A phase-change composite fiber with precise temperature control and its preparation method and application

The electrochemical hydrogen evolution expansion-impregnation method is used to fill polyethylene glycol into carbon nanotube fibers, which solves the problems of low thermal conductivity and poor mechanical properties of phase change materials, and achieves two-way regulation and efficient energy storage of phase change composite fibers. Suitable for temperature control in different environments.

CN115852701BActive Publication Date: 2024-10-18SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI

Patent Information

Application Number
CN202211524144.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-10-18
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

Existing phase change materials have problems such as low thermal conductivity, liquid leakage, poor mechanical properties, delayed phase change, poor thermal stability, and phase change expansion, making it difficult to meet the needs of energy storage and temperature control.

Method used

Polyethylene glycol is filled into the nanopores of carbon nanotube fibers through the electrochemical hydrogen evolution expansion-impregnation method to form a polyethylene glycol/carbon nanofiber composite structure, which precisely controls the phase transition temperature of the phase change composite fiber and combines the carbon Nanotube network assembly structure improves mechanical, electrical and thermal conductivity properties.

Benefits of technology

The phase change composite fiber has achieved excellent mechanical properties, electrical conductivity and thermal conductivity, has two-way temperature regulation performance, is suitable for temperature control in different environments, and has a simple and efficient process, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852701B_ABST
    Figure CN115852701B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a phase-change composite fiber with precise temperature control, wherein the carbon nanotube fiber is expanded by the electrolytic water hydrogen evolution technology, and then the phase change material is filled into the network skeleton structure of the carbon nanotube fiber in combination with in-situ impregnation-stretching to form a carbon nanotube phase-change composite fiber, and at the same time, the temperature control range of the composite fiber is further broadened by selecting the type and composite ratio of the phase change material. By adopting the technical solution of the present invention, the high strength, high conductivity, and high thermal conductivity of the carbon nanotube fiber nanostructure network skeleton can be fully utilized, and the phase change heat storage characteristics of the phase change material can be combined to prepare a carbon nanotube phase-change composite fiber with excellent mechanical, electrical, thermal, high phase change latent heat, and wide temperature range control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inorganic nanomaterials, and in particular to a method for preparing a phase-change composite fiber with precise temperature regulation. Background Art

[0002] Energy crisis and environmental pollution have become global problems and major challenges facing my country's development. Thermal energy storage is a new environmentally friendly and energy-saving technology that can solve the imbalance of energy supply in time and space and is an important means of low-carbon environmental protection (Renewable and Sustainable Energy Reviews, 2019, 108, F398-422; CN114574998A; CN104910334A, etc.). Among many energy technologies, phase change materials use phase change latent heat to store and release energy, which has become a very active research direction in energy science and materials science in recent years.

[0003] Phase change energy storage materials store and release energy through solid-solid, solid-liquid, solid-gas or liquid-gas phase changes, and can be divided into inorganic and organic categories. At present, phase change materials mainly have problems such as low thermal conductivity, liquid leakage, poor mechanical properties, phase change delay, poor thermal stability and phase change expansion. Compared with inorganic phase change materials, organic phase change materials have a wide phase change temperature range, stable chemical properties, high latent heat, etc., and have great potential in improving energy utilization and regulating temperature (CN113403834A; CN106048761A; J.Phys.Chem.C, 2011, 115, 8753-8758; J.Mater.Chem.A, 201, 4, 17042-17049, etc.). Compounding phase change materials with other materials can effectively overcome the defects of single phase change materials and give full play to the advantages of each component. Since carbon materials have the characteristics of good thermal conductivity, high chemical stability and low density, the composite of porous carbon, carbon fiber, carbon nanotubes, graphene, etc. with organic phase change materials has become a new research direction. Studies have shown that the thermal properties and stability of phase change materials can be improved by dispersing and adding nanocarbon, but the comprehensive performance advantages of nanocarbon materials have not yet been fully utilized (Energy Environ. Sci., 2020, 13, 4498-4535; Chemical Engineering Journal, 2019, 356, 641-661). By compounding the nano-assembly structure with the phase change material, with the help of the excellent electrothermal performance and network binding effect of the carbon nanotube network assembly structure, the bottleneck problems such as easy agglomeration, poor orientation and low content of nano units in the dispersion method can be effectively overcome, and the comprehensive performance of force, heat and electricity can be significantly improved (Adv. Mater., 2018, 30, 1801754; CN108587571A). For example, a Chinese invention patent (CN 110804301A) discloses a polyethylene glycol / hydroxypropyl cellulose carbon nanotube composite solid-solid phase change material and a preparation method thereof, which is prepared by chemical grafting reaction of polyethylene glycol (PEG), isocyanate (MDI), and hydroxypropyl cellulose (HPC). The phase change process of the phase change material is solid-solid phase change, the phase change temperature is 32 to 54°C, and the phase change enthalpy value is 99.5-130.8 J / g.

