oven, but the heat resistance of the laminate with the above-mentioned polyethylene resin as the sealant layer is insufficient. Therefore, a paper cup has been proposed in which a polypropylene resin, which has higher heat resistance than polyethylene resin, is used as the sealant layer (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-95350 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, with the paper cup described in Patent Document 1, when the opening of the cup is closed with a lid material that can be opened by heat sealing, there are cases where the closed lid material cannot be peeled off from the opening or the paper peels off.
[0005] SUMMARY OF THE PRESENT EMBODIMENT In order to solve the above problems, an object of the present invention is to provide a container and a lid having good peeling properties. [Means for solving the problem]
[0006] The present invention solves the above problems by the following solving means. Note that, for ease of understanding, the following description will be given with reference numerals corresponding to the embodiments of the present invention, but the present invention is not limited thereto.
[0007] The first invention relates to a container (1) comprising a cup (10) having a body (11) and a bottom (12), and a lid (20) for closing an opening provided in the body, wherein the body and the bottom are made of a first laminate (100) having a first paper base layer (101) and a first sealant layer (102) provided on at least one side of the first paper base layer, the opening of the body is provided with a flange portion (13) formed by folding back the first laminate so that the first sealant layer is exposed, and the lid is made of a base layer (201) and a sealant layer (102) provided on at least one side of the base layer. the first laminate (200) having a sealant film layer (202) and a base layer (202A) joined to the flange portion, the sealant film layer having a base layer (202A) and a second sealant layer (202B) joined to the flange portion, the first sealant layer contains a polypropylene-based resin and has an MFR value of 15 g / 10 min or more and 60 g / 10 min or less, the base layer is made of a polyethylene-based resin, and the second sealant layer is mainly composed of a polyethylene-based resin and contains a tackifier or a polystyrene-based resin. It is.
[0008] A second invention is a container (1) of the first invention, characterized in that the base material layer (201) of the second laminate (200) is a second paper base material layer, and the second paper base material layer accounts for more than half of the total mass of the lid material.
[0009] A third invention is the container (1) of the first or second invention, characterized in that the sealing strength between the flange portion (13) of the cup and the lid material (20) is 8 kPa or more.
[0010] The fourth invention is a lid material (20) for closing the opening of a cup (10), the lid material being made of a second laminate (200) having a second paper base layer (201) and a sealant film layer (202) provided on one side of the second paper base layer, the sealant film layer having a base layer (202A) and a second sealant layer (202B) joined to the opening, the base layer being made of a polyethylene-based resin, the second sealant layer being mainly composed of a polyethylene-based resin and containing a tackifier or a polystyrene-based resin, and the second paper base layer accounting for more than half of the total mass of the lid material. Effect of the Invention
[0011] According to the present invention, it is possible to provide a container and a lid having good peeling properties. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a perspective view of a container according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a lid and a cup heat-sealed to a flange portion. [Diagram 3] FIG. 2 is a diagram illustrating a layer structure of a first laminate used in a cup. [Figure 4] FIG. 2 is a diagram illustrating the layer structure of a second laminate used in the lid material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The container having a lid material of the present invention will be described below with reference to the drawings. FIG. 1 is a perspective view of a container according to an embodiment. FIG. 2 is a cross-sectional view of the lid and cup heat-sealed to the flange portion. Note that the following figures, including Fig. 1, are schematic views, and the size and shape of each part are appropriately exaggerated for ease of understanding. Furthermore, as described below, the body 11 and the lid 20 are composed of a first laminate and a second laminate having multiple layers, but Fig. 2 shows only the first sealant layer 102 and the second sealant layer 202B located on the inner side of the cup, and omits the other layers.
[0014] (container) 1, container 1 includes cup 10 and lid 20, and can accommodate contents such as food in the container portion of cup 10 and seal with lid 20. Container 1 of this embodiment can heat and cook the contents stored in cup 10 while still in cup 10 by using a microwave oven. For this reason, cup 10 and lid 20 are each made of a heat-resistant material so as not to cause phenomena such as foaming or melting when heated.
[0015] (10 cups) The cup 10 is a vessel formed into a truncated cone shape, and is composed of a body 11, a bottom 12, and a flange 13. The body 11, bottom 12, and flange 13 of the cup 10 are formed using a first laminate 100 including a first paper base layer 101 as a constituent material. Details of the first laminate 100 will be described later. The body 11 is a cylindrical portion that forms the peripheral side surface of the truncated cone of the cup 10, with a bottom 12 disposed on one end edge of the cylinder and a flange portion 13 formed on the other end edge. The bottom portion 12 is a member that constitutes the bottom portion of the cup 10, and is formed from a separate member from the body portion 11.
[0016] The flange portion 13 is formed on the edge of the opening of the cup 10, and is formed by folding back the edge of the first laminate 100 constituting the body portion 11 towards the outside of the cup 10, as shown in Fig. 2. Therefore, the flange portion 13 is formed integrally with the body portion 11. In this way, by providing the flange portion 13 on the body portion 11, the rigidity of the opening of the cup 10 can be increased, and deformation of the cup 10 when the cup 10 is carried can be suppressed. Furthermore, by providing the flange portion 13, the lid member 20 can be easily joined to the cup 10. Here, a first sealant layer 102 (described later) is provided on one surface of the first laminate 100, and the first laminate 100 constituting the body 11 and the bottom 12 is disposed so that the first sealant layer 102 is located on the inner side of the cup 10, as shown in Fig. 2. Therefore, the first sealant layer 102 is exposed on the surface of the flange 13 formed by folding back the edge of the body 11.
[0017] (Lid material 20) Lid material 20 is a member that seals the opening of cup 10, and is removably joined to flange portion 13 provided on cup 10. Lid material 20 is formed using second laminate 200 as a constituent material, and is joined to flange portion 13 of cup 10 such that second sealant layer 202B provided on one surface of second laminate 200 is positioned on the cup 10 side, as shown in Fig. 2. Details of second laminate 200 will be described later. Here, as described above, the first sealant layer 102 of the first laminate 100 is exposed on the surface of the flange portion 13, and this first sealant layer 102 is heat sealed to the second sealant layer 202B of the second laminate 200 that constitutes the lid material, thereby making it possible to peelably seal the opening of the cup 10 with the lid material 20.
