Resin composition, secondary coating material for optical fiber, optical fiber, and method for producing optical fiber
A resin composition with urethane (meth)acrylate, monomer, and hydrophobic zirconium oxide addresses filler settlement and stability issues, enhancing the lateral pressure characteristics and storage stability of optical fibers by forming a high Young's modulus resin layer.
Patent Information
- Application Number
- JP2021528146
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-18
- Filing Date
- 2020-06-10
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-10
AI Technical Summary
Existing resin compositions for optical fiber secondary coating layers face issues with filler settlement and decreased storage stability, which affect the lateral pressure characteristics of the optical fiber.
A resin composition containing a base resin with urethane (meth)acrylate, a monomer, a photopolymerization initiator, and hydrophobic zirconium oxide, with a zirconium content of 0.5% to 65% by mass, is used to form a secondary resin layer, enhancing the Young's modulus and improving storage stability and lateral pressure characteristics.
The resin composition achieves excellent storage stability and improved lateral pressure characteristics in optical fibers by forming a smooth resin layer with high Young's modulus, reducing stress during curing and enhancing the fiber's resistance to bending-induced transmission loss.
Smart Images

Figure 0007567789000004 
Figure 0007567789000001 
Figure 0007567789000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition, a secondary coating material for an optical fiber, an optical fiber, and a method for manufacturing an optical fiber. This application claims priority to Japanese Application No. 2019-112622, filed on June 18, 2019, and incorporates by reference all of the contents of said Japanese application. [Background technology]
[0002] In general, optical fibers have a resin coating layer for protecting a glass fiber that is an optical transmission medium. Optical fibers are required to have excellent lateral pressure characteristics in order to reduce an increase in transmission loss induced by minute bending that occurs when lateral pressure is applied to the optical fiber.
[0003] The coating resin layer can be formed using an ultraviolet-curable resin composition containing an oligomer, a monomer, a photopolymerization initiator, etc. For example, Patent Document 1 discusses improving the lateral pressure characteristics of an optical fiber by forming a resin layer using an ultraviolet-curable resin composition containing a filler made of synthetic quartz. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-219550 A Summary of the Invention
[0005] A resin composition according to one embodiment of the present disclosure is a resin composition including a base resin containing an oligomer, a monomer, and a photopolymerization initiator including a urethane (meth)acrylate, and hydrophobic zirconium oxide, and the content of the zirconium oxide is 0.5 mass% or more and 65 mass% or less based on the total amount of the resin composition. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Problem that this disclosure aims to solve] The coating resin layer generally includes a primary resin layer and a secondary resin layer. The resin composition forming the secondary resin layer is required to improve the lateral pressure characteristics of the optical fiber by increasing the Young's modulus. However, in the case of a resin composition containing a filler, the filler may settle, resulting in a decrease in the storage stability of the resin composition.
[0008] An object of the present disclosure is to provide a resin composition with which an optical fiber having excellent storage stability and excellent lateral pressure characteristics can be produced, and an optical fiber having excellent lateral pressure characteristics.
[0009] [Effects of this disclosure] According to the present disclosure, it is possible to provide a resin composition capable of producing an optical fiber having excellent storage stability and excellent lateral pressure characteristics, and an optical fiber having excellent lateral pressure characteristics.
[0010] [Description of the embodiments of the present disclosure] First, the contents of the embodiments of the present disclosure will be listed and described. A resin composition according to one aspect of the present disclosure is a resin composition including a base resin containing an oligomer, a monomer, and a photopolymerization initiator containing urethane (meth)acrylate, and hydrophobic zirconium oxide, and the content of the zirconium oxide is 0.5 mass% or more and 65 mass% or less based on the total amount of the resin composition.
[0011] Zirconium oxide can increase the Young's modulus of the resin layer, and can also release the reaction heat generated when the resin composition is cured, thereby reducing the stress generated in the resin layer during curing. By including zirconium oxide in a specific range, the resin composition can have excellent storage stability and a smooth resin layer can be formed. In addition, by using the resin composition according to this embodiment as an ultraviolet-curable resin composition for optical fiber coating, an optical fiber having excellent lateral pressure characteristics can be produced.
[0012] In order to form a resin layer having a high Young's modulus, the average primary particle size of zirconium oxide may be 100 nm or less.
[0013] The zirconium oxide may include tetragonal zirconium oxide, since this makes it easier to form a resin layer with a high Young's modulus.