[0004] However, in fact, in the prior art, organic phase change materials still have the following disadvantages: 1. Organic phase change materials will undergo solid-liquid phase change during the phase change process, making it difficult to maintain a certain form and prone to leakage during the phase change process; 2. Phase change fibers prepared by filling powdered carbon materials (carbon black, carbon nanotubes, graphene, etc.) into phase change materials and then using spinning technology usually have poor mechanical properties and are difficult to meet subsequent use requirements; 3. The carbon material in the powdered carbon / phase change material composite fiber does not form a continuous phase, which results in large contact resistance and contact thermal resistance, and thus has limited improvement in the electrical conductivity and thermal conductivity of the material; 4. Graphene aerogels and other carbon material assemblies and phase change material composite fibers also have problems such as poor mechanical strength and poor toughness, which is not conducive to subsequent processing; 5. The thermal enthalpy of phase change composite fibers is low; 6. The sensitivity to temperature control is low; 7. The processing method of phase change composite materials in the prior art is complex, which is not conducive to promotion and application. Summary of the invention

[0005] The present invention discloses a phase-change composite fiber with precise temperature control and a preparation method thereof. The carbon nanotube assembly structure is used as a skeleton to be composited with a polymer phase-change material. By composited with the phase-change material and the network assembly structure of the carbon nanotube fiber, the phase transition temperature of the phase-change composite fiber can be precisely controlled to adapt to temperature control in different environments. At the same time, it also has excellent electromechanical properties to solve the defects of the phase-change materials and phase-change composite materials in the prior art, such as poor mechanical properties, low thermal conductivity and low electrical conductivity.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a method for preparing a phase change composite fiber with precise temperature control, wherein the electrolysis of water is controlled by an electric current method to carry out hydrogen evolution expansion-impregnation of carbon nanotube fibers, and polyethylene glycol is filled into the nanopores of the carbon nanotube fibers to form the phase change composite fiber having a polyethylene glycol / carbon nanofiber composite structure.

[0007] Specifically, the steps include:

[0008] S1. Prepare electrolyte solution; add concentrated sulfuric acid solution to polyethylene glycol solution, stir and mix well;

[0009] S2. Hydrogen evolution expansion - in-situ impregnation: The electrolyte solution configured in S1 is added to an electrolytic cell, the anode is an inert electrode, the cathode is a carbon nanotube fiber, the carbon nanotube fiber is immersed in the electrolyte solution, and the carbon nanotube fiber is expanded by controlling the electrolysis of water by an electric current method, so that the phase change material fully penetrates into the interior of the carbon nanotube fiber to obtain a phase change composite fiber I;

[0010] S3 stretching: the hydrogen evolution expansion - in-situ impregnation of the phase change composite fiber I pulled out from the electrolyte solution, under the action of surface tension so that the surface of the phase change composite fiber has a dense structure, to obtain a phase change composite fiber II;

[0011] Due to the effect of surface tension, the structure of the phase change material / carbon nanotube fiber becomes denser, which is more conducive to the conversion and transfer of heat of the phase change material.

[0012] S4. Post-treatment: removing excess electrolyte solution from the surface of the phase change composite fiber II, and vacuum drying to obtain the final phase change composite fiber product.

[0013] Preferably, in S1, the concentration of the polyethylene glycol solution is 10-20wt%; and / or the polyethylene glycol is any one of PEG600 to 6000 or a mixture of more than one; and / or the polyethylene glycol solution is a mixed solution of PEG600 and / or PEG1500; more preferably, the mass ratio of PEG600 to PEG1500 is 0.5 to 2:1.

[0014] Preferably, in S2, the carbon nanotube fibers are prepared by a floating catalyst chemical deposition method (CVD).

[0015] Preferably, in S1, the electrolyte preparation step comprises: (1) preparing an electrolyte solution: slowly adding concentrated sulfuric acid to deionized water in a cold water bath, fixing the volume, and stirring until uniform, which is recorded as solution A;

[0016] (2) Preparation of polyethylene glycol (PEG) solution: Add polyethylene glycol to deionized water and stir until completely dissolved, referred to as solution B;

[0017] (3) Preparing an electrolyte solution: adding solution A to solution B and stirring until the mixture is uniform to obtain the electrolyte solution.

[0018] Preferably, the temperature control conditions of the phase change composite fiber are 8-57°C and the thermal enthalpy is 110-183 J·g -1 .