[0018] From the viewpoint of ensuring a more reliable bond between the lid material 20 and the cup 10 (flange portion 13), the bond width t of the lid material 20 on the flange portion 13 in the cross section shown in FIG. 2 is preferably 1 mm or more and 4 mm or less. If the bond width t is less than 1 mm, the bond area of the lid material 20 becomes too narrow, the lid material 20 cannot be stably bonded to the cup 10, and the sealing strength decreases, which is undesirable. If the bond width t exceeds 4 mm, the width dimension of the flange portion 13 must also be increased, which undesirably results in an excessively large outer shape of the cup 10. If the bond area of the lid material 20 becomes too large, it may be difficult to peel off the lid material 20, which is undesirable.
[0019] (First laminate) Next, the first laminate 100 constituting the cup 10 will be described. FIG. 3 is a diagram illustrating the layer structure of the first laminate used in the cup. The first laminate 100 is a component that constitutes the body 11, bottom 12, and flange 13 of the cup 10, and is composed of, in order from the inner side of the cup 10, a first sealant layer 102, a first paper base layer 101, and a surface resin layer 103.
[0020] The first paper substrate layer 101 is a paper substrate that serves as the base of the first laminate 100, and may be, for example, uncoated paper, craft paper, or recycled paper of known origin. The basis weight of the first paper substrate layer 101 is set to 150 g / m2 from the viewpoint of favorable molding of the cup 10. 2 More than 350g / m 2 It is preferable that the weight is less than 180 g / m 2 More than 240g / m 2 It is more preferable that the basis weight of the first paper base layer 101 is 150 g / m 2 If the basis weight of the first paper base layer 101 is less than 350 g / m, the buckling strength of the molded cups is not sufficient, and if a part of the cup breaks due to the pressure when stacked, the cups become stuck together and cannot be removed, or even a slight drop can cause the flanges to deform, making handling difficult, which is not preferable. 2If it is larger than this, it is not preferable because the curling of the flange portion cannot be stably performed at high speed.
[0021] The first sealant layer 102 is the layer located on the innermost side of the cup 10, and has heat sealability, which is an adhesive property when heated. The first sealant layer 102 is mainly composed of polypropylene (PP) resin from the viewpoint of combining good heat resistance and heat sealability. Examples of the polypropylene resin used in the first sealant layer 102 include homopolypropylene, random polypropylene, and block polypropylene. Copolymer polypropylene in which a part of propylene is replaced with another monomer may also be used. In the present invention, it is preferable to use a homopolymer from the viewpoint of obtaining high heat resistance. Furthermore, the MFR (melt flow rate) value of the polypropylene resin forming the first sealant layer 102 is desirably 15 g / 10 min or more and 60 g / 10 min or less, more desirably 30 g / 10 min or more and 50 g / 10 min or less, and even more desirably 35 g / 10 min or more and 45 g / 10 min or less.
[0022] If the MFR value is less than 15 g / 10 min, when forming the first sealant layer 102 by extrusion molding on the first paper base layer 101, the fluidity of the resin when molten is low, which is undesirable as it reduces adhesion to the first paper base layer 101. If the MFR value is greater than 60 g / 10 min, a neck-in phenomenon occurs in which the extruded resin becomes narrower than the effective width of the die, making it difficult to form the first laminate 100, and phenomena such as foaming and melting during heating may also occur, which is undesirable.
[0023] From the viewpoint of being heat-sealed without gaps by heating, the thickness of the first sealant layer 102 is desirably 15 μm to 50 μm, and more desirably 20 μm to 40 μm. If the thickness of the first sealant layer 102 is 15 μm or more, for example, when the body portion 11 is produced using the first laminate 100, the heat seal strength can be sufficiently maintained in the joining of the edges of the body portion 11. Also, sufficient pinhole resistance can be ensured. Furthermore, by making the thickness of the first sealant layer 102 50 μm or less, it is possible to minimize the amount of plastic used while maintaining the stiffness of the original body fabric. Furthermore, when creating blanks for the body 11 and bottom 12 by punching, it is possible to minimize the occurrence of burrs and punching defects. For the first sealant layer 102, for example, PHA03A manufactured by SunAllomer Corporation, which is a homopolymer type polypropylene resin and has an MFR value of 42 g / 10 min, can be used.
[0024] The surface resin layer 103 is the layer located on the outermost side of the cup 10, and protects the outer surface of the first paper base layer 101. The surface resin layer 103 also has heat sealability, which means adhesive properties when heated. From the viewpoint of preventing curling of the first laminate 100, the surface resin layer 103 is desirably formed of the same material as the first sealant layer 102, to the same thickness, and by the same method. The outer surface of the first paper base layer 101 may be printed, and in that case, it is preferable that the surface resin layer 103 is transparent or nearly transparent so that the printed content can be visually recognized.
[0025] (Second laminate) Next, the second laminate 200 constituting the lid member 20 will be described. FIG. 4 is a diagram illustrating the layer structure of the second laminate used in the lid. As shown in Figure 4, the second laminate 200 is formed by laminating, in order from the inner side of the cup 10, a sealant film layer 202, an adhesive layer 205, a first resin layer 203, an adhesive layer 205, a second paper base layer 201, an adhesive layer 205, a printing layer 206, and a second resin layer 204.
