Polyamide resin composition for three-dimensional modeling and three-dimensionally modeled molded body thereof
A polyamide resin composition with novolac type phenolic resin addresses warping and deformation issues in 3D printing, achieving precise and strong molded products with low water absorption.
Patent Information
- Application Number
- JP2021122591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-07-27
AI Technical Summary
Conventional thermoplastic resins used in FDM 3D printing, such as polycarbonate resin, ABS resin, and polylactic acid, suffer from warping and deformation due to shrinkage, limiting the accuracy of molded products, and polyamide resin compositions with novolac-type phenolic resin have not been effectively used in 3D printing.
A polyamide resin composition containing 60-95% polyamide resin and 5-40% novolac type phenolic resin, with specific polyamide types and resin properties, is formulated to suppress warping and foaming in 3D printing, ensuring low water absorption and high strength.
The composition achieves suppressed warping, reduced foaming, and improved mechanical strength in 3D printed products, with a water absorption rate of 2.2% or less, enhancing product precision and appearance.
Smart Images

Figure 0007567709000003 
Figure 0007567709000001 
Figure 0007567709000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide resin composition for three-dimensional modeling. [Background technology]
[0002] One method of manufacturing three-dimensional molded products is to use a 3D printer, a device for manufacturing three-dimensional objects. A 3D printer produces three-dimensional objects by stacking two-dimensional layers in sequence based on three-dimensional coordinate data.
[0003] 3D printers use a variety of methods, including fused deposition modeling (hereinafter referred to as "FDM"), liquid vat photopolymerization, and inkjet printing, with FDM being the most widely used of these. In the FDM method, a filament-shaped raw material composition is heated and melted while being continuously extruded from a nozzle onto an XY flat table, where it is deposited. The filaments are then stacked in the Z-axis direction, fusing as they are deposited, and solidifying into one piece as they cool.
[0004] As raw materials used in the FDM method, thermoplastic resins such as polycarbonate resin, ABS resin, polycarbonate ABS resin, and polylactic acid have been used because of the need for melt fluidity. On the other hand, a polyamide resin composition containing a polyamide resin composition and a novolac-type phenolic resin is known as a resin composition having good melt fluidity in injection molding (see Patent Document 1). A similar composition is known to have low water absorption and excellent mechanical properties (see Patent Documents 2 and 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2011-500875 [Patent Document 2] Japanese Patent Application Publication No. 188456 / 1983 [Patent Document 3] JP 2016-113603 A Summary of the Invention [Problem to be solved by the invention]
[0006] Thermoplastic resins such as polycarbonate resin, ABS resin, polycarbonate ABS resin, and polylactic acid that have been used in conventional FDM methods tend to warp and deform due to effects such as thermal shrinkage when the molten thermoplastic resin is extruded from a nozzle and solidifies into a three-dimensional molded product, making it difficult to obtain molded products with high precision. A polyamide resin composition containing a polyamide resin composition and a novolac-type phenolic resin has been used in injection molding, but no attempt has been made to mold it with a 3D printer.
[0007] Therefore, an object of the present invention is to provide a polyamide resin composition for three-dimensional modeling which, when molded with a 3D printer, suppresses warping of the molded product, suppresses foaming when extruded from a nozzle, resulting in a molded product with a good appearance, low water absorption, and satisfactory strength. [Means for solving the problem]
[0008] The present invention includes, for example, the following [1] to [8]. [1] A polyamide resin composition for three-dimensional printing, comprising, based on 100 mass% of the polyamide resin composition for three-dimensional printing, 60 to 95 mass% of a polyamide resin (A) and 5 to 40 mass% of a novolac-type phenolic resin (B). [2] The polyamide resin composition for three-dimensional printing according to [1], wherein the polyamide resin (A) comprises an aliphatic copolyamide (A-1). [3] The polyamide resin composition for three-dimensional printing according to [1], wherein the polyamide resin (A) is at least one selected from the group consisting of polyamide 6, polyamide 6 / 66, polyamide 6 / 12, and polyamide 6 / 66 / 12. [4] The polyamide resin composition for three-dimensional printing according to any one of [1] to [3], wherein the novolac phenolic resin (B) has a softening point of 110 to 150°C. [5] The polyamide resin composition for 3D printing according to any one of [1] to [4], wherein an ISO 527 Type A tensile test piece obtained by injection molding the polyamide resin composition for 3D printing has a water absorption rate of 2.2% or less when immersed in water at 40°C for 24 hours. [6] The polyamide resin composition for 3D printing according to any one of [1] to [5], wherein an ISO 527 type A tensile test specimen obtained by 3D printing the polyamide resin composition for 3D printing using a 3D printer is left for 24 hours under conditions of 23°C and 50% RH, and then placed on a surface plate. When one end of a width direction side is fixed with a weight, the amount of warping of the other end of the width direction side from the surface of the surface plate is 30 mm or less. [7] A monofilament for three-dimensional printing obtained by molding the polyamide resin composition for three-dimensional printing according to any one of [1] to [6]. [8] A molded article obtained by three-dimensionally molding the polyamide resin composition for three-dimensional printing according to any one of [1] to [6] or the monofilament for three-dimensional printing according to claim 7 using a 3D printer. Effect of the Invention
[0009] When the polyamide resin composition for 3D modeling of the present application is molded using a 3D printer, warping of the molded product is suppressed, and foaming when extruded from a nozzle is suppressed, resulting in a molded product with a good appearance, low water absorption, and satisfactory strength. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram illustrating an example of a 3D printer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention relates to a polyamide resin composition for three-dimensional printing (hereinafter also referred to as "polyamide resin composition"), which contains 60 to 95 mass% of polyamide resin (A) and 5 to 40 mass% of novolac type phenolic resin (B) based on 100 mass% of the polyamide resin composition for three-dimensional printing. In this specification, "three-dimensional modeling" refers to modeling using a 3D printer.
