Method for producing carbon fiber bundle with sizing agent and carbon fiber reinforced composite material
The sizing agent for carbon fibers, composed of urethane, epoxy, and ester compounds, addresses the issue of insufficient matrix resin impregnation and handling in high-speed forming methods, enhancing mechanical properties and processing ease of carbon fiber bundles.
Patent Information
- Application Number
- JP2022015044
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-10-17
- Filing Date
- 2022-02-02
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2037-10-30
AI Technical Summary
Existing sizing agents for carbon fibers fail to provide sufficient matrix resin impregnation, handling properties, and mechanical properties, especially in high-speed forming methods like filament winding, leading to inadequate composite material performance.
A sizing agent for carbon fibers comprising components (A), (B), and (C), including urethane, epoxy, and ester compounds, with specific molecular structures and ratios, enhances matrix resin impregnation, handling, and mechanical properties.
The sizing agent improves matrix resin impregnation, interfacial adhesion, and dispersion within the resin, resulting in carbon fiber bundles with enhanced mechanical properties and processing ease.
Smart Images

Figure 0007567822000046 
Figure 0007567822000001 
Figure 0007567822000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a sizing agent for carbon fibers, an aqueous dispersion of a sizing agent for carbon fibers, carbon fibers having a sizing agent attached thereto, and carbon fiber bundles having a sizing agent attached thereto. This application claims priority based on Japanese Patent Application No. 2016-211672, filed in Japan on October 28, 2016, and Japanese Patent Application No. 2017-200941, filed in Japan on October 17, 2017, the contents of which are incorporated herein by reference. [Background technology]
[0002] One type of fiber-reinforced composite material is a carbon fiber-reinforced resin composite material (hereinafter sometimes referred to as "carbon fiber composite material") formed from a reinforcing material made of carbon fiber and a matrix resin. As the matrix resin, various resins such as epoxy resin, unsaturated polyester resin, vinyl ester resin, and phenol resin are used, and among them, epoxy resin is widely used. Generally, carbon fibers are used as carbon fiber bundles in which several thousand to several tens of thousands of single fibers having a diameter of about 5 to 8 μm are bundled together, and it is not easy to impregnate the carbon fiber bundles with a matrix resin.
[0003] When the impregnation with the matrix resin is insufficient, the excellent properties of the carbon fiber as a reinforcing material may not be fully exhibited.
[0004] In particular, in recent years, molding methods with excellent productivity, such as the filament winding (hereinafter sometimes abbreviated as "FW") molding method and the pultrusion (hereinafter sometimes abbreviated as "PT") molding method, have come to be applied to carbon fiber composite materials. In these molding methods, it is desired to pull out the carbon fiber bundle at high speed from a bobbin around which the carbon fiber bundle is wound, and impregnate the bundle with the matrix resin in a short time in the processing step that involves rollers, guides, etc.
[0005] Conventionally, a sizing agent has been added to carbon fibers for the purpose of improving the handleability in processing steps and the wettability with a matrix resin.
[0006] For example, Patent Documents 1 and 2 disclose sizing agents made of epoxy compounds with different surface free energies as sizing agents that improve the impregnation of carbon fiber bundles with matrix resins. Furthermore, Patent Documents 3 and 4 disclose carbon fiber bundles to which a urethane-modified compound has been added for the purpose of improving abrasion resistance. Furthermore, Patent Document 5 discloses a sizing agent made of a urethane-modified epoxy resin and a bisphenol A ethylene oxide adduct for the purpose of improving the handleability of carbon fiber bundles in processing steps. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2003 / 010383 [Patent Document 2] JP 2008-280624 A [Patent Document 3] Japanese Patent Application Publication No. 58-013781 [Patent Document 4] Japanese Patent Application Publication No. 01-314785 [Patent Document 5] JP 2008-274520 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, the carbon fiber bundles to which the sizing agents described in Patent Documents 1 and 2 have been applied may be difficult to sufficiently impregnate with the matrix resin in a high-speed molding method such as filament winding, and the mechanical properties of the obtained composite material may be insufficient. The carbon fiber bundles to which the sizing agents described in Patent Documents 3 and 4 have been applied have excellent abrasion resistance, and therefore the handleability in the processing step of the carbon fiber bundles is good, but the impregnation with the matrix resin may be insufficient. Similarly, in the case of a carbon fiber bundle using the sizing agent described in Patent Document 5, the handleability in the processing step is good, but the impregnation with the matrix resin may be difficult in a high-speed molding method such as filament winding.
[0009] In other words, there is a problem that a sizing agent capable of providing carbon fibers and carbon fiber bundles that are excellent in resin impregnation in the processing step, in handleability, and in the mechanical properties of the composite material has not yet been obtained. Furthermore, the sizing agent is required to improve the impregnation of the matrix resin into the carbon fibers, in particular the property of making it easier for the carbon fibers to be uniformly dispersed in the matrix resin, as well as to improve the bundling of the carbon fibers (rigidity of the carbon fibers) and the interfacial adhesion between the carbon fibers and the matrix resin.
[0010] One aspect of the present invention has been made in view of the above circumstances, and has an object to provide a sizing agent for carbon fiber and an aqueous dispersion of the sizing agent that can provide carbon fibers and carbon fiber bundles that are excellent in impregnation with a matrix resin, in handleability in processing, and in mechanical properties of a composite material. Another object of the present invention is to provide sizing-agent-adhered carbon fibers and sizing-agent-adhered carbon fiber bundles to which the sizing agent has been applied, and further to provide carbon fiber-reinforced composite materials that are excellent in mechanical properties.
[0011] Another aspect of the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a sizing agent for carbon fiber, and an aqueous dispersion of a sizing agent for carbon fiber, which can provide carbon fibers and carbon fiber bundles that are excellent in all of the following: impregnation with a matrix resin, bundling ability, interfacial adhesion with the matrix resin, and ease of dispersion in the matrix resin. Another object of the present invention is to provide a sizing-agent-adhered carbon fiber and a sizing-agent-adhered carbon fiber bundle to which the carbon fiber sizing agent has been applied. [Means for solving the problem]
[0012] The present invention includes the following aspects. [1] A sizing agent for carbon fibers comprising component (A), component (B), and component (C), the component (A) is at least one selected from the group consisting of components (A-1), (A-2), and (A-3); The component (A-1) is a urethane compound having a structure represented by the following formula (1-1) in the molecule, [ka] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer of 1 to 50.] The component (A-2) is an ester compound having a structure represented by the following formula (1-2) in the molecule, [ka] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n1 represents an integer from 1 to 50.] The component (A-3) is an amide compound having a structure represented by the following formula (1-3) in the molecule, [ka] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R, R1, and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer from 1 to 49.] The component (B) is an epoxy compound selected from the group consisting of an epoxy compound represented by the following formula (2), an epoxy compound represented by the following formula (3), and an epoxy compound represented by the following formula (4), [ka] [In the formula, m represents an integer of 1 to 5.] [ka] [In the formula, R3 and R4 each independently represent a hydrogen atom or a saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms, and p represents an integer of 0 to 5.] [ka] [In the formula, q represents an integer of 0 to 5.] The sizing agent for carbon fibers, wherein the component (C) is a bisphenol type epoxy compound or an aliphatic epoxy compound. [2] The sizing agent for carbon fiber according to [1], wherein the component (A) contains a component (A-1), and the component (A-1) has an epoxy group in the molecule. [3] The sizing agent for carbon fiber according to [1] or [2], wherein the component (A) includes component (A-1), the content of the component (A-1) is 10 to 60 parts by mass, the content of the component (B) is 15 to 55 parts by mass, and the content of the component (C) is 20 to 75 parts by mass, relative to 100 parts by mass in total of the components (A), (B), and (C), and the total of the component (A-1), (B), and (C) is 50% by mass or more, relative to the total mass of the sizing agent for carbon fiber. [4] The sizing agent for carbon fiber according to [3], further comprising an aliphatic ester compound, the content of the aliphatic ester compound being 5 to 20 mass% relative to the total mass of the sizing agent for carbon fiber. [5] The sizing agent for carbon fiber according to [3] or [4], further comprising a surfactant, the content of the surfactant being 10 to 25 mass% relative to the total mass of the sizing agent for carbon fiber. [6] The sizing agent for carbon fiber according to [5], wherein the surfactant is an anionic surfactant represented by the following formula (5): [ka] [In the formula, R5 and R6 each independently represent a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; and r represents an integer of 5 to 25.] [7] The sizing agent for carbon fiber according to [1], wherein the component (A) contains a component (A-2), and the component (A-2) has an epoxy group in the molecule. [8] The sizing agent for carbon fiber according to [1] or [7], wherein the component (A) contains a component (A-2), and the component (A-2) has a structure represented by the following formula (1-2)' in the molecule: [ka] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; Y represents a methylene group, a 1,1-ethylene group, a 2,2-propylene group, -SO2-, an oxygen atom, a sulfur atom, or a single bond; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n1 and n2 each independently represent an integer from 1 to 50.] [9] The sizing agent for carbon fiber according to any one of [1], [7], and [8], wherein the component (A) includes component (A-2), and the content of the component (A-2) is 40 to 80 parts by mass, the content of the component (B) is 10 to 40 parts by mass, and the content of the component (C) is 10 to 30 parts by mass, relative to 100 parts by mass in total of the contents of the components (A), (B), and (C).
[10] The sizing agent for carbon fiber according to [9], further comprising a surfactant, the content of the surfactant being 5 to 30 mass % relative to the total mass of the sizing agent for carbon fiber.
[11] The sizing agent for carbon fiber according to
[10] , wherein the surfactant is a nonionic surfactant.
[12] A sizing agent for carbon fiber according to any one of [1] to
[11] , and water, An aqueous dispersion of a sizing agent for carbon fiber in which the sizing agent for carbon fiber is dispersed in water.
[13] A sizing-agent-adhered carbon fiber bundle comprising carbon fiber and a sizing agent for carbon fiber, the sizing-agent-adhered carbon fiber bundle having a spontaneous dispersion rate of 3 or more as measured by a spontaneous dispersion test.
