Separator with functional layer for electrochemical element, and electrochemical element

A single functional layer with inorganic particles and particulate polymer on electrochemical device separators addresses manufacturing complexity and adhesion issues, improving electrolyte pourability and heat resistance for enhanced electrochemical device performance.

JP7567787B2Active Publication Date: 2024-10-16ZEON CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021524816
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-03
Filing Date
2020-05-29
Publication Date
2024-10-16
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

Conventional separators for electrochemical devices require a separate heat-resistant layer and adhesive layer, leading to a complex manufacturing process and insufficient adhesion between components, which affects electrolyte pourability and heat resistance.

Method used

A single functional layer is introduced, comprising inorganic particles and a particulate polymer with a maximum surface height of 2.5 μm or more, featuring convex portions with particulate polymer on the surface, to enhance process adhesion, heat resistance, and electrolyte pourability.

Benefits of technology

The functional layer simplifies manufacturing, improves adhesion between components, enhances electrolyte pourability, and maintains excellent heat resistance, resulting in better electrochemical device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567787000002
    Figure 0007567787000002
  • Figure 0007567787000003
    Figure 0007567787000003
  • Figure 0007567787000004
    Figure 0007567787000004
Patent Text Reader

Abstract

This separator including a functional layer for an electrochemical element is provided with a separator substrate and a functional layer for an electrochemical element, the functional layer being disposed on at least one surface of the separator substrate. This functional layer for an electrochemical element contains inorganic particles and a particulate polymer. The maximum height Sz of the surface of the functional layer for an electrochemical element is 2.5 µm or greater. The functional layer for an electrochemical element has surface protrusions containing the particulate polymer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator with a functional layer for an electrochemical device, and an electrochemical device. [Background technology]

[0002] Electrochemical devices such as lithium ion secondary batteries and electric double layer capacitors are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications.

[0003] Here, for example, a lithium ion secondary battery generally includes battery components such as a positive electrode, a negative electrode, and a separator that isolates the positive electrode from the negative electrode to prevent a short circuit between the positive electrode and the negative electrode.

[0004] In recent years, further improvements in the separator have been investigated in order to further improve the performance of lithium ion secondary batteries. Specifically, for example, Patent Document 1 proposes a separator in which a heat-resistant layer containing non-conductive particles and a binder is formed on a separator substrate, and an adhesive layer containing a specific particulate polymer is further provided on the heat-resistant layer. Patent Document 1 also reports that the use of a separator having an adhesive layer on the heat-resistant layer can satisfactorily bond the separator and electrodes, thereby improving the battery characteristics of a secondary battery. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2013 / 151144 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the production of the above-mentioned conventional separator having a heat-resistant layer and an adhesive layer, it is necessary to sequentially form the heat-resistant layer on the separator substrate and the adhesive layer on the heat-resistant layer, making the production process complicated.

[0007] In response to such problems, it is conceivable that, for example, instead of a heat-resistant layer and an adhesive layer provided separately, a single layer capable of simultaneously exhibiting heat resistance and adhesive properties (hereinafter, such a layer will be referred to as a "functional layer") could be formed on the separator substrate, thereby simplifying the separator manufacturing process and increasing productivity.

[0008] Therefore, the present inventors have focused on the fact that if a composition containing a component contributing to heat resistance and a component contributing to adhesion is used, the resulting functional layer can simultaneously exhibit heat resistance and adhesion. However, the present inventors have studied and found that a functional layer formed using a composition that is a simple mixture of a component contributing to heat resistance and a component contributing to adhesion has insufficient adhesion between members during the manufacturing process of an electrochemical element (hereinafter also referred to as "process adhesion"). In addition, since there is a trade-off between heat resistance and adhesion, it has become clear that it is difficult to form a functional layer that can exhibit excellent heat resistance while ensuring sufficient adhesion. Furthermore, an electrochemical element manufactured using a functional layer is required to have good electrolyte pourability (hereinafter referred to as "electrolyte pourability") when manufacturing an electrochemical element.

[0009] Therefore, an object of the present invention is to provide a separator with a functional layer for an electrochemical element, which has excellent process adhesion and heat resistance, and is provided with a functional layer that can improve electrolyte injectability. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to achieve the above object, and have found that by forming a functional layer for electrochemical elements, which contains inorganic particles and a particulate polymer, has a maximum surface height Sz of a predetermined value or more, and has protrusions containing a particulate polymer on the surface, on a separator substrate, a separator with a functional layer for electrochemical elements, which has excellent process adhesion and heat resistance and can improve electrolyte injection properties, can be obtained, and have completed the present invention.

[0011] That is, the present invention aims to advantageously solve the above problems, and the separator with functional layer for electrochemical elements of the present invention is a separator with functional layer for electrochemical elements comprising a separator substrate and a functional layer for electrochemical elements arranged on at least one surface of the separator substrate, the functional layer for electrochemical elements comprising inorganic particles and a particulate polymer, the maximum height Sz of the surface of the functional layer for electrochemical elements being 2.5 μm or more, and the functional layer for electrochemical elements having a convex portion containing the particulate polymer on the surface. In this way, by forming a functional layer for electrochemical elements comprising inorganic particles and a particulate polymer, having a maximum height Sz of a surface of a predetermined value or more, and having a convex portion containing the particulate polymer on the separator substrate, a separator with functional layer for electrochemical elements having excellent process adhesion and heat resistance and good electrolyte injectability can be provided. In this specification, the "maximum surface height Sz" conforms to ISO25178. In addition, in the present invention, a "protrusion" refers to a portion of the surface of the functional layer that protrudes 1 μm or more from the plane of the arithmetic mean height Sa of the functional layer. Here, the protrusion "containing a particulate polymer on its surface" refers to a state in which a particulate polymer is exposed on the surface of the protrusion of the functional layer when the separator with the functional layer is observed alone. The "protrusion containing a particulate polymer on its surface" of the functional layer can be confirmed by SEM-EDX (scanning electron microscope-energy dispersive X-ray analysis).

[0012] Here, in the separator with a functional layer for electrochemical devices of the present invention, the maximum height Rz of the surface of the functional layer for electrochemical devices is preferably 1.6 μm or more. In this way, if the maximum height Rz of the surface of the functional layer for electrochemical devices is equal to or greater than the above-mentioned predetermined value, the process adhesion of the functional layer can be further improved. In this specification, the "maximum surface height Rz" conforms to JIS B 0601.

[0013] In addition, in the separator with a functional layer for electrochemical devices of the present invention, the arithmetic mean height Sa of the surface of the functional layer for electrochemical devices is preferably 0.2 μm or more. In this way, if the arithmetic mean height Sa of the surface of the functional layer for electrochemical devices is equal to or more than the above-mentioned predetermined value, the process adhesion of the functional layer can be further improved. In this specification, the "arithmetic mean height Sa" conforms to ISO25178.

[0014] Furthermore, in the separator with a functional layer for electrochemical devices of the present invention, the volume ratio of the inorganic particles to the particulate polymer in the functional layer for electrochemical devices (inorganic particles / particulate polymer) is preferably 1.1 or more and 2.1 or less. In this way, when the volume ratio of the inorganic particles to the particulate polymer in the functional layer for electrochemical devices is within the above-mentioned predetermined range, the functional layer has a good balance between process adhesion and heat resistance.

[0015] In addition, in the separator with a functional layer for an electrochemical device of the present invention, the particulate polymer preferably has an electrolyte swelling degree of 1 to 15. In this way, when the electrolyte swelling degree of the particulate polymer is within the above-mentioned predetermined range, the adhesiveness of the functional layer in the electrolyte can be increased, and the electrochemical properties of an electrochemical device including the functional layer can be improved.

[0016] Furthermore, in the separator with a functional layer for an electrochemical device of the present invention, it is preferable that the particulate polymer satisfies the following 1) or 2). 1) The glass transition temperature of the particulate polymer is 15° C. or higher and 90° C. or lower. 2) The melting point of the particulate polymer is 50° C. or higher. In this way, if the glass transition temperature of the particulate polymer is within the above-mentioned range, the blocking of the functional layer can be suppressed while ensuring good adhesion of the functional layer. Also, if the melting point of the particulate polymer is 50°C or higher, even if the particulate polymer contains a crystalline polymer, the good adhesion of the functional layer can be ensured. In the present invention, the "glass transition temperature" and the "melting point" can be measured by the method described in the Examples of this specification.

[0017] In the separator with a functional layer for an electrochemical element of the present invention, the particulate polymer preferably contains an epoxy group-containing unsaturated monomer unit. In this way, if the particulate polymer contains an epoxy group-containing unsaturated monomer unit, the adhesiveness of the functional layer in the electrolyte can be increased, and the storage characteristics of an electrochemical element having the functional layer can be improved.

[0018] Furthermore, in the separator with functional layer for electrochemical element of the present invention, the content ratio of the epoxy group-containing unsaturated monomer unit in the particulate polymer is preferably 0.5% by mass or more and 30.0% by mass or less. In this way, if the content ratio of the epoxy group-containing monomer unit in the particulate polymer is equal to or more than the above-mentioned predetermined value, the adhesiveness of the functional layer in the electrolyte can be increased and the storage characteristics of the electrochemical element equipped with the functional layer can be improved, and if the content ratio of the epoxy group-containing monomer unit in the particulate polymer is equal to or less than the above-mentioned predetermined value, the particulate polymer can be stably produced.

[0019] The present invention has an object to advantageously solve the above problems, and the electrochemical element of the present invention is characterized by comprising the above-mentioned separator with functional layer for electrochemical element. In this way, by comprising the separator with functional layer for electrochemical element of the present invention, it is possible to provide an electrochemical element that can exhibit excellent electrochemical properties. Effect of the Invention

[0020] According to the present invention, it is possible to provide a separator with a functional layer for an electrochemical element, which has excellent process adhesion and heat resistance, and is provided with a functional layer that can improve electrolyte injectability. Moreover, according to the present invention, it is possible to provide an electrochemical element capable of exhibiting excellent electrochemical properties. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a separator with a functional layer for an electrochemical element according to the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of a separator with a functional layer for an electrochemical element according to the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing still another example of a separator with a functional layer for an electrochemical element according to the present invention. [Figure 4] FIG. 4 is a schematic plan view showing an example of the configuration of a functional layer when the surface of the functional layer of the separator with a functional layer for an electrochemical element according to the present invention is viewed in plan. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment of the present invention will be described in detail. Here, the separator with a functional layer for an electrochemical device of the present invention can be used when producing the electrochemical device of the present invention. The electrochemical device of the present invention is an electrochemical device that includes at least the separator with a functional layer for an electrochemical device of the present invention.

[0023] (Separator with functional layer for electrochemical elements) The separator with a functional layer for an electrochemical element of the present invention (hereinafter also simply referred to as a "separator with a functional layer") comprises a separator substrate and a predetermined functional layer for an electrochemical element disposed on at least one surface of the separator substrate. According to the present invention, it is possible to provide a separator with a functional layer for an electrochemical element that has excellent process adhesion and heat resistance and is provided with a functional layer that can improve electrolyte injectability.

[0024] <Separator substrate> The separator substrate is not particularly limited, and may be, for example, one described in JP 2012-204303 A. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred, from the viewpoint that the overall thickness of the separator with the functional layer can be reduced, thereby increasing the ratio of the electrode active material in the lithium ion secondary battery and increasing the capacity per volume.

[0025] <Functional layers for electrochemical devices> The functional layer for electrochemical elements (hereinafter simply referred to as "functional layer") provided in the separator with a functional layer of the present invention contains inorganic particles and a particulate polymer, and may further contain other components, as desired. The functional layer for electrochemical elements provided in the separator with a functional layer of the present invention has a maximum surface height Sz of a predetermined value or more, and has convex portions on the surface that contain a particulate polymer. The functional layer provided in the separator with a functional layer of the present invention has excellent process adhesion and heat resistance, and can improve electrolyte injection properties.

[0026] <<Properties of the functional layer>> [Maximum height Sz] Here, the maximum height Sz of the surface of the functional layer must be 2.5 μm or more, preferably 5.0 μm or more, more preferably 7.5 μm or more, preferably 15.0 μm or less, and more preferably 10.0 μm or less. If the maximum height Sz of the surface of the functional layer is above the lower limit, the functional layer can exhibit excellent process adhesion. On the other hand, if the maximum height Sz of the surface of the functional layer is below the upper limit, the process adhesion of the functional layer can be further improved. [Maximum height Rz] The maximum surface height Rz of the functional layer is preferably 1.6 μm or more, more preferably 2.5 μm or less, and more preferably 2.0 μm or less. If the maximum surface height Rz of the functional layer is within the above-mentioned range, the process adhesion of the functional layer can be further improved. [Arithmetic mean height Sa] Furthermore, the arithmetic mean height Sa of the surface of the functional layer is preferably 0.2 μm or more, more preferably 0.4 μm or more, and is preferably 1.0 μm or less, and more preferably 0.8 μm or less. If the arithmetic mean height Sa of the surface of the functional layer is within the above-mentioned range, the process adhesion of the functional layer can be further improved.