[0012] <<Polyamide resin composition for 3D modeling>> <Polyamide resin (A)> The polyamide resin composition for three-dimensional modeling contains a polyamide resin (A). Examples of the polyamide resin (A) include aliphatic homopolyamide resin (A-2), aliphatic copolyamide resin (A-1), aromatic homopolyamide resin (A-4) and aromatic copolyamide resin (A-3). These may be used alone or in combination of two or more. Among these, from the viewpoint of molding processability, the polyamide resin (A) preferably contains at least one selected from the group consisting of aliphatic homopolyamide resin (A-2) and aliphatic copolyamide resin (A-1), and more preferably contains aliphatic copolyamide resin (A-1).
[0013] (A-1) Aliphatic copolyamide resin The aliphatic copolyamide resin (A-1) is a polyamide resin composed of two or more aliphatic structural units. The aliphatic copolyamide resin (A-1) is a copolymer of a monomer selected from the group consisting of a combination of a diamine and a dicarboxylic acid, lactam, and aminocarboxylic acid. Here, the combination of a diamine and a dicarboxylic acid is regarded as one type of monomer by combining one type of diamine and one type of dicarboxylic acid.
[0014] Examples of diamines include aliphatic diamines such as ethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, and 2,2,4 / 2,4,4-trimethylhexamethylenediamine; Examples of the diamines include alicyclic diamines such as 1,3- / 1,4-cyclohexyldiamine, bis(4-aminocyclohexyl)methane, bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, (3-methyl-4-aminocyclohexyl)propane, 1,3- / 1,4-bisaminomethylcyclohexane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, and norbornanedimethyleneamine. Among these, from the viewpoint of polymerization productivity, at least one selected from the group consisting of aliphatic diamines is preferred, at least one selected from the group consisting of linear aliphatic diamines is more preferred, and hexamethylenediamine is even more preferred. These diamines may be used alone or in appropriate combination of two or more.
[0015] Examples of dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedionic acid, dodecanedionic acid, tridecanedionic acid, tetradecanedionic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosanedioic acid; and alicyclic dicarboxylic acids such as 1,3- / 1,4-cyclohexanedicarboxylic acid, dicyclohexanemethane-4,4'-dicarboxylic acid, and norbornanedicarboxylic acid. Among these, aliphatic dicarboxylic acids are preferred, and at least one selected from the group consisting of adipic acid, sebacic acid, and dodecanedionic acid is more preferred, and at least one selected from adipic acid and dodecanedionic acid is even more preferred. These dicarboxylic acids may be used alone or in combination of two or more.
[0016] Examples of lactams include ε-caprolactam, enantholactam, undecane lactam, α-pyrrolidone, α-piperidone, laurolactam, etc. Among these, from the viewpoint of polymerization production, at least one selected from the group consisting of ε-caprolactam, undecane lactam, and laurolactam is preferred. These lactams may be used alone or in suitable combination of two or more.
[0017] Examples of aminocarboxylic acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. Among these, from the viewpoint of polymerization production, at least one selected from the group consisting of 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid is preferred. These aminocarboxylic acids may be used alone or in appropriate combination of two or more.
[0018] Specific examples of the aliphatic copolymer polyamide resin (A-1) include caprolactam / hexamethylenediaminoadipic acid copolymer (polyamide 6 / 66), caprolactam / hexamethylenediaminoazelaic acid copolymer (polyamide 6 / 69), caprolactam / hexamethylenediaminosebacic acid copolymer (polyamide 6 / 610), caprolactam / hexamethylenediaminoundecanoic acid copolymer (polyamide 6 / 611), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 612), caprolactam / aminoundecanoic acid copolymer (polyamide 6 / 613), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 614), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 615), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 616), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 617), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 618), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 619), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 620), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 621), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 622), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 623), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 624), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 625), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 626), caprolactam / hex Examples of the aliphatic copolymer polyamide include capric acid copolymer (polyamide 6 / 11), caprolactam / laurolactam copolymer (polyamide 6 / 12), caprolactam / hexamethylenediaminoadipic acid / laurolactam copolymer (polyamide 6 / 66 / 12), caprolactam / hexamethylenediaminoadipic acid / hexamethylenediaminosebacic acid copolymer (polyamide 6 / 66 / 610), caprolactam / hexamethylenediaminoadipic acid / hexamethylenediaminododecanedicarboxylic acid copolymer (polyamide 6 / 66 / 612), etc. The aliphatic copolymer polyamide resin (A-1) may be used alone or as a mixture of two or more kinds.
[0019] Among these, from the viewpoints of suppressing the water absorption rate of the molded product, suppressing warping and foaming of the molded product produced by a 3D printer, and maintaining the mechanical strength, at least one selected from the group consisting of polyamide 6 / 66, polyamide 6 / 12, and polyamide 6 / 66 / 12 is preferred, at least one selected from the group consisting of polyamide 6 / 12 and polyamide 6 / 66 / 12 is more preferred, and polyamide 6 / 66 / 12 is particularly preferred.