[0014] The secondary coating material for an optical fiber according to an embodiment of the present disclosure includes the resin composition described above. By using the resin composition according to this embodiment for the secondary resin layer, a coating resin layer having excellent lateral pressure characteristics can be formed.
[0015] An optical fiber according to one aspect of the present disclosure includes a glass fiber including a core and a cladding, a primary resin layer that contacts the glass fiber and covers the glass fiber, and a secondary resin layer that covers the primary resin layer, the secondary resin layer being made of a cured product of the resin composition. The zirconium oxide content in the secondary resin layer is 0.5% by mass or more and 65% by mass or less based on the total amount of the secondary resin layer. By applying the resin composition according to this embodiment to the secondary resin layer, the lateral pressure characteristics of the optical fiber can be improved.
[0016] The method for producing an optical fiber according to an embodiment of the present disclosure includes a coating step of coating the resin composition on the outer periphery of a glass fiber composed of a core and a cladding, and a curing step of curing the resin composition by irradiating the resin composition with ultraviolet light after the coating step, thereby making it possible to produce an optical fiber having excellent lateral pressure characteristics.
[0017] [Details of the embodiment of the present disclosure] Specific examples of the resin composition and optical fiber according to the embodiment of the present disclosure will be described with reference to the drawings as necessary. Note that the present invention is not limited to these examples, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims. In the following description, the same elements in the description of the drawings will be given the same reference numerals, and duplicated descriptions will be omitted.
[0018] <Resin composition> The resin composition according to the present embodiment contains a base resin containing an oligomer, a monomer, and a photopolymerization initiator including a urethane (meth)acrylate, and hydrophobic zirconium oxide.
[0019] (Zirconium oxide) The zirconium oxide (zirconia) according to this embodiment is a hydrophobic zirconia particle whose surface has been hydrophobically treated. The hydrophobizing treatment according to this embodiment means that a hydrophobic group is introduced to the surface of the zirconium oxide. Zirconium oxide before the hydrophobizing treatment usually has a hydroxyl group on the surface and is hydrophilic. Zirconium oxide having a hydrophobic group introduced therein has excellent dispersibility in a resin composition. The hydrophobic group may be a reactive group such as a (meth)acryloyl group, or a non-reactive group such as a hydrocarbon group. When zirconium oxide has a reactive group, it becomes easier to form a resin layer having a high Young's modulus.
[0020] The zirconia particles according to this embodiment are dispersed in a dispersion medium. By using the zirconia particles dispersed in a dispersion medium, the zirconia particles can be uniformly dispersed in the resin composition, and the storage stability of the resin composition can be improved. The dispersion medium is not particularly limited as long as it does not inhibit the curing of the resin composition. The dispersion medium may be reactive or non-reactive.
[0021] As the reactive dispersion medium, monomers such as (meth)acryloyl compounds and epoxy compounds may be used. As the (meth)acryloyl compounds, for example, 1,6-hexanediol di(meth)acrylate, EO modified bisphenol A di(meth)acrylate, polyethylene glycol di(meth)acrylate, PO modified bisphenol A di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, (meth)acrylic acid adduct of propylene glycol diglycidyl ether, (meth)acrylic acid adduct of tripropylene glycol diglycidyl ether, and (meth)acrylic acid adduct of glycerin diglycidyl ether may be used. As the dispersion medium, (meth)acryloyl compounds exemplified as monomers described later may be used.
[0022] As the non-reactive dispersion medium, a ketone solvent such as methyl ethyl ketone (MEK), an alcohol solvent such as methanol (MeOH), or an ester solvent such as propylene glycol monomethyl ether acetate (PGMEA) may be used. In the case of a non-reactive dispersion medium, the resin composition may be prepared by mixing the base resin and the zirconia particles dispersed in the dispersion medium, and then removing a part of the dispersion medium. The zirconia particles dispersed in the non-reactive dispersion medium are more likely to reduce the cure shrinkage of the resin composition than the zirconia particles dispersed in a reactive dispersion medium.
[0023] The zirconia particles dispersed in the dispersion medium remain dispersed in the resin layer even after the resin composition is cured. When a reactive dispersion medium is used, the zirconia particles are mixed into the resin composition together with the dispersion medium, and are incorporated into the resin layer while maintaining the dispersed state. When a non-reactive dispersion medium is used, at least a part of the dispersion medium is evaporated from the resin composition, but the zirconia particles remain dispersed in the resin composition and remain dispersed in the resin layer after curing. When the zirconia particles present in the resin layer are observed with an electron microscope, they are observed as dispersed primary particles.