[14] The sizing-agent-adhered carbon fiber bundle according to
[13] , containing 0.1 to 5.0 mass% of the sizing agent for carbon fiber according to any one of [1] to
[11] relative to the total mass of the sizing-agent-adhered carbon fiber bundle.
[15] A method for producing a carbon fiber reinforced composite material, comprising impregnating a sizing-agent-attached carbon fiber bundle according to
[13] or
[14] with a thermosetting resin composition and heat curing the thermosetting resin composition.
[16] A method for producing a carbon fiber reinforced pressure vessel, comprising: impregnating a sizing-agent-adhered carbon fiber bundle according to
[13] or
[14] with a thermosetting resin composition by a filament winding method, and heat-curing the thermosetting resin composition to produce a carbon fiber reinforced pressure vessel. Effect of the Invention
[0013] In one aspect of the present invention, by using a carbon fiber sizing, it is possible to obtain carbon fibers and carbon fiber bundles with a sizing agent attached thereto, which are excellent in impregnation with a matrix resin, handleability in processing steps, and mechanical properties of the composite material.
[0014] In another aspect of the present invention, by using a carbon fiber sizing, it is possible to obtain carbon fibers and carbon fiber bundles with a sizing agent attached thereto, which are excellent in terms of impregnation with a matrix resin, bundling ability, interfacial adhesion with the matrix resin, and ease of dispersion within the matrix resin. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a schematic diagram of an apparatus for measuring the opening rate A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <Carbon fiber sizing agent> <Component (A)> In the present invention, the component (A) is at least one selected from the group consisting of the components (A-1), (A-2), and (A-3). The component (A-1) used in the carbon fiber sizing agent of the present invention is a urethane compound having a structure of formula (1-1) in the molecule. The component (A-1) preferably has at least two or more epoxy groups in one molecule.
[0017] [ka]
[0018] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer of 1 to 50. It is preferable that one of R1 and R2 is a methyl group and the other is a hydrogen atom.]
[0019] Component (A-1) can be obtained by reacting a polyhydroxy compound mixture (polyol mixture) containing a polyhydroxy compound having a hydroxyethyloxy group, a hydroxypoly(ethyleneoxy) group, a hydroxyisopropyloxy group or a hydroxypoly(isopropyloxy) group (hereinafter referred to as polyhydroxy compound A) with a diisocyanate compound. As polyhydroxy compound A, it is preferable to use a polyhydroxy compound having a hydroxyisopropyloxy group or a hydroxypoly(isopropyloxy) group.
[0020] The component (A-1) having an epoxy group in the molecule can be obtained by reacting a urethane compound having a structure represented by formula (1-1)' with an epoxy compound having a hydroxy group.
[0021] [ka]
[0022] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer of 1 to 50. It is preferable that one of R1 and R2 is a methyl group and the other is a hydrogen atom.]
[0023] The urethane compound having a structure represented by formula (1-1)' in the molecule can be obtained by mixing a polyhydroxy compound mixture (polyol mixture) containing a polyhydroxy compound A with a diisocyanate compound such that the isocyanate group in the diisocyanate compound is in excess relative to 1 mol of hydroxy group in the polyol mixture, and reacting them at 40 to 140°C. As polyhydroxy compound A, it is preferable to use a polyhydroxy compound having a hydroxyisopropyloxy group or a hydroxypoly(isopropyloxy) group.
[0024] When reacting a polyhydroxy compound mixture (polyol mixture) containing a polyhydroxy compound A with a diisocyanate compound, it is also possible to use a urethane polymerization catalyst in order to promote the reaction, for example, an organometallic compound such as dioctyltin dilaurate, dibutyltin dilaurate, stannous octoate, stannous octoate, lead octoate, lead naphthenate, or zinc octoate, or a tertiary amine compound such as triethylenediamine or triethylamine.
[0025] Examples of polyhydroxy compounds other than the polyhydroxy compound A include polyester polyols, polycarbonate polyols, polyesteramide polyols, acrylic polyols, and polyurethane polyols, and among these, polyether polyols can be preferably used. The polyhydroxy compounds may be used alone or in combination.
[0026] As the polyhydroxy compound having the hydroxyisopropyleneoxy group or hydroxypoly(isopropyloxy) group, a compound in which propylene oxide is added to a polyhydric alcohol so as to obtain a desired molecular weight (molecular weight of 100 to 10,000) is preferably used.
[0027] Examples of the polyhydric alcohol include dihydric alcohols such as ethylene glycol, propylene glycol, and 1,4-butylene glycol, and examples of the trihydric alcohol include glycerin, trioxyisobutane, 1,2,3-butanetriol, 1,2,3-pentanetriol, 2-methyl-1,2,3-propanetriol, 2-methyl-2,3,4-butanetriol, 2-ethyl-1,2,3-butanetriol, 1,2,4-butanetriol, and 2,3,4-pentanetriol. Examples of the polyhydric alcohol include erythritol, 2,3,4-hexanetriol, pentamethylglycerin, 1,2,4-pentanetriol, etc., examples of the tetrahydric alcohol include erythritol, 1,2,3,4-pentanetetraol, 2,3,4,5-hexatetraol, 1,2,3,5-pentanetetraol, 1,3,4,5-hexanetetraol, etc., examples of the pentahydric alcohol include xylitol, arabitol, etc., and examples of the hexahydric alcohol include sorbitol, mannitol, etc. Among these, the preferred polyhydric alcohols are dihydric to tetrahydric alcohols.
[0028] Diisocyanate compounds include propane-1,2-diisocyanate, 2,3-dimethylbutane-2,3-diisocyanate, 2-methylpentane-2,4-diisocyanate, octane-3,6-diisocyanate, 3,3-dinitropentane-1,5-diisocyanate, octane-1,6-diisocyanate, 1,6-hexamethylene diisocyanate (HDI), trimethylhexamethylene diisocyanate, lysine diisocyanate, and tolylene diisocyanate (TD). I), xylylene diisocyanate, metatetramethylxylylene diisocyanate, isophorone diisocyanate (3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate), 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane, diphenylmethane-4,4'-diisocyanate (MDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), hydrogenated tolylene diisocyanate, and mixtures thereof.
[0029] Furthermore, when X in formula (1-1) is a divalent aromatic group, and when the diisocyanate is an aromatic diisocyanate such as tolylene diisocyanate (TDI) or xylylene diisocyanate, the sizing agent for carbon fiber of the present invention has a strong interaction with the carbon fiber surface and is also excellent in compatibility with a matrix resin having an aromatic ring that has excellent heat resistance, which is preferable.
[0030] The diisocyanate may be used alone or in combination with a plurality of diisocyanates. Furthermore, polyisocyanates having three or more isocyanate groups in one molecule, such as triisocyanates and tetraisocyanates, may be used in combination. Examples of epoxy compounds having a hydroxy group include epoxy resins having a hydroxy group, such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, resorcinol type epoxy resins, bisphenol S type epoxy resins, polyethylene glycol type epoxy resins which are reaction products of polyhydric alcohols with the halogen-containing epoxides, and polypropylene glycol type epoxy resins. Of these, from the viewpoint of improving compatibility with the matrix resin, bisphenol A type epoxy resins or bisphenol F type epoxy resins having a hydroxy group are preferably used.
[0031] Component (A-1) having an epoxy group in the molecule can be obtained, for example, by mixing a urethane compound having an isocyanate residue and a structure represented by formula (1-1)' in the molecule with an epoxy compound having a hydroxy group, and reacting them at 40 to 140° C. In this case, the amount of hydroxy groups in the epoxy compound having a hydroxy group is set to 1 to 10 mol per 1 mol of isocyanate residue in the urethane compound having a structure represented by formula (1-1)' in the molecule. In order to promote the reaction, it is also possible to use a urethane polymerization catalyst, for example, an organometallic compound such as dioctyltin dilaurate, dibutyltin dilaurate, stannous octoate, stannous octoate, lead octoate, lead naphthenate, or zinc octoate, or a tertiary amine compound such as triethylenediamine or triethylamine.
[0032] Component (A-1) is a compound that has a urethane bond in its molecule, has strong interaction with the carbon fiber surface, and is flexible. In the process of impregnating and curing a carbon fiber bundle with a matrix resin, the inclusion of component (A-1) in the sizing agent attached to the surface of the carbon fiber single fiber makes it possible to form a flexible interfacial layer that is firmly attached to the surface of the carbon fiber single fiber. As a result, when carbon fibers with a sizing agent containing component (A) attached thereto are used as reinforcing fibers in a composite material, the mechanical properties of the composite material become good. Component (A-1) having an epoxy group in the molecule has an epoxy group and a urethane bond in the molecule, and is a compound that has strong interaction with the carbon fiber surface and is flexible. In the process of impregnating and curing a carbon fiber bundle with a matrix resin, by including component (A-1) having an epoxy group in the molecule in the sizing agent attached to the surface of the carbon fiber single fiber, it becomes possible to form a flexible interfacial layer that is firmly attached to the surface of the carbon fiber single fiber, and as a result, when the carbon fiber to which the sizing agent containing component (A) is attached is used as a reinforcing fiber of a composite material, the mechanical properties of the composite material become particularly good.
[0033] As the raw material of the sizing agent containing component (A-1), commercially available products such as ADEKA RESIN EPU-73B (manufactured by ADEKA CORPORATION) and ADEKA RESIN EPU-78-11 (manufactured by ADEKA CORPORATION) can be used, but many of these commercially available products contain bisphenol type epoxy resins that do not have the structure of formula (1-1) in the molecule, such as bisphenol A type epoxy resins and bisphenol F type epoxy resins. In the present invention, bisphenol type epoxy resins that do not have the structure of formula (1-1) in the molecule correspond to component (C) described later. Component (A-1) contained in ADEKA RESIN EPU-73B and ADEKA RESIN EPU-78-11 has an epoxy group in the molecule.
[0034] The component (A-2) is an ester compound having the structure of the following formula (1-2) in the molecule.
[0035] [ka]
[0036] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n1 represents an integer from 1 to 50.]