[0026] The second paper substrate layer 201 is a paper substrate that serves as the base of the second laminate 200, and may be, for example, uncoated paper, coated paper, or wood-free paper. The basis weight of the second paper substrate layer 201 is set to 40 g / m2 in order to ensure the flexibility of the lid material 20 that can be peeled off from the cup 10. 2 More than 100g / m 2 It is preferable that the thickness is less than 70 g / m 2 More than 90g / m 2 It is more preferable that the basis weight of the first paper base layer 101 is 40 g / m 2 If the basis weight of the first paper base layer 101 is less than 100 g / m, the thickness of the cover material 20 is too thin and the cover material 20 may curl in an unintended direction, which is not preferable. 2 If it is larger than this, the thickness of the lid material 20 becomes too thick, the flexibility of the lid material 20 decreases, and the workability of opening the container 1 decreases, which is undesirable. Here, the lid material 20 formed from this second laminate 200 is formed so that the second paper base layer 201 accounts for more than half of the total mass of the entire lid material 20. As a result, the lid material 20 (second laminate 200) can reduce the amount of fossil fuel used and reduce the environmental burden.
[0027] The sealant film layer 202 is the layer of the lid material 20 located closest to the cup 10. The sealant film layer 202 is a film in which a base layer 202A and a second sealant layer 202B are laminated in this order from the first resin layer 203 side. The sealant film layer 202 is bonded to the first resin layer 203 by, for example, a dry lamination method via an adhesive layer 205 made of a lamination adhesive. The lamination adhesive used may be a conventionally known adhesive, such as a urethane adhesive, an acrylic adhesive, or an isocyanate adhesive. The base layer 202A is a base material that is the foundation of the sealant film layer 202, and may be made of, for example, a polyethylene-based resin, a polypropylene-based resin, or the like, with the use of a polyethylene-based resin being particularly desirable.
[0028] The second sealant layer 202B is the layer of the lid material 20 closest to the cup 10, and has heat sealability, which is an adhesive property when heated. The second sealant layer 202B is mainly composed of a polyethylene resin, and further contains a tackifier or a polystyrene resin. Here, the main component refers to a component whose content in the target layer (here, the second sealant layer 202B) is 41% or more by mass, preferably 50% or more, and more preferably 60% or more. Examples of the polyethylene-based resin include low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE). In addition to these homopolymers, copolymerized polyolefins in which part of the ethylene is replaced with other monomers may also be used. Specifically, examples include ethylene-vinyl acetate copolymer (EVA), ethylene-methyl acrylate copolymer (EMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-butyl acrylate copolymer (EBA), and ethylene-methyl methacrylate copolymer (EMMA). The content of the polyethylene-based resin in the second sealant layer 202B is preferably 41% by mass or more and 95% by mass or more.
[0029] Examples of the tackifier include aliphatic hydrocarbon resins including alicyclic hydrocarbon resins (alicyclic resins), aromatic hydrocarbon resins, rosins, polyterpene resins, and the like. Examples of the aliphatic hydrocarbon resin include polymers mainly composed of monoolefins or diolefins having 4 to 5 carbon atoms, such as butene-1, butadiene, isobutylene, and 1,3-pentadiene; resins polymerized from cyclic monomers, such as resins polymerized by cyclizing and dimerizing diene components in cyclopentadiene and spent C4 to C5 fractions, and resins obtained by intracyclic hydrogenation of aromatic hydrocarbon resins. Examples of the aromatic hydrocarbon resin include resins mainly composed of vinyl aromatic hydrocarbons, such as α-methyltoluene, vinyltoluene, and indene. Examples of the rosins include rosin, polymerized rosin, rosin glycerin ester, hydrogenated rosin glycerin ester, polymerized rosin glycerin ester, rosin pentaerythritol ester, hydrogenated rosin pentaerythritol ester, and polymerized rosin pentaerythritol ester. Examples of polyterpene resins include hydrogenated terpene resins, terpene-phenol copolymer resins, dipentene polymers, α-pinene polymers, β-pinene polymers, α-pinene-phenol copolymer resins, etc. Further examples of synthetic resin tackifiers other than those mentioned above include acid-modified C5 petroleum resins, C5 / C9 copolymer petroleum resins, xylene resins, coumarone-indene resins, etc. Polystyrene-based resins are resins mainly composed of styrene, such as styrene homopolymers, copolymers of styrene with acrylonitrile or methyl methacrylate, or rubber-modified versions of these. Specific examples include polystyrene, impact-resistant polystyrene (rubber-blended polystyrene), AS resin (SAN), ABS, and SMA (styrene-maleic anhydride polymer). The content of the tackifier or polystyrene resin in the second sealant layer 202B is preferably 1 to 30 mass %, and more preferably 2 to 15 mass %, because this makes it easier to obtain good adhesion to the adherend and suitable film-forming properties.
[0030] From the viewpoint of being heat-sealed without gaps by heating, the thickness of the second sealant layer 202B is desirably 5 μm to 20 μm, and more desirably 8 μm to 15 μm. If the thickness of the second sealant layer 202B is 5 μm or more, for example, when the lid material 20 is heat-sealed to the flange portion 13 of the cup 10, the bonding strength (sealing strength) between the flange portion 13 and the lid material 20 can be sufficiently ensured. Furthermore, by making the thickness of the second sealant layer 202B 20 μm or less, the amount of plastic used can be minimized, and the amount of fossil fuel-derived materials used in the lid material 20 can be reduced as much as possible. Here, the sealing strength between the flange portion 13 and the lid material 20 is desirably 8 kPa or more in order to ensure sufficient airtightness by the lid material. If the sealing strength is less than 8 kPa, the airtightness by the lid material may be insufficient, or a part of the lid material 20 may peel off from the flange portion 13, which is undesirable.
[0031] The sealant film layer 202 may have an intermediate layer having a predetermined function between the base layer 202A and the second sealant layer 202B. For example, the intermediate layer may be provided to improve the adhesion between the base layer 202A and the second sealant layer 202B or to adjust the overall thickness of the sealant film layer 202. If the intermediate layer is to improve the adhesion between the base layer 202A and the second sealant layer 202B, it may be made of, for example, LLDPE or LDPE. If the overall thickness of the sealant film layer 202 is to be adjusted, it may be made of, for example, the same resin as the base layer 202A. A plurality of intermediate layers may be provided according to the needs of the required functions, etc.