[0020] The production equipment for the aliphatic copolyamide resin (A-1) may be a known polyamide production equipment such as a batch reaction vessel, a single- or multi-vessel continuous reaction equipment, a tubular continuous reaction equipment, a kneading reaction extruder such as a single-screw kneading extruder or a twin-screw kneading extruder. The polymerization method may be a known method such as melt polymerization, solution polymerization or solid-phase polymerization, and may be polymerized by repeating normal pressure, reduced pressure and increased pressure operations. These polymerization methods may be used alone or in combination as appropriate.
[0021] From the viewpoints of moldability and mechanical properties, the relative viscosity of the aliphatic copolyamide resin (A-1) is preferably 2.3 or more and 5.0 or less, more preferably 2.4 or more and 5.0 or less, even more preferably 2.4 or more and 4.5 or less, and particularly preferably 2.4 or more and 4.2 or less, as measured in accordance with JIS K 6920-2 by dissolving 1 g of the aliphatic copolyamide in 100 ml of 96% concentrated sulfuric acid at 25°C.
[0022] The terminal amino group concentration of the aliphatic copolyamide resin (A-1) is determined by dissolving it in a mixed solvent of phenol and methanol and performing neutralization titration. The terminal amino group concentration of the aliphatic copolyamide resin (A-1) is preferably 30 μmol / g or more, more preferably 30 μmol / g or more and 50 μmol / g or less. If the terminal amino group concentration is within the above range, it is preferable from the viewpoint of adhesion with other resins.
[0023] (A-2) Aliphatic homopolyamide resin The aliphatic homopolyamide resin (A-2) is a polyamide resin consisting of one kind of aliphatic structural unit. The aliphatic homopolyamide resin (A-2) may consist of one kind of lactam or an aminocarboxylic acid which is a hydrolyzate of the lactam, or may consist of a combination of one kind of diamine and one kind of dicarboxylic acid. Here, the combination of diamine and dicarboxylic acid is regarded as one kind of monomer.
[0024] Examples of lactams include the same ones as those exemplified as raw materials for the aliphatic copolyamide resin (A-1). Among these, from the viewpoint of polymerization production, one selected from the group consisting of ε-caprolactam, undecane lactam and laurolactam is preferred. Examples of aminocarboxylic acids include those exemplified as raw materials for the aliphatic copolyamide resin (A-1). Among these, from the viewpoint of polymerization production, one selected from the group consisting of 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid is preferred.
[0025] Examples of diamines include those exemplified as raw materials for the aliphatic copolyamide resin (A-1). Among these, from the viewpoint of polymerization productivity, aliphatic diamines are preferred, and hexamethylenediamine is more preferred.
[0026] The dicarboxylic acid may be the same as those exemplified as the raw material of the aliphatic copolyamide resin (A-1). Among these, an aliphatic dicarboxylic acid is preferred, more preferably one selected from the group consisting of adipic acid, sebacic acid and dodecanedioic acid, and even more preferably adipic acid or dodecanedioic acid.
[0027] Specific examples of the aliphatic homopolyamide resin (A-2) include polycaprolactam (polyamide 6), polyenantholactam (polyamide 7), polyundecane lactam (polyamide 11), polylaurolactam (polyamide 12), polyhexamethylene adipamide (polyamide 66), polytetramethylene dodecamide (polyamide 412), polypentamethylene azelamide (polyamide 59), polypentamethylene sebacamide (polyamide 510), polypentamethylene dodecamide (polyamide 512), polyhexamethylene azelamide (polyamide 69), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polynonane, Examples of the polyamide include methylene adipamide (polyamide 96), polynonamethylene azelamide (polyamide 99), polynonamethylene sebacamide (polyamide 910), polynonamethylene dodecamide (polyamide 912), polydecamethylene adipamide (polyamide 106), polydecamethylene azelamide (polyamide 109), polydecamethylene decamamide (polyamide 1010), polydecamethylene dodecamide (polyamide 1012), polydodecamethylene adipamide (polyamide 126), polydodecamethylene azelamide (polyamide 129), polydodecamethylene sebacamide (polyamide 1210), polydodecamethylene dodecamide (polyamide 1212), and polyamide 122. The aliphatic homopolyamide resin (A-2) may be used alone or as a mixture of two or more kinds.
[0028] Among these, from the viewpoint of polymerization productivity, the aliphatic homopolyamide resin (A-2) is preferably at least one selected from the group consisting of polyamide 6, polyamide 11, polyamide 12, polyamide 66, polyamide 610, and polyamide 612, more preferably at least one selected from polyamide 6, polyamide 11, polyamide 12, polyamide 610, and polyamide 612, and even more preferably polyamide 6.
[0029] The production apparatus and polymerization method for the aliphatic homopolyamide resin (A-2) may be the same as those exemplified in the section for the aliphatic copolyamide resin (A-1).
[0030] The relative viscosity of the aliphatic homopolyamide resin (A-2) is measured at 25°C in accordance with JIS K 6920-2 by dissolving 1g of the aliphatic homopolyamide in 100ml of 96% concentrated sulfuric acid. The relative viscosity of the aliphatic homopolyamide is preferably 2.3 to 5.0, more preferably 2.4 to 5.0, and even more preferably 2.4 to 4.5. From the viewpoint of further improving the effects of the present invention, it is particularly preferably 2.4 to 4.2. When it is 2.3 or more, molding is easier, and when it is 5.0 or less, better mechanical properties of the polyamide resin can be maintained.
[0031] The terminal amino group concentration of the aliphatic homopolyamide resin (A-2) is determined by dissolving it in a mixed solvent of phenol and methanol and performing neutralization titration. The terminal amino group concentration of the aliphatic homopolyamide resin (A-2) is preferably 30 μmol / g or more, more preferably 30 μmol / g or more and 50 μmol / g or less.
