Optical fiber manufacturing method

By forming a glass fiber with a high-modulus second resin coating layer and controlling atmospheric particles and static electricity, the method stabilizes optical fibers against breakage during manufacturing.

JP7567698B2Active Publication Date: 2024-10-16SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2021116168
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-14
Publication Date
2024-10-16
Estimated Expiration
2041-07-14

AI Technical Summary

Technical Problem

Optical fibers with small diameters are prone to breakage during manufacturing due to particles in the atmosphere adhering to the fiber and applying local stress, leading to disconnection issues.

Method used

A method involving the formation of a glass fiber with a two-layer resin coating, where the second resin coating layer has a Young's modulus of 900 MPa or more, and maintaining an atmosphere with a target particle density of 1060 particles/m³, along with static electricity neutralization, to prevent particle adhesion and stress application.

Benefits of technology

The method effectively reduces the frequency of optical fiber breakage, maintaining manufacturing efficiency by preventing particle-induced stress on the glass fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567698000003
    Figure 0007567698000003
  • Figure 0007567698000004
    Figure 0007567698000004
  • Figure 0007567698000005
    Figure 0007567698000005
Patent Text Reader

Abstract

To suppress breakage of an optical fiber.SOLUTION: A method for manufacturing an optical fiber includes the steps of: forming a glass fiber; forming a resin coating layer so as to cover the outer periphery of the glass fiber; curing the resin coating layer using a predetermined curing device; conveying the optical fiber obtained by curing the resin coating layer by a plurality of guide rollers and a capstan; and winding the optical fiber by a bobbin. In the step of forming the resin coating layer, a first resin coating layer and a second resin coating layer as resin coating layers are formed in this order from a central axis side to an outer peripheral side of the glass fiber. Between the step of forming the resin coating layer and the step of winding the optical fiber, a density of particles having a size of 1 / 4 times or more the thickness of the second resin coating layer in the atmosphere is set to 1,060 pieces / m3 or less.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing an optical fiber. [Background technology]

[0002] 2. Description of the Related Art Optical fibers in which the outer periphery of a glass fiber is covered with a resin coating layer are known (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-6797 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to suppress breakage of optical fibers. [Means for solving the problem]

[0005] According to one aspect of the present disclosure, forming a glass fiber; forming a resin coating layer so as to cover an outer periphery of the glass fiber; curing the resin coating layer using a predetermined curing device; a step of conveying the optical fiber having the cured resin coating layer by a plurality of guide rollers and a capstan; winding the optical fiber on a bobbin; having In the step of forming the resin coating layer, forming a first resin coating layer and a second resin coating layer in this order from a central axis side to an outer periphery side of the glass fiber as the resin coating layer; During the process from forming the resin coating layer to winding the optical fiber, The density of particles having a size equal to or greater than 1 / 4 the thickness of the second resin coating layer in the atmosphere is set to 1060 particles / m 3 The following A method for manufacturing an optical fiber is provided. Effect of the Invention

[0006] According to the present disclosure, breakage of optical fibers can be suppressed. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an optical fiber according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram showing an optical fiber manufacturing apparatus according to an embodiment of the present disclosure. [Diagram 3] FIG. 3 is a graph showing the frequency of wire breakage versus the thickness of the second resin coating layer. [Figure 4] FIG. 4 is a graph showing the frequency of disconnections versus the target particle density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Description of the embodiments of the present disclosure] <Knowledge gained by the inventors> First, the findings of the inventors will be described.

[0009] In recent years, in order to pack multiple optical fibers at high density in an optical cable, there has been a demand for optical fibers with a smaller outer diameter. Specifically, the outer diameter of some optical fibers in recent years is 200 μm or less.

[0010] In the manufacturing process of such a small-diameter optical fiber, the optical fiber is more susceptible to breakage than optical fibers with a conventional outer diameter. If the optical fiber breaks during the manufacturing process, the manufacturing efficiency of the optical fiber decreases. For this reason, a new manufacturing method was required.

[0011] In order to address the above-mentioned issues, we have focused on particles present in the atmosphere during the manufacturing process and conducted a study.

[0012] When particles present in the atmosphere adhere to the optical fiber during the manufacturing process, the particles become interposed between the optical fiber and a guide roller or capstan that transports the optical fiber. At this time, the optical fiber is transported with a certain tension, so that the particles that have adhered to the optical fiber are locally pressed against the resin coating layer. This may result in localized stress being applied to the glass fiber. In such a case, damage such as cracks may occur in the glass fiber. As a result, the optical fiber may break due to the damage to the glass fiber.