[0037] The main chain of component (A-2) may terminate with a carboxy group or an alcoholic hydroxy group.
[0038] Component (A-2) can be obtained by mixing and reacting a mixture of polyhydroxy compounds (polyol mixture) containing polyhydroxy compound A with a dicarboxy compound or a carboxylic acid anhydride (hereinafter, sometimes simply referred to as acid anhydride).
[0039] The component (A-2) preferably has a structure represented by formula (1-2)' in the molecule.
[0040] [ka]
[0041] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; Y represents a methylene group, a 1,1-ethylene group, a 2,2-propylene group, -SO2-, an oxygen atom, a sulfur atom, or a single bond; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n1 and n2 each independently represent an integer from 1 to 50.]
[0042] Component (A-2) may have an epoxy group in the molecule. Component (A-2) having an epoxy group can be obtained by reacting component (A-2') having a structure represented by the following formula (1-2)'' with an epoxy compound having two or more epoxy groups in one molecule.
[0043] [ka]
[0044] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n1 represents an integer from 1 to 50.]
[0045] The component (A-2') having a structure represented by formula (1-2)'' in the molecule (i.e., the component (A-2) having a carboxy group at the end of the main chain) can be obtained by mixing and reacting a mixture of polyhydroxy compounds containing polyhydroxy compound A (polyol mixture) with a dicarboxy compound or a carboxylic acid anhydride (hereinafter, sometimes simply referred to as acid anhydride) such that the carboxylic acid in the dicarboxy compound or acid anhydride is in excess relative to the hydroxy groups in the polyol mixture.
[0046] Component (A-2), whose main chain has an alcoholic hydroxy group at its end, can be obtained by mixing and reacting a polyol mixture with a dicarboxy compound or an acid anhydride such that there is a shortage of carboxylic acid in the dicarboxy compound or the acid anhydride relative to the hydroxy groups in the polyol mixture.
[0047] As the polyhydroxy compound other than the polyhydroxy compound A, polyester polyols, polycarbonate polyols, polyesteramide polyols, acrylic polyols, polyurethane polyols, and polyether polyols having hydroxyl groups at their terminals can be used. The polyhydroxy compounds may be used alone or in combination. As the polyhydroxy compound A, a compound obtained by adding ethylene oxide or propylene oxide to a bisphenol so as to obtain a desired molecular weight (mass average molecular weight of 100 to 10,000) can be preferably used, and a component (A-2) having a structure represented by formula (1-2)' in the molecule can be obtained. In the present invention, the mass average molecular weight is a value measured by gel permeation chromatography (GPC) and calculated as a standard polystyrene.
[0048] Examples of the bisphenols include bisphenol F, bisphenol E, bisphenol A, bisphenol S, 4,4'-oxydiphenol, 4,4'-thioxydiphenol, and 4,4'-biphenol. The phenylene group of the bisphenols may have a substituent. Examples of bisphenols having a phenylene group with a substituent include various bis-xylenols and bis-orthocresols. Among these, bisphenol F and bisphenol A are preferred, and bisphenol A is more preferred. As the polyhydroxy compound A, a compound in which ethylene oxide or propylene oxide is added to a polyhydric alcohol so as to give a desired molecular weight (mass average molecular weight of 100 to 10,000) is also preferably used.
[0049] Examples of the polyhydric alcohol include dihydric alcohols such as ethylene glycol, propylene glycol, 1,4-butylene glycol, and 1,4-dihydroxymethylbenzene, and examples of the trihydric alcohol include glycerin, trioxyisobutane, 1,2,3-butanetriol, 1,2,3-pentanetriol, 2-methyl-1,2,3-propanetriol, 2-methyl-2,3,4-butanetriol, 2-ethyl-1,2,3-butanetriol, 1,2,4-butanetriol, 2, Examples of the polyhydric alcohol include 3,4-pentanetriol, 2,3,4-hexanetriol, pentamethylglycerin, 1,2,4-pentanetriol, etc., examples of the tetrahydric alcohol include erythritol, 1,2,3,4-pentanetetraol, 2,3,4,5-hexatetraol, 1,2,3,5-pentanetetraol, 1,3,4,5-hexanetetraol, etc., examples of the pentahydric alcohol include xylitol, arabitol, etc., and examples of the hexahydric alcohol include sorbitol, mannitol, etc. Among these, the preferred polyhydric alcohols are dihydric to tetrahydric alcohols.
[0050] Examples of the dicarboxy compound include terephthalic acid, isophthalic acid, and mixtures thereof. Examples of the acid anhydride include phthalic anhydride. These dicarboxylic acids and acid anhydrides may have a substituent such as a methyl group or an ethyl group.
[0051] Furthermore, when X in formula (1-2) is a divalent aromatic group, that is, when the dicarboxy compound is an aromatic dicarboxy compound such as terephthalic acid or isophthalic acid, the sizing agent for carbon fiber of the present invention has a strong interaction with the carbon fiber surface and is also excellent in compatibility with a matrix resin having an aromatic ring that has excellent heat resistance, which is preferable. The dicarboxy compound may be used alone or in combination with a plurality of dicarboxy compounds.Furthermore, a polycarboxylic acid having three or more carboxy groups in one molecule may be used in combination.
[0052] Examples of epoxy compounds having two or more epoxy groups in one molecule include epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, resorcinol type epoxy resins, bisphenol S type epoxy resins, polyol type epoxy resins which are reaction products of polyhydric alcohols and halogen-containing epoxides, polyethylene glycol type epoxy resins, polypropylene glycol type epoxy resins, etc. Among these, from the viewpoint of improving compatibility with the matrix resin, bisphenol A type epoxy resins or bisphenol F type epoxy resins are preferably used.
[0053] The component (A-3) used in the sizing agent for carbon fiber of the present invention is an amide compound having a structure of formula (1-3) in the molecule.
[0054] [ka]
[0055] [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R, R1, and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer from 1 to 49.]
[0056] Component (A-3) can be obtained by reacting a carboxylic acid obtained by oxidizing the hydroxymethyl groups at the molecular terminals of a mixture of polyhydroxy compounds (polyol mixture) containing polyhydroxy compound A to form carboxy groups, with a diamino compound. Examples of diamino compounds include propane-1,2-diamine, 2,3-dimethylbutane-2,3-diamine, 2-methylpentane-2,4-diamine, octane-3,6-diamine, 3,3-dinitropentane-1,5-diamine, octane-1,6-diamine, 1,6-hexamethylenediamine, trimethylhexamethylenediamine, lysinediamine, tolylenediamine, xylylenediamine, meta-tetramethylxylylenediamine, isophoronediamine (3-aminomethyl-3,5,5-trimethylcyclohexylamine), 1,3- or 1,4-bis(aminomethyl)cyclohexane, diphenylmethane-4,4'-diamine, dicyclohexylmethane-4,4'-diamine, hydrogenated tolylenediamine, and mixtures thereof.
[0057] <Ingredient (B)> Component (B) is an epoxy compound selected from the group consisting of epoxy compounds represented by the following formula (2), epoxy compounds represented by the following formula (3), and epoxy compounds represented by the following formula (4).
[0058] [ka]
[0059] [In the formula, m represents an integer of 1 to 5.]
[0060] [ka]
[0061] [In the formula, R3 and R4 each independently represent a hydrogen atom or a saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms; and p represents an integer of 0 to 5.]
[0062] [ka]
[0063] [In the formula, q represents an integer of 0 to 5.]
[0064] Component (B) may be an epoxy compound selected from the group consisting of the epoxy compound represented by the above formula (2), the epoxy compound represented by the above formula (3), and the epoxy compound represented by the above formula (4), and one type may be used or multiple types may be mixed and used. Generally, industrially available epoxy resins are mixtures of compounds in which m, p, and q in the above formulas (2), (3), and (4) are different integers, and the mixtures may be expressed by indicating decimal places for m, p, and q in the above formulas (2), (3), and (4). Examples of component (B) are given below, but the present invention is not limited to these.
[0065] As the epoxy compound represented by formula (2) of component (B), commercially available products such as the EPICLON HP7200 series (manufactured by DIC Corporation) can be used. As the epoxy compound represented by formula (3) of component (B), commercially available products such as jER157S70 (manufactured by Mitsubishi Chemical Corporation) and jER157S60 (manufactured by Mitsubishi Chemical Corporation) can be used. As the epoxy compound represented by formula (4) of component (B), commercially available products such as jER1032H60 (manufactured by Mitsubishi Chemical Corporation) and jER1032S50 (manufactured by Mitsubishi Chemical Corporation) can be used.
[0066] The bisphenol epoxy compound or aliphatic epoxy compound of component (C) may be a bisphenol epoxy resin such as a bisphenol A epoxy resin or a bisphenol F epoxy resin, or a glycidyl ether-terminated epoxy resin formed by the reaction of an aliphatic alcohol or polyol with epichlorohydrin. In addition, it is preferable that the epoxy equivalent is 160 to 400 g / eq, the number average molecular weight is 340 to 800, and the viscosity at 50°C is 100 mPa·s or more and 10,000 mPa·s or less. In addition, the viscosity can be measured by the "Viscosity measurement method using a cone-plate type rotational viscometer" in JIS Z8803 (2011). As component (C), bisphenol type epoxy compounds are preferred, and bisphenol A type epoxy resins and bisphenol F type resins are more preferred because they are versatile. As the aliphatic epoxy compound, commercially available products such as EPIOL G-100 (manufactured by NOF Corp.) as a glycerin triglycidyl ether, and Denacol, EX-612, EX-614, and EX-622 (all manufactured by Nagase ChemteX Corp.) as a sorbitol polyglycidyl ether can be used.
[0067] In one aspect of the present invention, the content of component (A) is preferably 10 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the total of components (A), (B) and (C). When the amount of component (A) contained in the total of 100 parts by mass of components (A), (B) and (C) is 10 parts by mass or more, impregnation of the matrix resin into the carbon fiber bundle of the present invention is good, and at the same time, when the carbon fiber bundle is used as a reinforcing fiber of a composite material, the mechanical properties of the composite material are good. When the amount of component (A) is 60 parts by mass or less, the handleability of the carbon fiber bundle in processing steps such as FW molding is good. A range of 15 parts by mass or more and 40 parts by mass or less is more preferable.