[0032] The first resin layer 203 is a resin layer provided between the second paper base layer 201 and the sealant film layer 202, and is composed of, for example, a PET resin film (thickness 12 μm), and this film is bonded to the second paper base layer 201 by a dry lamination method via an adhesive layer 205 made of a lamination adhesive. The first resin layer 203 can be made of the above-mentioned PET resin, polyester resin such as PBT resin, polyamide resin, polypropylene resin, etc. The first resin layer 203 is preferably a stretched plastic film, and more preferably a biaxially stretched plastic film, and for example, a biaxially stretched PET film, a biaxially stretched PBT film, OPP, ONY, etc. can be used. The thickness of the first resin layer 203 is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 12 μm or more. The thickness of the first resin layer 203 is preferably 50 μm or less, and more preferably 25 μm or less. If the thickness of the first resin layer 203 is less than 5 μm, the processability in the bonding process with other materials is poor, and even if bonding is possible, the resin may peel off or break in a later process or during use, making it impossible to function as a lid material, which is not preferable. If the thickness of the first resin layer 203 is greater than 50 μm, the heat is difficult to propagate, narrowing the stable area of the seal, or the resin is too rigid, impairing the flexibility as a lid material, which is not preferable.
[0033] The second resin layer 204 is a resin layer provided on the surface of the second paper base layer 201 opposite to the first resin layer 203, and is made of, for example, a PET resin film (thickness 12 μm) similar to the above-mentioned first resin layer 203. The second resin layer 204 is bonded to the second paper base layer 201 by a dry lamination method via an adhesive layer 205 made of a lamination adhesive. The second resin layer 204 can be made of the above-mentioned PET resin, polyester resin such as PBT resin, polyamide resin, polypropylene resin, etc. The second resin layer 204 is preferably a stretched plastic film, more preferably a biaxially stretched plastic film, and for example, a biaxially stretched PET film, a biaxially stretched PBT film, OPP, ONY, etc. can be used. The thickness of the second resin layer 204 is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 12 μm or more. The thickness of the second resin layer 204 is preferably 50 μm or less, and more preferably 25 μm or less. If the thickness of the second resin layer 204 is less than 5 μm, it is not preferable because it is not suitable as a printing base material due to poor dimensional stability and has low strength, which makes it difficult to process in the bonding process with other materials. If the thickness of the second resin layer 204 is greater than 50 μm, it is not preferable because heat is not easily transmitted, which narrows the stable area of the seal, or the rigidity of the resin is too strong, which impairs the flexibility as a lid material. In this way, by arranging the first resin layer 203 and the second resin layer 204 so as to sandwich the second paper base layer 201, when the second laminate 200 is formed into a sheet, the amount of resin present on the front and back of the second paper base layer 201 can be made approximately equal, and curling of the second laminate 200 can be significantly suppressed. The second resin layer 204 is the layer located on the outermost side of the lid material 20, and protects the outer surface of the second paper base layer 201. In this embodiment, the second resin layer 204 has a printed layer 206 on its inner surface that displays information about the contents of the container 1. Therefore, the surface of the second resin layer 204 on which the printed layer 206 is provided is bonded to the second paper base layer 201 via an adhesive layer 205. It is desirable that the second resin layer 204 be transparent or nearly transparent so that the printed content of the printed layer 206 can be visually confirmed. In the above description, the printed layer 206 is provided on the inner surface of the second resin layer 204, but the present invention is not limited to this and may be provided on the outer surface of the second paper base layer 201. In this case, the second resin layer 204 is bonded to the printed layer 206 provided on the second paper base layer 201 via the adhesive layer 205.
[0034] Here, from the viewpoint of improving the peeling characteristics of the lid 20 and the cup 10, the sealant film layer 202 is desirably formed mainly in any one of the following modes.
[0035] (First embodiment of sealant film layer 202) The sealant film layer 202 of the first embodiment has a two-layer structure in which a second sealant layer 202B and a base layer 202A are laminated in this order from the cup 10 side. In this embodiment, the base layer 202A is preferably made of a polyethylene resin. The second sealant layer 202B of this embodiment contains a tackifier with a polyethylene resin as the main component, from the viewpoint of ensuring a good balance between heat sealability with the first sealant layer 102 of the cup 10 (first laminate 100) and ease of peeling. The thickness of the second sealant layer 202B is preferably 15% to 35% of the thickness of the base layer 202A. If the thickness of the second sealant layer 202B is less than 15% of the thickness of the base layer 202A, the second sealant layer 202B will break when heat-sealing with the first sealant layer 102 of the cup 10, and good peeling properties will not be obtained, which is not preferable. Also, if the thickness of the second sealant layer 202B is more than 35% of the thickness of the base layer 202A, the material cost will increase, which is not preferable.
[0036] The polyethylene resin that is the main component of the second sealant layer 202B is preferably linear low density polyethylene (LLDPE), and in this case, from the viewpoint of improving adhesion to the adherend, it is desirable for the MFR to be greater than 7 g / 10 min. The tackifier contained in the second sealant layer 202B contains at least one of an alicyclic resin and a rosin ester resin. In the present invention, the tackifier is added to the second sealant layer 202B to adjust the sealing property. It is preferable to use a tackifier made of a mixture of an alicyclic resin and a rosin ester resin. The tackifier is preferably contained in an amount of 1 to 30% by mass with respect to the total mass of the second sealant layer 202B. In addition to the above materials, an anti-blocking agent, a slip agent, etc. may be added to the second sealant layer 202B.