[0019] The phase-change composite fiber prepared by the above-mentioned technical solution has a precise control effect on temperature. The phase-change composite fiber prepared by uniformly compounding with the phase-change material by electrochemical hydrogen evolution expansion has excellent mechanical properties, electrical conductivity and thermal conductivity. At the same time, it can have a wide temperature control range and is suitable for different working environments. It can store energy by electrothermal means when the light intensity is weak, and release heat to maintain the temperature when necessary, and has a two-way temperature regulation performance. The phase-change composite fiber is used in wearable temperature-regulating fabrics, which can release / store heat to maintain the temperature of the living body according to the external temperature, and has broad market application prospects.

[0020] Similarly, the above technical solution can also be applied to other phase change materials, that is, polyethylene glycol can also be other organic phase change materials or inorganic phase change materials; the organic phase change material includes any one of polyols, paraffin, and fatty acids; the inorganic phase change material includes hydrated salts or molten salts.

[0021] In summary, the present invention uses a carbon nanotube assembly structure as a skeleton to composite with a polyethylene glycol phase change material, and efficiently controls the content of the phase change material entering the carbon nanotube network through the hydrogen evolution expansion method. By mixing and compounding phase change materials of different molecular weights with the carbon nanotube network assembly structure, the phase transition temperature of the composite phase change fiber is precisely controlled to adapt to temperature control in different environments, while also having excellent mechanical, electrical and thermodynamic properties.

[0022] The technical effects of the technical solution of the present invention are as follows:

[0023] 1. By adopting the technical solution of the present invention, the high strength, high electrical and thermal conductivity of carbon nanotube fibers are utilized, and the phase change material is uniformly compounded through electrochemical hydrogen evolution expansion to prepare a phase change composite fiber with excellent mechanical properties, electrical conductivity and thermal conductivity.

[0024] 2. By adopting the technical solution of the present invention, carbon nanotubes also have excellent light-to-heat conversion performance. In practical applications, they can store heat as long as there is light. At the same time, they can also store energy through electric heating when the light intensity is weak, and release heat to maintain the temperature when necessary, with two-way temperature control performance.

[0025] 3. By adopting the technical solution of the present invention, the phase change material is filled into the nanopores in the carbon nanotube fiber by the method of hydrogen evolution expansion, and at the same time combined with the in-situ impregnation and stretching process, the phase change material is more densely filled in the carbon nanotube fiber, so that the composite phase change material of the phase change material / carbon nanotube fiber structure has heat storage capacity, and can further more accurately control the temperature.

[0026] 4. The phase change composite fiber prepared by adopting the technical solution of the present invention not only has excellent electrical conductivity, thermal conductivity and mechanical strength, but also does not involve toxic and hazardous substances in the process of phase change composite fiber, is efficient, green, energy-saving and environmentally friendly, and its application in wearable temperature regulating fabrics has broad market prospects.

[0027] 5. By adopting the technical solution of the present invention, the temperature range for preparing phase change composite fibers is wider, the preparation method is simple and efficient, continuous production can be expanded, and industrialization can be realized; different phase change materials and / or different proportions of phase change materials can be used according to the needs of the use environment to achieve a phase change composite material with precise temperature control performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of the structure of the device for preparing phase change composite fibers in Example 1 of the present invention.

[0029] Figure 2 Process flow chart for preparing phase change composite fibers in Example 1 of the present invention.

[0030] Figure 3a These are plan SEM images and cross-sectional SEM images of the carbon nanotube fibers used in Example 1 of the present invention at different magnifications.

[0031] Figure 3b These are the planar SEM images and cross-sectional SEM images of the phase change composite fiber prepared in Comparative Example 1 of the present invention at different magnifications.

[0032] Figure 3c These are planar SEM images and cross-sectional SEM images of the phase change composite fiber prepared in Example 1 of the present invention at different magnifications.

[0033] Figure 4a , Figure 4b , Figure 4c and Figure 4d They are respectively diagrams characterizing changes in the thermodynamic properties of the phase change material of the phase change composite fiber prepared in Example 1 of the present invention at different ratios.

[0034] Figure 5 This is a diagram showing the conductivity change of the phase change material added to the phase change composite fiber prepared in Example 1 of the present invention at different ratios.

[0035] Figure 6 This is a graph showing the change in tensile strength at different ratios of the added phase change material of the phase change composite fiber prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0037] The present invention provides a phase-change composite fiber with precise temperature control, which is formed by electrolyzing water to expand and impregnate carbon nanotube fibers with hydrogen, and filling polyethylene glycol into the nanopores of the carbon nanotube fibers to form the phase-change composite fiber with a polyethylene glycol / carbon nanofiber composite structure.