[0032] (A-3) Aromatic copolyamide resin Aromatic polyamide is an aromatic polyamide resin containing at least one aromatic monomer component, for example, a polyamide resin obtained by polycondensation of aliphatic dicarboxylic acid and aromatic diamine, aromatic dicarboxylic acid and aliphatic diamine, or aromatic dicarboxylic acid and aromatic diamine. Aromatic copolymer polyamide resin (A-3) is a polyamide resin consisting of two or more kinds of structural units among the above aromatic polyamide resins. Here, a combination of diamine and dicarboxylic acid is regarded as one kind of monomer by a combination of one kind of diamine and one kind of dicarboxylic acid.
[0033] Examples of the aliphatic diamines and aliphatic dicarboxylic acids used as raw materials include the same as those exemplified as the raw materials for the aliphatic copolyamide (A-1) described above, and also include those exemplified as the alicyclic diamines and alicyclic dicarboxylic acids. These aliphatic diamines and aliphatic dicarboxylic acids may be used alone or in appropriate combination of two or more. Examples of the aromatic diamine include metaxylylenediamine and paraxylylenediamine, and examples of the aromatic dicarboxylic acid include naphthalenedicarboxylic acid, terephthalic acid, isophthalic acid, and phthalic acid. These aromatic diamines and aromatic dicarboxylic acids may be used alone or in appropriate combination of two or more. The aromatic copolyamide resin may contain structural units derived from lactam or aminocarboxylic acid, and examples of the lactam or aminocarboxylic acid include the same as those exemplified as the raw materials for the aliphatic copolyamide (A-1) described above. These lactams and aminocarboxylic acids may be used alone or in combination of two or more.
[0034] Specific examples of the aromatic copolymer polyamide resin (A-3) include (polyamide 66 / 6T), polyhexamethylene terephthalamide / polycaproamide copolymer (polyamide 6T / 6), polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (polyamide 66 / 6I), polyhexamethylene isophthalamide / polycaproamide copolymer (polyamide 6I / 6), polydodecaamide, Polyhexamethylene terephthalamide copolymer (polyamide 12 / 6T), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (polyamide 66 / 6T / 6I), polyhexamethylene adipamide / polycaproamide / polyhexamethylene isophthalamide copolymer (polyamide 66 / 6 / 6I), polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (polyamide 6T / 6I), polyhexamethylene terephthalamide / poly(2-methylpentamethylene terephthalamide) copolymer (polyamide 6T / M5T), etc. The aromatic copolymer polyamide resin (A-3) may be used alone or in combination of two or more. Among these, polyamide 6T / 6I is preferred.
[0035] The production apparatus and polymerization method for the aromatic copolyamide resin (A-3) may be the same as those exemplified in the section for the aliphatic copolyamide resin (A-1).
[0036] The degree of polymerization of the aromatic copolyamide resin (A-3) in the present invention is not particularly limited, but from the viewpoints of moldability and mechanical properties, the relative viscosity measured at 25°C according to JIS K 6920-2 is preferably from 2.3 to 5.0, more preferably from 2.4 to 5.0, even more preferably from 2.4 to 4.5, and particularly preferably from 2.4 to 4.2.
[0037] The terminal amino group concentration of the aromatic copolymer polyamide resin (A-3) is determined by dissolving it in a mixed solvent of phenol and methanol and performing neutralization titration. The terminal amino group concentration of the aromatic copolymer polyamide resin (A-3) is preferably 20 μmol / g or more and 60 μmol / g or less.
[0038] (A-4) Aromatic homopolyamide resin The aromatic homopolyamide resin (A-4) is an aromatic polyamide resin consisting of one type of structural unit derived from an aromatic monomer component, for example, a polyamide resin obtained by polycondensation of aliphatic dicarboxylic acid and aromatic diamine, aromatic dicarboxylic acid and aliphatic diamine, or aromatic dicarboxylic acid and aromatic diamine as raw materials. Here, the combination of diamine and dicarboxylic acid is regarded as one type of monomer by the combination of one type of diamine and one type of dicarboxylic acid.
[0039] Examples of the aliphatic diamines and aliphatic dicarboxylic acids as the raw materials include the same as those exemplified as the raw materials for the aliphatic copolyamide (A-1), and also include those exemplified as the alicyclic diamines and alicyclic dicarboxylic acids. Examples of the aromatic diamine include metaxylylenediamine and paraxylylenediamine, and examples of the aromatic dicarboxylic acid include naphthalenedicarboxylic acid, terephthalic acid, isophthalic acid, and phthalic acid.
[0040] Specific examples of the aromatic homopolyamide resin (A-4) include polynonamethylene terephthalamide (polyamide 9T), polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene isophthalamide (polyamide 6I), polyxylylene adipamide (polyamide MXD6), etc. The aromatic homopolyamide resin (A-4) may be used alone or in combination of two or more.
[0041] The production apparatus and polymerization method for the aromatic homopolyamide resin (A-4) may be the same as those exemplified in the section for the aliphatic copolyamide resin (A-1).
[0042] The degree of polymerization of the aromatic homopolyamide resin (A-4) in the present invention is not particularly limited, but from the viewpoints of moldability and mechanical properties, the relative viscosity measured at 25°C in accordance with JIS K 6920-2 is preferably from 2.3 to 5.0, more preferably from 2.4 to 5.0, even more preferably from 2.4 to 4.5, and particularly preferably from 2.4 to 4.2.