[0013] As a result of extensive research into the particles, the inventors have found that the relationship between specific particles in the atmosphere and the thickness of the second resin coating layer affects the frequency of breakage of the optical fiber.

[0014] The present disclosure is based on the above findings made by the present inventors.

[0015] [Details of the embodiment of the present disclosure] Next, an embodiment of the present disclosure will be described below with reference to the drawings. Note that the present disclosure is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0016] <One embodiment of the present disclosure> (1) Optical fiber An optical fiber 10 according to an embodiment of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a schematic cross-sectional view showing the optical fiber according to the present embodiment.

[0017] In the following, the "axial direction" of the glass fiber 100 refers to the direction along the central axis of the glass fiber 100, which can be rephrased as the longitudinal direction of the glass fiber 100. The "radial direction" of the glass fiber 100 refers to the direction perpendicular to the axial direction of the glass fiber 100, which can be rephrased as the transverse direction of the glass fiber 100 in some cases. The "circumferential direction" of the glass fiber 100 refers to the direction along the outer periphery of the glass fiber 100 (the circumferential direction in FIG. 1). The same terms as those for the glass fiber 100 can be used for the optical fiber 10.

[0018] 1, the optical fiber 10 of this embodiment is configured as a linear body in which, for example, the outer periphery of a glass fiber 100 is covered with a resin coating layer 200. That is, the optical fiber 10 has, for example, the glass fiber 100 and the resin coating layer 200 in this order from the central axis side of the glass fiber 100 toward the outer periphery side.

[0019] The term "optical fiber 10" used herein includes the optical fiber strand before being colored and the optical fiber core wire after being colored. In the following, the optical fiber 10 will be described as an optical fiber strand, for example.

[0020] [Glass fiber] The glass fiber 100 is configured as, for example, an optical transmission body that transmits light introduced into the optical fiber 10 along the axial direction of the optical fiber 10. The glass fiber 100 is also called, for example, a "bare optical fiber." The glass fiber 100 has, for example, silica (SiO2) glass as a base material (main component) and has a core 120 and a cladding 140.

[0021] [Resin coating layer] The resin coating layer 200 is provided, for example, so as to cover the outer periphery of the glass fiber 100 and is configured to protect the glass fiber 100 .

[0022] In this embodiment, the resin coating layer 200 has, for example, a first resin coating layer (primary resin coating layer) 220 and a second resin coating layer (secondary resin coating layer) 240.

[0023] The first resin coating layer 220 is provided, for example, so as to cover the outer periphery of the clad 140 of the glass fiber 100 and is in contact with the outer periphery of the clad 140. The second resin coating layer 240 is provided, for example, so as to cover the outer periphery of the first resin coating layer 220 and is in contact with the outer periphery of the first resin coating layer 220.

[0024] The first resin coating layer 220 and the second resin coating layer 240 are formed, for example, as a cured product obtained by curing an ultraviolet-curable resin composition by ultraviolet irradiation. Examples of the base resin in the ultraviolet-curable resin composition include urethane acrylate.

[0025] In this embodiment, the Young's modulus of the second resin coating layer 240 is preferably, for example, 900 MPa or more. If the Young's modulus of the second resin coating layer 240 is less than 900 MPa, when particles present in the atmosphere adhere to the optical fiber 10 during the manufacturing process, the particles are likely to be locally pushed into the second resin coating layer 240 by contact with the guide roller 552 of the conveying unit 550 described later. For this reason, excessive stress may be applied to the glass fiber 10. As a result, the optical fiber 10 may be easily broken. In contrast, in this embodiment, by setting the Young's modulus of the second resin coating layer 240 to 900 MPa or more, that is, by hardening the second resin coating layer 240, even if particles present in the atmosphere adhere to the optical fiber 10 during the manufacturing process, it is possible to suppress the particles from being locally pushed into the second resin coating layer 240. This makes it possible to suppress the application of excessive stress to the glass fiber 10. As a result, it is possible to stably suppress the breakage of the optical fiber 10.

[0026] There is no particular upper limit to the Young's modulus of the second resin coating layer 240. For example, it is preferably 1400 MPa or less.

[0027] The Young's modulus of the first resin coating layer 220 is preferably, for example, not less than 0.15 MPa and not more than 1.2 MPa.

[0028] In this embodiment, the optical fiber 10 is configured to have, for example, a small diameter. Specifically, the outer diameter of the above-mentioned resin coating layer 200 (i.e., the outer diameter of the second resin coating layer 240) is, for example, 190 μm or less. This allows a plurality of optical fibers 10 to be densely packed as an optical cable.