[0037] (Second embodiment of sealant film layer 202) The sealant film layer 202 of the second embodiment has a two-layer structure in which a second sealant layer 202B and a base layer 202A are laminated in this order from the cup 10 side. The base layer 202A of this embodiment contains linear low density polyethylene (LLDPE) and low density polyethylene (LDPE), and it is desirable for the linear low density polyethylene (LLDPE) content to be greater than the low density polyethylene (LDPE) content. In order to ensure a good balance between heat sealability with the first sealant layer 102 of the cup 10 (first laminate 100) and ease of peeling, the second sealant layer 202B of this embodiment contains a polyethylene (PE) resin as a main component, polypropylene resin, and polystyrene resin. Also, the second sealant layer 202B is preferably made of, in descending order of content, polyethylene resin, polypropylene resin, and polystyrene resin. In addition to the above materials, an anti-blocking agent and a slip agent may be added to the second sealant layer 202B.
[0038] (Another form of the second laminate) The second laminate 200 may be provided with a barrier resin layer instead of the first resin layer 203. That is, the second laminate 200 may be provided with a sealant film layer 202, an adhesive layer 205, a barrier resin layer, an adhesive layer 205, a second paper base layer 201, an adhesive layer 205, a printed layer 206, and a second resin layer 204, which are laminated in this order from the cup 10 side. This allows the second laminate 200 to be provided with barrier properties against oxygen and water vapor. The barrier resin layer may be a film obtained by depositing a metal oxide on a resin film such as PET. Examples of inorganic oxides that can be used for the deposition layer include aluminum oxide and titanium oxide, which are metal oxides of the above metals, and silica, which is an oxide of silicon (Si). In particular, it is preferable to provide a deposition film of aluminum oxide for packaging. An example of a film in which a metal oxide is deposited can be IB-PET (thickness 12 μm) manufactured by Dai Nippon Printing Co., Ltd.
[0039] In addition, the second laminate 200 may omit the second resin layer 204 depending on the application of the lid material 20. That is, the second laminate 200 may be configured such that, in order from the cup 10 side, the sealant film layer 202, the adhesive layer 205, the first resin layer 203, the adhesive layer 205, the second paper base material layer 201, and the printing layer 206 are laminated. In this case, since the amount of resin differs between the front and back of the second paper base material layer 201, if the second paper base material layer 201 is in a sheet-like form, curling occurs, making it difficult to use. However, if the second laminate 200 is wound and supplied and heat-sealed directly to the cup in-line, it can be used as a lid material even in this form.
[0040] Furthermore, the second laminate 200 may omit the first resin layer 203 and use a substrate other than paper, i.e., a substrate layer made of resin, as the second paper substrate layer 201, depending on the application of the lid material 20. In this case, the second laminate 200 is formed by laminating a sealant film layer 202, an adhesive layer 205, a substrate layer, an adhesive layer 205, a printing layer 206, and a second resin layer 204 in this order from the cup 10 side. In this case, the material of the base layer can be selected depending on the application, and a PET resin film (for example, 12 μm thick) or a biaxially oriented nylon film (for example, 15 μm thick) can be used.
[0041] (Selection of sealant film layer) Next, the selection of the sealant film layer 202 provided on the second laminate 200 constituting the lid material 20 will be described. Eight types of test specimens (test specimens 1 to 8) having sealant film layers with different layer configurations and materials were prepared as test specimens corresponding to the lid material, and each test specimen was heat-sealed to the flange portion 13 of the above-mentioned cup 10, and the sealing state and peeling properties between the test specimen and the cup (flange portion) were evaluated. In this evaluation, the sealant film layer of the test specimen that was evaluated as being good in both sealing strength and peeling properties was applied to the lid material 20.
[0042] For each specimen, the base layer side of the sealant film layer was bonded to a 12 μm thick PET resin film by the dry lamination method. The first laminate 100 constituting the cup 10 has a first paper base layer 101 with a basis weight of 220 g / m 2 The cup base paper was used, and the first sealant layer 102 and surface resin layer 103 were formed on each side of the first paper base layer 101 using a homopolymer type polypropylene resin (PHA03A, MFR=42g / 10min, manufactured by Sun Allomer Co., Ltd.) with a thickness of 20 μm.
[0043] Each test specimen was heat sealed to the flange 13 of the cup 10 at 150°C or 160°C for 1 second under 0.3 MPa, and the sealing strength of each test specimen to the flange and the peeling properties of each test specimen after sealing were evaluated when peeled from the flange. Details of the sealant film layer used for each test specimen and the evaluation results are summarized in Table 1 below. Here, as described above, if the sealing strength is 8 kPa or more, the lid material (test specimen) is sufficiently heat-sealed to the cup 10, and sufficient airtightness can be ensured. The sealing strength was measured using a sealing strength measuring device (Sun Scientific, SEAL TESTER FKT-100J). Using the measuring device, a needle was inserted into the bottom 12 of the cup 10 to allow air to flow in, and the maximum pressure until the heat seal between the cup and the lid material (test specimen) burst or air escaped was measured. The measuring device was set to a pressure of 0.07 MPa, and the air flow rate was set to apply a pressure of 0.013 MPa for 10 seconds. The peeling properties were evaluated by a subject's sensory assessment of whether the test piece heat-sealed to the cup could be peeled off with his or her hands with ease.
[0044] [Table 1]
[0045] As shown in Table 1, the sealant film layer of specimen 1 is made of 30μm thick Easy Peel Film 7601EA manufactured by Toray Advanced Film Co., Ltd., and has a two-layer structure consisting of a base layer and a second sealant layer laminated in that order. The base layer is made of polyethylene resin, and the second sealant layer is made of a resin in which a polybutene resin is added to a polyethylene resin. The peeling morphology of specimen 1 is the "cohesion" type. Here, "cohesion" type refers to a morphology in which the specimen (lid material) and the cup peel off due to internal destruction of the second sealant layer. When heat-sealing test piece 1 at 150°C, the sealing strength was less than 8 kPa, and sufficient sealing strength was not obtained. Regarding the peeling properties, the adhesion of test piece 1 to the cup was too weak, and it was in a so-called temporary state. Furthermore, even when heat-sealing test piece 1 at 160°C, the sealing strength was less than 8 kPa, and sufficient sealing strength was not obtained. Regarding the peeling properties, the adhesion of test piece 1 to the cup was too weak, being in a so-called temporary state.