[0027] [Convex portion containing particulate polymer on the surface] The functional layer has protrusions on the surface thereof, the protrusions including a particulate polymer, the details of which will be described later. Here, the area ratio of the particulate polymer to the surface of the convex portion is preferably 10% or more, more preferably 50% or more, and particularly preferably 100%. If the area ratio of the particulate polymer to the surface of the convex portion is equal to or more than the above-mentioned predetermined value, the process adhesion of the functional layer can be further improved. The area ratio of the particulate polymer to the surface of the convex portion can be measured by measuring the separator surface with SEM-EDX and performing element mapping of C, Al, etc.

[0028] In addition, when the surface of the functional layer is viewed in plan, the ratio of the area (occupied area of ​​the convex portion) of the surface of the functional layer per unit area of ​​the surface of the functional layer, which is occupied by the convex portion containing the particulate polymer on the surface, is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. If the ratio of the occupied area of ​​the convex portion is equal to or greater than the lower limit, the process adhesion of the functional layer can be further improved. On the other hand, if the ratio of the occupied area of ​​the convex portion is equal to or less than the upper limit, the pourability can be further improved. The ratio of the occupied area of ​​the convex portion can be measured by calculating the area of ​​the portion protruding by 1 μm or more from the surface of the reference arithmetic mean height Sa using a laser displacement meter microscope (manufactured by Keyence, model: VK-X1000).

[0029] The above-mentioned convex portion will be described in further detail below with reference to figures showing specific examples of the separator with a functional layer according to the present invention.

[0030] Fig. 1 is a schematic cross-sectional view showing an example of a separator with a functional layer according to the present invention. As shown in Fig. 1, the functional layer 1 is formed on a separator substrate 2, and contains inorganic particles 11 and a particulate polymer 12. Here, a plurality of inorganic particles 11 are stacked in the thickness direction of the functional layer 1 to form an inorganic particle layer 13. The particulate polymer 12 is embedded in the inorganic particle layer 13, and a part of the particulate polymer 12 protrudes from the surface of the inorganic particle layer 13 (functional layer 1) to form a convex portion.

[0031] FIG. 2 is a schematic cross-sectional view showing another example of a separator with a functional layer according to the present invention. As shown in FIG. 2, the functional layer 1 is formed on a separator substrate 2 and contains inorganic particles 11 and a particulate polymer 12. Here, a plurality of inorganic particles 11 are overlapped in the thickness direction of the functional layer 1 to form an inorganic particle layer 13. The inorganic particle layer 13 is formed on the entire surface of the separator substrate 2. Then, a convex portion made of a plurality of particulate polymers 12 is formed on the inorganic particle layer 13. Although not shown, the shape of the convex portion when the functional layer 1 is viewed in plan is not particularly limited, and may be, for example, a dot shape, a line shape (stripes), a circle shape (crater outer ring shape), or the like.

[0032] FIG. 3 is a schematic cross-sectional view showing yet another example of a separator with a functional layer according to the present invention. As shown in FIG. 3, the functional layer 1 is formed on a separator substrate 2 and contains inorganic particles 11 and a particulate polymer 12. Here, a plurality of inorganic particles 11 overlap in the thickness direction of the functional layer 1 to form an inorganic particle layer 13. The inorganic particle layer 13 is not formed on the entire surface of the separator substrate 2, but is formed only on a part of the separator substrate 2. That is, a part of the separator substrate 2 is not covered by the inorganic particle layer 13 and is exposed. Although not shown, the shape of the inorganic particle layer 13 when the functional layer 1 is viewed in plan is not particularly limited, and may be, for example, a dot shape, a line shape (stripes), a circular shape (crater outer ring shape), or the like. Furthermore, an aggregate consisting of a plurality of particulate polymers 12 is arranged so as to cover at least a part of the surface of the inorganic particle layer 13. As a result, the inorganic particle layer 13 and the particulate polymer 12 covering at least a part of the inorganic particle layer 13 are integrated to form a convex portion. The shape of the aggregate of the particulate polymers 12 when the functional layer 1 is viewed in plan is not particularly limited and may be dot-like, linear (striped), circular (crater outer ring-like), etc. The shape of the aggregate of the particulate polymers 12 when the functional layer 1 is viewed in plan may be the same as or different from the shape of the inorganic particle layer 13.

[0033] In any of the cases of Figs. 1 to 3, the thickness of the inorganic particle layer 13 is preferably 0.5 µm or more, more preferably 0.8 µm or more, even more preferably 1 µm or more, and preferably 6 µm or less, more preferably 5 µm or less, and even more preferably 4 µm or less. If the thickness of the inorganic particle layer 13 is equal to or more than the above lower limit, the heat resistance of the functional layer can be improved. On the other hand, if the thickness of the inorganic particle layer 13 is equal to or less than the above upper limit, a decrease in the energy density of an electrochemical element including the functional layer can be suppressed. In addition, the adhesion of the functional layer can be improved.

[0034] <<Inorganic particles>> The inorganic particles contained in the functional layer are used to increase the heat resistance of the functional layer. In general, in the functional layer, a plurality of inorganic particles are stacked in the thickness direction of the functional layer to form an inorganic particle layer. In the functional layer, the inorganic particle layer and the particulate polymer described later in detail may or may not overlap in the thickness direction of the functional layer.

[0035] [Area occupied by inorganic particles] 4 is a schematic plan view showing an example of the configuration of the functional layer for electrochemical devices according to the present invention, when the surface of the functional layer for electrochemical devices is viewed in plan view. As shown in FIG. 4, the functional layer 1 includes a particulate polymer 12 and an inorganic particle layer 13.

[0036] When the surface of the functional layer is viewed in plan, the ratio of the area occupied by the inorganic particles per unit area of ​​the surface of the functional layer (the area occupied by the inorganic particles) is preferably more than 90%, more preferably 92% or more, even more preferably 93% or more, and preferably 99% or less, more preferably 98% or less, and even more preferably 97% or less. If the ratio of the area occupied by the inorganic particles is more than 90%, the heat resistance of the functional layer can be excellent. In addition, the electrochemical characteristics (particularly, the output characteristics) and the electrolyte injection property of the electrochemical element having the functional layer can be improved. On the other hand, if the ratio of the area occupied by the inorganic particles is equal to or less than the above upper limit, the functional layer can be given excellent adhesion.

[0037] [Volume average particle size of inorganic particles] The volume average particle diameter (D50) of the inorganic particles is preferably 0.1 μm or more, more preferably 0.2 μm or more, even more preferably 0.3 μm or more, and preferably 1 μm or less, more preferably 0.9 μm or less, and even more preferably 0.8 μm or less. If the volume average particle diameter of the inorganic particles is equal to or greater than the above lower limit, the inorganic particles are densely packed in the functional layer. Therefore, the decrease in ion conductivity in the functional layer can be suppressed, and the electrochemical characteristics (particularly, output characteristics) of the electrochemical element can be further improved. In addition, if the volume average particle diameter of the inorganic particles is equal to or less than the above upper limit, the functional layer can exhibit excellent heat resistance even when the thickness of the inorganic particle layer is reduced, so that the capacity of the electrochemical element can be increased.

[0038] [Inorganic particle materials] Here, the material of the inorganic particles is preferably one that exists stably in the environment in which the electrochemical element is used and is electrochemically stable. From this viewpoint, preferred materials for the inorganic particles include oxide particles such as aluminum oxide (alumina), aluminum oxide hydrate (boehmite (AlOOH)), gibbsite (Al(OH)3), silicon oxide, magnesium oxide (magnesia), magnesium hydroxide, calcium oxide, titanium oxide (titania), barium titanate (BaTiO3), ZrO, and alumina-silica composite oxide; nitride particles such as aluminum nitride and boron nitride; covalent crystal particles such as silicon and diamond; sparingly soluble ion crystal particles such as barium sulfate, calcium fluoride, and barium fluoride; clay particles such as talc and montmorillonite; and the like. Among these, aluminum oxide, boehmite, titanium oxide, and barium sulfate are preferred, and aluminum oxide is more preferred. In addition, these inorganic particles may be subjected to element substitution, surface treatment, solid solution formation, and the like as necessary. These inorganic particles may be used alone or in combination of two or more kinds in any ratio.

[0039] <<Particulate polymer>> The particulate polymer contained in the functional layer is not particularly limited, so long as a functional layer can be formed on the separator substrate such that the maximum surface height Sz is a predetermined value or more and the functional layer has protrusions containing the particulate polymer on the surface.

[0040] [Mixing ratio of inorganic particles and particulate polymer] The volume ratio of the inorganic particles to the particulate polymer in the functional layer (inorganic particles / particulate polymer) is preferably 1.1 or more, more preferably 1.4 or more, and is preferably 2.1 or less, and more preferably 1.6 or less. If the volume ratio of the inorganic particles to the particulate polymer is within the above-mentioned range, the balance between the heat resistance and the adhesiveness of the functional layer is good.

[0041] In addition, the mass ratio of the inorganic particles to the particulate polymer in the functional layer (inorganic particles / particulate polymer) is preferably 55 / 45 or more, more preferably 60 / 40 or more, even more preferably 65 / 35 or more, and is preferably 95 / 5 or less, more preferably 93 / 7 or less, and even more preferably 90 / 10 or less. If the mixing ratio of the inorganic particles to the particulate polymer is within the above-mentioned specified range in terms of mass ratio, the balance between the heat resistance and adhesion of the functional layer will be better.

[0042] In addition, the particulate polymer contained in the functional layer may be one type alone, or may be a mixture of multiple types at any ratio.When multiple types of particulate polymers are used, the "particulate polymer" in the volume ratio and mass ratio of the inorganic particles and the particulate polymer described above refers to the total amount of the multiple types of particulate polymers.

[0043] [Specific Examples of Particulate Polymers] Here, when the functional layer of the separator with a functional layer of the present invention has the configuration shown in FIG. 1 described above, particulate polymers that the functional layer may suitably contain are described in detail below as follows: a particulate polymer (X) having a volume average particle diameter larger than the thickness of the inorganic particle layer, and a particulate polymer (Y) having a volume average particle diameter smaller than the thickness of the inorganic particle layer. [[Particulate polymer (X)]] The particulate polymer (X) that can be suitably contained in the functional layer of the separator with a functional layer of the present invention has a volume average particle diameter larger than the thickness of the inorganic particle layer described above. The particulate polymer (X) is a component that can exhibit good adhesiveness when the separator with a functional layer is bonded to other members (electrodes, etc.) via the functional layer. The particulate polymer (X) may be in a particle shape or any other shape after bonding the members together via the functional layer. Furthermore, the particulate polymer (X) may be a crystalline polymer or a non-crystalline polymer, or a mixture thereof.

[0044] -Volume average particle size of particulate polymer (X)- The particulate polymer (X) preferably has a volume average particle diameter of 1.0 μm or more, more preferably 2.5 μm or more, even more preferably 5.0 μm or more, particularly preferably more than 5.0 μm, and preferably 10.0 μm or less, more preferably 9.0 μm or less, and even more preferably 8.0 μm or less. If the volume average particle diameter of the particulate polymer (X) is equal to or greater than the above lower limit, the particulate polymer (X) is more likely to protrude from the inorganic particles on the surface in the thickness direction of the functional layer, so that better adhesion can be obtained. In addition, the heat resistance of the functional layer is improved. Furthermore, when a member having a functional layer is bonded to another member, a gap is secured between the inorganic particle layer and the other member in the thickness direction of the functional layer. Then, the electrolyte is injected through this gap, so that the electrolyte injection property is improved. Here, the reason why the heat resistance of the functional layer is improved as described above is not clear, but it is presumed as follows. That is, in order to improve the heat resistance, the proportion of inorganic particles in the functional layer needs to be high. In addition, since the particulate polymer (X) protrudes from the inorganic particles on the thickness direction surface of the functional layer, the ratio of the inorganic particles in the inorganic particle layer appears to be high, which is considered to increase the heat resistance. In addition, if the volume average particle diameter of the particulate polymer (X) is not more than the above upper limit, good adhesion of the functional layer can be obtained and the blocking resistance of the functional layer can be improved. Here, the volume average particle size of the particulate polymer (X) can be adjusted by the type and amount of the metal hydroxide used in preparing the particulate polymer (X). The metal hydroxide will be described in detail later. The "volume average particle size" can be measured by the method described in the Examples of this specification.