[0029] The outer circumferential diameter of the resin coating layer 200 is preferably, for example, 160 μm or more.

[0030] Considering the relationship between the outer circumferential diameter of the first resin coating layer 220 and the outer circumferential diameter of the second resin coating layer 240 described above, the thickness of the second resin coating layer 240 is preferably, for example, not less than 10 μm and not more than 25 μm.

[0031] (2) Optical fiber manufacturing equipment Next, an optical fiber manufacturing apparatus 50 according to this embodiment will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing the configuration of the optical fiber manufacturing apparatus according to this embodiment.

[0032] 2, optical fiber manufacturing apparatus 50 of this embodiment includes, for example, a drawing furnace 510, a fiber position measuring unit 522, a cooling unit 523, an outer diameter measuring unit 524, a resin coating unit 530, a curing unit 540, a conveying unit 550, a bobbin 560, a control unit 590, a clean booth 620, and an air conditioning system 640. The equipment members other than the control unit 590, the clean booth 620, and the air conditioning system 640 are provided in this order.

[0033] Hereinafter, in each device member of optical fiber production apparatus 50, the side closer to gripping mechanism 512 will be referred to as the "upstream" side, and the side closer to bobbin 560 will be referred to as the "downstream" side.

[0034] The draw furnace 510 is configured to form the glass fiber 100 .

[0035] The inside of the furnace tube 514 is heated and the softened glass is stretched, thereby forming a glass fiber 100 having a small diameter.

[0036] The fiber position measuring unit 522 is configured to measure the horizontal position of the glass fiber 100 .

[0037] Cooling device 523 is configured to cool the glass fiber 100 formed in draw furnace 510 .

[0038] The outer diameter measuring unit 524 is configured to measure the outer diameter of the glass fiber 100 before it is resin-coated.

[0039] The resin coating device 530 is configured to form a resin coating layer 200 so as to cover the outer periphery of the glass fiber 100. The resin coating layer 200 has a die that applies an ultraviolet-curable resin composition to the outer periphery of the glass fiber 100 while inserting the glass fiber 100 therethrough.

[0040] In this embodiment, the resin coating device 530 has two dies for forming the first resin coating layer 220 and the second resin coating layer 240 in this order from the central axis side of the glass fiber 100 toward the outer periphery side.

[0041] The curing device 540 is configured to irradiate the resin coating layer 200 with ultraviolet rays to cure the resin coating layer 200 .

[0042] The conveying section 550 is configured to convey the optical fiber 10 with the resin coating layer 200 cured. Specifically, the conveying section 550 has, for example, a plurality of guide rollers 552, 556, and a capstan 554. The immediately below roller 552a, which is one of the plurality of guide rollers 552, is located, for example, immediately below the curing device 540. The capstan 554 is, for example, provided downstream of the immediately below roller 552a, and configured to convey (pull) the optical fiber 10 with a predetermined tension while holding the optical fiber 10 between the belt and the roller. The screening rollers 552c, 552d, and 552e of the plurality of guide rollers 552 are provided downstream of the capstan 554, and configured to apply a screening tension to the optical fiber 10 together with the capstan 554. The guide roller 556 is provided downstream of the screening roller 552e, and configured to adjust the tension of the optical fiber 10 by moving up and down in response to fluctuations in the tension of the optical fiber 10.

[0043] The bobbin 560 is provided, for example, downstream of the guide roller 556 and configured to wind up the optical fiber 10.

[0044] The control unit 590 is configured, for example, to be connected to and control each unit of the optical fiber manufacturing apparatus 50. The control unit 590 is configured, for example, as a computer.

[0045] In this embodiment, the environment from the resin coating device 530 to the bobbin 560 is maintained so as to satisfy the requirement of the target particle density in the atmosphere, which will be described later.

[0046] Specifically, the optical fiber manufacturing apparatus 50 includes, for example, a clean booth 620 and an air conditioning system 640 .

[0047] The clean booth 620 is provided, for example, so as to surround the area from the resin coating device 530 to the bobbin 560. The clean booth 620 has, for example, a resin plate or a resin film that separates the area from the resin coating device 530 to the bobbin 560 from the other areas.

[0048] The air conditioning system 640 is configured to, for example, suck air in the clean booth 620, remove particles through a filter, and supply the purified air to the clean booth 620. Examples of the filter in the air conditioning system 640 include a HEPA filter (High Efficiency Particulate Air Filter) and a ULPA filter (Ultra Low Penetration Air Filter). The air conditioning system 640 is configured to, for example, maintain the pressure in the clean booth 620 at a higher pressure than the pressure in an area outside the clean booth 620.