[0038] The specific implementation of the present invention is described in detail using polyethylene glycol as an example. The melting and crystallization temperatures of pure polyethylene glycol are single and fixed. For example, the melting temperature of pure PEG1500 is 53.5°C, and the crystallization temperature is 22.4°C. The melting temperature of pure PEG600 is 27.8°C, and the crystallization temperature is 0.6°C. This means that heat energy can only be stored and released when the ambient temperature reaches the phase change temperature, which makes it difficult to meet the temperature control requirements of different environments. The present invention mixes two polyethylene glycols of different molecular weights in different mass ratios according to different use environments, and then compounds them with carbon nanotube fibers to prepare phase change composite fibers that can achieve precise temperature control.

[0039] Based on this, the preparation method of phase change composite fiber with precise temperature regulation function includes the following steps:

[0040] S1. Prepare electrolyte solution:

[0041] (1) Preparation of electrolyte: Take 98% concentrated sulfuric acid, slowly add the concentrated sulfuric acid into deionized water with a glass rod in a cold water bath while stirring, make up to volume, and stir until uniform, which is recorded as solution A;

[0042] (2) preparing a polyethylene glycol (PEG) solution: accurately weighing polyethylene glycol and adding it to deionized water, placing it in a water bath at 30° C., and stirring it with a magnetic stirrer until it is completely dissolved, which is referred to as solution B; preferably, the polyethylene glycol solution has a mass volume concentration of 10 to 20 wt %; wherein the polyethylene glycol solution is PEG600 to 6000, preferably, a mixed solution of PEG600 and PEG1500; more preferably, the mass ratio of PEG600 to PEG1500 is 1:0.5 to 2;

[0043] (3) preparing an electrolyte solution: adding solution A to solution B and stirring until the mixture is completely mixed to obtain an electrolyte solution;

[0044] S2. Hydrogen evolution expansion of carbon nanotube fibers - in-situ impregnation: the electrolyte solution configured in S1 is added to an electrolytic cell, the anode is an inert electrode, the cathode is a carbon nanotube fiber, and the carbon nanotube fiber is expanded by controlling the electrolysis of water by an electric current method, so that the polyethylene glycol fully penetrates into the carbon nanotube fiber to obtain a phase change composite fiber I; preferably, the carbon nanotube fiber is prepared by a floating catalyst chemical deposition method (CVD);

[0045] S3 stretching: pulling the phase change composite fiber I out of the electrolyte solution, so that the surface of the phase change composite fiber has a dense structure under the action of surface tension, to obtain a phase change composite fiber II;

[0046] In some embodiments, the dipping and stretching processes are performed simultaneously.

[0047] S4. Post-treatment: removing excess electrolyte solution from the surface of the phase change composite fiber II and vacuum drying to obtain the final phase change composite fiber product.

[0048] Furthermore, in S2, the current is generally fixed between 10 and 180 mA, and the voltage varies with the current. The carbon nanotube fibers in the present invention can expand rapidly within a few seconds, or can maintain the expansion state all the time, so there is no specific requirement for the power-on time.

[0049] The temperature of the phase change composite fiber prepared by the above method is 8-57°C and the thermal enthalpy is 110-183 J·g -1 .

[0050] The technical scheme of the present invention is further described in detail below through specific examples. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0051] Example 1

[0052] This embodiment provides a phase change composite fiber with precise temperature control, using a method for electrolytic hydrogen evolution and expansion of carbon nanotube fibers, see Figure 1 , the carbon nanotube fiber is fully soaked in the water bath and then enters the electrolytic tank. In the electrolytic tank, the carbon nanotube fiber is connected to the negative electrode of the power supply, and a polyethylene glycol solution with sulfuric acid is added as an electrolyte solution as an expansion bath, and is connected to the positive electrode of the power supply through a platinum electrode, so that the carbon nanotube fiber as the cathode, the anode, and the polyethylene glycol sulfuric acid solution as the electrolyte form an electrochemical system. After the system works, the gas generated by the electrolysis of water and hydrogen evolution causes the carbon nanotube fiber to produce uniform instantaneous expansion in the longitudinal direction or / radial direction and from the inside to the outside, and at the same time, the phase change material molecules enter the surface and / or micropores of the expanded carbon nanotube fiber. After sufficient impregnation, the polyethylene glycol enters and fills the micropores inside the carbon nanotube fiber.

[0053] A motor-driven winder is provided at the end to wind up the carbon nanotube fiber expanded by hydrogen evolution through the fiber winder. Through physical stretching, the filling structure of polyethylene glycol in the micropores of the carbon nanotube fiber becomes denser.