[0024] The crystal structure of the zirconia particles may be tetragonal or cubic. From the viewpoint of increasing the Young's modulus of the resin layer, the zirconia particles may contain tetragonal zirconia.
[0025] From the viewpoint of increasing the Young's modulus of the resin layer, the average primary particle size of the zirconia particles is preferably 0.5 nm to 100 nm, more preferably 1 nm to 80 nm, and even more preferably 1.5 nm to 70 nm. The average primary particle size can be measured, for example, by image analysis of an electron microscope photograph, a light scattering method, or the like. The dispersion medium in which the primary particles of the zirconia particles are dispersed appears transparent to the naked eye when the particle size of the primary particles is small. When the particle size of the primary particles is relatively large (40 nm or more), the dispersion medium in which the primary particles are dispersed appears cloudy, but no sediment is observed.
[0026] The content of zirconium oxide (zirconia particles) in the resin composition is 0.5% by mass or more and 65% by mass or less, based on the total amount of the resin composition, and may be 1% by mass or more and 60% by mass or less, 5% by mass or more and 55% by mass or less, or 10% by mass or more and 50% by mass or less. When the content of zirconium oxide is 0.5% by mass or more, it is easy to form a resin layer having excellent lateral pressure characteristics. When the content of zirconium oxide is 65% by mass or less, it is easy to form a resin layer having excellent storage stability and toughness of the resin composition.
[0027] (Base resin) The base resin according to the present embodiment contains an oligomer, a monomer, and a photopolymerization initiator that contain a urethane (meth)acrylate. Here, the term "(meth)acrylate" refers to an acrylate or a corresponding methacrylate. The same applies to (meth)acrylic acid.
[0028] As the urethane (meth)acrylate, an oligomer obtained by reacting a polyol compound, a polyisocyanate compound, and a hydroxyl group-containing (meth)acrylate compound can be used.
[0029] Examples of polyol compounds include polytetramethylene glycol, polypropylene glycol, and bisphenol A-ethylene oxide addition diol. Examples of polyisocyanate compounds include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane 4,4'-diisocyanate. Examples of hydroxyl group-containing (meth)acrylate compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 1,6-hexanediol mono(meth)acrylate, pentaerythritol tri(meth)acrylate, 2-hydroxypropyl (meth)acrylate, and tripropylene glycol mono(meth)acrylate.
[0030] In general, an organic tin compound is used as a catalyst when synthesizing urethane (meth)acrylate. Examples of the organic tin compound include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexyl mercaptoacetate), dibutyltin bis(isooctyl mercaptoacetate), and dibutyltin oxide. In terms of easy availability or catalytic performance, it is preferable to use dibutyltin dilaurate or dibutyltin diacetate as a catalyst.
[0031] A lower alcohol having 5 or less carbon atoms may be used during synthesis of the urethane (meth)acrylate. Examples of the lower alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-2-butanol, and 2,2-dimethyl-1-propanol.
[0032] From the viewpoint of increasing the Young's modulus of the resin layer, the oligomer may further contain an epoxy (meth)acrylate. As the epoxy (meth)acrylate, an oligomer obtained by reacting an epoxy resin having two or more glycidyl groups with a compound having a (meth)acryloyl group can be used.
[0033] The monomer may be a monofunctional monomer having one polymerizable group or a polyfunctional monomer having two or more polymerizable groups. Two or more kinds of monomers may be mixed and used.
[0034] Examples of the monofunctional monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, 2 ... Octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, phenoxydiethylene glycol acrylate, phenoxypolyethylene glycol (meth)acrylate, 4-tert-butylcyclohexanol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentene (Meth)acrylate monomers such as dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, and isobornyl (meth)acrylate; (meth)acrylic acid, (meth)acrylic acid dimer, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, ω-carboxy-polycaprolactone, carboxyl group-containing monomers such as lactone (meth)acrylate; heterocycle-containing (meth)acrylates such as N-(meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N-acryloylpiperidine, N-methacryloylpiperidine, N-(meth)acryloylpyrrolidine, 3-(3-pyridine)propyl (meth)acrylate, and cyclic trimethylolpropane formal acrylate; maleimide-based monomers such as maleimide, N-cyclohexylmaleimide, and N-phenylmaleimide;Amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; aminoalkyl(meth)acrylate monomers such as aminoethyl(meth)acrylate, aminopropyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and tert-butylaminoethyl(meth)acrylate; and succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide.