[0049] Furthermore, in this embodiment, at least one of the multiple guide rollers 552, the capstan 554, and the bobbin 560 is configured to be able to eliminate static electricity so as to satisfy the requirement for the amount of static electricity of the optical fiber 10 after winding, which will be described later.

[0050] Specifically, for example, ionizers 580 (590a to 580h) are provided on each of the plurality of guide rollers 552, capstan 554, and bobbin 560. Ionizers 580 are configured to, for example, blow ionized air onto an object to neutralize the object.

[0051] (3) Optical fiber manufacturing method Next, a method for manufacturing the optical fiber 10 according to this embodiment will be described with reference to Fig. 2. In the following, steps are abbreviated as "S".

[0052] The manufacturing method of the optical fiber 10 of this embodiment includes, for example, a glass fiber forming step (drawing step) S100, a cooling step S200, a resin coating layer forming step S300, a hardening step S400, a conveying step S500, and a winding step S600. These steps are continuously performed in this order in the optical fiber manufacturing apparatus 50. Each component of the optical fiber manufacturing apparatus 50 is controlled by a control unit 590.

[0053] [S100: Wire drawing process] First, the glass preform G is introduced into the furnace core tube 514 of the drawing furnace 510, and the glass preform G in the furnace core tube 514 is heated by the heating element 516. After the glass preform G is heated, the softened glass is drawn from the lower end of the glass preform G to form a glass fiber 100 having a small diameter.

[0054] [S200: Cooling process] Next, the glass fiber 100 formed in the drawing furnace 510 is introduced into a cooling device 523 and air-cooled.

[0055] At this time, the feed rate of the glass base material and the like are controlled so that the outer diameter of the glass fiber 100 before resin coating, measured by the outer diameter measuring unit 524, remains constant.

[0056] [S300: Resin coating layer formation process] Next, a resin coating layer 200 is formed by a resin coating device 530 so as to cover the outer periphery of the glass fiber 100 .

[0057] At this time, in this embodiment, as the resin coating layer 200, a first resin coating layer 220 and a second resin coating layer 240 are continuously formed in this order from the central axis side of the glass fiber 100 toward the outer periphery side.

[0058] In this embodiment, the outer circumferential diameter of the resin coating layer 200 is set to, for example, 190 μm or less.

[0059] [S400: Hardening process] Next, the resin coating layer 200 is irradiated with ultraviolet light by the curing device 540 to cure the resin coating layer 200. At this time, in this embodiment, the first resin coating layer 220 and the second resin coating layer 240 are cured simultaneously. By setting the Young's modulus of the cured second resin coating layer 240 to 900 MPa or more, the resin coating layer 200 can be made less susceptible to damage by particles.

[0060] [S500: Transportation process] Next, the optical fiber 10 with the cured resin coating layer 200 is transported by the transport unit 550. Specifically, in the transport unit 550, the optical fiber 10 is transported through the direct below roller 552a, the guide roller 552b, the capstan 554, the screening rollers 552c, 552d, and 552e, and the guide roller 556 with a predetermined tension.

[0061] [S600: Winding process] Next, the optical fiber 10 is wound around the bobbin 560 .

[0062] In this embodiment, during the resin coating layer forming step S300 to the winding step S600, for example, the density of particles having a size (particle diameter) of 1 / 4 or more times the thickness of the second resin coating layer 240 in the atmosphere is set to 1060 particles / m 3 The density of the particles is also called the "target particle density." If CF (cubic feet) is used as the unit, the above-mentioned target particle density corresponds to 30 particles / CF or less.

[0063] In this embodiment, the target particle density is set to 1060 particles / m 3 By setting it to the value below, the probability that particles having a large ratio of size to the thickness of the second resin coating layer 240 will adhere to the optical fiber 10 can be reduced.

[0064] The lower limit of the target particle density is not particularly limited, since the lower the better.

[0065] The above-mentioned target particle density is adjusted, for example, by the type of filter of the air conditioning system 640, the number of filters of the air conditioning system 640, the intake speed of the air conditioning system 640, the supply speed of clean air of the air conditioning system 640, the pressure inside the clean booth 620, etc.

[0066] In this embodiment, in the steps from the transport step S500 to the winding step S600, at least one of the guide rollers 552, the capstan 554, and the bobbin 560 is neutralized so that the absolute value of the static electricity of the entire optical fiber 10 after winding onto the bobbin 560 is 6 kV or less. By neutralizing each part so as to satisfy the above-mentioned requirements for the static electricity amount, adhesion of particles to the optical fiber 10 due to charging of the optical fiber 10 can be suppressed.