[0054] After the carbon nanotube fiber undergoes hydrogen expansion-in-situ impregnation-stretching process, it is pulled out from the electrolyte solution through a winder to obtain a phase change composite fiber. By adjusting the mixing ratio of PEG with different molecular weights, the intelligent function of precise temperature control of the composite fiber is achieved. Specifically, the steps of the preparation method of the phase change composite fiber with precise temperature control include:

[0055] 1. Provide carbon nanotube fibers, which are prepared by a floating catalyst chemical deposition method (CVD). This embodiment uses carbon nanotube fibers prepared by Suzhou JEDI Nanotechnology Co., Ltd.

[0056] 2. Prepare electrolyte solution:

[0057] (1) Prepare the electrolyte: Accurately measure 900 mL of deionized water in a 2L beaker, accurately measure 54.35 mL of 98% concentrated sulfuric acid, and slowly add sulfuric acid to the deionized water with a glass rod while stirring in a cold water bath. Finally, add deionized water to 1000 mL and stir until uniform. This is called solution A.

[0058] (2) Prepare a 15 wt% polyethylene glycol (PEG) solution: accurately measure 425 mL of deionized water in a 500 mL beaker, accurately weigh 75 g of polyethylene glycol, and place in a 30° C. water bath with magnetic stirring for 1 h until completely dissolved, which is recorded as solution B. In this embodiment, the polyethylene glycol is a mixture of PEG600 and PEG1500, and accurately weigh 50 g of PEG600 and 25 g of PEG1500 and dissolve them in 425 mL of deionized water to prepare a polyethylene glycol mixed solution (solution B) with a mass ratio of 2:1.

[0059] (3) Prepare electrolyte solution: add 10 mL of A solution into solution B and stir until completely mixed to obtain an electrolyte solution.

[0060] 3. Electrolysis of water to release hydrogen to expand carbon nanotube fibers and in-situ impregnation: 500 mL of electrolyte is added to the electrolytic cell, the anode is an inert electrode, and the cathode is the carbon nanotube fiber. The current method is used for control (the voltage changes with the current control), and the mixed electrolyte solution is charged with electricity to release hydrogen to expand the carbon nanotube fiber, so that the polyethylene glycol is filled into the nanopores of the carbon nanofiber.

[0061] 4. Stretching: The impregnated polyethylene glycol / carbon nanotube fibers are pulled out of the solution through a winding motor. Due to the effect of surface tension, the structure of the polyethylene glycol / carbon nanotube fibers becomes denser, which is more conducive to the conversion and transfer of heat of the phase change material. Preferably, the stretching speed of the winding motor is 25 cm / min.

[0062] 5. Post-treatment: remove excess electrolyte solution on the surface of the polyethylene glycol / carbon nanotube fiber through a wire drawing die, dry it at 50°C in vacuum to obtain the final product of the phase change composite fiber.

[0063] Example 2

[0064] The difference between this embodiment and embodiment 1 is that in step 2-(2), a 15 wt% polyethylene glycol (PEG) solution is prepared by accurately weighing 37.5 g PEG600 and 37.5 g PEG1500 and dissolving them in 425 mL deionized water to prepare a 1:1 polyethylene glycol mixed solution (B solution).

[0065] Example 3

[0066] The difference between this embodiment and embodiment 1 is that in step 2-(2), a 15 wt% polyethylene glycol (PEG) mixed solution is prepared by accurately weighing 25 g PEG600 and 50 g PEG1500 and dissolving them in 425 mL deionized water to prepare a 1:2 polyethylene glycol mixed solution (B solution).

[0067] Example 4

[0068] The difference between this embodiment and embodiment 1 is that in step 2-(2), the concentration of the polyethylene glycol (PEG) mixed solution is 10 wt %.

[0069] Example 5

[0070] The difference between this embodiment and embodiment 1 is that in step 2-(2), the concentration of the polyethylene glycol (PEG) mixed solution is 20 wt %.

[0071] Example 6

[0072] The difference between this embodiment and embodiment 1 is that in step 2-(2), the preparation of the polyethylene glycol (PEG) mixed solution includes using deionized water as a solvent to prepare a PEG1500 solution with a concentration of 15 wt%.

[0073] Electrolysis of water to expand the fiber process: Take 500mL of electrolyte and add it to the electrolytic cell, the anode is the platinum electrode, and the cathode is the carbon nanotube fiber. Adjust the current to 50mA, electrolyze water to release hydrogen to expand the carbon nanotube fiber to achieve ultra-high lossless expansion, and at the same time in-situ impregnation of PEG1500 to prepare phase change composite fibers.