[0043] The polyamide resin (A) preferably has a relative viscosity of 2.3 to 5.0, more preferably 2.4 to 5.0, and even more preferably 2.4 to 4.5, measured at 25°C by dissolving 1g of the polyamide resin in 100ml of 96% concentrated sulfuric acid according to JIS K 6920-2. From the viewpoint of further improving the effects of the present invention, it is particularly preferably 2.4 to 4.2. If it is 2.3 or more, molding processing is easier. Also, if it is 5.0 or less, better mechanical properties of the polyamide resin can be obtained.
[0044] When the polyamide resin (A) contains two or more polyamide resins having different relative viscosities (for example, at least one aliphatic homopolyamide resin (A-2) and at least one aliphatic copolymer polyamide resin (A-1)), the relative viscosity of the polyamide resin (A) is preferably measured as described above. However, when the relative viscosity of each polyamide resin and its mixing ratio are known, the relative viscosity of the polyamide resin (A) may be determined by multiplying each relative viscosity by the mixing ratio and adding up the values, and the average value calculated may be used as the relative viscosity of the polyamide resin (A).
[0045] The terminal amino group concentration of the polyamide resin (A), as determined by dissolving the resin in a mixed solvent of phenol and methanol and performing neutralization titration, is preferably in the range of 30 μmol / g or more, more preferably in the range of 30 μmol / g to 110 μmol / g, and even more preferably in the range of 30 μmol / g to 70 μmol / g. If it is 30 μmol / g or more, it is possible to obtain good adhesion to the reinforcing material, sufficient melt viscosity and impact resistance. Also, if it is 110 μmol / g or less, it is possible to obtain good moldability.
[0046] When the polyamide resin (A) contains two or more polyamide resins having different terminal amino group concentrations (for example, at least one aliphatic homopolyamide resin (A-2) and at least one aliphatic copolymer polyamide resin (A-1)), the terminal amino group concentration in the polyamide resin (A) is preferably measured by the above-mentioned neutralization titration. However, when the terminal amino group concentrations of each polyamide resin and their mixing ratios are known, the terminal amino group concentration of the polyamide resin (A) may be determined by adding up the values obtained by multiplying each terminal amino group concentration by the mixing ratio.
[0047] The polyamide resin (A) is contained in an amount of 60 to 95% by mass, preferably 70 to 85% by mass, and more preferably 70 to 78% by mass, based on 100% by mass of the polyamide resin composition for 3D printing. If the content of polyamide resin (A) is less than the above range, the mechanical properties of the polyamide resin are reduced, whereas if it is more than the above range, the water absorption rate of the molded product is increased, and the molded product produced by the 3D printing device has large warpage and foaming.
[0048] <Novolac-type phenolic resin (B)> The novolac-type phenolic resin (B) may be one produced by condensation polymerization of phenols and aldehydes in the presence of an acid catalyst, but does not include resol-type phenol-formaldehyde resins produced by condensation polymerization of phenols and aldehydes in the presence of an alkaline catalyst.
[0049] Here, examples of the phenols used in the production of the novolac phenolic resin (B) include monohydric or polyhydric phenols such as phenol, cresol, trimethylphenol, xylenol, resorcinol, catechol, butylphenol, octylphenol, nonylphenol, phenylphenol, dihydroxybenzene, bisphenol A, and naphthol, as well as their substituted derivatives. These may be used alone or in combination of two or more. Among these, phenol and cresol are preferred, and phenol is more preferred.
[0050] Specific examples of aldehydes used in the production of the novolac phenolic resin (B) include formaldehyde, acetaldehyde, propionaldehyde, butylaldehyde, glyoxal, n-propanal, n-butanal, isopropanal, isobutylaldehyde, 3-methyl-n-butanal, benzaldehyde, p-tolylaldehyde, and 2-phenylacetaldehyde, and these may be used alone or in combination of two or more. Among these, formaldehyde and acetaldehyde are preferred, and formaldehyde is more preferred.
[0051] The acid catalyst is not particularly limited, but examples thereof include oxalic acid, hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, paratoluenesulfonic acid, phenolsulfonic acid, formic acid, maleic acid, zinc acetate, and zinc octoate.
[0052] Among such novolac type phenolic resins (B), a phenol formaldehyde resin represented by the following formula (1) is preferred from the viewpoints of mechanical properties and heat resistance. [ka] In the above formula (1), n is preferably an integer of 1 to 200, more preferably an integer of 1 to 50, and even more preferably an integer of 5 to 20.
[0053] The number average molecular weight of the novolac phenolic resin (B) is preferably 100 to 20,000, more preferably 300 to 15,000, from the viewpoint of moldability and heat resistance. The number average molecular weight is calculated based on the hydroxyl value measured in accordance with JIS K 1557. Specifically, the hydroxyl value is measured, and calculated by the terminal group quantitative method using (56.1×1000×valence) / hydroxyl value (in this formula, the unit of hydroxyl value is [mgKOH / g]). In the formula, the valence is the number of hydroxyl groups in one molecule.
[0054] From the viewpoints of moldability and heat resistance, the softening point of the novolak phenolic resin (B) is preferably 50 to 250° C., more preferably 70 to 200° C., further preferably 110 to 150° C., particularly preferably 110 to 130° C., and most preferably 120 to 130° C. The softening point is a value determined by a ring and ball softening point measurement based on JIS K6910.