[0067] Note that the "static charge amount of the entire optical fiber 10 after being wound around the bobbin 560" referred to here can be rephrased as the static charge amount of the entire optical fiber 10 in a state where it is wound around the bobbin 560. The reason why the static charge amount of the entire optical fiber 10 after being wound is specified is because it is not possible to measure the static charge amount of the optical fiber 10 during the transportation process of the optical fiber 10. As described above, satisfying the static charge amount of the entire optical fiber 10 after being wound corresponds to suppressing the accumulation of static charge of the optical fiber 10 during the transportation process of the optical fiber 10.

[0068] The lower limit of the amount of static electricity in the optical fiber 10 after winding is not particularly limited, since the lower the better.

[0069] As a specific method of removing static electricity, for example, ionized air having a polarity opposite to the polarity to which the optical fiber 10 is charged is blown by each ionizer 580 against at least one of the guide rollers 552, the capstan 554, and the bobbin 560. It is preferable that the ionized air is blown at a location on the target object with which the optical fiber 10 comes into contact. This method can cancel out the static electricity of the optical fiber 10. As a result, the optical fiber 10 can be stably removed from the static electricity.

[0070] In this embodiment, for example, it is preferable to neutralize at least one of the plurality of guide rollers 552 and the capstan 554 located upstream of the bobbin 560 by the ionizer 580. Since the optical fiber 10 is transported upstream of the bobbin 560, the optical fiber 10 tends to approach particles in the atmosphere. Therefore, by actively neutralizing the optical fiber 10 upstream of the bobbin 560 as described above, adhesion of particles to the optical fiber 10 can be stably suppressed even during a period in which the optical fiber 10 may approach particles in the atmosphere.

[0071] Furthermore, in this embodiment, it is more preferable to neutralize the capstan 554 by the ionizer 580c, for example. In the capstan 554, the optical fiber 10 rubs between the belt and the roller, so that the optical fiber 10 is likely to be charged. Therefore, by actively neutralizing the capstan 554 as described above, it is possible to stably suppress the charging of the optical fiber 10. As a result, it is possible to stably suppress the adhesion of particles to the optical fiber 10.

[0072] In this embodiment, it is most preferable to neutralize all of the guide rollers 552, the capstan 554, and the bobbin 560 by the ionizers 580. This can reliably prevent the optical fiber 10 from being charged during transportation, and can reliably prevent particles from adhering to the optical fiber 10.

[0073] In this manner, the optical fiber 10 of the present embodiment is manufactured.

[0074] (4) Effects of this embodiment According to this embodiment, one or more of the following advantages are achieved.

[0075] (a) In the process from the resin coating layer forming step S300 to the winding step S600 of this embodiment, the density of particles having a size equal to or greater than 1 / 4 the thickness of the second resin coating layer 240 in the atmosphere is set to 1060 particles / m 3 The following applies.

[0076] Target particle density is 1060 particles / m 3 If the thickness exceeds 1 / 2 mm, there is a high probability that particles having a large size ratio relative to the thickness of the second resin coating layer 240 will adhere to the optical fiber 10. If such large particles adhere to the optical fiber 10, the particles are likely to be locally pushed into the second resin coating layer 240 by contact with the guide rollers 552 of the conveying section 550, etc. This may result in excessive stress being applied to the glass fiber 100. As a result, the optical fiber 10 may become more susceptible to breakage.

[0077] In contrast, in this embodiment, the target particle density is set to 1060 particles / m 3 By setting the ratio as below, it is possible to reduce the probability that particles having a large ratio of size to the thickness of the second resin coating layer 240 will adhere to the optical fiber 10. By suppressing the adhesion of particles, it is possible to suppress the particles from being locally pushed into the second resin coating layer 240. This makes it possible to suppress the application of excessive stress to the glass fiber 100. As a result, it is possible to stably suppress breakage of the optical fiber 10.

[0078] By reducing the frequency of breakage of the glass fiber 100 in this manner, it is possible to suppress a decrease in the manufacturing efficiency of the optical fiber 10.

[0079] (b) In the resin coating layer forming step S300 of this embodiment, the Young's modulus of the second resin coating layer 240 is set to 900 MPa or more. That is, by hardening the second resin coating layer 240, even if particles present in the atmosphere during the manufacturing process adhere to the optical fiber 10, it is possible to suppress localized pushing of the particles into the second resin coating layer 240. This makes it possible to suppress application of excessive stress to the glass fiber 100. As a result, breakage of the optical fiber 10 can be stably suppressed.