[0045] - Ratio of volume average particle diameter of particulate polymer (X) to thickness of inorganic particle layer - In addition, the ratio of the volume average particle diameter of the particulate polymer (X) to the thickness of the inorganic particle layer (volume average particle diameter of the particulate polymer (X) / thickness of the inorganic particle layer) is preferably 1.1 or more, more preferably 1.2 or more, even more preferably 1.3 or more, even more preferably 1.5 or more, even more preferably 3.0 or more, preferably 10.0 or less, more preferably 5.0 or less, even more preferably 4.5 or less, and even more preferably 4.0 or less. If the ratio of the volume average particle diameter of the particulate polymer (X) to the thickness of the inorganic particle layer is the above lower limit or more, the particulate polymer (X) is more likely to protrude from the surface of the inorganic particles on the thickness direction surface of the inorganic particle layer, so that better adhesion can be exhibited. In addition, if the ratio of the volume average particle diameter of the particulate polymer (X) to the thickness of the inorganic particle layer is the above lower limit or more, the particulate polymer (X) is more stably held in the functional layer, so that the components such as the particulate polymer (X) constituting the functional layer are more suppressed from falling off from the functional layer (powder falling), and a more uniform functional layer can be maintained.

[0046] -Mixing ratio of inorganic particles and particulate polymer (X)- The volume ratio of the inorganic particles to the particulate polymer (X) in the functional layer (inorganic particles / particulate polymer) is preferably 55 / 45 or more, more preferably 60 / 40 or more, even more preferably 65 / 35 or more, preferably 95 / 5 or less, more preferably 80 / 20 or less, even more preferably 75 / 25 or less, and particularly preferably 70 / 30 or less. If the volume ratio of the inorganic particles to the particulate polymer (X) is within the above-mentioned range, the balance between the heat resistance and adhesiveness of the functional layer is good.

[0047] In addition, the mass ratio of the inorganic particles to the particulate polymer (X) in the functional layer (inorganic particles / particulate polymer) is preferably 49 / 51 or more, more preferably 58 / 42 or more, even more preferably 64 / 39 or more, and is preferably 99 / 1 or less, more preferably 94 / 6 or less, and even more preferably 91 / 9 or less. If the mass ratio of the inorganic particles to the particulate polymer (X) is within the above-mentioned range, the balance between the heat resistance and the adhesiveness of the functional layer is improved.

[0048] -Glass transition temperature of particulate polymer (X)- The glass transition temperature (Tg) of the particulate polymer (X) is preferably 15° C. or higher, more preferably 20° C. or higher, even more preferably 30° C. or higher, particularly preferably 40° C. or higher, and is preferably 90° C. or lower, more preferably 80° C. or lower. If the glass transition temperature of the particulate polymer (X) is the above lower limit or higher, the occurrence of blocking of the functional layer can be suppressed, for example, during storage of an electrochemical device having a functional layer. On the other hand, if the glass transition temperature of the particulate polymer (X) is the above upper limit or lower, good adhesion of the functional layer can be obtained even when members are pressed and bonded together via the functional layer. The "glass transition temperature" can be measured by the method described in the Examples of this specification.

[0049] -Melting point of particulate polymer (X)- Furthermore, the melting point (Tm) of the particulate polymer (X) is preferably 50° C. or higher, more preferably 100° C. or higher. If the melting point of the particulate polymer (X) is above the lower limit, good adhesion of the functional layer can be ensured even when the particulate polymer (X) contains a crystalline polymer. In addition, when the particulate polymer (X) has both a glass transition temperature and a melting point, from the viewpoint of further improving the adhesiveness of the functional layer, it is preferable that the melting point of the particulate polymer (X) is not less than the above lower limit. The "melting point" can be measured by the method described in the Examples of this specification.

[0050] - Swelling degree of particulate polymer (X) in electrolyte - Furthermore, the electrolyte swelling degree of the particulate polymer (X) is preferably 1.0 times or more, more preferably 1.2 times or more, even more preferably 1.3 times or more, and is preferably 15 times or less, more preferably 10 times or less, even more preferably 7 times or less. If the electrolyte swelling degree of the particulate polymer (X) is the above lower limit or more, the adhesive strength of the functional layer in the electrolyte can be strengthened. On the other hand, if the electrolyte swelling degree of the particulate polymer (X) is the above upper limit or less, the resistance of the functional layer in the electrolyte is reduced, and the electrochemical properties of the electrochemical element having the functional layer can be improved. The "degree of swelling in an electrolyte solution" can be measured by the method described in the Examples of this specification.

[0051] -Composition of particulate polymer (X)- As described above, the particulate polymer (X) is not particularly limited in composition as long as the volume average particle diameter is larger than the thickness of the inorganic particle layer.Therefore, as the particulate polymer (X), for example, a known polymer that can be used as a binder when forming a functional layer can be used.

[0052] Examples of the monomer unit constituting the particulate polymer (X) include an aromatic vinyl monomer unit, a (meth)acrylic acid ester monomer unit, a fluorine-containing monomer unit, and a crosslinkable monomer unit. In the present invention, "(meth)acrylic" means acrylic and / or methacrylic. In the present invention, when a polymer "contains a monomer unit", it means that the polymer obtained by using the monomer contains a repeating unit derived from the monomer.

[0053] --Aromatic vinyl monomer unit-- Here, examples of aromatic vinyl monomers capable of forming aromatic vinyl monomer units include, but are not limited to, styrene, α-methylstyrene, styrenesulfonic acid, butoxystyrene, vinylnaphthalene, and the like, with styrene being preferred among them. These aromatic vinyl monomers may be used alone or in combination of two or more kinds in any ratio.

[0054] The content of the aromatic vinyl monomer unit in the particulate polymer (X) is preferably 30% by mass or more, more preferably 50% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less, when the total monomer units in the particulate polymer are taken as 100% by mass. If the content of the aromatic vinyl monomer unit is equal to or more than the lower limit, the elasticity of the particulate polymer (X) is improved, the strength of the functional layer obtained is ensured, and the adhesion of the functional layer to the substrate can be improved. On the other hand, if the content of the aromatic vinyl monomer unit is equal to or less than the upper limit, the flexibility of the particulate polymer (X) is increased, and the adhesion of the functional layer to the substrate can be improved. In the present invention, the "content ratio of each monomer unit" is 1 It can be measured using nuclear magnetic resonance (NMR) techniques such as H-NMR.

[0055] --(Meth)acrylic acid ester monomer unit-- Examples of (meth)acrylic acid ester monomers capable of forming the (meth)acrylic acid ester monomer unit include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, butyl acrylates such as n-butyl acrylate and t-butyl acrylate, octyl acrylates such as pentyl acrylate, hexyl acrylate, heptyl acrylate, and 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate. and methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, butyl methacrylate such as n-butyl methacrylate and t-butyl methacrylate, octyl methacrylate such as pentyl methacrylate, hexyl methacrylate, heptyl methacrylate and 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, and other methacrylic acid alkyl esters. Among these, n-butyl acrylate, 2-ethylhexyl acrylate, and methyl methacrylate are preferred, and n-butyl acrylate is more preferred. These (meth)acrylic acid ester monomers may be used alone or in combination of two or more kinds in any ratio.

[0056] The content of the (meth)acrylic acid ester monomer unit in the particulate polymer (X) is preferably 10% by mass or more, preferably 80% by mass or less, more preferably 75% by mass or less, when the total repeating units of the particulate polymer are taken as 100% by mass. If the content of the (meth)acrylic acid ester monomer unit is equal to or more than the lower limit, the glass transition temperature of the particulate polymer (X) is prevented from excessively decreasing, and the blocking resistance of the resulting functional layer can be improved. On the other hand, if the content of the (meth)acrylic acid ester monomer unit is equal to or less than the upper limit, the adhesion between the functional layer and the substrate can be improved.

[0057] --Fluorine-containing monomer unit-- Examples of fluorine-containing monomers capable of forming fluorine-containing monomer units are not particularly limited, and include, for example, vinylidene fluoride, tetrafluoroethylene, hexafluoropropylene, vinyl chloride trifluoride, vinyl fluoride, perfluoroalkyl vinyl ether, etc. Among these, vinylidene fluoride is preferred. These fluorine-containing monomers may be used alone or in combination of two or more kinds in any ratio.

[0058] Here, when the particulate polymer (X) contains a fluorine-containing monomer unit, from the viewpoint of ensuring better adhesion of the functional layer, the particulate polymer (X) is preferably a fluorine-containing polymer using vinylidene fluoride as a fluorine-containing monomer.Among them, the fluorine-containing polymer is preferably a homopolymer of vinylidene fluoride, a copolymer of vinylidene fluoride and other fluorine-containing monomers copolymerizable therewith, or a copolymer of vinylidene fluoride and other fluorine-containing monomers copolymerizable therewith and monomers copolymerizable therewith.And, among the fluorine-containing polymers, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), polyvinyl fluoride, and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer are preferred.

[0059] --Cross-linking monomer unit-- Furthermore, the particulate polymer (X) may contain a crosslinkable monomer unit in addition to the above monomer unit. Here, the crosslinkable monomer unit is a monomer unit that can form a crosslinked structure during or after polymerization by heating or irradiation with energy rays. The particulate polymer (X) may contain, as the crosslinkable monomer unit, either an epoxy group-containing unsaturated monomer unit or a crosslinkable monomer unit other than an epoxy group-containing unsaturated monomer unit. However, from the viewpoint of increasing the adhesion of the functional layer in the electrolyte and improving the storage characteristics of the electrochemical element, it is preferable that the particulate polymer (X) contains at least an epoxy group-containing unsaturated monomer unit.

[0060] =Epoxy group-containing unsaturated monomer unit= Here, examples of the epoxy group-containing unsaturated monomer capable of forming the epoxy group-containing unsaturated monomer unit include unsaturated glycidyl ethers such as vinyl glycidyl ether, allyl glycidyl ether, butenyl glycidyl ether, o-allylphenyl glycidyl ether, and glycidyl (2-butenyl) ether; and monoepoxides of dienes or polyenes such as butadiene monoepoxide, chloroprene monoepoxide, 4,5-epoxy-2-pentene, 3,4-epoxy-1-vinylcyclohexene, and 1,2-epoxy-5,9-cyclododecadiene. alkenyl epoxides such as 3,4-epoxy-1-butene, 1,2-epoxy-5-hexene, and 1,2-epoxy-9-decene; glycidyl acrylate, glycidyl methacrylate, glycidyl crotonate, glycidyl-4-heptenoate, glycidyl sorbate, glycidyl linoleate, glycidyl-4-methyl-3-pentenoate, glycidyl ester of 3-cyclohexene carboxylic acid, glycidyl ester of 4-methyl-3-cyclohexene carboxylic acid, and the like. Among these, from the viewpoint of further increasing the adhesion of the functional layer in the electrolyte and further improving the storage characteristics of the electrochemical element, it is preferable to use unsaturated glycidyl ethers and glycidyl esters of unsaturated carboxylic acids, and it is more preferable to use allyl glycidyl ether, glycidyl (2-butenyl) ether, and glycidyl methacrylate. These epoxy group-containing unsaturated monomers may be used alone or in combination of two or more kinds in any ratio.

[0061] The content ratio of the epoxy group-containing unsaturated monomer unit in the particulate polymer (X) is preferably 0.5% by mass or more, more preferably 2.0% by mass or more, even more preferably 10.0% by mass or more, preferably 30.0% by mass or less, more preferably 25.0% by mass or less, and even more preferably 20.0% by mass or less, when the amount of all monomer units in the particulate polymer (X) is taken as 100% by mass. If the content ratio of the epoxy group-containing unsaturated monomer unit in the particulate polymer (X) is above the lower limit, the adhesion of the functional layer in the electrolyte can be further improved, and the storage characteristics of the electrochemical element can be further improved. On the other hand, if the content ratio of the epoxy group-containing unsaturated monomer unit is below the upper limit, the particulate polymer (X) can be stably produced.

[0062] =Crosslinkable monomer units other than epoxy group-containing unsaturated monomer units= In addition, examples of monomers that can form crosslinkable monomer units other than epoxy group-containing unsaturated monomer units include polyfunctional monomers having two or more polymerization reactive groups in the monomer. Examples of such polyfunctional monomers include divinyl compounds such as divinylbenzene; di(meth)acrylic acid ester compounds such as diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate; and tri(meth)acrylic acid ester compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate. Among them, ethylene glycol dimethacrylate is preferred. These crosslinkable monomers may be used alone or in combination of two or more kinds in any ratio.

[0063] The content ratio of crosslinkable monomer units other than epoxy group-containing unsaturated monomer units in the particulate polymer (X) is preferably 0.02% by mass or more, preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1% by mass or less, when the amount of all monomer units in the particulate polymer (X) is 100% by mass. If the content ratio of crosslinkable monomer units in the particulate polymer (X) is within the above range, the elution of the particulate polymer (X) into the electrolyte can be sufficiently suppressed.

[0064] --Other monomer units-- And, the particulate polymer (X) may contain other monomer units other than aromatic vinyl monomer units, (meth)acrylic acid ester monomer units, fluorine-containing monomer units, and crosslinkable monomer units.Here, the other monomer units are not particularly limited, but for example, include nitrile group-containing monomer units and acid group-containing monomer units described in the section of "particulate polymer (Y)" below.