[0055] Commercially available products of such novolak type phenolic resins include HF-4M and NC58 manufactured by Meiwa Kasei. In 100% by mass of the polyamide resin composition for three-dimensional printing, the novolac type phenolic resin (B) is contained in an amount of 5 to 40% by mass, preferably 5 to 35% by mass, and more preferably 22 to 30% by mass. If the amount of the novolac type phenolic resin is less than the above range, the water absorption rate of the molded product increases, and the molded product produced by the three-dimensional printing device has a large warp and a large amount of foaming due to water absorption. If the content of the novolac type phenolic resin is more than the above range, the mechanical properties of the polyamide itself are impaired.
[0056] <Additives> The polyamide resin composition for 3D modeling may contain, as optional components, appropriate functionality-imparting agents such as dyes, pigments, fibrous reinforcements, particulate reinforcements, plasticizers, antioxidants, heat resistance agents, foaming agents, weather resistance agents, crystal nucleating agents, crystallization accelerators, release agents, lubricants, antistatic agents, flame retardants, flame retardant assistants, and colorants, depending on the purpose, etc. The optional additives are contained in an amount of preferably 0.01 to 45% by mass, and more preferably 0.05 to 30% by mass, based on 100% by mass of the polyamide resin composition for 3D modeling.
[0057] The polyamide resin composition for three-dimensional printing may contain a resin other than the polyamide resin (A) and the novolac phenolic resin (B), preferably in an amount of 20% by mass or less.
[0058] <Method of manufacturing polyamide resin composition for three-dimensional modeling> The method for producing the polyamide resin composition for three-dimensional modeling is not particularly limited, and for example, the following method can be applied. For mixing the polyamide resin (A), the novolac phenolic resin (B), and other optional components, a commonly known melt kneader such as a single-screw or twin-screw kneader, a Banbury mixer, a kneader, or a mixing roll may be used. For example, any of the following methods may be used: a method in which all raw materials are mixed using a twin-screw kneader, and then melt-kneaded; a method in which some raw materials are mixed, then melt-kneaded, and then the remaining raw materials are mixed and melt-kneaded; or a method in which some raw materials are mixed, and then the remaining raw materials are mixed using a side feeder during melt-kneading.
[0059] <Characteristics of polyamide resin composition for 3D modeling> A type A tensile test piece obtained by injection molding a polyamide resin composition for 3D printing according to ISO 527 at a molding temperature of 250°C and a mold temperature of 40°C when the polyamide resin (A) contains polyamide 6, or at a molding temperature of 220°C and a mold temperature of 40°C when the polyamide resin (A) does not contain polyamide 6, is stored at room temperature after molding so as not to absorb water, and then the initial weight (W0) is measured, the piece is immersed in water at 40°C for 24 hours, and after removal, any adhering moisture is wiped off, the weight (W1) is measured, and the water absorption calculated by ((W1-W0) / W0) x 100 is preferably 2.2% or less, and more preferably 2.0% or less. In this way, the polyamide resin composition for three-dimensional modeling has a suppressed water absorption rate.
[0060] A type A tensile test specimen obtained by 3D printing the polyamide resin composition for 3D modeling according to the shape of ISO527 using a 3D printer was left for 24 hours under conditions of 23°C and 50% RH, and then the test specimen was placed on a surface plate and one end of the width direction side was fixed with a 30 mm wide, 200 g weight. The amount of warping of the other end of the width direction side from the surface of the surface plate was measured with a ruler, and the amount of warping obtained was preferably 30 mm or less, and more preferably 20 mm or less. In this way, the polyamide resin composition for 3D modeling can suppress warping of molded articles obtained by 3D modeling using a 3D printer, making it possible to obtain molded products with good precision.
[0061] <Filament for 3D modeling> The filament for three-dimensional printing is produced by using the polyamide resin composition for three-dimensional printing. The method for producing the filament for three-dimensional printing is not particularly limited, but the filament can be obtained by molding the polyamide resin composition for three-dimensional printing by a known molding method such as extrusion molding, or by using the polyamide resin composition for three-dimensional printing as filament during production. Specifically, in a method for producing a filament for 3D modeling from the polyamide resin composition for 3D modeling, for example, when the filament for 3D modeling is obtained by extrusion molding, the temperature setting is preferably the melting point or glass transition temperature (Tg) of the polyamide resin composition for 3D modeling plus 5 to 100°C, preferably 10 to 80°C.
[0062] The diameter of the filament for three-dimensional modeling is determined by the device, but in the case of a 1.75 mm specification, the range of 1.65 to 1.85 mm is preferable, and in the case of a 3.00 mm specification, the range of 2.90 to 3.10 mm is preferable.
[0063] In order to prevent blocking between the filaments for 3D modeling before melting, a blocking agent may be applied or coated onto the surface of the filaments for 3D modeling.
[0064] Examples of the blocking agent that can be used here include silicone-based blocking agents, inorganic fillers such as talc, fatty acid metal salts, etc. These blocking agents may be used alone or in combination of two or more.
[0065] Preferred forms of the filament include a wound body in which the filament is wound around a bobbin or the like, and a cartridge in which the filament is housed in a container.
[0066] <3D modeling method> A molded body can be produced by modeling a polyamide resin composition for 3D modeling or a filament for 3D modeling (hereinafter also referred to as "material for 3D modeling") using a 3D printer, which is a device for producing 3D objects.
[0067] The 3D printer is not particularly limited, but an FDM device is preferred. As shown in FIG. 1, an FDM 3D printer usually includes a raw material supply unit, a gear 2, a tube 3, a nozzle 4 equipped with a heater 6, and a table 5. The heater and the nozzle may be separate.