[0046] The sealant film layer of specimen 2 is a 30μm thick Easy Peel Film 7601ED manufactured by Toray Advanced Film Co., Ltd., and has a two-layer structure consisting of a base layer and a second sealant layer laminated in that order. The base layer is made of polyethylene resin, and the second sealant layer is made of a resin in which polybutene resin is added to polyethylene resin. The peeling mode of specimen 2 is the "cohesion" type. When heat-sealing was performed at 150°C on specimen 2, the sealing strength was less than 8 kPa, and sufficient sealing strength was not obtained. Regarding the peeling properties, the adhesion of specimen 1 to the cup was too weak, being in a so-called temporary state. In addition, even when heat-sealing test piece 2 at 160°C, the sealing strength was 8 kPa, which was sufficient, but in terms of peeling properties, the adhesion of test piece 1 to the cup was too weak, and it was in a so-called temporary state.
[0047] The sealant film layer of the specimen 3 has a thickness of 30 μm and is a two-layer structure in which a base layer and a second sealant layer are laminated in this order. A polyethylene resin is used for the base layer, and a polyethylene resin containing a tackifier is used for the second sealant layer. The sealant film layer of the specimen 3 corresponds to the first aspect of the sealant film layer 202 described above. The peeling mode of the specimen 3 is an "interface" type. Here, the "interface" type refers to a mode in which the specimen (lid material) and the cup are peeled off due to destruction at the bonding interface between the second sealant layer and the first sealant layer on the cup side. When test piece 3 was heat sealed at 150°C, the sealing strength was 10 kPa, which was sufficient. Furthermore, the peeling characteristics were also good, as the test subject was able to easily peel test piece 3 from the cup. In addition, when test piece 3 was heat sealed at 160°C, the sealing strength was 9 kPa, which was sufficient. Furthermore, the peeling characteristics were also good, as the test subject was able to easily peel test piece 3 from the cup.
[0048] The sealant film layer of specimen 4 has a thickness of 30 μm and is a two-layer structure in which a base layer and a second sealant layer are laminated in this order. A polyethylene-based resin is used for the base layer, and a resin containing a polyethylene-based resin, a polypropylene resin, a polystyrene-based resin, etc. is used for the second sealant layer. The sealant film layer of specimen 4 corresponds to the second aspect of the sealant film layer 202 described above. The peeling mode of specimen 4 is an "aggregation" type. When test piece 4 was heat sealed at 150°C, the sealing strength was 9 kPa, which was sufficient. Furthermore, the peeling characteristics were also good, as the test subject was able to easily peel test piece 4 from the cup. Furthermore, when heat-sealing test piece 4 at 160°C, the sealing strength was 10 kPa, which was sufficient, but the peeling properties were confirmed to be good, as the test subject was able to easily peel test piece 4 from the cup. It was confirmed that some fibrous sealant material, so-called whiskers, remained on the peeled surface, but this was at a level that would not cause any problems in practical use.
[0049] The sealant film layer of specimen 5 is 50 μm thick and has a two-layer structure in which a base layer and a second sealant layer are laminated in that order. The base layer is made of polypropylene resin, and the second sealant layer is made of high-density polyethylene (HDPE) and polypropylene resin. The peeling mode of specimen 5 is the "cohesion" type. When specimen 5 was heat sealed at 150°C, the sealing strength was 8 kPa, which was sufficient. However, regarding the peeling properties, when specimen 5 was peeled off from the cup, it was confirmed that part of the resin (polypropylene resin) of the first sealant layer provided on the flange of the cup remained on the specimen side (PP elongation). Even when test specimen 5 was heat sealed at 160°C, the sealing strength was 11 kPa, which was sufficient. However, regarding the peeling properties, when test specimen 5 was peeled off from the cup, it was confirmed that part of the resin (polypropylene resin) of the first sealant layer provided on the flange of the cup remained on the test specimen side (PP elongation).
[0050] The sealant film layer of specimen 6 is 50μm thick and has a multi-layer structure in which a base layer, multiple intermediate layers, and a second sealant layer are laminated in that order. The base layer is made of high density polyethylene (HDPE), the intermediate layer is made of high density polyethylene (HDPE), and the second sealant layer is made of high density polyethylene (HDPE) and polypropylene resin. The peeling mode of specimen 6 is the "cohesion" type. When test specimen 6 was heat sealed at 150°C, the sealing strength was 11 kPa, which was sufficient. However, when test specimen 6 was peeled from the cup, the test specimen tore and a part of it remained on the cup side, a phenomenon known as paper peeling, was confirmed. When specimen 6 was heat sealed at 160°C, the sealing strength was 14 kPa, which was sufficient. However, regarding the peeling properties, when specimen 6 was peeled off from the cup, it was confirmed that part of the resin (polypropylene resin) of the first sealant layer provided on the flange of the cup remained on the specimen side (PP elongation).
[0051] The sealant film layer of specimen 7 is made of TAF650C manufactured by Mitsui Chemicals Tohcello Co., Ltd., with a thickness of 30 μm, and has a three-layer structure in which a base layer, an intermediate layer, and a second sealant layer are laminated in this order. A special polyethylene resin is used for the base layer, a homopolymer type polypropylene resin is used for the intermediate layer, and a resin in which a polypropylene resin is added to a polyethylene resin is used for the second sealant layer. Here, the special polyethylene resin of the base layer is made by adding a polymer alloy (compatibilizer) to a polyethylene resin, or a random type polypropylene resin is added to a polyethylene resin, in order to structure adhesion with the homopolymer type polypropylene resin of the intermediate layer. The peeling mode of specimen 7 is the "aggregation" type. When test specimen 7 was heat sealed at 150°C, the sealing strength was 9 kPa, which was sufficient. However, when test specimen 7 was peeled from the cup, the test specimen tore and a part of it remained on the cup side, a phenomenon known as paper peeling, was confirmed. When the test specimen 7 was heat sealed at 160° C., the sealing strength exceeded 15 kPa, which was sufficient, but in terms of peeling properties, the test specimen 7 could not be peeled off from the cup (not peelable).