[0065] =Nitrile group-containing monomer unit= Here, examples of nitrile group-containing monomers capable of forming nitrile group-containing monomer units include α,β-ethylenically unsaturated nitrile monomers. Specifically, the α,β-ethylenically unsaturated nitrile monomers are not particularly limited as long as they are α,β-ethylenically unsaturated compounds having nitrile groups, and examples thereof include acrylonitrile; α-halogenoacrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkylacrylonitriles such as methacrylonitrile and α-ethylacrylonitrile; and the like. These nitrile group-containing monomers may be used alone or in combination of two or more kinds in any ratio.

[0066] The content ratio of the nitrile group-containing monomer unit in the particulate polymer (X) is preferably 3% by mass or more, more preferably 4% by mass or more, even more preferably 6% by mass or more, preferably 30% by mass or less, more preferably 27% by mass or less, and even more preferably 25% by mass or less, when the total repeating units in the particulate polymer (X) are taken as 100% by mass. If the content ratio of the nitrile group-containing monomer unit is equal to or more than the lower limit, the binding force of the particulate polymer (X) can be improved and the peel strength of the functional layer can be increased. On the other hand, if the content ratio of the nitrile group-containing monomer unit is equal to or less than the upper limit, the flexibility of the particulate polymer (X) can be increased.

[0067] The content of other monomer units in the particulate polymer (X) is preferably 0% by mass or more, preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less. If the content of other monomer units is 10% by mass or less, the stability of the functional layer composition used to form the functional layer can be suppressed from decreasing.

[0068] -Preparation of particulate polymer (X)- The particulate polymer (X) can be prepared by polymerizing a monomer composition containing the above-mentioned monomers in an aqueous solvent such as water. Here, the ratio of each monomer in the monomer composition is usually the same as the ratio of each monomer unit in the particulate polymer (X).

[0069] The polymerization method is not particularly limited, and any method such as suspension polymerization, emulsion polymerization aggregation, or pulverization can be used. Among them, from the viewpoint of efficiently preparing the particulate polymer (X), suspension polymerization and emulsion polymerization aggregation are preferred, and suspension polymerization is more preferred. In addition, any reaction such as radical polymerization or living radical polymerization can be used as the polymerization reaction.

[0070] In addition, the monomer composition used in preparing the particulate polymer (X) may contain other additives such as a chain transfer agent, a polymerization regulator, a polymerization reaction retarder, a reactive fluidizing agent, a filler, a flame retardant, an antiaging agent, and a colorant in any amount.

[0071] Here, as an example, a method for preparing the particulate polymer (X) by suspension polymerization will be described.

[0072] --Preparation of particulate polymer (X) by suspension polymerization-- (1) Preparation of monomer composition First, monomers capable of forming monomer units constituting the desired particulate polymer (X) and other compounding ingredients added as required are mixed to prepare a monomer composition.

[0073] (2) Droplet formation Next, the monomer composition is dispersed in water, a polymerization initiator is added, and then droplets of the monomer composition are formed. The method for forming the droplets is not particularly limited, and for example, the droplets can be formed by shearing and stirring an aqueous medium containing the monomer composition using a dispersing machine such as an emulsifying disperser.

[0074] In this case, examples of the polymerization initiator used include oil-soluble polymerization initiators such as t-butylperoxy-2-ethylhexanoate, azobisisobutyronitrile, etc. The polymerization initiator may be added after the monomer composition is dispersed in water and before droplets are formed, or may be added to the monomer composition before it is dispersed in water.

[0075] From the viewpoint of stabilizing the droplets of the monomer composition formed in water, it is preferable to form the droplets of the monomer composition by adding a dispersion stabilizer to the water. In this case, the dispersion stabilizer may be, for example, a metal hydroxide such as magnesium hydroxide, or sodium dodecylbenzenesulfonate.

[0076] (3) Polymerization Then, after forming droplets of the monomer composition, the water containing the formed droplets is heated to initiate polymerization, thereby forming a particulate polymer (X) in the water. At this time, the polymerization reaction temperature is preferably 50° C. or more and 95° C. or less. The polymerization reaction time is preferably 1 hour or more and 10 hours or less, preferably 8 hours or less, more preferably 6 hours or less.

[0077] (4) Washing, filtering, dehydrating and drying processes After the polymerization is completed, the water containing the particulate polymer (X) is washed, filtered and dried in a conventional manner to obtain the particulate polymer (X).

[0078] [[Particulate polymer (Y)]] In addition to the particulate polymer (X), the functional layer may further contain a particulate polymer (Y) having a volume average particle diameter smaller than the thickness of the inorganic particle layer and functioning as a binder. The particulate polymer (Y) as a binder is a component that can suppress components such as inorganic particles and particulate polymer (X) contained in the functional layer from falling off from the functional layer.

[0079] -Composition of particulate polymer (Y)- Here, the composition of the particulate polymer (Y) is not particularly limited, and may be, for example, a known polymer that is water-insoluble and dispersible in a dispersion medium such as water, such as a thermoplastic elastomer and a binder resin such as polyvinylidene fluoride (PVDF).As the thermoplastic elastomer, a conjugated diene polymer and an acrylic polymer are preferable, and an acrylic polymer is more preferable.

[0080] Here, the conjugated diene polymer refers to a polymer containing a conjugated diene monomer unit. Specific examples of the conjugated diene polymer include, but are not limited to, copolymers containing aromatic vinyl monomer units and aliphatic conjugated diene monomer units, such as styrene-butadiene copolymer (SBR), butadiene rubber (BR), acrylic rubber (NBR) (copolymers containing acrylonitrile units and butadiene units), and hydrogenated products thereof. Moreover, the acrylic polymer refers to a polymer containing a (meth)acrylic acid ester monomer unit. These particulate polymers (Y) may be used alone or in combination of two or more kinds in any ratio.

[0081] The acrylic polymer that can be preferably used as the particulate polymer (Y) is not particularly limited, and examples thereof include a monomer containing the above-mentioned (meth)acrylic acid ester monomer unit, a crosslinkable monomer unit, and an acid group-containing monomer unit described below.

[0082] Examples of the acid group-containing monomer capable of forming the acid group-containing monomer unit include a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, a monomer having a phosphoric acid group, and a monomer having a hydroxyl group.

[0083] Examples of the monomer having a carboxylic acid group include monocarboxylic acid and dicarboxylic acid. Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid. Examples of the dicarboxylic acid include maleic acid, fumaric acid, and itaconic acid. Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. In this specification, "(meth)allyl" means allyl and / or methallyl, and "(meth)acrylic" means acrylic and / or methacrylic. Furthermore, examples of monomers having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. In this specification, "(meth)acryloyl" means acryloyl and / or methacryloyl. Examples of monomers having a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. These acid group-containing monomers may be used alone or in combination of two or more kinds in any ratio.

[0084] The proportion of (meth)acrylic acid ester monomer units in the acrylic polymer is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 58% by mass or more, and is preferably 98% by mass or less, more preferably 97% by mass or less, even more preferably 96% by mass or less. By making the proportion of (meth)acrylic acid ester monomer units equal to or greater than the lower limit of the above range, the peel strength of the functional layer can be increased. Also, by making it equal to or less than the upper limit, the electrochemical properties of an electrochemical element having a functional layer can be improved.

[0085] The proportion of the crosslinkable monomer unit in the acrylic polymer is preferably 0.1% by mass or more, more preferably 1.0% by mass or more, and is preferably 3.0% by mass or less, more preferably 2.5% by mass or less. By making the proportion of the crosslinkable monomer unit equal to or more than the above limit, the electrochemical properties of the electrochemical element having the functional layer can be further improved. By making the proportion of the crosslinkable monomer unit equal to or less than the above upper limit, the peel strength of the functional layer can be further increased.

[0086] The proportion of the acid group-containing monomer unit in the acrylic polymer is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less. By making the proportion of the acid group-containing monomer unit equal to or more than the lower limit, the dispersibility of the particulate polymer (Y) in the functional layer can be increased, and the electrochemical properties of the electrochemical element having the functional layer can be sufficiently improved. In addition, by making the proportion of the acid group-containing monomer unit equal to or less than the upper limit, the amount of residual moisture in the functional layer can be reduced, and the electrochemical properties of the electrochemical element can be sufficiently improved.

[0087] Furthermore, the acrylic polymer may contain other monomer units. Examples of other monomers that can form other monomer units that can be contained in the acrylic polymer include aliphatic conjugated diene monomers such as 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, and 2-chloro-1,3-butadiene; aromatic vinyl monomers and nitrile group-containing monomers described in the section "Composition of Particulate Polymer (X)", olefin monomers such as ethylene and propylene; halogen atom-containing monomers such as vinyl chloride and vinylidene chloride; vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; vinyl ether monomers such as methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether; vinyl ketone monomers such as methyl vinyl ketone, ethyl vinyl ketone, butyl vinyl ketone, hexyl vinyl ketone, and isopropenyl vinyl ketone; and heterocycle-containing vinyl compound monomers such as N-vinylpyrrolidone, vinylpyridine, and vinylimidazole. Among these, the other monomer is preferably acrylonitrile. These other monomers may be used alone or in any combination of two or more at any ratio. The content of the other monomer units in the acrylic polymer may be appropriately adjusted.

[0088] -Glass transition temperature of particulate polymer (Y)- The glass transition temperature (Tg) of the particulate polymer (Y) is preferably -100°C or higher, more preferably -90°C or higher, even more preferably -80°C or higher, even more preferably -40°C or higher, preferably less than 30°C, more preferably 20°C or lower, and even more preferably 15°C or lower. If the glass transition temperature of the particulate polymer (Y) is above the lower limit, the adhesiveness and strength of the particulate polymer (Y) can be increased. On the other hand, if the glass transition temperature of the particulate polymer (Y) is below the upper limit or below the upper limit, the flexibility of the functional layer can be further increased.

[0089] -Volume average particle size of particulate polymer (Y)- In addition, the volume average particle size of the particulate polymer (Y) is not particularly limited as long as it is smaller than the volume average particle size of the particulate polymer (X) and smaller than the thickness of the inorganic particle layer. More specifically, the volume average particle diameter of the particulate polymer (Y) is preferably 0.05 μm or more, more preferably 0.10 μm or more, and preferably 0.8 μm or less, and more preferably 0.5 μm or less. If the volume average particle diameter of the particulate polymer (Y) is equal to or greater than the lower limit, clogging of the separator can be suppressed. On the other hand, if the volume average particle diameter of the particulate polymer (Y) is equal to or less than the upper limit, the adhesive strength between the particles constituting the functional layer and between the functional layer and the separator substrate can be increased.

[0090] -Content of particulate polymer (Y)- The content of the particulate polymer (Y) in the functional layer is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.5 parts by mass or more, and preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of inorganic particles. If the content of the particulate polymer (Y) is equal to or more than the above lower limit, it is possible to sufficiently prevent components such as the particulate polymer (X) from falling off the functional layer and to sufficiently increase the peel strength of the functional layer. On the other hand, if the content of the particulate polymer (Y) is equal to or less than the above upper limit, it is possible to suppress the decrease in the ion conductivity of the functional layer and the decrease in the electrochemical properties of the electrochemical element.

[0091] -Preparation of particulate polymer (Y)- The particulate polymer (Y) is not particularly limited, and can be prepared, for example, by polymerizing a monomer composition containing the above-mentioned monomers in an aqueous solvent such as water. Here, the ratio of each monomer in the monomer composition is usually the same as the ratio of each monomer unit in the binder.

[0092] The polymerization method and the polymerization reaction are not particularly limited, and for example, the polymerization methods and polymerization reactions exemplified as the polymerization methods for the particulate polymer (X) described above can be used.

[0093] <<Other ingredients>> The functional layer may also contain other components in addition to the inorganic particles and particulate polymers described above. Here, the other components that may be contained in the functional layer are not particularly limited as long as they do not affect the electrochemical reaction in the electrochemical element, and examples of such other components include known additives such as dispersants, viscosity adjusters, and wetting agents. These other components may be used alone or in combination of two or more. In addition, the functional layer may contain a binder other than the above-mentioned particulate polymer (Y). Such a binder is not particularly limited as long as it does not fall under the category of particulate polymer, and for example, a water-soluble polymer such as polyvinyl alcohol can be used.

[0094] <<Method for forming functional layers for electrochemical devices>> The method for forming the functional layer is not particularly limited, and for example, the functional layer can be formed using a functional layer composition obtained by mixing the above-mentioned inorganic particles, a particulate polymer, water as a dispersion medium, and other components used as necessary.