[0080] (c) In the steps from the transport step S500 to the winding step S600 of this embodiment, at least one of the multiple guide rollers 552, the capstan 554, and the bobbin 560 is de-electrified so that the absolute value of the static electricity of the entire optical fiber 10 after winding onto the bobbin 560 is 6 kV or less.

[0081] Here, during the transportation of the optical fiber 10 by the guide rollers 552 and the capstan 554 and the winding of the optical fiber 10 by the bobbin 560 (collectively referred to as the transportation process of the optical fiber 10), the optical fiber 10 comes into contact with various parts. For this reason, the optical fiber 10 is easily charged.

[0082] The absolute value of the static electricity amount of the entire optical fiber 10 after winding being less than 6 kV corresponds to the accumulation of static electricity in the optical fiber 10 during the above-mentioned transport process of the optical fiber 10. As described above, if the optical fiber 10 is charged during the transport process of the optical fiber 10, particles are likely to adhere to the optical fiber 10 due to static electricity during the transport process of the optical fiber 10. When particles adhere to the optical fiber 10, excessive stress may be applied to the glass fiber 100 due to the particles being pushed into the resin coating layer 200 as described above. As a result, the optical fiber 10 may become more susceptible to breakage.

[0083] In contrast, reducing the amount of static electricity in the entire optical fiber 10 after winding, as in the present embodiment, corresponds to suppressing the accumulation of static electricity in the optical fiber 10 during the transport process of the optical fiber 10. By suppressing the accumulation of static electricity in the optical fiber 10, it is possible to suppress adhesion of particles to the optical fiber 10 caused by charging of the optical fiber 10. This makes it possible to suppress the application of excessive stress to the glass fiber 10 caused by pushing particles into the resin coating layer 200. As a result, it is possible to stably suppress breakage of the optical fiber 10.

[0084] (d) In this embodiment, the outer diameter of the resin coating layer 200 of the optical fiber 10 is 190 μm or less. When manufacturing such a small-diameter optical fiber 10, the optical fiber 10 is likely to break due to adhesion of particles having a size equal to or greater than ¼ the thickness of the second resin coating layer 240, as in the examples described below. Therefore, the above-described manufacturing method is particularly effective for manufacturing an optical fiber 10 in which the outer diameter of the resin coating layer 200 is 190 μm or less.

[0085] <Other embodiments of the present disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above-described embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.

[0086] In the above embodiment, the optical fiber 10 is illustrated and described as an optical fiber wire before being colored, but as described above, the optical fiber 10 may be an optical fiber core wire after being colored. That is, the optical fiber 10 may have a colored layer covering the outer periphery of the resin coating layer 200.

[0087] In the above embodiment, the resin coating layer 200 is configured with two layers, but the present invention is not limited to this. The resin coating layer 200 may be configured with only one layer, or may be configured with three or more layers.

[0088] In the above embodiment, the case where all of (i), (ii), and (iii) below are implemented has been described, but the present invention is not limited to this case. (i) During the resin coating layer forming process S300 to the winding process S600, the density of particles having a size equal to or greater than 1 / 4 the thickness of the second resin coating layer 240 in the atmosphere is set to 1060 particles / m 3 The following applies. (ii) The Young's modulus of the second resin coating layer 240 is set to 900 MPa or more. (iii) In the steps from the transporting step S500 to the winding step S600, at least one of the multiple guide rollers 552, the capstan 554, and the bobbin 560 is de-electrified so that the absolute value of the static electricity of the entire optical fiber 10 after winding around the bobbin 560 is 6 kV or less. By implementing at least (i), the above-mentioned effects can be obtained to a certain extent. However, the above-mentioned effects can be obtained more stably by implementing at least one of (ii) and (iii) in addition to (i).

[0089] In the above embodiment, the clean booth 620 is used to separate the area from the resin coating device 530 to the bobbin 560 from the other areas, and the air conditioning system 640 is used to reduce the target particle density in the clean booth 620, but the present invention is not limited to this. The air conditioning system may be used to reduce the target particle density in the entire clean room in which the optical fiber manufacturing apparatus 50 is installed.