[0052] The sealant film layer of specimen 8 is 9501E manufactured by Toray Advanced Film Co., Ltd., 30 μm thick, and has a two-layer structure with a base layer and a second sealant layer laminated in that order. The base layer is made of polypropylene resin, and the second sealant layer is made of a resin in which polypropylene resin is added to polyethylene resin. The peeling mode of specimen 8 is the "cohesion" type. When test specimen 8 was heat sealed at 150°C, the sealing strength was 14 kPa, which was sufficient. However, regarding the peeling characteristics, when test specimen 8 was peeled from the cup, it was confirmed that part of the resin (polypropylene resin) of the first sealant layer provided on the flange portion of the cup remained on the test specimen side (PP elongation). When the test piece 8 was heat sealed at 160° C., the sealing strength exceeded 15 kPa, which was sufficient. However, in terms of peeling properties, the test piece 7 could not be peeled from the cup (not peelable).
[0053] From the above evaluation results, it was confirmed that the sealant film layers of test specimens 3 and 4 out of the eight test specimens, i.e., the first and second aspects of the sealant film layer 202 described above, had good sealing strength and peel characteristics.
[0054] (Evaluation of sealing strength between lid and cup, and opening strength) Next, lids (Examples 1 and 2) having the sealant film layers of the above test specimens 3 and 4 were actually produced and heat sealed to the flange portion 13 of the cup 10, and the sealing strength, opening strength, and peeling properties were evaluated. The evaluation results are summarized in Table 2 below. The cup 10 used in the evaluation was the same as the cup used for selecting the sealant film layer described above. The lid materials of each of the examples and comparative examples used in the evaluation were heat-sealed to the flange portion 13 of the cup 10 by pressing at 0.3 MPa for 1 second at 150°C, 160°C, 170°C, or 180°C.
[0055] The sealing strength was measured by the same method as that used in the selection of the sealant film layer described above. The opening strength is the force required to peel off the lid material heat-sealed to the cup. The opening strength was measured by using a force gauge (FGPX-5, manufactured by Nidec-Shimpo) to place the cup with the lid material facing up and measure the strength when opening at a peel angle (angle with respect to the top surface of the lid material) of 45 degrees. In addition, a film chuck (6FC-20, manufactured by Nidec-Shimpo) was used as an attachment for the measurement. In general, an opening strength of 6.0N or more and 18N or less is sufficient for practical use. If the opening strength is less than 6.0N, the lid material will peel off too easily from the cup, which is undesirable because it will cause problems such as the lid material peeling off unintentionally. If the opening strength is greater than 18N, the lid material will not peel off from the cup, or even if it does peel off, the lid material or the cup may be damaged, which is undesirable. The peeling properties were evaluated in the same manner as in the evaluation of peeling properties performed in the selection of the second sealant layer described above. A rating of "O" was given if the lid could be easily peeled off from the cup, and a rating of "X" was given if the adhesion of the lid to the cup was too weak or too strong and the lid could not be peeled off. The sealing strength and opening strength were measured using three lids from each Example and Comparative Example, and the average values were used as the measurement results.
[0056] [Table 2]
[0057] The second laminate constituting each of the lid materials of Examples 1, 2, and the comparative example used in this evaluation is configured by laminating, from the inner side of the cup, a sealant film layer, a first resin layer, a second paper base layer, and a second resin layer. Here, the first resin layer, the second paper base layer, and the second resin layer are configured in the same manner in Examples 1 and 2 and the Comparative Example. That is, the first resin layer is configured from a PET resin film with a thickness of 12 μm, and the second paper base layer is configured from a PET resin film with a basis weight of 80 g / m 2The first resin layer is made of uncoated paper, and the second resin layer is made of a PET resin film having a thickness of 12 μm. The first resin layer, the second paper base layer, and the second resin layer of each example and comparative example are bonded via an adhesive layer made of a lamination adhesive by a dry lamination method. A predetermined printed layer is formed on the second paper base layer side of the second resin layer.
[0058] The lid material of Example 1 has the sealant film layer (first aspect of the sealant film layer 202) used in the above-mentioned test piece 3. That is, the sealant film layer of Example 1 is formed of a two-layer structure having a thickness of 30 μm, in which a polyethylene resin is used for the base layer and a resin in which a tackifier is added to a polyethylene resin is used for the second sealant layer. The sealant film layer of Example 1 is bonded to the first resin layer by a dry lamination method via an adhesive layer made of a lamination adhesive. As shown in the evaluation results in Table 2, the lid of Example 1 had a seal strength of 9.7 kPa and an open strength of 7.1 N when heat sealed at 150°C, confirming that it had sufficient seal strength and open strength. In addition, regarding the peeling properties, the subjects were able to easily peel the lid from the cup, confirming that there were no practical problems, and the evaluation was "good." Furthermore, when heat sealed at 160°C, the sealing strength was 9.0 kPa and the opening strength was 7.3 N, confirming that the seal strength and opening strength were sufficient. Regarding peeling properties, although a small amount of polypropylene resin from the cup side remained on the lid side, the subject was able to easily peel the lid from the cup, confirming that there was no problem in practical use, and the evaluation was given as "Good." When heat sealed at 170°C, the sealing strength was 9.0 kPa and the opening strength was 7.0 N, confirming that the sealing strength and opening strength were sufficient. In addition, regarding the peeling properties, the subject was able to easily peel the lid from the cup, confirming that there were no practical problems, and the evaluation was "Good." When heat sealed at 180°C, the sealing strength was 10.7 kPa and the opening strength was 8.4 N, confirming that the sealing strength and opening strength were sufficient. In addition, regarding the peeling properties, the subject was able to easily peel the lid from the cup, confirming that there were no practical problems, and the evaluation was "Good."