[0068] In an FDM 3D printer, the material for 3D modeling is fed from a raw material supply section, sent into a tube 3 by a pair of opposing gears 2, heated and melted by a heater 6, and extruded from a nozzle 4.
[0069] The temperature to which the material for 3D modeling is heated to melt is not particularly limited, but is preferably equal to or higher than the melting point or glass transition temperature (Tg) of the polyamide resin composition for 3D modeling and equal to or lower than the melting point or glass transition temperature (Tg) +300°C. Specifically, the temperature is preferably set to the melting point or glass transition temperature (Tg) plus 5 to 100°C, preferably 10 to 80°C.
[0070] The molten 3D modeling material extruded from nozzle 4 is deposited on table 5, which defines the XY axis directions, as two-dimensional layers sliced based on the three-dimensional coordinate data. These two-dimensional layers are then stacked sequentially in the Z axis direction to obtain a 3D modeled object.
[0071] The molding speed is preferably 10 to 100 mm / sec.
[0072] <Uses of molded bodies obtained by 3D modeling> The uses of the molded articles obtained by 3D modeling of the polyamide resin composition for 3D modeling or the filaments for 3D modeling are not particularly limited, and suitable uses include automobile parts such as spoilers, air intake ducts, intake manifolds, resonators, fuel tanks, gas tanks, hydraulic oil tanks, fuel filler tubes, fuel delivery pipes, and various other hoses, tubes, and tanks, machine parts such as power tool housings and pipes, electric and electronic parts such as tanks, tubes, hoses, and films, household and office supplies, building material-related parts, and furniture parts.
[0073] In addition, since the polyamide resin composition for three-dimensional modeling has excellent gas barrier properties, it is suitable for use in molded products that come into contact with high-pressure gas, such as tanks, tubes, hoses, films, etc. The type of gas is not particularly limited and examples thereof include hydrogen, nitrogen, oxygen, helium, methane, butane, propane, etc., with less polar gases being preferred, and hydrogen, nitrogen, and methane being particularly preferred. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0075] The test pieces used in the measurements were prepared in the following manner. (1) Creating test pieces by injection molding The polyamide resin compositions were injection molded according to ISO 527 to prepare Type A tensile test specimens at a cylinder temperature of 250°C and a mold temperature of 40°C for polyamide 6, and at a cylinder temperature of 220°C and a mold temperature of 40°C for the other copolymer polyamides.
[0076] (2) Modeling using a 3D printer (2-1) Creating filament The polyamide resin composition is extruded using an extruder at a cylinder temperature of 230°C from a nozzle with a diameter of 3 mm. The resin is then wound up and the filament diameter is adjusted to 1.75 mm to create a filament for use in a 3D printer. (2-2) Modeling with a 3D printer The 3D printer used was a Value3D MagiX MF-2200D manufactured by Muto Industries Ltd., with a nozzle diameter of 0.5 mm, a nozzle heater of 240°C, a table temperature of 110°C, a layer pitch of 0.3 mm, a modeling speed of 72 mm / sec, and no cooling fan. Using the filament obtained in (2-1), the molten filament was layered sequentially on the table based on the three-dimensional coordinate data to obtain a model.
[0077] The values shown in the examples and Table 1 were measured by the following methods. (3)Measurement method <Relative viscosity> The value is measured in accordance with JIS K6920-2 by dissolving 1 g of polyamide in 100 ml of 96% concentrated sulfuric acid at 25°C.
[0078] <Softening point temperature> The softening point temperature is a value determined by a ring and ball softening point measurement based on JIS K6910.
[0079] <Water absorption rate> The polyamide resin composition was injection molded under the above (1) conditions to obtain a type A tensile test piece, which was stored at room temperature to prevent water absorption after molding, and the initial weight (W0) was measured. The dried test piece was then immersed in water at 40°C for 24 hours and in water at 80°C for 24 hours. After removal, the moisture was wiped off and the weight (W1) was measured, and the water absorption was calculated by ((W1-W0) / W0)×100.
[0080] <Warping of 3D printed products> The polyamide resin composition was molded into a shape according to ISO527 according to the above-mentioned (2) 3D printer molding method, and the obtained test piece was left for 24 hours under conditions of 23°C and 50% RH. Next, the test piece was placed on a surface plate, and one end of the width direction side was fixed with a 30 mm wide, 200 g weight, and the amount of warping up from the surface of the surface plate was measured with a finger.
[0081] <Bubble foam coming from a 3D printer nozzle> The polyamide resin composition was made into filaments by the method described above in (2-1). The obtained filaments were left at 23°C and 50% RH for 24 hours, 100 hours, and 240 hours, and used as humidity-conditioned filaments after 24 hours, 100 hours, and 240 hours. The moisture-conditioned filament was fed into the 3D printer at a feed rate of 300 mm / min, and the foaming state of the resin emerging from the nozzle of the 3D printer was visually confirmed. The foaming was evaluated according to the following criteria. ×: A lot of foaming is observed △: A little foaming is observed 〇: No foaming observed When the moisture-conditioned filament was used after 24 hours, the filament was rated as passing if no foaming was observed.
[0082] <Mechanical properties of 3D printer-made products> Regarding the mechanical properties in the Z-axis direction, the polyamide resin composition was molded into a test piece shape conforming to ISO178 according to the 3D printer molding method described above in (2), and the tensile strength and nominal tensile break strain were measured using an Instron tensile testing machine, Model 5567, under the conditions of a chuck distance of 20 mm and a test speed of 5 mm / min. Regarding the mechanical properties in the XY axis direction, the polyamide resin composition was molded into a type A test piece shape conforming to ISO527 according to the above-mentioned (2) 3D printer molding method, and the tensile strength and nominal tensile break strain were measured using an Instron tensile testing machine, model 5567, under the conditions of a chuck distance of 115 mm and a test speed of 5 mm / min. The XY axis direction refers to the table surface on which the model is being shaped, and the Z axis direction refers to the direction perpendicular to the plane defined by the XY axes.