[0090] In the above embodiment, during the resin coating layer forming step S300 to the winding step S600, the density of particles having a size equal to or greater than 1 / 4 the thickness of the second resin coating layer 240 in the atmosphere is set to 1060 particles / m 3Although the following case has been described, the present invention is not limited to this case. Instead of adjusting the target particle density, the thickness of the second resin coating layer 240 may be adjusted. That is, the thickness of the second resin coating layer 240 may be set to, for example, four times or more the size of the most abundant particles (for example, more than 30 particles / CF) present in the atmosphere. However, since the thickness of the second resin coating layer 240 is determined by the specifications of the optical fiber 10, it is preferable to adjust the target particle density as described above. EXAMPLES

[0091] Next, examples according to the present disclosure will be described. These examples are merely examples of the present disclosure, and the present disclosure is not limited to these examples.

[0092] (1) Fabrication of optical fiber Each sample optical fiber was produced under the following conditions.

[0093] When preparing each sample, the target particle density in the atmosphere was adjusted by changing the opening and closing state of the clean booth.

[0094] [Common conditions] Glass fiber outer diameter: 125μm Outer diameter of optical fiber (outer diameter of second resin coating layer): 180 μm Number of resin coating layers: 2 layers Manufacturing equipment: Configuration shown in Figure 2

[0095] [Experiment 1] Thickness of the second resin coating layer: 5 to 30 μm (the outer diameter of the second resin coating layer is fixed at 180 μm) Particle size: 3.75μm or 5μm Particle density: 30 particles / CF Young's modulus of the second resin coating layer: 900MPa Neutralization by ionizers in the transport section and bobbin: None

[0096] [Experiment 2] Thickness of the second resin coating layer: 20 μm Target particle density: 0 to 50 particles / CF Young's modulus of the second resin coating layer: 900MPa Neutralization by ionizers in the transport section and bobbin: None

[0097] [Experiment 3] Thickness of the second resin coating layer: 20 μm Target particle density: 30 particles / CF Young's modulus of the second resin coating layer: 800 to 2000 MPa Ionizers for static elimination in the transport section and bobbin: Yes Amount of static electricity on the optical fiber after winding (absolute value): 6 kV

[0098] [Experiment 4] Thickness of the second resin coating layer: 20 μm Target particle density: 30 particles / CF Young's modulus of the second resin coating layer: 900MPa Ionizers for charge removal in the transfer section and bobbin: yes or no Amount of static electricity on optical fiber after winding (absolute value): 0.3 to 30 kV (Sample B4-2 was not subjected to static elimination.)

[0099] (2) Evaluation [Target particle density] The particle density in the clean booth surrounding the area from the resin coating device to the bobbins was measured using a particle counter (Met One Model 237B). This particle counter can detect the size and number of particles contained in 1CF of air.

[0100] [Static electricity amount] The absolute value of the static electricity quantity of the optical fiber after it was wound around the bobbin was measured by a static electricity quantity meter.

[0101] [Measurement of frequency of wire breakage] During the manufacturing process of the optical fiber for each sample described above, the number of breaks in the optical fiber was measured. For each sample, the number of breaks per 1000 km was calculated as the "break frequency (times / Mm)." As a result, a break frequency of less than 5 times / Mm was evaluated as "good," and a break frequency of 5 times / Mm or more was evaluated as "poor."

[0102] (3) Results [Experiment 1] The results of Experiment 1 regarding the dependency of the thickness of the second resin coating layer will be described with reference to FIG.

[0103] As shown in Figure 3, in the manufacture of optical fibers in an atmosphere in which particles of a certain size are present, the frequency of breakage of the optical fiber gradually increased as the thickness of the second resin coating layer became thinner from a certain threshold value. In addition, a comparison of particles of different sizes revealed that the threshold thickness of the second resin coating layer at which the frequency of breakage of the optical fiber becomes 5 times / mm or more is about four times the particle size, and is proportional to the particle size.

[0104] [Experiment 2] The results of Experiment 2 regarding the dependency of the target particle density are explained with reference to FIG.

[0105] As shown in Figure 4, as the density of particles having a size of 1 / 4 or more times the thickness of the second resin coating layer in the atmosphere (target particle density) increases from a certain threshold, the frequency of optical fiber breakage gradually increases. It was found that the threshold of the target particle density at which the frequency of optical fiber breakage becomes 5 times / mm or more is 30 particles / CF.

[0106] From the results of Experiments 1 and 2, it was confirmed that the frequency of optical fiber breakage can be reduced by setting the density of particles having a size of 1 / 4 or more times the thickness of the second resin coating layer in the atmosphere to 30 particles / CF or less between the resin coating layer formation process and the winding process.

[0107] [Experiment 3] The results of Experiment 3 regarding the dependency of the Young's modulus of the second resin coating layer will be described with reference to Table 1 below.