[0095] The method for preparing the composition for the functional layer is not particularly limited, and can be prepared, for example, by mixing the above-mentioned particulate polymer, inorganic particles, water as a dispersion medium, and other components used as necessary. When the particulate polymer is prepared by polymerizing a monomer composition in water, the particulate polymer may be mixed with other components as it is in the form of an aqueous dispersion. When the particulate polymer is mixed in the form of an aqueous dispersion, the water in the aqueous dispersion may be used as a dispersion medium.

[0096] Here, the method of mixing the above-mentioned components is not particularly limited, but in order to efficiently disperse each component, it is preferable to use a disperser as a mixing device to perform mixing. The disperser is preferably a device that can uniformly disperse and mix the above-mentioned components. Examples of the disperser include a ball mill, a sand mill, a pigment disperser, a crusher, an ultrasonic disperser, a homogenizer, and a planetary mixer.

[0097] The functional layer composition can be formed on a suitable substrate, for example. The method for forming a functional layer on a substrate using the functional layer composition is not particularly limited, and may be, for example, 1) A method in which a composition for a functional layer is applied to the surface of a substrate and then dried 2) A method of immersing a substrate in a composition for a functional layer and then drying the substrate 3) A method in which a composition for a functional layer is applied onto a release substrate, dried to form a functional layer, and the resulting functional layer is transferred onto the surface of the substrate. The functional layer may be formed on only one side of the substrate, or on both sides of the substrate.

[0098] Among these, the method 1) is preferred because the thickness of the functional layer can be easily controlled. The method 1) may include, for example, a step of applying a functional layer composition onto a substrate (application step) and a step of drying the functional layer composition applied onto the substrate to form a functional layer (functional layer formation step).

[0099] [Coating process] In the coating process, the method for coating the functional layer composition onto the substrate is not particularly limited, and examples thereof include the doctor blade method, reverse roll method, direct roll method, gravure method, extrusion method, and brush coating method.

[0100] [Functional layer formation process] In the functional layer forming step, the method for drying the functional layer composition on the substrate is not particularly limited and may be any known method, such as drying with warm air, hot air, or low humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams, etc. The drying conditions are not particularly limited, but the drying temperature is preferably 50 to 150° C., and the drying time is preferably 1 to 30 minutes.

[0101] Furthermore, the functional layer formed on the substrate can be suitably used as a single layer that simultaneously functions as a heat-resistant layer that enhances the heat resistance of the substrate and as an adhesive layer that firmly bonds components together.

[0102] Furthermore, a substrate having a functional layer formed using the functional layer composition as described above (hereinafter, sometimes referred to as a "substrate with functional layer") can be produced in less labor and time than a substrate having a conventional heat-resistant layer and adhesive layer, and therefore has high productivity.

[0103] [Maximum thickness of functional layer] The maximum thickness of the functional layer formed by applying the functional layer composition to the substrate is preferably 1.0 μm or more, more preferably 1.5 μm or more, even more preferably 2.0 μm or more, particularly preferably 2.5 μm or more, most preferably 5.0 μm or more, preferably 10.0 μm or less, more preferably 9.0 μm or less, and even more preferably 8.0 μm or less. If the maximum thickness of the functional layer is above the lower limit, the heat resistance of the functional layer is extremely good. On the other hand, if the maximum thickness of the functional layer is below the upper limit, the ion diffusibility of the functional layer can be ensured, and the electrochemical characteristics (output characteristics) of the electrochemical element can be further sufficiently improved. In this specification, the "maximum thickness of the functional layer" can be measured, for example, using a field emission scanning electron microscope (FE-SEM).

[0104] <Method for manufacturing separator with functional layer for electrochemical element> The separator with a functional layer for electrochemical elements of the present invention can be manufactured, for example, by using a separator substrate as the substrate and forming a functional layer on the separator substrate in the method for forming a functional layer described above in the section "Functional layer for electrochemical elements."

[0105] (Electrochemical element) The electrochemical device of the present invention is required to include at least the separator with a functional layer for electrochemical devices of the present invention. Therefore, the electrochemical device of the present invention may include components other than the functional layer of the present invention as long as the effects of the present invention are not significantly impaired.

[0106] The electrochemical device of the present invention is not particularly limited, and may be, for example, a lithium ion secondary battery or an electric double layer capacitor, and is preferably a lithium ion secondary battery.

[0107] Hereinafter, a lithium ion secondary battery will be described as an example of the electrochemical element of the present invention. The lithium ion secondary battery according to the present invention comprises the functional layer of the present invention described above. More specifically, the lithium ion secondary battery comprises a positive electrode, a negative electrode, a separator with a functional layer of the present invention, and an electrolyte. The functional layer may be formed on only one side of the separator substrate, or on both sides of the separator substrate.

[0108] In the lithium ion secondary battery according to the present invention, the positive electrode and the separator substrate, and / or the negative electrode and the separator substrate are firmly bonded in the electrolyte by the functional layer. Therefore, the increase in the distance between the electrodes due to repeated charging and discharging is suppressed, and the battery characteristics such as cycle characteristics are good. In addition, in this lithium ion secondary battery, the heat resistance of the separator substrate is improved by the functional layer. Furthermore, this lithium ion secondary battery can be manufactured with high productivity by shortening the time required for manufacturing the separator, compared to the case where a separator having a conventional heat-resistant layer and an adhesive layer is used.

[0109] As the above-mentioned positive electrode, negative electrode, and electrolyte, known positive electrodes, negative electrodes, and electrolytes used in lithium ion secondary batteries can be used.

[0110] <Positive and negative electrodes> Specifically, the electrodes (positive and negative electrodes) may be electrodes formed by forming an electrode mixture layer on a current collector. The current collector may be made of a metal material such as iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, or platinum. Among these, it is preferable to use a current collector made of copper as the current collector for the negative electrode. It is also preferable to use a current collector made of aluminum as the current collector for the positive electrode. Furthermore, a layer containing an electrode active material and a binder may be used as the electrode mixture layer.

[0111] <Electrolyte> As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte, for example, a lithium salt is used in a lithium ion secondary battery. As the lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. are listed. Among them, LiPF6, LiClO4, and CF3SO3Li are preferred because they are easily dissolved in a solvent and show a high degree of dissociation. Note that one type of electrolyte may be used alone, or two or more types may be used in combination. Usually, the lithium ion conductivity tends to be higher as the supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0112] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. For example, in lithium ion secondary batteries, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), methyl ethyl carbonate (ethyl methyl carbonate (EMC)), vinylene carbonate, and the like; esters such as γ-butyrolactone, methyl formate, and the like; ethers such as 1,2-dimethoxyethane, tetrahydrofuran, and the like; sulfur-containing compounds such as sulfolane, dimethyl sulfoxide, and the like; and the like are suitably used.

[0113] A mixture of these solvents may also be used. Among them, carbonates are preferred because they have a high dielectric constant and a wide stable potential range. Generally, the lower the viscosity of the solvent used, the higher the lithium ion conductivity tends to be, so the lithium ion conductivity can be adjusted by the type of solvent. The concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. Known additives may also be added to the electrolytic solution.

[0114] <Method of manufacturing lithium-ion secondary battery> The lithium ion secondary battery as the electrochemical element of the present invention can be produced, for example, by stacking the above-mentioned positive electrode and negative electrode via a separator with a functional layer, wrapping or folding the stack as necessary, placing the stack in a battery container, injecting an electrolyte into the battery container, and sealing the container. Here, the battery container may be filled with an expand metal, a fuse, an overcurrent prevention element such as a PTC element, a lead plate, or the like as necessary to prevent pressure rise inside the battery and overcharging and discharging. The shape of the battery may be any of, for example, a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, and the like. EXAMPLES

[0115] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In addition, in a polymer produced by copolymerizing multiple types of monomers, the ratio of a structural unit formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified.

[0116] In the examples and comparative examples, the glass transition temperature, melting point, volume average particle size, electrolyte swelling degree, thickness of inorganic particle layer, ratio of volume average particle size of particulate polymer (X) to thickness of inorganic particle layer, mixing ratio (volume ratio and mass ratio) of inorganic particles and particulate polymer, ratio of area occupied by convex portion, area ratio of particulate polymer occupying the surface of convex portion, maximum height Sz, Rz of the surface of functional layer, arithmetic mean height Sa of the surface of functional layer were measured by the following methods. In addition, the process adhesion of the functional layer, adhesion of the functional layer in electrolyte, blocking resistance of the functional layer, heat resistance of the functional layer, electrolyte injection property, cycle characteristics of secondary battery, output characteristics of secondary battery, and storage characteristics of secondary battery were measured and evaluated by the following methods.

[0117] <Glass transition temperature> The particulate polymer (X) and particulate polymer (Y) (binder) prepared in the examples and comparative examples were used as the measurement samples. 10 mg of the measurement sample was weighed into an aluminum pan, and a differential scanning calorimetry (DSC) curve was obtained by using a differential thermal analysis measuring device (SII NanoTechnology's "EXSTAR DSC6220"), using an empty aluminum pan as a reference, at a measurement temperature range of -100°C to 500°C, at a heating rate of 10°C / min, and under the conditions specified in JIS Z 8703. The baseline immediately before the endothermic peak of the DSC curve where the differential signal (DDSC) is 0.05 mW / min / mg or more appears and the tangent of the DSC curve at the inflection point that first appears after the endothermic peak were intersected by the differential scanning calorimetry (DSC) curve during this heating process, as the glass transition temperature (°C).

[0118] <Melting point> The melting point (Tm) of the particulate polymer (X) prepared in Example 5 was measured as follows. First, the particulate polymer was melted by heating, and the melted polymer was quenched with dry ice, thereby obtaining an amorphous polymer. Then, the melting point (Tm) was measured by using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode) using the amorphous polymer as a test specimen.

[0119] <Volume average particle size> <<Volume average particle size of particulate polymer (X)>> The particulate polymer (X) prepared in the examples and comparative examples was used as a measurement sample. 0.1 g of the measurement sample was weighed out and placed in a beaker, and 0.1 mL of an alkylbenzene sulfonic acid aqueous solution (manufactured by Fujifilm Corporation, "Drywell") was added as a dispersant. 10 to 30 mL of a diluent (manufactured by Beckman Coulter, Inc., "Isoton II") was further added to the beaker, and the mixture was dispersed for 3 minutes using a 20 W (Watt) ultrasonic disperser. Then, the volume average particle size of the measurement sample was determined using a particle size measuring device (manufactured by Beckman Coulter, Inc., "Multisizer") under the following conditions: aperture diameter: 20 μm, medium: Isoton II, number of particles measured: 100,000.

[0120] <<Volume average particle size of binder (particulate polymer (Y))>> The volume average particle diameter of the binder (particulate polymer (Y)) prepared in the examples was measured by a laser diffraction method. Specifically, an aqueous dispersion solution (adjusted to a solid content concentration of 0.1% by mass) containing the prepared binder was used as a sample. Then, in the particle size distribution (volume basis) measured using a laser diffraction type particle size distribution measuring device (manufactured by Beckman Coulter, Inc., "LS-230"), the particle diameter D50 at which the cumulative volume calculated from the small diameter side becomes 50% was taken as the volume average particle diameter.

[0121] <<Volume average particle size of inorganic particles>> In the particle size distribution (volume basis) measured by a laser diffraction method, the particle size (D50) at which the cumulative volume calculated from the small diameter side becomes 50% was defined as the volume average particle size of the inorganic particles.

[0122] <Electrolyte swelling rate> The aqueous dispersion containing the particulate polymer (X) prepared in the examples and comparative examples was placed in a polytetrafluoroethylene petri dish and dried at 25°C for 48 hours to prepare a powder. Approximately 0.2 g of the obtained powder was pressed at 200°C and 5 MPa for 2 minutes to obtain a film. The obtained film was then cut into 1 cm squares to obtain a test piece. The mass W0 of this test piece was measured. Moreover, the above-mentioned test piece was immersed in an electrolyte solution for 72 hours at 60° C. Thereafter, the test piece was taken out of the electrolyte solution, the electrolyte solution on the surface of the test piece was wiped off, and the mass W1 of the test piece after the immersion test was measured. Using the measured masses W0 and W1, the degree of swelling in the electrolyte S (times) was calculated as S=W1 / W0. The electrolyte used was a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC), and vinylene carbonate (VC) (volume ratio: EC / DEC / VC = 68.5 / 30 / 1.5) with LiPF6 dissolved as a supporting electrolyte at a concentration of 1 mol / L.

[0123] <Thickness of inorganic particle layer> The cross section of the separator with the functional layer was observed using the field emission scanning electron microscope (FE-SEM) and the thickness of the inorganic particle layer was calculated from the SEM image obtained. The thickness of the inorganic particle layer was defined as the distance from the surface of the separator substrate coated with the slurry composition to the inorganic particle farthest in the vertical direction.

[0124] <Ratio of volume average particle diameter of particulate polymer (X) to thickness of inorganic particle layer> Based on the volume average particle diameter of the particulate polymer (X) obtained as described above and the thickness of the inorganic particle layer, the ratio of the volume average particle diameter of the particulate polymer (X) to the thickness of the inorganic particle layer (volume average particle diameter of the particulate polymer (X) / thickness of the inorganic particle layer) was determined.