[0068] In another aspect of the present invention, the content of component (A) is preferably 10 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total of components (A), (B) and (C). When the content of component (A) is 10 parts by mass or more, impregnation of the matrix resin into the sizing-agent-adhered carbon fiber bundle of the present invention is good, and at the same time, when the carbon fiber bundle is used as a reinforcing fiber of a composite material, the sizing-agent-adhered carbon fiber bundle has good mechanical properties. When the content of the component (A) is 90 parts by mass or less, the handleability of the carbon fiber bundle in processing steps such as FW molding is good. The content of component (A) is more preferably from 40 parts by mass to 80 parts by mass.
[0069] In one aspect of the present invention, the content of component (B) is preferably 15 parts by mass or more and 55 parts by mass or less per 100 parts by mass of the total of components (A), (B) and (C). When the amount of component (B) contained in the total of 100 parts by mass of components (A), (B) and (C) is 15 parts by mass or more, the carbon fiber bundle of the present invention can be easily handled in processing steps such as FW molding. When the amount is 55 parts by mass or less, the carbon fiber bundle can be easily impregnated with the matrix resin. A range of 20 parts by mass or more and 45 parts by mass or less is more preferable.
[0070] In another aspect of the present invention, the content of component (B) is preferably 2 parts by mass or more and 70 parts by mass or less per 100 parts by mass of the total of components (A), (B) and (C). When the content of component (B) is 2 parts by mass or more, the carbon fiber bundle of the present invention has good handleability in processing steps such as FW molding. When the content of component (B) is 70 parts by mass or less, the impregnation of the matrix resin into the carbon fiber bundles having the sizing agent attached thereto is excellent. The content of component (B) is more preferably from 10 parts by mass to 40 parts by mass.
[0071] In one aspect of the present invention, the content of component (C) is preferably 20 parts by mass or more and 75 parts by mass or less per 100 parts by mass of the total of components (A), (B) and (C). When the amount of component (C) contained in the total of 100 parts by mass of components (A), (B) and (C) is 20 parts by mass or more, the impregnation of the matrix resin into the carbon fiber bundle of the present invention is good, and when it is 75 parts by mass or less, the handleability of the carbon fiber bundle in processing steps such as FW molding is good. 40 parts by mass or more and 60 parts by mass or less are more preferable.
[0072] In another aspect of the present invention, the content of component (C) is preferably 2 parts by mass or more and 70 parts by mass or less per 100 parts by mass of the total of components (A), (B) and (C). When the content of component (C) is 2 parts by mass or more, the impregnation of the matrix resin into the carbon fiber bundle having the sizing agent of the present invention is favorable. If the content of component (C) is 70 parts by mass or less, the handleability of the carbon fiber bundle in processing steps such as FW molding will be good. The content of component (C) is more preferably from 10 parts by mass to 30 parts by mass.
[0073] The sizing agent for carbon fibers of the present invention may contain an aliphatic ester as component (D) in addition to components (A), (B) and (C). The content of the component (D) is preferably 5% by mass or more and 20% by mass or less based on the total mass of the sizing agent for carbon fiber. By containing the component (D), the handleability of the sizing agent-attached carbon fiber bundle during processing can be improved.
[0074] Component (D) is not particularly limited as long as it is an aliphatic carboxylate ester, but is preferably an aliphatic ester obtained by dehydration condensation of an aliphatic monocarboxylic acid having 8 to 21 carbon atoms and an aliphatic alcohol. Specific examples include the Exsepar series (Kao Corporation). More specific examples include Exsepar EH-S and Exsepar SS (both product names of Kao Corporation).
[0075] The sizing agent of the present invention may further contain a surfactant such as a nonionic surfactant or an anionic surfactant as component (E). Component (E) contained in the sizing agent for carbon fiber of the present invention is used for dispersing the above-mentioned components (A), (B), and (C), the optional component (D), and other components in water. One type of surfactant may be used alone, or two or more types may be used in combination.
[0076] In order to apply a carbon fiber sizing agent to carbon fibers, the carbon fiber sizing agent can be dispersed in water or an organic solvent having low solubility and used, or the sizing agent can be dissolved in an organic solvent having high solubility and used. The use of the compound dispersed in water is easier to handle and is superior to the use of the compound dissolved in an organic solvent. An example of an organic solvent with low solubility is ethanol. An example of an organic solvent having high solubility is acetone.
[0077] The content of the component (E) can be appropriately determined taking into consideration the stability of the aqueous dispersion in which the sizing agent for carbon fiber is dispersed in water. The content of the component (E) is preferably from 5 to 30 mass %, and more preferably from 10 to 25 mass %, based on the total mass of the sizing agent for carbon fiber. If the content is 5% by mass or more, the stability of the aqueous dispersion of the sizing agent is good, and if the content is 30% by mass or less, the effect of the sizing agent is well exhibited.
[0078] Examples of the nonionic surfactant include aliphatic nonionic surfactants such as ethylene oxide adducts of higher alcohols, ethylene oxide adducts of fatty acids, ethylene oxide adducts of polyhydric alcohol fatty acid esters, fatty acid esters of glycerol, fatty acid esters of sorbitol and sorbitan, and fatty acid esters of pentaerythritol. Examples of the phenolic nonionic surfactant include alkylphenolic nonionic surfactants and polycyclic phenolic nonionic surfactants. Block polymers of ethylene oxide and propylene oxide (so-called Pluronic type) are preferably used.
[0079] As the anionic surfactant, a compound having an ammonium ion as a counter ion and an alkylene oxide added thereto, and having a phenol group as a hydrophobic group, is preferred. As the anionic surfactant, surfactants such as carboxylates, sulfates, sulfonates, and phosphates can be used, among which sulfates are preferred.
[0080] As the anionic surfactant, one having a structure represented by the following formula (5) is preferably used.
[0081] [ka]
[0082] [In the formula, R5 and R6 each independently represent a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. r represents an integer of 5 to 25.]
[0083] <Aqueous dispersion of sizing agent for carbon fiber> The aqueous dispersion of the sizing agent for carbon fiber of the present invention contains the sizing agent for carbon fiber of the present invention and water. In addition to these, it may contain other components. The other components contained in the aqueous dispersion for sizing carbon fiber of the present invention are blended within a range that does not impair the function exerted by the sizing agent for carbon fiber of the present invention, and examples thereof include (poly)ester compounds, (poly)urethane compounds, (poly)amide compounds, and (poly)imide compounds.
[0084] The aqueous dispersion of the sizing agent for carbon fibers of the present invention can be prepared by mixing the sizing agent for carbon fibers and the surfactant to obtain a homogeneous mixture, and gradually adding water with stirring to effect phase inversion emulsification. In this specification, the term "dispersion" refers to a state in which the sizing agent is in the form of particles or micelles of about 1 nm to 10 μm suspended in a dispersion medium such as water or an organic solvent, forming a suspension.
[0085] The sizing treatment of adhering the carbon fiber sizing agent of the present invention to the surface of carbon fiber can be carried out by applying the sizing agent to the carbon fiber by a method of immersing the carbon fiber in a sizing agent solution for carbon fiber or a dispersion of the sizing agent for carbon fiber via a roller, a method of contacting the carbon fiber with a roller to which the sizing agent solution for carbon fiber or the dispersion of the sizing agent for carbon fiber is attached, or the like, and then drying the carbon fiber. The amount of the sizing agent attached to the surface of the carbon fiber can be adjusted by adjusting the concentration or the amount of squeezing of the sizing agent solution for carbon fiber or the dispersion of the sizing agent for carbon fiber. Drying can be carried out by using hot air, a hot plate, a heated roller, various infrared heaters, or the like.
[0086] In addition, the sizing agent concentration in the aqueous dispersion of the sizing agent for carbon fiber of the present invention, i.e., the concentration of components other than volatile components (such as water that is dried and removed in the sizing treatment) in the aqueous dispersion of the sizing agent for carbon fiber, is usually adjusted to a concentration of about 10 to 50 mass%. The concentration may be less than 10 mass% at the preparation stage of the aqueous dispersion of the sizing agent for carbon fiber, but the proportion of water in the aqueous dispersion of the sizing agent for carbon fiber increases, which may be uneconomical in terms of transportation and storage from the preparation of the aqueous dispersion of the sizing agent for carbon fiber to its use (sizing treatment of carbon fiber). Therefore, when using the aqueous dispersion of the sizing agent for carbon fiber (sizing treatment of carbon fiber), the aqueous dispersion of the sizing agent for carbon fiber is diluted to a concentration of 0.1 to 10 mass% relative to the total mass of the aqueous dispersion of the sizing agent for carbon fiber so as to obtain a desired amount of sizing agent attached.
[0087] <Carbon fiber with sizing agent> The sizing-agent-adhered carbon fiber of the present invention has the sizing agent for carbon fiber of the present invention adhered to the surface of the carbon fiber. The adhesion of the sizing agent for carbon fiber of the present invention improves the handleability of the carbon fiber bundle in processing steps such as impregnation of the carbon fiber bundle with a matrix resin and FW molding. The amount of the sizing agent for carbon fibers applied is preferably 0.1 to 5.0 mass %, more preferably 0.2 to 3.0 mass %, based on the total mass of the carbon fibers with the sizing agent applied thereto.
[0088] The carbon fiber to which the carbon fiber sizing agent of the present invention is applied may be obtained from any raw material such as pitch, rayon, or polyacrylonitrile, and may be any of high strength type (low elastic modulus carbon fiber), medium-high elasticity carbon fiber, and ultra-high elasticity carbon fiber.
[0089] <Carbon fiber bundle with sizing agent> The sizing-adhered carbon fiber bundle of the present invention comprises carbon fibers and a sizing agent for carbon fibers, and is a carbon fiber bundle bundle bundled with the sizing agent, and has a spontaneous dispersion ratio of 3 or more as measured by a spontaneous dispersion test.