[0059] The lid material of Example 2 includes the sealant film layer (second embodiment of the sealant film layer 202) used in the above-mentioned test piece 4. That is, the sealant film layer of Example 2 is formed of a two-layer structure having a thickness of 30 μm, in which a polyethylene resin is used for the base layer and a resin in which a polypropylene resin, a polystyrene-based resin, or the like is added to a polyethylene resin is used for the second sealant layer. The sealant film layer of Example 2 is bonded to the first resin layer by a dry lamination method via an adhesive layer made of a lamination adhesive. The lid material of Example 2 had a seal strength of 7.3 kPa and an unsealing strength of 6.5 N when heat sealed at 150°C, and was confirmed to have sufficient unsealing strength, but the seal strength was below 8 kPa and was confirmed to be insufficient. In addition, regarding the peeling properties, although the subject was able to peel the lid material from the cup, it was confirmed that the adhesion of the lid material to the cup was too weak and insufficient for use as a product, and the evaluation was "x". However, when heat sealed at 160°C, the sealing strength was 8.0 kPa and the opening strength was 7.3 N, confirming that the seal strength and opening strength were sufficient. Regarding peeling properties, a small amount of polypropylene resin from the cup side was found to remain on the lid side, but the subject was able to easily peel the lid from the cup, confirming that there was no problem in practical use, and the evaluation was "Good". In addition, when heat sealed at 170°C, the sealing strength was 9.0 kPa and the opening strength was 8.0 N, confirming that the sealing strength and opening strength were sufficient. In addition, regarding the peeling properties, the subjects were able to easily peel the lid from the cup, confirming that there were no practical problems, and the evaluation was "Good." When heat sealed at 180°C, the sealing strength was 9.7 kPa and the opening strength was 8.7 N, confirming that the sealing strength and opening strength were sufficient. In addition, regarding the peeling properties, the subject was able to easily peel the lid from the cup, confirming that there were no practical problems, and the evaluation was "Good."
[0060] The comparative example of the lid material has a sealant film layer formed by co-extrusion of 10 μm of a blend resin of LDPE and α-olefin copolymer and 30 μm of a polyethylene resin in a first resin layer. That is, the sealant film layer in the comparative example is formed of a two-layer structure with a thickness of 40 μm, in which a polyethylene resin is used in the base layer and the above-mentioned blend resin (easy peel resin) is used in the second sealant layer. The lid material of the comparative example had a seal strength of 2.7 kPa and an unsealing strength of 3.1 N when heat sealed at 150°C, which means that sufficient seal strength and unsealing strength were not obtained. Regarding peeling properties, although the lid material could be peeled off from the cup by the subject, the adhesion of the lid material to the cup was too weak and it was confirmed to be insufficient for use as a product, and the evaluation was "X". In addition, when heat sealed at 160°C, the sealing strength was 3.0 kPa and the opening strength was 3.1 N, neither of which were sufficient. Regarding peeling properties, although the subject was able to peel the lid from the cup, the adhesion of the lid to the cup was too weak and it was confirmed that it was insufficient for use as a product, and the evaluation was "X". When heat sealed at 170°C, the sealing strength was 4.0 kPa and the opening strength was 3.5 N, neither of which were sufficient. Regarding peeling properties, although the subject was able to peel the lid from the cup, the adhesion of the lid to the cup was too weak and it was confirmed to be insufficient for use as a product, and the evaluation was "X". When heat sealed at 180°C, the sealing strength was 5.3 kPa and the opening strength was 5.0 N, neither of which were sufficient. On the other hand, regarding the peeling properties, the subjects were able to easily peel the lid from the cup, confirming that there were no practical problems, and the evaluation was "Good."
[0061] From the above, it was confirmed that the lid material of Example 1 had good sealing strength, opening strength, and peeling properties when heat sealed in the temperature range of 150° C. to 180° C. In addition, it was confirmed that the lid material of Example 2 had good sealing strength, opening strength, and peeling properties when heat sealed in the temperature range of 160° C. to 180° C. In contrast, it was confirmed that the lid materials of the comparative examples were unable to provide sufficient sealing strength, opening strength, and peeling properties in any heat sealing temperature range. [Explanation of symbols]
[0062] 1 container 10 cups 11. Torso 12 Bottom 13 Flange 20 Lid material 100 First laminate 101 1st paper base layer 102 First sealant layer 103 Surface resin layer 200 Second laminate 201 2nd paper base layer 202 Sealant film layer 202A Base Layer 202B Second sealant layer 203 1st resin layer 204 2nd resin layer 205 Adhesive layer 206 Printing layer
Claims
1. A container comprising a cup having a body and a bottom, and a lid for closing an opening provided in the body, The body and the bottom are made of a first laminate having a first paper base layer and a first sealant layer provided on at least one surface side of the first paper base layer, the opening of the body portion includes a flange portion formed by folding back the first laminate so as to expose the first sealant layer, The lid material is made of a second laminate having a base layer and a sealant film layer provided on at least one surface side of the base layer, The sealant film layer has a base layer and a second sealant layer bonded to the flange portion, the first sealant layer contains a polypropylene resin, and the MFR value of the polypropylene resin is 30 g / 10 min or more and 50 g / 10 min or less; The base layer is made of a polyethylene resin, The second sealant layer is mainly composed of a polyethylene-based resin and contains a tackifier or a polystyrene-based resin; A container characterized by:
2. The base material layer of the second laminate is a second paper base material layer, The second paper base layer accounts for more than half of the total mass of the lid material.
2. The container according to claim 1 ,
3. The sealing strength between the flange portion of the cup and the lid material is 8 kPa or more; 3. The container according to claim 1 or 2, characterized in that
Citation Information
Patent Citations
Adhesive for sealant and film for lid material
CN108070330A
Cover material for paper made cup
JP1997066586A
Easily unsealable container
JP2000264367A
Paper cup for use in microwave oven
JP2003095350A
Resin composition and film for lid material
JP2020158763A