[0125] <Mixing ratio of inorganic particles and particulate polymer> From the amounts of inorganic particles (alumina) and particulate polymer charged when the slurry composition was prepared, the mixing ratio (volume ratio and mass ratio) of the inorganic particles (alumina) to the particulate polymer (X), and the mixing ratio (volume ratio and mass ratio) of the inorganic particles (alumina) to the total amount of the particulate polymer (X) and the particulate polymer (Y) were calculated. The density of alumina is 4 g / cm 3 It was calculated as:

[0126] <Proportion of the area occupied by the convex parts> The proportion of the area occupied by the convex parts was measured by using a laser displacement meter microscope (Keyence, model: VK-X1000) to calculate the area of ​​the parts protruding by 1 μm or more from the surface with the reference arithmetic mean height Sa.

[0127] <Area ratio of particulate polymer to the surface of the protrusions> The area ratio of the particulate polymer to the surface of the protrusions was measured by measuring the separator surface with SEM-EDX and performing element mapping of C and Al.

[0128] <Maximum height Sz, Rz, arithmetic mean height Sa of the functional layer surface> The separators with functional layers for electrochemical elements prepared in the examples and comparative examples were observed using a laser displacement meter microscope (Keyence, model: VK-X1000). 10 arbitrary 100 μm square areas on the surface of the functional layer were measured, and the maximum height Sz and arithmetic mean height Sa of the surface of the functional layer were calculated. In addition, the maximum height Rz of each of 10 contour curves drawn in parallel at equal intervals of 7 μm as viewed from above on an arbitrary 100 μm square area of ​​the surface of the functional layer was calculated, and the average value of these was taken as the measured value at one location, and the average value of the measured values ​​obtained by performing the same measurement at a total of 10 locations was taken as the maximum height Rz of the surface of the functional layer.

[0129] <Process adhesion of functional layer> The positive electrode, negative electrode, and separator with functional layer produced in the examples and comparative examples were each cut to a width of 10 mm and a length of 50 mm, and the positive electrode and the separator with functional layer were laminated so that the surface on the positive electrode composite layer side faced the separator with functional layer, and pressed using a roll press under conditions of a temperature of 70°C, a load of 8 kN / m, and a press speed of 30 m / min to obtain an integrated product in which the positive electrode and the separator with functional layer were integrated. The obtained integrated product was placed with the positive electrode current collector side facing down, and cellophane tape was attached to the surface of the electrode. The cellophane tape used was that specified in JIS Z1522. The cellophane tape was fixed to a horizontal test table. One end of the separator with the functional layer was then pulled vertically upward at a pulling speed of 50 mm / min and peeled off, and the stress was measured. The negative electrodes prepared in the examples and comparative examples were also subjected to the same operations as in the case of using the positive electrodes, and the stress was measured. The above-mentioned stress measurement was performed three times for each of the integrated positive electrode and separator with functional layer, and the integrated negative electrode and separator with functional layer, for a total of six times, and the average stress was calculated. The average value obtained was used as the peel strength (N / m). The calculated peel strength was then used to evaluate the process adhesion between the electrode and the separator with the functional layer according to the following criteria: A higher peel strength indicates that the functional layer has better process adhesion. A: Peel strength 3N / m or more B: Peel strength 2N / m or more and less than 3N / m C: Peel strength less than 2N / m

[0130] <Adhesion of functional layer in electrolyte> The negative electrodes and separators with functional layers prepared in the examples and comparative examples were each cut to a width of 10 mm and a length of 50 mm, and the negative electrodes and separators with functional layers were laminated so that the surface of the negative electrode composite layer faced the separator with functional layer. They were then pressed at a press speed of 30 m / min using a roll press with a temperature of 70°C and a load of 10 kN / m, and then immersed in an electrolyte and left for 24 hours to obtain test pieces. After that, the test piece was removed from the electrolyte, and a polyethylene terephthalate (PET) film was placed on the separator side to prevent evaporation of the electrolyte. Cellophane tape was attached to the surface of the negative electrode with the current collector side facing down. The cellophane tape used was specified in JIS Z1522. The cellophane tape was fixed to a horizontal test table. One end of the separator substrate was pulled vertically upward at a pulling speed of 50 mm / min and peeled off, and the stress was measured. The above measurement was carried out three times, and the average of the three stresses obtained was calculated as the peel strength (N / m), which was evaluated as the adhesiveness of the functional layer in the electrolyte according to the following criteria: The higher the peel strength, the better the adhesiveness of the functional layer in the electrolyte. A: Peel strength 0.30N / m or more B: Peel strength 0.15N / m or more and less than 0.30N / m C: Peel strength less than 0.15N / m

[0131] <Blocking resistance of functional layer> The separator with functional layer prepared in the examples and comparative examples was cut into two pieces with a size of 4 cm wide x 4 cm long to prepare test pieces. The two obtained test pieces were stacked with the functional layer sides facing each other, and then pressed for 2 minutes at a temperature of 40°C and a pressure of 5 MPa to obtain a pressed body. One end of the obtained pressed body was fixed, and the other end of the pressed body was pulled vertically upward at a tensile speed of 50 mm / min to peel it off, and the stress obtained was measured, and the obtained stress was taken as the blocking strength. The blocking strength was evaluated according to the following criteria. The smaller the blocking strength, the better the functional layer suppresses the occurrence of blocking, that is, the higher the blocking resistance of the functional layer. A: Less than 4N / m B: 4N / m or more and less than 6N / m C: 6N / m or more

[0132] <Heat resistance of functional layer> The separators with functional layers produced in the examples and comparative examples were cut into squares measuring 12 cm wide x 12 cm long, and a square measuring 10 cm on a side was drawn inside the resulting square to prepare a test piece. The test piece was then placed in a thermostatic chamber at 150°C and left for 1 hour, after which the change in area of ​​the square drawn inside [= {(area of ​​square before leaving - area of ​​square after leaving) / area of ​​square before leaving} x 100%] was calculated as the thermal shrinkage rate, and evaluated according to the following criteria. A smaller thermal shrinkage rate indicates better heat resistance of the separator with functional layers. A: Heat shrinkage rate is less than 3% B: Heat shrinkage rate is 3% or more and less than 5% C: Heat shrinkage rate is 5% or more

[0133] <Electrolyte injection performance> An electrolyte solution was injected into the lithium ion secondary batteries produced in the examples and comparative examples. The inside of the lithium ion secondary batteries was then reduced in pressure to -100 kPa and kept in that state for 1 minute. Heat sealing was then performed. After 10 minutes, the electrodes (positive electrodes) were disassembled and the state of electrolyte impregnation in the electrodes was visually confirmed. Evaluation was then performed according to the following criteria. The greater the portion of the electrode impregnated with electrolyte, the higher the electrolyte injectability. A: The electrolyte is impregnated on all sides of the electrode. B: The part of the electrode that is not impregnated with electrolyte is 1 cm 2 Less than 100% of the surface area is impregnated (except for all surfaces). C: The part of the electrode that is not impregnated with electrolyte is 1 cm 2 More than

[0134] <Cycle characteristics of secondary batteries> The lithium ion secondary batteries produced in the examples and comparative examples were left to stand at 25°C for 5 hours after injecting the electrolyte. Next, the batteries were charged to a cell voltage of 3.65V at 25°C and 0.2C at a constant current, and then aged at 60°C for 12 hours. Then, the batteries were discharged to a cell voltage of 3.00V at 25°C and 0.2C at a constant current. Then, the batteries were CC-CV charged (upper cell voltage 4.20V) at 0.2C at a constant current, and CC discharged to 3.00V at 0.2C at a constant current. This charge and discharge at 0.2C was repeated three times. Thereafter, 100 cycles of charge and discharge were performed at a cell voltage of 4.20-3.00 V and a charge and discharge rate of 1.0 C in an environment of 25° C. In this case, the discharge capacity of the first cycle was defined as X1, and the discharge capacity of the 100th cycle was defined as X2. The capacity retention rate ΔC′=(X2 / X1)×100(%) was calculated using the discharge capacity X1 and the discharge capacity X2, and evaluated according to the following criteria: The larger the capacity retention rate ΔC′, the better the cycle characteristics of the secondary battery. A: Capacity retention rate ΔC´ is 93% or more B: Capacity retention rate ΔC' is 90% or more and less than 93% C: Capacity retention rate ΔC' is 87% or more and less than 90%

[0135] <Output characteristics of secondary batteries> The lithium ion secondary batteries produced in the examples and comparative examples were charged at constant current and constant voltage (CCCV) up to 4.3 V in an atmosphere at a temperature of 25° C. to prepare cells. The prepared cells were discharged to 3.0 V by a constant current method of 0.2 C and 1.5 C to obtain the electric capacity. Then, the discharge capacity retention rate represented by the ratio of electric capacities (= (electric capacity at 1.5 C / electric capacity at 0.2 C) × 100 (%)) was obtained. This measurement was performed on five lithium ion secondary battery cells. Then, the average value of the discharge capacity retention rate of each cell was obtained and evaluated according to the following criteria. A higher value of the discharge capacity retention rate indicates that the secondary battery has better output characteristics. A: The average discharge capacity retention rate is 90% or more B: The average discharge capacity retention rate is 85% or more and less than 90% C: Average discharge capacity retention rate is 75% or more and less than 85%

[0136] <Storage characteristics of secondary batteries> The lithium ion secondary batteries manufactured in each Example and Comparative Example were charged to 4.2V at constant current and constant voltage (CCCV) in a thermostatic chamber set at a temperature of 25°C. The temperature of the thermostatic chamber was then raised to 60°C and stored for one month. The temperature of the thermostatic chamber was then lowered to 25°C, and the battery was cooled for 2 hours, after which it was discharged at a constant current of 0.2C to 3V, and then CC-CV charged (upper cell voltage 4.20V) again at a constant current of 0.2C, and CC discharged to 3.00V at a constant current of 0.2C. The ratio of the discharge capacity at 0.2C before and after storage at 60°C was taken as the storage characteristic and was evaluated according to the following criteria. The higher the value of the storage characteristic, the better the storage characteristic of the secondary battery. A: Storage characteristics are 93% or more B: Storage characteristics: 90% to less than 93% C: Storage properties are less than 90%

[0137] Example 1 <Preparation of Particulate Polymer (X1)> <<Preparation of Monomer Composition (X1)>> A monomer composition (X1) was prepared by mixing 81.9 parts of styrene as an aromatic vinyl monomer, 18 parts of 2-ethylhexyl acrylate as a (meth)acrylic acid ester monomer, and 0.1 parts of ethylene glycol dimethacrylate as a crosslinkable monomer.

[0138] <<Preparation of metal hydroxides>> A colloidal dispersion (X1) containing magnesium hydroxide as a metal hydroxide was prepared by gradually adding, with stirring, an aqueous solution of 5.6 parts of sodium hydroxide dissolved in 50 parts of ion-exchanged water to an aqueous solution of 8.0 parts of magnesium chloride dissolved in 200 parts of ion-exchanged water.

[0139] <<Suspension polymerization method>> A particulate polymer (X1) was prepared by a suspension polymerization method. Specifically, the monomer composition (X1) obtained as described above was added to the colloidal dispersion (X1) containing the magnesium hydroxide, and after further stirring, 2.0 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corp., "Perbutyl O") was added as a polymerization initiator to obtain a mixed solution. The obtained mixed solution was stirred at a high shear rate of 15,000 rpm for 1 minute using an in-line emulsifying disperser (manufactured by Pacific Machinery Works, "Cavitron") to form droplets of the monomer composition (X1) in the colloidal dispersion (X1) containing magnesium hydroxide.

[0140] Then, the above-mentioned colloidal dispersion (X1) containing magnesium hydroxide was placed in a reactor, and the temperature was raised to 90° C. to carry out a polymerization reaction for 5 hours, thereby obtaining an aqueous dispersion containing a particulate polymer (X1). The volume average particle size and the degree of swelling in an electrolyte solution of the particulate polymer (X1) were measured using the aqueous dispersion containing the particulate polymer (X1). The results are shown in Table 1.

[0141] Further, while stirring the aqueous dispersion containing the particulate polymer (X1), sulfuric acid was dropped at room temperature (25°C) to perform acid washing until the pH became 6.5 or less. Then, filtration and separation were performed, and 500 parts of ion-exchanged water was added to the obtained solid matter to reslurry it, and water washing treatment (washing, filtration and dehydration) was repeated several times. Then, filtration and separation were performed, and the obtained solid matter was placed in a container of a dryer and dried at 40°C for 48 hours to obtain a dried particulate polymer (X1). The glass transition temperature of the resulting particulate polymer (X1) was measured, and the results are shown in Table 1.