[0090] (Spontaneous Dispersibility Test Method) The spontaneous dispersibility test is carried out by the following method. The carbon fiber bundle is cut in the longitudinal direction of the fibers to a length of 2.5 cm to prepare a test specimen. At this time, in order to cut without disturbing the shape of the carbon fiber bundle, the carbon fiber bundle pulled out 30 cm from the bobbin is placed on a cutting mat without twisting or disturbance, and then cut with a razor while maintaining its shape. The width of the specimen is measured at both ends and at the center in the fiber length direction, and the average width W0 is calculated. Bisphenol A type epoxy resin (viscosity at 25°C: 11 to 15 Pa·s) kept at a temperature of 44 to 46°C is used as the evaluation liquid for the spontaneous dispersibility test. The evaluation liquid for the spontaneous dispersibility test is placed in a petri dish and kept at a temperature in the range of 44 to 46°C in the absence of convection. The test specimen is floated on the spontaneous dispersibility test evaluation liquid, and this time is set as 0 seconds. After 60 seconds, the widths of both ends and the center of the test specimen in the longitudinal direction are measured, and the average width W is calculated. The increase rate (average width W / average width W0) of the average width of the test specimen during the measurement period (60 seconds) is regarded as the spontaneous dispersion rate of each test specimen. A spontaneous dispersibility test is carried out on 20 specimens taken from the same carbon fiber bundle, and the average spontaneous dispersibility rate of each specimen is regarded as the spontaneous dispersibility rate of the carbon fiber bundle. Since the spontaneous dispersibility test causes the sizing agent to dissolve in the test solution, a new test solution must be used for each measurement of the spontaneous dispersibility test.
[0091] The evaluation liquid for the spontaneous dispersibility test needs to be liquid in the range of 44 to 46°C. Therefore, a bisphenol A type epoxy resin with a viscosity of 11 to 15 Pa·s at 25°C can stably maintain a liquid state in the range of 44 to 46°C. Commercially available bisphenol A type epoxy resins with the above-mentioned viscosity characteristics include jER828 (manufactured by Mitsubishi Chemical Corporation), EPICLON 850S (manufactured by DIC Corporation), ADEKA RESIN EP-4100 (manufactured by ADEKA Corporation), etc.
[0092] The sizing-agent-attached carbon fiber bundle is preferably made of the sizing-agent-attached carbon fiber of the present invention.
[0093] If a liquid other than bisphenol A type epoxy resin (viscosity at 25°C: 11 to 15 Pa·s) is used as the liquid for evaluating spontaneous dispersibility, the measurement results will differ.
[0094] The carbon fiber bundle of the present invention is characterized in that each filament of the carbon fiber bundle spontaneously disperses without the application of an external force due to the interaction with the matrix resin composition. The sizing agent that can be used for the carbon fiber bundle of the present invention is characterized in that it has excellent wettability with the matrix resin composition, dissolves quickly in the matrix resin composition, and has a surface free energy of a solution in which the sizing agent is dissolved in the matrix resin composition that is lower than the surface free energy of the matrix resin composition alone. Here, the surface free energy of the liquid can be measured by the Wilhelmy method, etc. The wettability can be measured by the dynamic contact angle between the carbon fiber filament to which the sizing agent is attached and the matrix resin composition.
[0095] The spontaneous dispersion of carbon fiber bundles in the spontaneous dispersion test is understood as the following phenomenon. First, when a carbon fiber bundle is floated in the evaluation liquid, the sizing agent attached to the carbon fiber filaments dissolves in the evaluation liquid. As the sizing agent dissolves in the evaluation liquid, the amount of sizing agent that was binding the carbon fiber bundle decreases, and the binding force between the carbon fiber filaments decreases. Immediately after a carbon fiber bundle (specimen) is floated in the evaluation liquid and the sizing agent attached to the carbon fiber bundle dissolves in the evaluation liquid, an "evaluation liquid in which the sizing agent is dissolved at a high concentration" is present near the carbon fiber bundle.
[0096] This "evaluation liquid in which the sizing agent is dissolved at a high concentration" has a lower surface free energy than the evaluation liquid (in which the sizing agent is not dissolved) that is separated from the test specimen.
[0097] If we focus on the carbon fiber filaments located at the edge of the test specimen, the concentration of sizing agent in the evaluation liquid on the carbon fiber bundle side is high, while the concentration of sizing agent on the opposite side (outside the carbon fiber bundle) is low, so a force acts in the direction of spreading the carbon fiber bundle.
[0098] When the force spreading the carbon fiber bundle exceeds the binding force between the filaments of the carbon fiber bundle, the group of carbon fiber filaments in contact with the evaluation liquid spreads in the width direction.
[0099] The diffusion of the sizing agent dissolved in the evaluation liquid into the evaluation liquid acts in the direction of eliminating the concentration difference, but as the carbon fiber filaments in contact with the evaluation liquid expand in the width direction, carbon fiber filaments that were inside the thickness direction of the carbon fiber bundle and had not previously been in contact with the evaluation liquid come into contact with the evaluation liquid, and the sizing agent dissolves in the evaluation liquid from the filaments that have newly come into contact with the evaluation liquid, increasing the concentration of the sizing agent in the evaluation liquid, maintaining the concentration difference, and the width of the carbon fiber bundle continues to expand above the evaluation liquid.
[0100] The sizing-adhered carbon fiber bundle of the present invention is characterized in that the opening ratio A measured by the following method is 150% or less. The opening ratio A of 150% or less provides excellent handleability in processing steps such as filament winding molding. In the processing step, excessive opening of the carbon fiber bundle on the rollers or guides for transporting the carbon fiber bundle is suppressed, which suppresses the occurrence of fluctuations in tow width during the processing step due to breakage of the ends of the carbon fiber bundle, facilitating uniform processing and providing excellent handleability, which is preferable. In addition, the opening ratio A is preferably 110% or more. If the opening ratio A is 110% or less, the binding force between the filaments in the carbon fiber bundle by the sizing agent is strong, and it may be difficult to impregnate the carbon fiber bundle with a matrix resin.
[0101] The opening ratio A described in the present invention is defined by the following formula. {(Tow width when spread) / (Tow width on bobbin)}×100(%) The "tow width on the bobbin" is measured by placing a ruler on three points, excluding the folded-back parts of the traverse and any parts showing visible changes in appearance, and is obtained as the average value. Furthermore, the "tow width when spread" is obtained by the following method. As shown in Figure 1, a device 10 for measuring the spread rate A is used. The carbon fiber bundle is unwound from a carbon fiber bundle (bobbin 1) wound cylindrically on a paper tube with a traverse, and is guided via rollers to a spreading device consisting of three spreading bars 2 (steel cylinder, diameter 10 mm, hard chrome plating, Vickers hardness 1000, surface roughness Ra: 0.8 μm), and spread by contacting each spreading bar at a wrap angle of 60°. This carbon fiber bundle is transported by a driving roller 3 while maintaining the spread tow width, and the tow width is measured non-contact with a laser-type length measuring sensor 4 under a tension of 1.0 cN / tex. The unwinding tension is 0.30 cN / tex, and the running speed of the carbon fiber bundle is 10 m / min. The output of the laser length measuring sensor is captured once every 100 ms, and the average value for 10 minutes is defined as the "tow width at the time of spreading."
[0102] In addition, the carbon fiber bundle with a sizing agent of the present invention preferably contains the sizing agent for carbon fiber of the present invention. The carbon fiber bundle with a sizing agent for carbon fiber of the present invention has good handleability in processing steps such as FW molding due to the carbon fiber sizing agent of the present invention being applied, and the carbon fiber bundle is impregnated with resin well. In addition, the mechanical properties of a carbon fiber composite material molded product produced using the carbon fiber bundle with a sizing agent for carbon fiber of the present invention is good. In the present invention, the term "carbon fiber bundle with a sizing agent attached" refers to a carbon fiber bundle in which the sizing agent is dispersed and held throughout the interior and surface of the carbon fiber bundle, in a form in which the sizing agent covers at least a portion of the surface of each carbon fiber constituting the carbon fiber bundle or in a form in which the sizing agent connects the gaps between the carbon fibers.
[0103] In particular, when the sizing agent for carbon fiber of the present invention contains component (D), the carbon fiber bundle having the sizing agent thereon has excellent abrasion resistance and is easy to handle in the processing step.
[0104] The carbon fiber bundle containing the carbon fiber sizing agent of the present invention and having the sizing agent attached thereto has excellent abrasion resistance against mechanical friction and has little fuzz, and therefore is easy to handle in processing steps such as weaving, and can provide a fiber base material such as a woven fabric or a multiaxial warp knit with little fuzz.
[0105] Furthermore, the carbon fiber bundles coated with a sizing agent containing the carbon fiber sizing agent of the present invention have excellent abrasion resistance against mechanical friction, are less likely to fluff, and are well impregnated with a matrix resin into the carbon fiber bundles. Therefore, even when the carbon fiber bundles are passed through rollers or guides in processes such as filament winding molding and pultrusion molding, no fluff or winding around rollers occurs, and the carbon fiber bundles can be easily impregnated with a matrix resin in a short time, so that the excellent productivity of these molding methods is not impaired.
[0106] The sizing-agent-adhered carbon fiber bundle containing the carbon fiber sizing agent of the present invention can be impregnated with a matrix resin composition to be processed into a carbon fiber composite material in the form of an intermediate material such as a unidirectional prepreg, cross prepreg, towpreg, short fiber sheet prepreg, short fiber mat prepreg, etc. The matrix resin composition is not particularly limited, but examples thereof include epoxy resins, acrylic resins, which are radical polymerization resins, vinyl ester resins, unsaturated polyester resins, thermoplastic acrylic resins, and further phenolic resins.
[0107] <Carbon fiber composite material> The carbon fiber composite material of the present invention is a carbon fiber composite material formed using carbon fibers coated with a sizing agent containing the carbon fiber sizing agent of the present invention, and radical polymerization resins such as epoxy resins, acrylic resins, unsaturated polyester resins, and vinyl ester resins, and phenolic resins can be used as the matrix resin. A carbon fiber composite material molded article can be obtained by molding the carbon fiber composite material.