[0074] Example 7

[0075] The difference between this embodiment and embodiment 6 is that in step 2-(2), the preparation of the polyethylene glycol (PEG) mixed solution includes using deionized water as a solvent to prepare a PEG600 solution with a concentration of 15 wt%.

[0076] Example 8

[0077] The difference between this embodiment and embodiment 6 is that in step 2-(2), the preparation of the polyethylene glycol (PEG) mixed solution includes using deionized water as a solvent to prepare a PEG2000 solution with a concentration of 15 wt%.

[0078] Electrolysis of water to expand the fiber process: Take 500ml of electrolyte and add it to the electrolytic cell, the anode is the platinum electrode, and the cathode is the carbon nanotube fiber. Adjust the current to 50mA, electrolyze water to release hydrogen to expand the carbon nanotube fiber to achieve ultra-high lossless expansion, and at the same time in-situ impregnation of PEG2000 to prepare phase change composite fibers.

[0079] Example 9

[0080] The difference between this embodiment and embodiment 6 is that in step 2-(2), the preparation of the polyethylene glycol (PEG) mixed solution includes using deionized water as a solvent to prepare a PEG3500 solution with a concentration of 15 wt%.

[0081] Example 10

[0082] The difference between this embodiment and embodiment 6 is that in step 2-(2), the preparation of the polyethylene glycol (PEG) mixed solution includes using deionized water as a solvent to prepare a PEG6000 solution with a concentration of 15 wt%.

[0083] Comparative Example 1

[0084] The difference between this comparative example and Example 1 is that in step 4, the expanded carbon nanotube fibers are immersed in an electrolyte solution, the carbon nanotube fibers are immersed in a mixed electrolyte solution and electrically expanded, so that the polyethylene glycol is filled into the nanopores of the carbon nanofibers, and then the filled carbon nanofibers are directly taken out of the electrolyte solution without being stretched.

[0085] The above embodiments were characterized in terms of microscopic morphology, thermodynamics, electrical properties and mechanical properties.

[0086] Thermodynamic properties include phase transition temperature and thermal enthalpy (phase change enthalpy) testing, which is done using differential scanning calorimetry (DSC) testing.

[0087] See also Figure 3a , are SEM microscopic morphology images of the original carbon nanotube fibers at different magnifications. It can be seen that there are many micropores in the carbon nanotube fibers and the fiber surface is uneven. The presence of these micropores makes the carbon nanofibers a good carrier for phase change materials.

[0088] Figure 3b The SEM microstructure of the phase change composite fiber prepared by hydrogen evolution expansion and impregnation with polyethylene glycol in Comparative Example 1 but not stretched is shown. It can be seen that the unstretched phase change composite fiber has a rougher surface and uneven diameter, and the micropores of the carbon nanotubes are not completely filled with polyethylene glycol.

[0089] See also Figure 3cThe SEM microscopic morphology of the composite phase change fiber of Example 1 at different magnifications shows that the nanopores of the carbon nanotube fiber (CNT&PEG Fiber) after hydrogen evolution expansion-impregnation treatment are filled with polyethylene glycol. It is obvious that the carbon nanotube fiber and polyethylene glycol have been fully composited, and the fiber surface is flat and the structure is dense. It can be seen from the figure that under the traction of the reel, polyethylene glycol fully fills the network micropores of the carbon nanotube, and the prepared phase change composite fiber is more dense.

[0090] pass Figure 3a-Figure 3b The SEM microscopic morphology shows that the impregnation-stretching process of the present invention can promote the filling of the phase change material in the carbon nanotubes, and the composite phase change fiber obtained by the technical solution of the present invention has a uniform surface and a denser structure, thereby improving the heat storage performance of the phase change material and achieving the purpose of precise temperature control.

[0091] See also Figure 4a , is the loading rate of polyethylene glycol on the carbon nanotube fiber under different expansion currents in Example 1. By comparing the effects of different currents on the polyethylene glycol loading on the fiber, it is found that when the expansion current is 50 mA, the loading rate of polyethylene glycol on the carbon nanotube fiber is 89%.

[0092] See also Figure 4b The heat flow curves of melting and crystallization of phase change composite fibers prepared by compounding different polyethylene glycol ratios of Examples 1-3, PEG1500 of Example 6 and PEG600 of Example 7 with carbon nanotubes, and pure PEG1500 and pure PEG600, measured by DSC method, were compared. It was found that the heat flow of the sample mixed with PEG600 and PEG1500 in proportion varies with the different ratios of the two.