[0035] Examples of polyfunctional monomers include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, di(meth)acrylate of an alkylene oxide adduct of bisphenol A, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, 1,4- Butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosanediol di(meth)acrylate, isopentyldiol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate, bisphenol A EO adduct di(meth)acrylate of Nol A, trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxy polypropoxy tri(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol Examples of the acrylate copolymer include acrylate copolymers such as acrylate copolymers, ...
[0036] The photopolymerization initiator can be appropriately selected from known radical photopolymerization initiators. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one (Omnirad 907, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins).
[0037] The resin composition may further contain a silane coupling agent, a leveling agent, a defoaming agent, an antioxidant, a sensitizer, and the like.
[0038] Silane coupling agents are not particularly limited as long as they do not interfere with the curing of the resin composition. Examples of silane coupling agents include tetramethyl silicate, tetraethyl silicate, mercaptopropyl trimethoxysilane, vinyl trichlorosilane, vinyl triethoxysilane, vinyl tris(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, 3-acryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-aminoethyl)-γ -aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, bis-[3-(triethoxysilyl)propyl]tetrasulfide, bis-[3-(triethoxysilyl)propyl]disulfide, γ-trimethoxysilylpropyldimethylthiocarbamyltetrasulfide, and γ-trimethoxysilylpropylbenzothiazyltetrasulfide.
[0039] The resin composition according to the present embodiment can be suitably used as a secondary coating material for an optical fiber. By using the resin composition according to the present embodiment for the secondary resin layer, a coating resin layer having excellent lateral pressure characteristics can be formed.
[0040] <Optical fiber> 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. The optical fiber 10 includes a glass fiber 13 including a core 11 and a cladding 12, and a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15 provided on the outer periphery of the glass fiber 13.
[0041] The cladding 12 surrounds the core 11. The core 11 and the cladding 12 mainly contain glass such as silica glass, and for example, the core 11 can be made of silica glass doped with germanium, and the cladding 12 can be made of pure silica glass or silica glass doped with fluorine.
[0042] 1, for example, the outer diameter (D2) of the glass fiber 13 is about 100 μm to 125 μm, and the diameter (D1) of the core 11 constituting the glass fiber 13 is about 7 μm to 15 μm. The thickness of the coating resin layer 16 is usually about 22 μm to 70 μm. The thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 5 μm to 50 μm.
[0043] When the outer diameter (D2) of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 60 μm to 70 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 10 μm to 50 μm, for example, the thickness of the primary resin layer 14 may be 35 μm and the thickness of the secondary resin layer 15 may be 25 μm. The outer diameter of the optical fiber 10 may be about 245 μm to 265 μm.
[0044] When the outer diameter (D2) of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 27 μm to 48 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 10 μm to 38 μm, for example, the thickness of the primary resin layer 14 may be 25 μm and the thickness of the secondary resin layer 15 may be 10 μm. The outer diameter of the optical fiber 10 may be about 179 μm to 221 μm.
[0045] When the outer diameter (D2) of the glass fiber 13 is about 100 μm and the thickness of the coating resin layer 16 is 22 μm to 37 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 5 μm to 32 μm, for example, the thickness of the primary resin layer 14 may be 25 μm and the thickness of the secondary resin layer 15 may be 10 μm. The outer diameter of the optical fiber 10 may be about 144 μm to 174 μm.
[0046] The resin composition according to the present embodiment can be applied to the secondary resin layer. The secondary resin layer can be formed by curing the resin composition containing the above-mentioned base resin and zirconium oxide. This can improve the lateral pressure characteristics of the optical fiber.
[0047] The content of zirconium oxide in the secondary resin layer is 0.5% by mass or more and 65% by mass or less, based on the total amount of the secondary resin layer, and may be 1% by mass or more and 60% by mass or less, 5% by mass or more and 55% by mass or less, or 10% by mass or more and 50% by mass or less.
[0048] The manufacturing method of the optical fiber according to this embodiment includes a coating step of coating the above-mentioned resin composition on the outer circumference of a glass fiber composed of a core and a cladding, and a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step.
[0049] The Young's modulus of the secondary resin layer is preferably 1150 MPa or more, more preferably 1200 MPa or more and 2700 MPa or less, and even more preferably 1300 MPa or more and 2600 MPa or less at 23° C. When the Young's modulus of the secondary resin layer is 1150 MPa or more, the lateral pressure characteristics are easily improved, and when it is 2700 MPa or less, appropriate toughness can be imparted to the secondary resin layer, making it less likely for cracks and the like to occur in the secondary resin layer.