[0108] <Method of manufacturing carbon fiber composite material> The method for producing a carbon fiber composite material of the present invention includes impregnating the sizing-agent-attached carbon fiber bundle of the present invention with a thermosetting resin composition, and then heat-curing the thermosetting resin composition. The proportion of the thermosetting resin composition is preferably 30 to 70 parts by mass, more preferably 40 to 60 parts by mass, per 100 parts by mass of the sizing agent-attached carbon fiber bundles. The heating conditions for heat curing the thermosetting resin composition are preferably 60 to 200° C., and more preferably 130 to 180° C. Furthermore, heating at the above temperature is preferably performed for 1 to 200 minutes, and more preferably 15 to 60 minutes.
[0109] <Manufacturing method of carbon fiber reinforced pressure vessel> The method for producing a carbon fiber reinforced pressure vessel of the present invention includes impregnating the sizing agent-applied carbon fiber bundle of the present invention with a thermosetting resin composition by a filament winding method, and then heat curing the thermosetting resin composition. In the filament winding method, the proportion of the thermosetting resin composition is preferably 30 to 70 parts by mass, and more preferably 40 to 60 parts by mass, per 100 parts by mass of the sizing agent-attached carbon fiber bundle. In the filament winding method, the heating conditions for heat-curing the thermosetting resin composition are preferably 60 to 200° C., and more preferably 130 to 180° C. Furthermore, heating at the above temperature is preferably performed for 30 to 200 minutes, and more preferably 60 to 150 minutes. EXAMPLES
[0110] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these in any way.
[0111] Tables 1 and 2 show the raw materials used in the examples and comparative examples.
[0112] [Table 1]
[0113] [Table 2]
[0114] Since the raw material composition A shown in Table 2 contains liquid bisphenol A type epoxy resin or bisphenol F type epoxy resin (both are component (C)) in addition to component (A), the content of component (A) is also shown. <Preparation of Preparation Composition 1> Preparation composition 1 was obtained by repeatedly extracting ADEKA RESIN EPU-73B shown in Table 2 with toluene and methanol. Table 3 shows the raw materials used in the reference examples.
[0115] [Table 3]
[0116] [Example 1-1] <Preparation of aqueous dispersion of sizing agent for carbon fiber> Ion-exchanged water was added to a sizing agent for carbon fiber prepared by mixing the A raw material composition and the components (B) to (E) shown in Tables 1 and 2 in the parts by mass shown in Table 4, and an aqueous dispersion of the sizing agent for carbon fiber was obtained by phase inversion emulsification using a homomixer. The concentration of the sizing agent in the aqueous dispersion was adjusted to 40% by mass.
[0117] Table 7 also lists the blending ratios of component (A), component (B), and component (C) in the sizing agent for carbon fiber obtained by mixing the raw materials in the parts by mass listed in Table 4. Note that this blending ratio is the parts by mass of each component relative to 100 parts by mass of the total of component (A), component (B), and component (C).
[0118] <Measurement of sizing agent concentration in aqueous dispersion> Approximately 2 g of the aqueous dispersion of the sizing agent was weighed into an aluminum petri dish (diameter 45 mm, depth 10 mm) and dried for 1 hour in a hot air dryer at 105°C, after which the components remaining in the petri dish were weighed. The mass of the aqueous dispersion of the sizing agent was designated W1, and the mass of the components remaining after drying was designated W2, and the concentration of the sizing agent in the aqueous dispersion was calculated using the following formula. Sizing agent concentration in aqueous dispersion of sizing agent (%) = {W2 / W1} x 100
[0119] <Carbon fiber sizing treatment> Carbon fiber bundle Pyrofil TRH50 18M (trade name, manufactured by Mitsubishi Chemical Corporation; number of filaments: 18,000, fiber diameter: 6 μm) to which no sizing agent was applied was immersed and passed through an immersion tank filled with an aqueous dispersion of a sizing agent, and then dried for 10 minutes in an atmosphere of 140° C., and then wound on a bobbin. At this time, the aqueous dispersion of the sizing agent adjusted to 40% by mass was diluted and used so that the concentration of the sizing agent in the aqueous dispersion of the sizing agent in the immersion tank was about 2.2% by mass.
[0120] <Measurement of the amount of sizing agent attached to carbon fiber bundle> The amount of sizing agent attached to the carbon fiber bundle after applying the sizing agent was measured by the Soxhlet extraction method using methyl ethyl ketone. The extraction time was 1 hour.
[0121] <Spontaneous dispersibility test> The spontaneous dispersibility was evaluated by the above-mentioned method, except that jER828 (manufactured by Mitsubishi Chemical Corporation) was used as the evaluation liquid.
[0122] <Pressure vessel construction and burst pressure measurement> The carbon fiber bundle to which the sizing agent was applied was wound around an aluminum liner (total length 540 mm, body length 415 mm, body outer diameter 163 mm, wall thickness at the center of the body 3 mm) with a capacity of 9 liters using a FW device. The aluminum liner used was made of a material obtained by heat-treating an aluminum material specified in A6061-T6 of JIS H 4040. The carbon fiber bundle was wound around a paper tube and the position was adjusted via a guide roll, and then a matrix resin composition was supplied to the carbon fiber bundle using a touch roll to be impregnated, and then the bundle was wound around the liner as follows. First, a hoop layer was formed on the body as the first layer in contact with the body of the liner, at an angle of 88.6° with respect to the direction of the rotation axis of the liner. Then, a helical layer was laminated at an angle of 11.0° with respect to the direction of the rotation axis of the liner to reinforce the mirror part of the liner, and thereafter, the layers described in Laminate Nos. 3 to 8 shown in Table 16 were formed in order to produce a container intermediate.
[0123] The obtained intermediate container was removed from the FW device and hung in a heating furnace. The temperature inside the furnace was raised to 135°C at 2°C / min, and then held at 135°C for 2 hours to harden. The temperature inside the furnace was then cooled to 60°C at 1°C / min to obtain a composite material reinforced pressure vessel. The evaluation results of the tank performance of the composite material reinforced pressure vessel (measurement results of burst pressure: tank burst unit (MPa)) are shown in Table 4. The matrix resin composition used was one in which 80 parts by mass of XN1045 was added to 100 parts by mass of jER828.
[0124] <Evaluation of resin impregnation state in the production of pressure vessels> The absorption of the matrix resin composition on the touch roll during the production of the pressure vessel and the voids in the cross section of the produced pressure vessel were observed and evaluated according to the following criteria. The results are shown in Table 7. ⊚: The matrix resin composition is well absorbed onto the touch roll, and almost no voids are observed in the cross section of the pressure vessel. ◯: The matrix resin composition is absorbed rather slowly onto the touch roll, but almost no voids are observed in the cross section of the pressure vessel. Δ: Absorption of the matrix resin composition onto the touch roll was rather slow, and voids were partially observed in the cross section of the pressure vessel. ×: The matrix resin composition is absorbed slowly onto the touch roll, and voids are observed in the cross section of the pressure vessel.
[0125] <Evaluation of processability of carbon fiber bundles in the manufacturing process of pressure vessels> The processability during the manufacture of the above pressure vessel was evaluated according to the following criteria, and the results are shown in Table 7. ⊚: Almost no accumulation of fuzz on the guide roll is observed. ◯: A small amount of fuzz has accumulated on the guide roll. Δ: A large amount of fuzz has accumulated on the guide roll, but no wrapping around the guide roll is observed. ×: A very large amount of fuzz accumulates on the guide roll, causing wrapping around the guide roll.
[0126] <Evaluation of fiber opening rate A> As shown in Figure 1, a device 10 for measuring the spread rate A was used. The carbon fiber bundle was unwound from a carbon fiber bundle (bobbin 1) that was wound cylindrically by adding a traverse onto a paper tube, and was introduced via rollers to a spreading device consisting of three spreading bars 2 (steel cylinder, diameter 10 mm, hard chrome plating, Vickers hardness 1000, surface roughness Ra: 0.8 μm), and was brought into contact with each spreading bar at a wrap angle of 60° for spreading processing. This carbon fiber bundle was transported by a driving roller 3 via rollers while maintaining the spread tow width, and the tow width was measured non-contact with a laser-type length measuring sensor 4 under a tension of 1.0 cN / tex. The unwinding tension was 0.30 cN / tex, and the running speed of the carbon fiber bundle was 10 m / min. The output of the laser length measuring sensor was captured once every 100 ms, and the average value for 10 minutes was taken as the "tow width at the time of spreading." The fiber opening rate A was calculated from the following formula. Spread rate A = {(tow width when spread) / (tow width on bobbin)} x 100 (%) The "tow width on the bobbin" in the above formula was measured with a ruler at three points excluding the folded parts of the traverse and any parts showing visible changes, and the average value was obtained.
[0127] <Evaluation of resin impregnation> The resin adhesion rate was measured and the resin impregnation property was evaluated by the following method. Using a FW device, resin was supplied to the carbon fiber bundle to which the sizing agent had been applied using a touch roller, and an aluminum liner (total length 540 mm, body length 415 mm, body outer diameter 163 mm, thickness at the center of the body 3 mm) was wound around it as a mandrel. The touch roller had a diameter of 200 mm, and the bottom 10 mm of the touch roller was immersed in the resin bath. A metal blade was attached to the touch roller, and the clearance between the roller and the blade was 0.1 mm. JER828 was used as the resin, and the temperature of the resin was set to 35°C by immersing the resin bath in warm water. The carbon fiber bundle with the sizing agent attached was brought into contact with the touch roller at a wrap angle of 50°. The tow width on the roll exit side just before the touch roller was adjusted to 5.5 x 10 mm with a metal guide of diameter 10 mm. -3 The tension of the carbon fiber bundle just before it contacted the touch roller was 1.2 cN / tex, and the winding speed was 10 / min.