[0142] <Preparation of aqueous dispersion containing binder (α) (particulate polymer (Y1))> To a reactor equipped with a stirrer, 70 parts of ion-exchanged water, 0.15 parts of sodium lauryl sulfate (manufactured by Kao Chemical Corporation, "EMAL (registered trademark) 2F") as an emulsifier, and 0.5 parts of ammonium persulfate as a polymerization initiator were supplied, the gas phase was replaced with nitrogen gas, and the temperature was raised to 60°C. Meanwhile, in another container, 50 parts of ion-exchanged water, 0.5 parts of sodium dodecylbenzenesulfonate as a dispersion stabilizer, 94 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 2 parts of methacrylic acid as an acid group-containing monomer, and 2 parts of acrylonitrile as a nitrile group-containing monomer, as well as 1 part of allyl methacrylate and 1 part of allyl glycidyl ether as crosslinkable monomers, were mixed to prepare a monomer composition (α). The obtained monomer composition (α) was continuously added to the above-mentioned reactor equipped with a stirrer over a period of 4 hours to carry out polymerization. The reaction was carried out at 60°C during the addition. After the addition was completed, the mixture was stirred at 70°C for an additional 3 hours, and then the reaction was terminated to obtain an aqueous dispersion containing a particulate binder (α) (particulate polymer (Y1)) as an acrylic polymer. The volume average particle size and glass transition temperature of the obtained binder (α) (particulate polymer (Y1)) were measured. The results are shown in Table 1.

[0143] <Preparation of Slurry Composition> 0.5 parts of polyacrylic acid as a dispersant was added to 100 parts of alumina (manufactured by Sumitomo Chemical Co., Ltd., "AKP3000", volume average particle diameter: 0.7 μm) as inorganic particles, 6 parts of an aqueous dispersion containing a binder (α) (particulate polymer (Y1)) in terms of solid content and 1.5 parts of carboxymethyl cellulose as a thickener were added, ion-exchanged water was added so that the solid content concentration was 55%, and the mixture was mixed using a ball mill to obtain a pre-mixing slurry. To 100 parts of the particulate polymer (X1), 0.2 parts of sodium dodecylbenzenesulfonate (Kao Chemical Co., Ltd., "Neopelex G-15") was added as an emulsifier, and ion-exchanged water was added and mixed to obtain a mixture with a solid content of 40%. The obtained mixture and the pre-mixing slurry obtained as described above were mixed so that the mixing ratio of the inorganic particles (alumina) and the particulate polymer (X1) was the mixing ratio shown in Table 1, and ion-exchanged water was added to obtain a solid content of 40%, to obtain a slurry composition (composition for functional layer). In addition, the mixing ratio (volume ratio and mass ratio) of the inorganic particles (alumina) to the total amount of the particulate polymer (X1) and the particulate polymer (Y1) was obtained from the charged amounts of the inorganic particles (alumina), the particulate polymer (X1), and the particulate polymer (Y1) when the slurry composition was prepared. The results are shown in Table 1.

[0144] <Preparation of separator with functional layer> A polyethylene microporous film (thickness: 12 μm) was prepared as a separator substrate. The slurry composition obtained as described above was applied to one side of this separator substrate by a bar coater method. Next, the separator substrate to which the slurry composition was applied was dried at 50° C. for 1 minute to form a functional layer. The same operation was performed on the other side of the separator substrate to prepare a separator with a functional layer provided on both sides of the separator substrate. The thickness of the inorganic particle layer in each functional layer was measured and all were 2.0 μm.

[0145] <Preparation of positive electrode> 100 parts of LiCoO2 (volume average particle diameter: 12 μm) as a positive electrode active material, 2 parts of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd., "HS-100") as a conductive material, 2 parts of polyvinylidene fluoride (manufactured by Kureha Corporation, "#7208") as a binder for the positive electrode composite layer in terms of solid content, and N-methylpyrrolidone as a solvent were mixed to a total solid content concentration of 70%. These were mixed using a planetary mixer to prepare a slurry composition for the positive electrode. The above-mentioned positive electrode slurry composition was applied to a 20 μm-thick aluminum foil as a current collector using a comma coater so that the film thickness after drying was about 150 μm, and then dried. This drying was performed by conveying the aluminum foil at a speed of 0.5 m / min in an oven at 60° C. for 2 minutes. Then, the aluminum foil was heated at 120° C. for 2 minutes to obtain a pre-press positive electrode raw material. This pre-press positive electrode raw material was rolled with a roll press to obtain a pre-press positive electrode having a positive electrode composite layer (thickness: 60 μm).

[0146] <Preparation of negative electrode> In a 5MPa pressure vessel equipped with a stirrer, 33 parts of 1,3-butadiene, 3.5 parts of itaconic acid, 63.5 parts of styrene, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, thoroughly stirred, and then heated to 50°C to start polymerization. When the polymerization conversion rate reached 96%, the reaction was stopped by cooling to obtain a mixture containing a binder (SBR) for the negative electrode composite layer. A 5% aqueous sodium hydroxide solution was added to the mixture containing the binder for the negative electrode composite layer, and the pH was adjusted to 8, after which unreacted monomers were removed by heating and reduced pressure distillation. Then, the mixture was cooled to 30°C or less to obtain an aqueous dispersion containing the desired binder for the negative electrode composite layer. 80 parts of artificial graphite (volume average particle size: 15.6 μm) as the negative electrode active material (1), 100 parts of silicon-based active material SiO x(Volume average particle size: 4.9 μm) 16 parts were blended, 2.5 parts of a 2% aqueous solution of carboxymethylcellulose sodium salt (manufactured by Nippon Paper Industries Co., Ltd., "MAC350HC") as a viscosity modifier was mixed in solid content equivalent, and ion-exchanged water was mixed to adjust the solid content concentration to 68%, and then further mixed at 25 ° C. for 60 minutes. The solid content concentration was further adjusted to 62% with ion-exchanged water, and then further mixed at 25 ° C. for 15 minutes to obtain a mixed liquid. 1.5 parts of the aqueous dispersion containing the binder for the negative electrode composite layer in solid content equivalent and ion-exchanged water were added to this mixed liquid, and the final solid content concentration was adjusted to 52%, and further mixed for 10 minutes to obtain a mixed liquid. This mixed liquid was defoamed under reduced pressure to obtain a negative electrode slurry composition with good fluidity. The above-mentioned negative electrode slurry composition was applied to a copper foil having a thickness of 20 μm as a current collector using a comma coater so that the film thickness after drying was about 150 μm, and then dried. This drying was performed by conveying the copper foil at a speed of 0.5 m / min in an oven at 60° C. for 2 minutes. Then, the copper foil was heated at 120° C. for 2 minutes to obtain a pre-press negative electrode raw material. This pre-press negative electrode raw material was rolled using a roll press to obtain a pre-press negative electrode having a negative electrode composite layer (thickness: 80 μm).

[0147] Using the separator with functional layer obtained as described above, the occupied area of ​​inorganic particles, the thickness of the inorganic particle layer, and the ratio of the volume average particle diameter of the particulate polymer to the thickness of the inorganic particle layer were obtained. In addition, the separator with functional layer was used to measure the maximum heights Sz and Rz of the surface of the functional layer, as well as the arithmetic mean height Sa. Furthermore, using the separator with functional layer obtained as described above, the positive electrode, and the negative electrode, the process adhesion of the functional layer, the adhesion of the functional layer in the electrolyte, the blocking resistance of the functional layer, the heat resistance of the functional layer, and the powder fall resistance of the functional layer were evaluated. The results are shown in Table 1. In addition, the cross-section of the separator with functional layer obtained as described above was analyzed by energy dispersive X-ray spectroscopy (SEM-EDX) (SEM body: Carl Zeiss ``Ultra-55'' -EDX: Bruker ``Quantax-400''), and it was confirmed that the functional layer had multiple protrusions containing particulate polymers on its surface.

[0148] <Production of lithium-ion secondary battery> The pressed positive electrode prepared as described above was cut into a rectangle of 49 cm x 5 cm, and placed so that the surface on the positive electrode composite layer side was facing up. The separator with functional layer cut to 120 cm x 5.5 cm was placed on the positive electrode composite layer so that the positive electrode was located on one side of the separator with functional layer in the longitudinal direction. Furthermore, the pressed negative electrode prepared as described above was cut into a rectangle of 50 cm x 5.2 cm, and placed on the separator with functional layer so that the surface on the negative electrode composite layer side faced the separator with functional layer and the negative electrode was located on the other side of the separator with functional layer in the longitudinal direction. Then, the obtained laminate was wound by a wound body to obtain a wound body. This wound body was pressed at 70℃ and 1MPa to make a flat body, then wrapped in an aluminum packaging material as the exterior of the battery, and electrolyte [solvent: ethylene carbonate / diethyl carbonate / vinylene carbonate (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 with a concentration of 1 mol)] was injected so that no air remained. Then, the opening of the aluminum packaging material was heat sealed at a temperature of 150℃ to produce a wound type lithium ion secondary battery with a capacity of 800mAh. The obtained lithium ion secondary battery was used to evaluate the electrolyte injection property, cycle characteristics, output characteristics, and storage characteristics of the secondary battery. The results are shown in Table 1.

[0149] Example 2 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X2) prepared as follows was used instead of the particulate polymer (X1), and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0150] <Preparation of particulate polymer (X2)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the colloidal dispersion (X2) containing magnesium hydroxide was used instead of the colloidal dispersion (X1) containing magnesium hydroxide as a metal hydroxide, to prepare the particulate polymer (X2). The colloidal dispersion (X2) containing magnesium hydroxide was prepared by gradually adding, with stirring, an aqueous solution of 7.0 parts of sodium hydroxide in 50 parts of ion-exchanged water to an aqueous solution of 10.0 parts of magnesium chloride in 200 parts of ion-exchanged water.

[0151] Example 3 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X3) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0152] <Preparation of particulate polymer (X3)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the colloidal dispersion (X3) containing magnesium hydroxide was used instead of the colloidal dispersion (X1) containing magnesium hydroxide as a metal hydroxide, to prepare the particulate polymer (X3). The colloidal dispersion (X3) containing magnesium hydroxide was prepared by gradually adding, with stirring, an aqueous solution of 5.6 parts of sodium hydroxide in 50 parts of ion-exchanged water to an aqueous solution of 8.0 parts of magnesium chloride in 200 parts of ion-exchanged water.

[0153] Example 4 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X4) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0154] <Preparation of particulate polymer (X4)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X4) was used instead of the monomer composition (X1), to prepare the particulate polymer (X4). The monomer composition (X4) was prepared by mixing 20.9 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 20 parts of acrylonitrile as a nitrile group-containing monomer, 59 parts of methyl methacrylate as a (meth)acrylic acid ester monomer, and 0.1 parts of ethylene glycol dimethacrylate as a crosslinkable monomer.

[0155] Example 5 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X5) prepared as follows, and a lithium ion secondary battery was obtained. Various measurements and evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0156] <Preparation of particulate polymer (X5)> After thoroughly replacing the inside of a 1L autoclave with nitrogen, 400g of deoxygenated pure water, 4g of ammonium perfluorodecanoate as an emulsifier, and poval as a dispersion stabilizer were charged, and the temperature was raised to 60°C while stirring at 100 rpm. Next, a mixed gas consisting of 90 parts of vinylidene fluoride (VDF) and 10 parts of hexafluoropropylene (HFP) was charged until the internal pressure reached 3 MPa (gauge pressure). Then, diisopropyl peroxydicarbonate was added as a polymerization initiator to start polymerization, and the reaction was continued for 3 hours. The reaction liquid was cooled and stirring was stopped, and the unreacted monomer was released to stop the reaction, and a latex of a fluorine-containing polymer was obtained as a particulate polymer (X5).

[0157] Example 6 In preparing the slurry composition, the mixing ratio of the inorganic particles (alumina) and the particulate polymer (X1) in the slurry composition was adjusted to 80:20 in volume ratio [inorganic particles (alumina):particulate polymer (X1)], and the same procedure as in Example 1 was used to prepare a separator with a functional layer, a positive electrode, and a negative electrode, and obtain a lithium ion secondary battery. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0158] Example 7 In preparing the slurry composition, the mixing ratio of the inorganic particles (alumina) and the particulate polymer (X1) in the slurry composition was adjusted to 60:40 in volume ratio [inorganic particles (alumina):particulate polymer (X1)], and the same procedure as in Example 1 was used to prepare a separator with a functional layer, a positive electrode, and a negative electrode, and obtain a lithium ion secondary battery. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0159] Example 8 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X6) prepared as follows, and a lithium ion secondary battery was obtained. Various measurements and evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0160] <Preparation of particulate polymer (X6)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X6) was used instead of the monomer composition (X1), to prepare the particulate polymer (X6). The monomer composition (X6) was prepared by mixing 60 parts of styrene as an aromatic vinyl monomer, 39.9 parts of 2-ethylhexyl acrylate as a (meth)acrylic acid ester monomer, and 0.1 part of ethylene glycol dimethacrylate as a crosslinkable monomer.