[0050] The zirconium oxide dispersed in the dispersion medium remains dispersed in the resin layer even after the resin layer is cured. When a reactive dispersion medium is used, the zirconium oxide is mixed into the resin composition together with the dispersion medium, and is incorporated into the resin layer while maintaining the dispersed state. When a non-reactive dispersion medium is used, at least a part of the dispersion medium volatilizes from the resin composition and disappears, but the zirconium oxide remains dispersed in the resin composition and remains dispersed in the resin layer after curing. When observed with an electron microscope, the zirconium oxide present in the resin layer is observed as dispersed primary particles.
[0051] The primary resin layer 14 can be formed, for example, by curing a resin composition containing a urethane (meth)acrylate, a monomer, a photopolymerization initiator, and a silane coupling agent. The resin composition for the primary resin layer can be formed using a conventionally known technique. The urethane (meth)acrylate, the monomer, the photopolymerization initiator, and the silane coupling agent may be appropriately selected from the compounds exemplified for the base resin above. However, the resin composition forming the primary resin layer has a different composition from the base resin forming the secondary resin layer.
[0052] In some cases, optical fibers are arranged in parallel and integrated with a ribbon resin to form an optical fiber ribbon, and the resin composition according to the present disclosure can also be used as a ribbon resin, which can improve the lateral pressure characteristics of the optical fiber ribbon in the same way as optical fibers. EXAMPLES
[0053] The present disclosure will be described in more detail below by showing the results of evaluation tests using examples and comparative examples according to the present disclosure. Note that the present disclosure is not limited to these examples.
[0054] [Resin composition for secondary resin layer] (Oligomer) As oligomers, urethane acrylate (UA) obtained by reacting polypropylene glycol having a molecular weight of 1000, 2,4-tolylene diisocyanate, and hydroxyethyl acrylate, and epoxy acrylate (EA) were prepared.
[0055] (monomer) As monomers, isobornyl acrylate (trade name "IBXA" manufactured by Osaka Organic Chemical Industry Co., Ltd.) and tripropylene glycol diacrylate (TPGDA, trade name "Viscoat #310HP" manufactured by Osaka Organic Chemical Industry Co., Ltd.) were prepared.
[0056] (Photopolymerization initiator) As photopolymerization initiators, 1-hydroxycyclohexyl phenyl ketone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide were prepared.
[0057] (Zirconium oxide) As zirconium oxide, a zirconia sol was prepared containing zirconia particles (Zr-1 to Zr-4) having the surface state and average primary particle size shown in Table 1. The hydrophobic zirconia particles had a main crystal system of tetragonal crystals and had methacryloyl groups.
[0058] [Table 1]
[0059] (Resin composition) A base resin was prepared by mixing 40 parts by mass of UA, 20 parts by mass of EA, 10 parts by mass of IBXA, 30 parts by mass of TPGDA, 0.5 parts by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 0.5 parts by mass of 1-hydroxycyclohexylphenyl ketone. Next, the zirconia sol was mixed with the base resin so as to obtain the content of the zirconia particles shown in Table 2 or Table 3, and then most of the MEK, which is the dispersion medium, was removed under reduced pressure to prepare the resin compositions of the examples and comparative examples. The total amount of the resin composition and the total amount of the cured product of the resin composition may be considered to be the same.
[0060] (Stability of Resin Composition) The resin composition was stirred while being heated at 45° C. for 30 minutes, and then allowed to stand at room temperature for 1 hour, and the appearance was visually inspected.
[0061] (Young's Modulus) The resin composition was applied onto a polyethylene terephthalate (PET) film using a spin coater, and then irradiated with 1000±100mJ / cm using an electrodeless UV lamp system (Heraeus's "VPS600 (D bulb)"). 2 The resin was cured under the above conditions to form a resin layer having a thickness of 200±20 μm on the PET film. The resin layer was peeled off from the PET film to obtain a resin film. The resin film was punched out into a dumbbell shape according to JIS K 7127 Type 5, and pulled at 23±2° C., 50±10% RH, using a tensile tester at a pulling speed of 1 mm / min and a gauge distance of 25 mm to obtain a stress-strain curve. The Young's modulus was determined by the 2.5% secant line. The resin composition of Comparative Example 1 had an increased viscosity, and it was not possible to produce a film.