[0093] See also Figure 4c , the comparison of the melting and crystallization temperatures of phase change composite fibers and pure polyethylene glycol, through comparison, it is found that compared with pure polyethylene glycol, the crystallization temperature of phase change composite fibers is increased by 5-10 ° C. Compared with pure polyethylene glycol, the increase in crystallization temperature is more conducive to the release of heat by phase change composite fibers. And by comparing the composites of polyethylene glycol and carbon nanotube fibers in different proportions, it is found that their melting and crystallization temperatures are also different. Among them, the highest is the sample of CNT / PEG1500, with a melting temperature of 57 ° C, which can meet the requirements of storing heat in a higher temperature environment to achieve temperature adjustment, and the crystallization temperature can reach 26 ° C, which can meet the requirements of releasing heat in room temperature environment to achieve temperature adjustment in practical applications; the smallest is the sample of CNT / PEG600, with a melting temperature of about 25 ° C, which can meet the requirements of heat storage and temperature adjustment in room temperature environment, and a crystallization temperature of about 8 ° C, which can meet the requirements of phase change temperature adjustment in a lower temperature environment in practical applications.

[0094] See also Figure 4d, is the thermal enthalpy test analysis of the phase change composite fiber prepared by combining the different polyethylene glycol ratios of Examples 1-3 and the PEG1500 of Example 6 and the PEG600 of Example 7 with the carbon nanotube fiber. It can be seen from the figure that when the mass ratio of pure PEG600, pure PEG1500, PEG600 and PEG1500 is 1:0.5-2, the thermal enthalpy value is 110-183 J.g -1 .

[0095] The above results show that the CNT / PEG phase change composite material prepared by compounding PEG600 and / or PEG1500 with carbon nanotubes has a temperature control sensitivity effect, and the composite phase change material obtained by compounding PEG600 and PEG1500 in different proportions with carbon nanotube fibers has a temperature control sensitivity effect, which can achieve precise temperature control in a wide temperature range (8-57°C), and the phase change composite material with different molecular weight PEG prepared in the embodiment has a higher thermal enthalpy. The phase change thermal enthalpy of the CNT / PEG1500 sample can reach up to 183 J·g -1 In addition, due to the relatively low thermal enthalpy of pure PEG600, the thermal enthalpy of the prepared phase change composite fibers was also reduced, but the lowest thermal enthalpy liquid reached 110 J·g -1 It can be seen that the CNT / PEG phase change composite fiber has good heat storage performance.

[0096] See also Figure 5 , which characterizes the electrical properties of the composite phase change materials prepared by combining different polyethylene glycol ratios of Examples 1-3, PEG1500 of Example 6, and PEG600 of Example 7 with carbon nanofibers. Pure polyethylene glycol is an electrical insulating material, and the phase change composite material prepared by the present invention has excellent electrical properties, which is due to the introduction of carbon nanotube fibers with high electrical conductivity, so that the insulating material obtains high electrical conductivity.

[0097] See also Figure 6 , which is the mechanical property characterization of the embodiment and the control example. As can be seen from the figure, due to the ultra-high polyethylene glycol loading rate in the phase change composite material, the mechanical strength of the composite material has decreased to a certain extent, but still maintains a mechanical strength of 500-1500MPa, and the elongation at break of the composite material is much higher than that of pure carbon nanotube fibers, providing excellent toughness performance for the phase change material, making it more conducive to weaving into wearable fabrics.

[0098] In addition, it was found through testing of Examples 8-10 that the performance parameters of the CNT composite phase change fibers were basically consistent with the rules of the above-mentioned embodiments, so the test results of Examples 8-10 are not described in detail here.

[0099] The above test results show that the phase change material of polyethylene glycol / carbon nanotube fiber structure obtained by the technical solution of the present invention has polyethylene glycol filled into the nanopores of carbon nanofibers to achieve a complete composite structure. The filling structure enables the carbon nanotube fiber to completely wrap the polyethylene glycol. When the expansion current is 50mA, the polyethylene glycol loading rate on the carbon nanotube fiber reaches more than 89%, so that the phase change material will not leak during the phase change process. The preparation process is simple, easy to operate, and low in cost. At the same time, the obtained phase change composite fiber can accurately control the temperature within an ultra-wide temperature range, and the maximum thermal enthalpy can reach 183J·g -1 The mechanical properties can still be maintained at 500-1500MPa, and the introduction of PEG enhances the elongation at break of the phase change composite material, expanding its application in the weaving field.

[0100] In summary, through the technical solution of the present invention, a simple process is adopted to obtain a phase change composite material with precise temperature control, high thermal enthalpy, excellent mechanical properties and electrical properties within an ultra-wide temperature range, and this processing process does not involve toxic and dangerous goods, and is efficient, green, energy-saving and environmentally friendly. It has a broad market prospect for application in wearable temperature-regulating fabrics. In particular, carbon nanotubes also have excellent light-heat conversion performance. In practical applications, they can store heat as long as there is light. At the same time, they can also store energy through electric heating when the light intensity is weak, and release heat to maintain the temperature when necessary, with two-way temperature regulation performance.