[0161] Example 9 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X7) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0162] <Preparation of particulate polymer (X7)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X7) was used instead of the monomer composition (X1), to prepare the particulate polymer (X7). The monomer composition (X7) was prepared by mixing 89.9 parts of styrene as an aromatic vinyl monomer, 10 parts of 2-ethylhexyl acrylate as a (meth)acrylic acid ester monomer, and 0.1 part of ethylene glycol dimethacrylate as a crosslinkable monomer.

[0163] Example 10 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were produced in the same manner as in Example 1, except that an aqueous dispersion containing a binder (β) (particulate polymer (Y2)) prepared as described below was used instead of the aqueous dispersion containing a binder (α) (particulate polymer (Y1)) to prepare the slurry composition, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0164] <Preparation of aqueous dispersion containing binder (β) (particulate polymer (Y2))> To a reactor equipped with a stirrer, 70 parts of ion-exchanged water, 0.15 parts of polyoxyethylene lauryl ether (manufactured by Kao Chemical Corporation, "EMULGEN (registered trademark) 120") as an emulsifier, and 0.5 parts of ammonium persulfate as a polymerization initiator were supplied, the gas phase was replaced with nitrogen gas, and the temperature was raised to 60°C. Meanwhile, in a separate vessel, 50 parts of ion-exchanged water, 0.5 parts of polyoxyethylene lauryl ether (manufactured by Kao Chemical Corporation, "Emulgen (registered trademark) 120") as an emulsifier, 70 parts of 2-ethylhexyl acrylate as a (meth)acrylic acid alkyl ester monomer, 25 parts of styrene as an aromatic vinyl monomer, 1.7 parts of allyl glycidyl ether and 0.3 parts of allyl methacrylate as crosslinkable monomers, and 3 parts of acrylic acid as an acid group-containing monomer were mixed to prepare a monomer composition (β). The obtained monomer composition (β) was continuously added to the above-mentioned reactor equipped with a stirrer over 4 hours to carry out polymerization. The reaction was carried out at 70°C during the addition. After the addition was completed, the mixture was stirred at 80°C for another 3 hours, and then the reaction was terminated to obtain an aqueous dispersion containing a particulate binder (β) (particulate polymer (Y2)). The volume average particle size and glass transition temperature of the binder (β) (particulate polymer (Y2)) were measured using the obtained aqueous dispersion containing the binder (β) (particulate polymer (Y2)). The results are shown in Table 1.

[0165] Example 11 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were produced in the same manner as in Example 1, except that an aqueous dispersion containing a binder (γ) (particulate polymer (Y3)) prepared as described below was used instead of the aqueous dispersion containing a binder (α) (particulate polymer (Y1)) to prepare the slurry composition, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0166] <Preparation of aqueous dispersion containing binder (γ) (particulate polymer (Y3))> A mixture containing 33 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 62 parts of styrene as an aromatic vinyl monomer, 4 parts of itaconic acid as a carboxylic acid group-containing monomer, 0.3 parts of t-dodecyl mercaptan as a chain transfer agent, and 0.3 parts of sodium lauryl sulfate as an emulsifier was charged into vessel A. Then, addition of the mixture from vessel A to pressure vessel B was started, and at the same time, addition of 1 part of potassium persulfate as a polymerization initiator to pressure vessel B was started to start the polymerization reaction. During this process, the reaction temperature was maintained at 75°C. In addition, 4 hours after the start of polymerization (i.e., after 70% of the above mixture had been added to pressure vessel B), 1 part of 2-hydroxyethyl acrylate (2-hydroxyethyl acrylate) as a hydroxyl group-containing monomer was added to pressure vessel B over 1 hour and 30 minutes. After 5 hours and 30 minutes from the start of polymerization, the addition of all the monomers was completed, and the mixture was then heated to 85° C. and reacted for 6 hours. When the polymerization conversion rate reached 97%, the mixture was cooled to stop the reaction, and a mixture containing a particulate polymer (γ1) was obtained. A 5% aqueous sodium hydroxide solution was added to the obtained mixture to adjust the pH to 8. Thereafter, unreacted monomers were removed by heating and reduced pressure distillation. Then, the mixture was cooled to obtain an aqueous dispersion (solid concentration: 40%) containing styrene-butadiene copolymer (SBR) as a particulate binder (γ) (particulate polymer (Y3)). The volume average particle size and glass transition temperature of the binder (γ) (particulate polymer (Y3)) were measured using the obtained aqueous dispersion containing the binder (γ) (particulate polymer (Y3)). The results are shown in Table 1.

[0167] Example 12 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were produced in the same manner as in Example 1, except that 1 part (solid content equivalent) of a water-soluble polymer, polyvinyl alcohol (Kuraray, "Kuraray Poval PVA110") was added as the binder (δ) instead of the aqueous dispersion of the binder (α) (particulate polymer (Y1)). A lithium ion secondary battery was obtained by producing the separator with a functional layer, a positive electrode, and a negative electrode in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0168] Example 13 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X8) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0169] <Preparation of particulate polymer (X8)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X8) was used instead of the monomer composition (X1), to prepare the particulate polymer (X8). The monomer composition (X8) was prepared by mixing 78.5 parts of styrene as an aromatic vinyl monomer, 20 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 1 part of glycidyl methacrylate (an epoxy group-containing unsaturated monomer) as a crosslinkable monomer, and 0.5 parts of ethylene glycol dimethacrylate.

[0170] Example 14 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X9) prepared as follows was used instead of the particulate polymer (X1), and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0171] <Preparation of particulate polymer (X9)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X9) was used instead of the monomer composition (X1), to prepare the particulate polymer (X9). The monomer composition (X9) was prepared by mixing 59.5 parts of styrene as an aromatic vinyl monomer, 20 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 20 parts of glycidyl methacrylate (an epoxy group-containing unsaturated monomer) as a crosslinkable monomer, and 0.5 parts of ethylene glycol dimethacrylate.

[0172] Example 15 In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X10) prepared as follows, and a lithium ion secondary battery was obtained. Various measurements and evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0173] <Preparation of particulate polymer (X10)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X10) was used instead of the monomer composition (X1) to prepare the particulate polymer (X10). The monomer composition (X10) was prepared by mixing 78.5 parts of styrene as an aromatic vinyl monomer, 20 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 1 part of allyl glycidyl ether (epoxy group-containing unsaturated monomer) as a crosslinkable monomer, and 0.5 parts of ethylene glycol dimethacrylate.

[0174] (Example 16) In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X11) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0175] <Preparation of particulate polymer (X11)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X11) was used instead of the monomer composition (X1) to prepare the particulate polymer (X11). The monomer composition (X11) was prepared by mixing 59.5 parts of styrene as an aromatic vinyl monomer, 20 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 20 parts of allyl glycidyl ether (an epoxy group-containing unsaturated monomer) as a crosslinkable monomer, and 0.5 parts of ethylene glycol dimethacrylate.

[0176] (Example 17) In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X12) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0177] <Preparation of particulate polymer (X12)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X12) was used instead of the monomer composition (X1) to prepare the particulate polymer (X12). The monomer composition (X12) was prepared by mixing 78.5 parts of styrene as an aromatic vinyl monomer, 20 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 1 part of glycidyl (2-butenyl) ether (an epoxy group-containing unsaturated monomer) as a crosslinkable monomer, and 0.5 parts of ethylene glycol dimethacrylate.

[0178] (Example 18) In preparing the slurry composition, a separator with a functional layer, a positive electrode, and a negative electrode were prepared in the same manner as in Example 1, except that the particulate polymer (X1) was replaced with the particulate polymer (X13) prepared as follows, and a lithium ion secondary battery was obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0179] <Preparation of particulate polymer (X13)> In preparing the particulate polymer, the same operation as in Example 1 was carried out except that the monomer composition (X13) was used instead of the monomer composition (X1) to prepare the particulate polymer (X13). The monomer composition (X13) was prepared by mixing 59.5 parts of styrene as an aromatic vinyl monomer, 20 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 20 parts of glycidyl (2-butenyl) ether (an epoxy group-containing unsaturated monomer) as a crosslinkable monomer, and 0.5 parts of ethylene glycol dimethacrylate.

[0180] Comparative Example 1 A separator with a functional layer, a positive electrode, and a negative electrode were produced in the same manner as in Example 2, except that the thickness of the inorganic particle layer was adjusted to 3.5 μm when the slurry composition was applied to the separator substrate to form a layer, and a lithium ion secondary battery was obtained. Various measurements and evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1. In addition, when the cross-section of the separator with functional layer obtained as described above was analyzed by energy dispersive X-ray spectroscopy (SEM-EDX) (SEM body: Carl Zeiss ``Ultra-55'' -EDX: Bruker ``Quantax-400''), no convex parts containing particulate polymer were confirmed on the surface of the functional layer.

[0181] [Table 1]

[0182] In addition, in Table 1, "ST" indicates styrene, "2EHA" indicates 2-ethylhexyl acrylate, "EDMA" stands for ethylene glycol dimethacrylate, "BA" indicates n-butyl acrylate; "PVdF-HFP" refers to fluoropolymer latex. "AN" indicates acrylonitrile, "MAA" stands for methacrylic acid; "MMA" indicates methyl methacrylate, "AGE" stands for allyl glycidyl ether. "AMA" stands for allyl methacrylate; "AA" indicates acrylic acid, "SBR" stands for styrene-butadiene copolymer; "GMA" refers to glycidyl methacrylate.

[0183] From Table 1, it can be seen that in Examples 1 to 18, in which a functional layer containing inorganic particles and a particulate polymer, having a maximum surface height Sz of a predetermined value or more, and having convex portions containing a particulate polymer on the surface, is formed on a separator substrate, a separator with a functional layer for electrochemical elements is obtained that has excellent process adhesion and heat resistance and can improve the electrolyte injection properties. On the other hand, the separator with functional layer for electrochemical elements of Comparative Example 1, in which the maximum surface height Sz of the functional layer is less than a specified value, has good heat resistance and electrolyte injection properties of the functional layer, but is poor in process adhesion of the functional layer. [Industrial Applicability]

[0184] According to the present invention, it is possible to provide a separator with a functional layer for an electrochemical element, which has excellent process adhesion and heat resistance, and is provided with a functional layer that can improve electrolyte injectability. Moreover, according to the present invention, it is possible to provide an electrochemical element capable of exhibiting excellent electrochemical properties. [Explanation of symbols]

[0185] 1. Functional Layer 2. Separator substrate 11 Inorganic particles 12 Particulate polymer 13 Inorganic particle layer

Claims

1. A separator with a functional layer for an electrochemical device, comprising a separator substrate and a functional layer for an electrochemical device disposed on at least one surface of the separator substrate, The functional layer for an electrochemical device includes inorganic particles and a particulate polymer, The maximum height Sz of the surface of the functional layer for electrochemical devices is 2.5 μm or more, the functional layer for electrochemical devices has a convex portion containing the particulate polymer on a surface thereof, The particulate polymer comprises an epoxy group-containing unsaturated monomer unit, and the particulate polymer comprises an epoxy group-containing unsaturated monomer unit.

2. A separator with a functional layer for an electrochemical element as described in claim 1, wherein the content of epoxy group-containing unsaturated monomer units in the particulate polymer is 0.5 mass% or more and 30.0 mass% or less.

3. 3. The separator with a functional layer for electrochemical devices according to claim 1, wherein the maximum height Rz of the surface of the functional layer for electrochemical devices is 1.6 μm or more.

4. 4. The separator with a functional layer for electrochemical devices according to claim 1, wherein the arithmetic mean height Sa of the surface of the functional layer for electrochemical devices is 0.2 μm or more.

5. The separator with a functional layer for electrochemical devices according to any one of claims 1 to 4, wherein the volume ratio of the inorganic particles to the particulate polymer in the functional layer for electrochemical devices (inorganic particles / particulate polymer) is 1.1 or more and 2.1 or less.

6. 6. The separator with a functional layer for an electrochemical element according to claim 1, wherein the particulate polymer has a degree of swelling in an electrolyte of 1 to 15 times.

7. The separator with a functional layer for an electrochemical element according to any one of claims 1 to 6, wherein the particulate polymer satisfies the following 1) or 2): 1) The glass transition temperature of the particulate polymer is 15° C. or higher and 90° C. or lower. 2) The melting point of the particulate polymer is 50° C. or higher.

8. An electrochemical device comprising the separator with a functional layer for electrochemical devices according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    JP2011258351A

  • Lithium secondary battery and lithium secondary battery pack

    JP2015082459A

  • Wound electrode element for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery using the same, and method for manufacturing wound electrode element for nonaqueous electrolyte secondary battery

    JP2016119221A

  • Battery separator

    JP2017152268A

  • Image forming device

    JP2019020578A