[0062] [Fabrication of optical fiber] (Resin composition for primary resin layer) As an oligomer, a urethane acrylate obtained by reacting polypropylene glycol having a molecular weight of 4000, isophorone diisocyanate, hydroxyethyl acrylate, and methanol was prepared. A resin composition for the primary resin layer was prepared by mixing 75 parts by mass of the urethane acrylate, 12 parts by mass of nonylphenol EO-modified acrylate, 6 parts by mass of N-vinyl caprolactam, 2 parts by mass of 1,6-hexanediol diacrylate, 1 part by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 1 part by mass of 3-mercaptopropyltrimethoxysilane.
[0063] (Optical Fiber) The resin composition for the primary resin layer and the resin composition for the example or comparative example were applied to the outer circumference of a glass fiber having a diameter of 125 μm, which is composed of a core and a clad, and then the resin composition was cured by irradiating with ultraviolet light to form a primary resin layer having a thickness of 35 μm and a secondary resin layer having a thickness of 25 μm on the outer circumference of the primary resin layer, thereby producing an optical fiber. The drawing speed was 1500 m / min.
[0064] (lateral pressure characteristics) The transmission loss of light with a wavelength of 1550 nm when the optical fiber 10 was wound in a single layer around a 280 mm diameter bobbin covered with sandpaper was measured by the OTDR (Optical Time Domain Reflectometer) method. In addition, the transmission loss of light with a wavelength of 1550 nm when the optical fiber 10 was wound in a single layer around a 280 mm diameter bobbin without sandpaper was measured by the OTDR method. The difference in the measured transmission losses was calculated, and the lateral pressure characteristic was judged to be "OK" when the transmission loss difference was 0.6 dB / km or less, and the lateral pressure characteristic was judged to be "NG" when the transmission loss difference was more than 0.6 dB / km. In Comparative Example 2, cracks occurred in the resin layer when the optical fiber was wound around the bobbin, and the lateral pressure characteristic could not be evaluated.
[0065] [Table 2]
[0066] [Table 3] [Explanation of symbols]
[0067] 10 Optical Fiber 11 cores 12 Clad 13 Glass Fiber 14 Primary resin layer 15 Secondary resin layer 16 Coating resin layer
Claims
1. a glass fiber including a core and a cladding; a primary resin layer that is in contact with and covers the glass fiber; A secondary resin layer that covers the primary resin layer, The optical fiber, wherein the secondary resin layer is made of a cured product of a resin composition containing a base resin containing an oligomer, a monomer, and a photopolymerization initiator including a urethane (meth)acrylate, and hydrophobic zirconium oxide, and the content of the zirconium oxide is 5 mass% or more and 60 mass% or less based on the total amount of the resin composition.
2. 2. The optical fiber of claim 1, wherein the zirconium oxide has an average primary particle size of 100 nm or less.
3. The optical fiber of claim 1 or 2, wherein the zirconium oxide comprises tetragonal zirconium oxide.
4. a glass fiber including a core and a cladding; a primary resin layer that is in contact with and covers the glass fiber; A secondary resin layer that covers the primary resin layer, The secondary resin layer contains hydrophobic zirconium oxide, The optical fiber, wherein the content of the zirconium oxide is 5 mass % or more and 60 mass % or less based on the total amount of the secondary resin layer.
5. A coating step of coating an outer periphery of a glass fiber including a core and a clad with a resin composition for a primary resin layer and a resin composition for a secondary resin layer; a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step to form a primary resin layer and a secondary resin layer; Including, A method for manufacturing an optical fiber, wherein the secondary resin layer is made of a cured product of a resin composition containing a base resin containing an oligomer, a monomer, and a photopolymerization initiator including a urethane (meth)acrylate, and hydrophobic zirconium oxide, and the content of the zirconium oxide is 5 mass% or more and 60 mass% or less based on the total amount of the resin composition.
6. The method for producing an optical fiber as described in claim 5, wherein the average primary particle size of the zirconium oxide is 100 nm or less.
7. The method for producing an optical fiber as described in claim 5 or claim 6, wherein the zirconium oxide comprises tetragonal zirconium oxide.
Citation Information
Patent Citations
Core wire for optical fiber tape
JP1996217495A
Radiation curable composition, its cured product and laminate
JP2006161030A
Composition for optical material
JP2008024735A
Radiation-curable coating composition
JP2010511770A
Coated optical fiber
JP2014219550A