[0083] [Examples 1 to 10, Comparative Examples 1 to 4] Each component listed in Table 1 was melt-kneaded in a twin-screw kneader ZSK32McPlus (manufactured by Coperion) with an L / D of 48 and a screw diameter of 32 mm at a cylinder temperature of 230°C, a screw rotation speed of 200 rpm, and a discharge rate of 50 kg / h to prepare pellets of a polyamide resin composition. The above-mentioned (1) test piece and (2) shaped article were prepared from the obtained pellets. The units of compositions in the tables are mass %, with the entire resin composition being 100 mass %.
[0084] The components used in Table 1 were as follows: PA6(1): Polyamide 6, relative viscosity 2.47 (Ube Industries, Ltd.) PA6(2): Polyamide 6, relative viscosity 3.37 (Ube Industries, Ltd.) PA6 / 66: Polyamide 6 / 66, relative viscosity 4.05, polyamide 6 85mol%, polyamide 66 15mol% (Ube Industries, Ltd.) PA6 / 12: Polyamide 6 / 12, relative viscosity 3.87, polyamide 6 80mol%, polyamide 12 20mol% (Ube Industries, Ltd.) PA6 / 66 / 12: Polyamide 6 / 66 / 12, relative viscosity 4.05, polyamide 6 80mol%, polyamide 66 10mol%, polyamide 12 10mol% (manufactured by Ube Industries, Ltd.) Novolac type phenolic resin (1): softening point temperature: 102°C, product name HF-4M (manufactured by Meiwa Kasei), structure represented by formula (1), n = approx. 6.7 Novolac type phenolic resin (2): softening point temperature: 125°C, product name NC58 (manufactured by Meiwa Kasei), structure represented by formula (1), n = approx. 14.6
[0085] [Table 1]
[0086] When the polyamide resin compositions of Examples 1 to 10 were molded using a 3D printer, the molded products were prevented from warping, and foaming during extrusion from a nozzle was suppressed, resulting in a good appearance, low water absorption, and satisfactory strength. In particular, the polyamide resin compositions of Examples 8 to 10 containing an aliphatic copolyamide further suppressed warpage of the molded articles, and also had high strength. Comparing Examples 3 and 4, it can be seen that warping is further suppressed when a polyamide resin having a relative viscosity within a specific range is used. Comparing Example 1 and Example 5, it is found that warpage is further suppressed when the softening point temperature of the novolac phenolic resin is within a specific range. Comparing Examples 1 to 3 with Examples 5 to 7, it is found that when the softening point temperature of the novolac phenolic resin is within a specific range, the strength is increased. [Industrial Applicability]
[0087] The polyamide resin composition for three-dimensional modeling of the present invention is suitably used for modeling using a 3D printer. [Explanation of symbols]
[0088] 1 filament 2 Gear 3 Tubes 4 Nozzles 5 Tables 6. Heater 7. FDM 3D Printer
Claims
1. A polyamide resin composition for three-dimensional printing, comprising 60 to 95 mass% of a polyamide resin (A) and 5 to 40 mass% of a novolac-type phenolic resin (B) based on 100 mass% of the polyamide resin composition for three-dimensional printing.
2. The polyamide resin composition for three-dimensional modeling according to claim 1, wherein the polyamide resin (A) contains an aliphatic copolyamide (A-1).
3. 2. The polyamide resin composition for three-dimensional modeling according to claim 1, wherein the polyamide resin (A) is at least one selected from the group consisting of polyamide 6, polyamide 6 / 66, polyamide 6 / 12, and polyamide 6 / 66 / 12.
4. The polyamide resin composition for three-dimensional modeling according to any one of claims 1 to 3, wherein the novolac type phenolic resin (B) has a softening point of 110 to 150°C.
5. The polyamide resin composition for three-dimensional modeling according to any one of claims 1 to 4, wherein an ISO527 Type A tensile test piece obtained by injection molding the polyamide resin composition for three-dimensional modeling has a water absorption rate of 2.2% or less when immersed in water at 40°C for 24 hours.
6. The polyamide resin composition for three-dimensional modeling according to any one of claims 1 to 5, wherein an ISO 527 Type A tensile test piece obtained by three-dimensionally modeling the polyamide resin composition for three-dimensional modeling using a 3D printer is left for 24 hours under conditions of 23°C and 50% RH, and then placed on a surface plate. When one end of a width direction side is fixed with a weight, the amount of warping of the other end of the width direction side from the surface of the surface plate is 30 mm or less.
7. A monofilament for three-dimensional modeling obtained by molding the polyamide resin composition for three-dimensional modeling according to any one of claims 1 to 6.
8. A molded article obtained by three-dimensionally molding the polyamide resin composition for three-dimensional modeling according to any one of claims 1 to 6 or the monofilament for three-dimensional modeling according to claim 7 using a 3D printer.
Citation Information
Patent Citations
Under-hood parts for automobile
JP1985188456A
Flame-retardant polyamide resin composition
JP2002129010A
Conductive polyamide resin composition
JP2005054087A
Flame retardant polyamide-based resin composition
JP2008050509A
Polyamide resin composition
JP2008540777A