[0128] As shown in Table 7, in Example 1-1, the processability in the pressure vessel production process was slightly poor, but the resin impregnation state was good, and the performance of the obtained pressure vessel was also good.
[0129] [Examples 2-1 to 24-1] A carbon fiber bundle subjected to a sizing treatment was obtained in the same manner as in Example 1-1, except that the raw material composition A shown in Tables 1 and 2 and the components (B) to (E) were mixed in the parts by mass shown in Tables 4 to 6. The obtained carbon fiber bundle was used to carry out the same evaluations as in Example 1-1. The results are shown in Tables 7 to 9. Tables 7 to 9 also show the blending ratios of component (A), component (B), and component (C) in the sizing agents for carbon fiber obtained by mixing the raw materials in the parts by mass shown in Tables 4 to 6. Note that these blending ratios are the parts by mass of each component relative to 100 parts by mass of the total of component (A), component (B), and component (C).
[0130] [Example 25-1] The same evaluation as in Example 1-1 was carried out using a carbon fiber bundle that had been sized in the same manner as in Example 2-1, except that PYROFIL TRH50 18M was replaced with PYROFIL TRH50 60M (product name: manufactured by Mitsubishi Chemical Corporation; filament count 60,000, fiber diameter 6 μm). The results are shown in Table 9.
[0131] [Example 26-1] The same evaluation as in Example 1-1 was carried out using a carbon fiber bundle that had been sized in the same manner as in Example 2-1, except that PYROFIL TRH50 18M was replaced with PYROFIL TR50D 12L (product name: manufactured by Mitsubishi Chemical Corporation; filament count 12000, fiber diameter 7 μm). The results are shown in Table 9.
[0132] [Comparative Examples 1-1 to 5-1] A carbon fiber bundle subjected to a sizing treatment was obtained in the same manner as in Example 1-1, except that the A raw material composition shown in Tables 1 and 2 and the components (B) to (E) were mixed in the parts by mass shown in Table 10. The obtained carbon fiber bundle was used to carry out the same evaluation as in Example 1-1. The results are shown in Table 11. Table 11 also shows the blending ratios of component (A), component (B), and component (C) in the sizing agent for carbon fiber obtained by mixing the raw materials in the parts by mass shown in Table 10. Note that this blending ratio is the parts by mass of each component relative to 100 parts by mass of the total of component (A), component (B), and component (C).
[0133] [Reference examples 1-1, 2-1] A carbon fiber bundle was obtained by sizing treatment in the same manner as in Example 1-1 except that the blending amounts shown in Table 12 were used, and the same evaluation was carried out using the obtained carbon fiber bundle. The resin impregnation state in the pressure vessel production process was poor and unsatisfactory. The process passability and the performance of the obtained pressure vessel were good. The results are shown in Table 12.
[0134] [Table 4]
[0135] [Table 5]
[0136] [Table 6]
[0137] [Table 7]
[0138] [Table 8]
[0139] [Table 9]
[0140] [Table 10]
[0141] [Table 11]
[0142] [Table 12]
[0143] Table 13 shows the raw materials used in Examples 1-2 to 10-2 and Comparative Examples 1-2 to 6-2.
[0144] [Table 13]
[0145] <Production Example of Ester A1> A bisphenol A-EO 80 mole adduct (80 moles of EO (ethylene oxide) added per mole of bisphenol A) was prepared by the following procedure. 228 parts by mass of bisphenol A, 1000 parts by mass of toluene, and 3 parts by mass of potassium hydroxide were charged into a pressure-resistant reactor, and 3520 parts by mass of EO were charged over 3 hours under conditions of 100°C and -0.1 MPa while adjusting the pressure so as not to exceed 0.5 MPa. After aging at 120°C for 1 hour, the pressure was reduced to -0.1 MPa, and toluene was distilled off. Thus, 3700 parts by mass of bisphenol A-EO 80 mole adduct was obtained.
[0146] 1580 parts by mass of bisphenol A EO adduct ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hereinafter abbreviated as "BPE-20") in which 2 moles of EO were added to 1 mole of bisphenol A, 996 parts by mass of terephthalic acid (alcohol / acid=5 / 6 molar ratio) and 2 parts by mass of tetraisopropoxy titanate were reacted in a reaction vessel under nitrogen flow at 170°C for 10 hours while distilling off water. 1590 parts by mass of the bisphenol A-EO 80 mole adduct was further added thereto, and the mixture was reacted for 10 hours at 180°C under reduced pressure to -0.1 MPa while distilling off water, to obtain 3900 parts by mass of ester A1.
[0147] <Production Example of Ester A2> A bisphenol A-40 mole EO adduct (40 moles of EO added per mole of bisphenol A) was prepared by the following procedure. 228 parts by mass of bisphenol A, 400 parts by mass of toluene, and 2 parts by mass of potassium hydroxide were charged into a pressure-resistant reactor, and 1760 parts by mass of EO were charged over 3 hours under conditions of 100°C and -0.1 MPa while adjusting the pressure so as not to exceed 0.5 MPa. After aging at 120°C for 1 hour, the pressure was reduced to -0.1 MPa, and toluene was distilled off. Thus, 1980 parts of bisphenol A-EO 40 mole adduct was obtained.
[0148] A mixture of 1264 parts by mass of BPE-20, 830 parts by mass of terephthalic acid (alcohol / acid=4 / 5 molar ratio), and 2 parts by mass of tetraisopropoxy titanate was reacted in a reaction vessel for 10 hours under nitrogen flow at 170° C. while distilling off water. 1928 parts by mass of the bisphenol A-EO 40 mole adduct was further added thereto, and the pressure was reduced to −0.1 MPa at 180° C., and the reaction was continued for 10 hours while distilling off water, to obtain 3800 parts by mass of ester A2.
[0149] [Example 1-2] <Preparation of aqueous dispersion of sizing agent for carbon fiber> The components (A) to (E) shown in Table 13 were mixed in the ratio (parts by mass) shown in the column of Example 1-2 in Table 14 to obtain a sizing agent for carbon fiber. Ion-exchanged water was added to the obtained sizing agent for carbon fiber, and an aqueous dispersion of the sizing agent for carbon fiber was obtained by phase inversion emulsification using a homomixer. The concentration of the sizing agent in the aqueous dispersion was adjusted to 30% by mass.
[0150] <Measurement of sizing agent concentration in aqueous dispersion> Approximately 2 g of the aqueous dispersion of the sizing agent was weighed into an aluminum petri dish (diameter 45 mm, depth 10 mm) and dried for 1 hour in a hot air dryer at 105°C, after which the components remaining in the petri dish were weighed. The mass of the aqueous dispersion of the sizing agent was designated W1, and the mass of the components remaining after drying was designated W2, and the concentration of the sizing agent in the aqueous dispersion was calculated using the following formula. Sizing agent concentration in aqueous dispersion of sizing agent (mass%) = {W2 / W1} x 100
[0151] <Carbon fiber sizing treatment> Carbon fiber bundle Pyrofil TRH50 30M (trade name, manufactured by Mitsubishi Chemical Corporation; filament count 30,000, fiber diameter 6 μm) to which no sizing agent was applied was immersed and passed through an immersion tank filled with an aqueous dispersion of a sizing agent, and then dried for 10 minutes in an atmosphere of 140° C., and then wound on a bobbin. At this time, the aqueous dispersion of the sizing agent adjusted to 30% by mass was diluted and used so that the concentration of the sizing agent in the aqueous dispersion of the sizing agent in the immersion tank was about 2.2% by mass.
[0152] <Measurement of the amount of sizing agent attached to carbon fiber bundle> The amount (mass%) of the carbon fiber sizing agent attached to the total mass of the carbon fiber with the sizing agent attached was measured by the Soxhlet extraction method using methyl ethyl ketone. The extraction time was 1 hour.
[0153] <Evaluation of resin impregnation> The resin adhesion rate was measured and the resin impregnation property was evaluated by the following method. Using a FW device, resin was supplied to the carbon fiber bundle to which the sizing agent had been applied using a touch roller, and an aluminum liner (total length 540 mm, body length 415 mm, body outer diameter 163 mm, thickness at the center of the body 3 mm) was wound around it as a mandrel. The touch roller was φ200 mm, and the bottom 10 mm of the touch roller was immersed in the resin bath. A metal blade was installed on the touch roller, and the clearance between the roller and the blade was 0.1 mm. jER828 was used as the resin, and the temperature of the resin was set to 35°C by immersing the resin bath in warm water. The carbon fiber bundle with the sizing agent attached was brought into contact with the touch roller at a wrap angle of 50°. In addition, the tow width on the roll exit side just before the touch roller was regulated to 9 mm with a φ10 metal guide. The tension of the carbon fiber bundle just before contacting the touch roller was 2 kgf, and the winding speed was 10 / min. The carbon fiber bundle wound around the mandrel was unwound and cut into five 1 m pieces, the mass of each was measured, and the average of the masses of the five pieces was taken as the "mass per unit length of the carbon fiber bundle after resin supply." Resin adhesion rate (%) = {(mass per unit length of carbon fiber bundle after resin supply -(mass per unit length of carbon fiber bundle) / (mass per unit length of carbon fiber bundle after resin supply)}×100 The "mass per unit length of the carbon fiber bundle" was calculated by unwinding the carbon fiber bundle from the carbon fiber bundle (spool) wound around a paper tube, cutting out five 1 m pieces, measuring the mass of each piece, and averaging the masses of the five pieces. The higher the resin adhesion rate, the higher the resin impregnation of the carbon fiber bundle. The evaluation was made as follows: 16% or more is O, 14% or more but less than 16% is △, and less than 14% is ×.
[0154] <Spontaneous dispersibility test> The spontaneous dispersibility was evaluated by the above-mentioned method, except that jER828 (manufactured by Mitsubishi Chemical Corporation) was used as the evaluation liquid.