[0101] In addition to the PEG used in the above embodiment, other organic or inorganic phase change materials can also be used by adopting the technical solution of the present invention. For example, the organic phase change material can also be any one or a combination of polyols, paraffin, and fatty acids; the inorganic phase change material includes hydrated salts or molten salts. By filling the carbon nanotubes with different proportions of phase change materials and combining the preparation process of the present invention, a composite phase change material with temperature control sensitivity can be prepared, which can also achieve the purpose of precise temperature control.

[0102] The above are only preferred embodiments of the present invention, which do not limit the protection scope of the present invention. For those skilled in the art, the present invention may have various modifications and changes. Within the spirit and principle of the present invention, changes, modifications, replacements, integrations and parameter changes to these embodiments by conventional substitutions or by being able to achieve the same functions without departing from the principles and spirit of the present invention all fall within the protection scope of the present invention.

Claims

1. Application of a phase change composite fiber capable of precise temperature adjustment in a temperature adjustable fabric, characterized in that: The carbon nanotube fibers are expanded by electrolyzing water to release hydrogen, and at the same time, the phase change material is filled into the nano-micropores of the carbon nanotube fibers by combining in-situ impregnation and stretching processes to form the phase change composite fiber having a phase change material / carbon nanofiber composite structure; The phase change material is a mixed solution of PEG600 and PEG1500; The mass ratio of PEG600 to PEG1500 is 1:0.5~2; After mixing two polyethylene glycols with different molecular weights and then compounding them with carbon nanotube fibers, the prepared phase-change composite fibers can be precisely controlled within a wide temperature range of 8 to 57°C. The temperature-adjustable fabric is woven from the phase-change composite fiber; The method for preparing the precisely temperature-controlled phase-change composite fiber comprises the following steps: S1. Prepare electrolyte solution: Mix concentrated sulfuric acid solution with phase change material and stir evenly; S2. Hydrogen evolution expansion-in-situ impregnation: the electrolyte solution configured in S1 is added to an electrolytic cell, the anode is an inert electrode, the cathode is a carbon nanotube fiber, the carbon nanotube fiber is immersed in the electrolyte solution, and the carbon nanotube fiber is expanded by controlling the electrolysis of water by an electric current method, so that the phase change material fully penetrates into the interior of the carbon nanotube fiber to obtain a phase change composite fiber I; S3. Stretching: pulling the phase change composite fiber I after hydrogen evolution expansion-in-situ impregnation out of the electrolyte solution, so that the surface of the phase change composite fiber has a dense structure under the action of surface tension, thereby obtaining a phase change composite fiber II; S4. Post-treatment: removing excess electrolyte solution from the surface of the phase change composite fiber II and vacuum drying to obtain the final phase change composite fiber product.

2. The use according to claim 1, characterized in that: In S1, the concentration of the phase change material is 10-20wt%.

3. The use according to claim 1, characterized in that: In S1, the step of preparing the electrolyte solution comprises: (1) Prepare the electrolyte: slowly add concentrated sulfuric acid into deionized water in a cold water bath, adjust the volume, and stir until uniform. This is referred to as solution A. (2) Prepare polyethylene glycol solution: Accurately weigh polyethylene glycol and add it to deionized water. Stir until completely dissolved. This is referred to as solution B. (3) Preparing an electrolyte solution: adding solution A to solution B and stirring until the mixture is uniform to obtain the electrolyte solution.

4. The use according to claim 1, characterized in that: The thermal enthalpy of the phase change composite fiber is 110-183 J·g -1 .

5. The use according to any one of claims 1 to 4, characterized in that: The carbon nanotube fibers are prepared by a floating catalyst chemical deposition method.

Citation Information

Patent Citations

  • Preparation method for energy-storing and temperature-adjusting phase-change material and fibres thereof

    CN104910334A

  • Encapsulated and networked regenerated cellulose phase-change fiber and preparation method thereof

    CN106048761A

  • Graphene aerogel intelligent phase-change fiber, and preparation method and application thereof

    CN108587571A

  • Polyethylene glycol / hydroxypropyl cellulose carbon nanotube composite solid-solid phase change material and preparation method thereof

    CN110804301A

  • High-strength and high-toughness carbon nanotube composite phase change fiber and preparation method and application thereof

    CN113403834A

Cited By

  • Carbon nano tube composite phase change energy storage material with customizable form and strong acid expansion impregnation composite preparation method of carbon nano tube composite phase change energy storage material