[0108] [Table 1]

[0109] In sample B3-1, in which the Young's modulus of the second resin coating layer was less than 900 MPa, the frequency of breakage of the optical fiber was 5 times / Mm or more.

[0110] In sample B3-1, when particles adhere to the optical fiber, the particles are easily pushed into the second resin coating layer, which is believed to be why the optical fiber in sample B3-1 is more susceptible to breakage.

[0111] In contrast, in Samples A3-1 to A3-4, in which the Young's modulus of the second resin coating layer was 900 MPa or more, the frequency of breakage of the optical fiber was less than 5 times / Mm. Also, in Samples A3-1 to A3-4, the frequency of breakage of the optical fiber tended to decrease as the Young's modulus of the second resin coating layer increased.

[0112] In samples A3-1 to A3-4, by setting the Young's modulus of the second resin coating layer to 900 MPa or more, even if particles adhere to the optical fiber, it was possible to suppress the particles from being locally pushed into the second resin coating layer. As a result, it was confirmed that in samples A3-1 to A3-4, it was possible to stably suppress breakage of the optical fiber 10.

[0113] [Experiment 4] The results of Experiment 4 regarding the dependence of the amount of static electricity are explained with reference to Table 2 below.

[0114] [Table 2]

[0115] In samples B4-1 and B4-2, in which the absolute value of the static electricity in the optical fiber after winding exceeded 6 kV, the frequency of breakage of the optical fiber was 5 times / Mm or more. In addition, in samples B4-1 and B4-2, the frequency of breakage of the optical fiber tended to increase as the absolute value of the static electricity in the optical fiber after winding increased.

[0116] In the samples B4-1 and B4-2, static electricity was accumulated in the optical fiber during the optical fiber transport process. This made it easier for particles to adhere to the optical fiber. As a result, it is believed that the optical fiber 10 in the samples B4-1 and B4-2 was more likely to break.

[0117] In contrast, in samples A4-1 to A4-3 in which the absolute value of the static electricity in the optical fiber after winding was 6 kV or less, the frequency of breakage of the optical fiber was less than 5 times / Mm. Also, in samples A4-1 to A4-3, the frequency of breakage of the optical fiber tended to decrease as the absolute value of the static electricity in the optical fiber after winding became lower.

[0118] In the samples A4-1 to A4-3, the accumulation of static electricity in the optical fiber during the optical fiber transport process could be suppressed. This made it possible to suppress the adhesion of particles to the optical fiber. As a result, it was confirmed that in the samples A4-1 to A4-3, the breakage of the optical fiber could be stably suppressed. [Explanation of symbols]

[0119] 10 Optical Fiber 50 Optical fiber manufacturing equipment 100 Glass Fiber 120 cores 140 Clad 200 Resin coating layer 220 1st resin coating layer 240 Second resin coating layer 430 Curing equipment 510 Wire drawing furnace 512 Gripping mechanism 514 Furnace tube 516 Heating element 518 Gas Supply Department 522 Fiber position measurement unit 523 Cooling device 524 Outer diameter measuring section 530 Resin coating device 540 Curing equipment 550 Transport section 552 Guide roller 552a Directly below roller 552b Guide roller 552c, 552d, 552e Screening Rollers 554 Capstan 555 Vibration suppressor 556 Guide Roller 560 Bobbin 580, 580a~580h Ionizer 590 Control Unit 620 Clean Booth 640 Air Conditioning System

Claims

1. forming a glass fiber; forming a resin coating layer so as to cover an outer periphery of the glass fiber; curing the resin coating layer using a predetermined curing device; a step of conveying the optical fiber having the cured resin coating layer by a plurality of guide rollers and a capstan; winding the optical fiber on a bobbin; having In the step of forming the resin coating layer, forming a first resin coating layer and a second resin coating layer in this order from a central axis side to an outer periphery side of the glass fiber as the resin coating layer; During the process from forming the resin coating layer to winding the optical fiber, The density of particles having a size equal to or greater than 1 / 4 the thickness of the second resin coating layer in the atmosphere is set to 1060 particles / m 3 The following A method for manufacturing optical fiber.

2. In the step of forming the resin coating layer, The Young's modulus of the second resin coating layer is set to 900 MPa or more. The method for producing the optical fiber according to claim 1 .

3. In the steps from the step of transporting the optical fiber to the step of winding the optical fiber, At least one of the guide rollers, the capstan, and the bobbin is neutralized so that the absolute value of the static electricity of the entire optical fiber after winding on the bobbin is 6 kV or less. The method for producing an optical fiber according to claim 1 or 2.