[0155] <Cantilever test> The cantilever value was measured by the following method and used as an index of the bundleability of the carbon fiber bundle. The larger the cantilever value, the higher the bundleability of the carbon fiber bundle. The cantilever value was judged as 24.0 cm or more as ○, 22.0 cm or more but less than 24.0 cm as △, and less than 22.0 cm as ×. (Step 1) The measurement is carried out in an air atmosphere at 25° C. A measurement table has a horizontal plane and a slope with an inclination angle of 45 degrees that slopes downward from one end (straight line) of the horizontal plane. The carbon fiber bundle is extended 30 cm from the bobbin onto the horizontal plane, and placed without twisting or disorder, and the end (straight line) of the test carbon fiber bundle is aligned with the boundary line A between the slope and the horizontal plane. At this time, the test carbon fiber bundle is placed with the surface that was on the surface side of the bobbin facing the horizontal plane. A pressure plate is placed on the test carbon fiber bundle, and the end (straight line) of the pressure plate is aligned with the boundary line A. (Step 2) Next, the pressure plate is moved horizontally toward the inclined surface at a speed of 0.5 cm / sec, and the movement of the pressure plate is stopped when the end of the test carbon fiber bundle comes into contact with the inclined surface. (Step 3) In step 2, measure the shortest distance between the point where the end of the carbon fiber bundle comes into contact with the slope and boundary line A. (Step 4) Steps 1 to 3 were performed 10 times, and the simple average of the obtained values was taken as the cantilever value.
[0156] <Evaluation of interfacial adhesion> 156 of the obtained carbon fiber bundles were aligned and arranged on the surface of a release paper coated with a matrix resin consisting of B-stage epoxy resin #350 (Mitsubishi Chemical Corporation, 130°C curing type), and then passed through a heated pressure roller to impregnate the carbon fiber bundles with the epoxy resin. A protective film was further laminated on top of the bundles, resulting in a resin content of approximately 33% by mass and a carbon fiber basis weight of 250 g / m. 2 A unidirectional (UD) prepreg with a width of 500 mm was fabricated. Next, a 2 mm thick UD laminate prepared from the UD prepreg was cured and molded to obtain a laminate as a carbon fiber composite material molded product. In the laminate obtained as the carbon fiber composite material molded product, the interfacial adhesion between the carbon fiber and the matrix resin was evaluated based on the 90° bending stress of the laminate (in accordance with ASTM-D-790). The higher the 90° bending stress, the better the adhesion between the carbon fiber and the matrix resin. The 90° bending stress was judged as ◯ for 135 MPa or more, △ for 125 MPa or more but less than 135 MPa, and × for less than 125 MPa. The results are shown in Table 14.
[0157] <Evaluation of fiber opening rate A> The opening ratio A was evaluated by the method described in Example 1-1.
[0158] [Examples 2-2 to 10-2, Comparative Examples 1-2 to 6-2] A carbon fiber bundle with a sizing agent was obtained in the same manner as in Example 1-2, except that the components (A) to (E) shown in Table 13 were mixed in the ratio (parts by mass) shown in Table 14 or 15. The obtained carbon fiber bundle with a sizing agent was used to carry out the same evaluation as in Example 1-2. The results are shown in Tables 14 and 15.
[0159] [Table 14]
[0160] [Table 15]
[0161] [Table 16] [Industrial Applicability]
[0162] In one aspect of the present invention, by using a carbon fiber sizing, it is possible to obtain carbon fibers and carbon fiber bundles with a sizing agent attached thereto, which are excellent in impregnation with a matrix resin, handleability in processing steps, and mechanical properties of the composite material.
[0163] In another aspect of the present invention, by using a carbon fiber sizing, it is possible to obtain carbon fibers and carbon fiber bundles with a sizing agent attached thereto, which are excellent in terms of impregnation with a matrix resin, bundling ability, interfacial adhesion with the matrix resin, and ease of dispersion within the matrix resin. [Explanation of symbols]
[0164] 1: A bobbin wound with carbon fiber bundles with sizing agent attached 2: Opening bar 3: Drive roller 4: Laser type length measuring sensor 10: Apparatus for measuring the opening ratio A
Claims
1. A sizing agent-attached carbon fiber bundle comprising carbon fibers and a sizing agent for carbon fibers, Contains component (A-1), component (B), and component (C), The component (A-1) is a urethane compound having a structure represented by the following formula (1-1) in the molecule: 【Chemistry 1】 [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer of 1 to 50.] The component (B) is an epoxy compound selected from the group consisting of epoxy compounds represented by the following formula (2) and epoxy compounds represented by the following formula (4), 【Chemistry 2】 [In the formula, m represents an integer of 1 to 5.] 【Chemistry 3】 [In the formula, q represents an integer of 0 to 5.] The component (C) is a bisphenol-type epoxy compound or an aliphatic epoxy compound, The spontaneous dispersion rate is 5.0 or more as measured by a spontaneous dispersion test using a bisphenol A type epoxy resin having a viscosity of 11 to 15 Pa·s at 25°C as an evaluation liquid. Carbon fiber bundle with sizing agent attached.
2. A sizing-agent-adhered carbon fiber bundle comprising carbon fibers and a sizing agent for carbon fibers, Contains component (A-1), component (B), and component (C), The component (A-1) is a urethane compound having a structure represented by the following formula (1-1) in the molecule: 【Chemistry 4】 [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer of 1 to 50.] The content of the component (B) is 15 to 40 parts by mass relative to 100 parts by mass of the total of the component (A-1), the component (B), and the component (C), The component (B) is an epoxy compound selected from the group consisting of an epoxy compound represented by the following formula (2), an epoxy compound represented by the following formula (3), and an epoxy compound represented by the following formula (4), 【Chemistry 5】 [In the formula, m represents an integer of 1 to 5.] 【Chemistry 6】 [In the formula, R3 and R4 each independently represent a hydrogen atom or a saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms, and p represents an integer of 0 to 5.] 【Chemistry 7】 [In the formula, q represents an integer of 0 to 5.] The component (C) is a bisphenol-type epoxy compound or an aliphatic epoxy compound, The spontaneous dispersion rate is 5.0 or more as measured by a spontaneous dispersion test using a bisphenol A type epoxy resin having a viscosity of 11 to 15 Pa·s at 25°C as an evaluation liquid. Carbon fiber bundle with sizing agent attached.
3. A sizing agent-attached carbon fiber bundle comprising carbon fibers and a sizing agent for carbon fibers, Contains component (A-1), component (B), and component (C), The component (A-1) is a urethane compound having a structure represented by the following formula (1-1) in the molecule: 【Chemistry 8】 [In the formula, X represents a divalent aromatic group, a divalent linear or branched aliphatic hydrocarbon group, or a divalent alicyclic hydrocarbon group; R1 and R2 each independently represent a methyl group or a hydrogen atom; and n represents an integer of 1 to 50.] The component (B) is an epoxy compound selected from the group consisting of epoxy compounds represented by the following formula (2) and epoxy compounds represented by the following formula (4), 【Chemistry 9】 [In the formula, m represents an integer of 1 to 5.] 【Chemistry 10】 [In the formula, q represents an integer of 0 to 5.] The component (C) is a bisphenol-type epoxy compound or an aliphatic epoxy compound, When the total amount of all components of the sizing agent for carbon fiber is 100 parts by mass, the content of component (A-1) is 7 to 49 parts by mass, the content of component (B) is 15 to 40 parts by mass, the content of component (C) is 21 to 68 parts by mass, and the total amount of component (A-1) and component (C) is 40 to 75 parts by mass, The spontaneous dispersion ratio measured by a spontaneous dispersion test using a bisphenol A type epoxy resin having a viscosity of 11 to 15 Pa·s at 25°C as an evaluation liquid is 3 or more. Carbon fiber bundle with sizing agent attached.
4. The carbon fiber bundle with a sizing agent applied thereto according to any one of claims 1 to 3, wherein the component (A-1) has an epoxy group in the molecule.
5. The sizing agent-adhered carbon fiber bundle according to any one of claims 1 to 4, wherein the viscosity of the component (C) at 50°C is 100 mPa·s or more and 10,000 mPa·s or less.
6. The sizing agent-attached carbon fiber bundle according to any one of claims 1 to 5, wherein the component (C) has an epoxy equivalent of 160 to 400 g / eq and a number average molecular weight of 340 to 800.
7. The sizing agent-adhered carbon fiber bundle according to any one of claims 1 to 6, further comprising an aliphatic ester compound, and a content of the aliphatic ester compound is 5 to 20 mass% relative to a total mass of the sizing agent for carbon fiber.
8. The sizing-agent-adhered carbon fiber bundle according to any one of claims 1 to 7, further comprising a surfactant, and a content of the surfactant is 10 to 25 mass% relative to a total mass of the sizing agent for carbon fiber.
9. The sizing agent-attached carbon fiber bundle according to claim 8, wherein the surfactant is an anionic surfactant represented by the following formula (5): 【Chemistry 11】 [In the formula, R5 and R6 each independently represent a hydrogen atom, an aliphatic hydrocarbon group having 1 to 18 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; and r represents an integer of 5 to 25.]
10. The sizing agent-attached carbon fiber bundle according to any one of claims 1 to 9, wherein the content of the sizing agent for carbon fiber is 0.1 to 5.0 mass% based on the total mass of the sizing agent-attached carbon fiber bundle.
11. A method for producing a carbon fiber reinforced composite material, comprising impregnating the sizing-adhered carbon fiber bundle according to any one of claims 1 to 10 with a thermosetting resin composition and heat curing the thermosetting resin composition.
12. A method for producing a carbon fiber reinforced pressure vessel, comprising: impregnating a sizing-agent-adhered carbon fiber bundle according to any one of claims 1 to 10 with a thermosetting resin composition by a filament winding method, and heat-curing the thermosetting resin composition to produce a carbon fiber reinforced pressure vessel.
Citation Information
Patent Citations
Carbon fiber composite emulsion sizing agent with low surface tension and high particle size stability and preparation method thereof
CN104562693B
Carbon fiber excellent in Anti-friction property
JP1983013781A
Carbon fiber and sizing agent therefor
JP1985065181A
Treating agent for fiber for composite material and production thereof
JP1989314785A
Sizing agent for carbon fiber and carbon fiber bundle
JP2008274520A